Carbon nanotube dispersion and method for producing same

WO2024247974A1PCT designated stage expired Publication Date: 2024-12-05ZEON CORP

Patent Information

Application Number
PCT/JP2024/019453
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-10
Filing Date
2024-05-27
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional carbon nanotube (CNT) dispersions face challenges in achieving high conductivity and stability over time in molded bodies, with existing methods falling short in optimizing the properties of CNT bundles for improved dispersibility and conductivity.

Method used

A CNT dispersion liquid is developed with specific characteristics, including CNT bundles of controlled average length, diameter, and aspect ratio, along with the use of a thickener such as cellulose polymers or polyvinylpyrrolidone, and a wet jet mill dispersion treatment to ensure optimal bundle distribution and stability.

Benefits of technology

The resulting CNT dispersion liquid achieves enhanced stability and conductivity in molded bodies, with improved dispersibility and conductivity due to the precise control of CNT bundle properties and processing conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The purpose of the present invention is to provide a carbon nanotube dispersion with which it is possible to form a molded body having excellent dispersion state stability over time and excellent conductivity, or with which it is possible to form a molded body having excellent conductivity. The present invention is a carbon nanotube dispersion comprising a plurality of carbon nanotubes, a solvent, and a thickener, wherein: the plurality of carbon nanotubes comprise single-wall carbon nanotubes; at least some of the plurality of carbon nanotubes form carbon nanotube bundles; when the carbon nanotube bundles are observed using a scanning electron microscope, the average length of the carbon nanotube bundles is more than 1.50 μm; the average diameter of the carbon nanotube bundles is 18.0 nm or less; among 100 carbon nanotube bundles, the number having a diameter of more than 30.0 nm is 15 or less; and when the carbon nanotube bundles are observed using an optical microscope, the average length of the carbon nanotube bundles is 8.0 μm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Carbon nanotube dispersion and method for producing same

[0001] The present invention relates to a carbon nanotube dispersion and a method for producing the same.

[0002] 2. Description of the Related Art Carbon nanotubes (hereinafter sometimes abbreviated as "CNTs") have been attracting attention as a material that has excellent properties such as electrical conductivity, thermal conductivity, and strength.

[0003] Although individual CNTs have excellent properties, their small outer diameters make them prone to bundling (forming into bundles) due to van der Waals forces. Therefore, conventionally, CNTs are first dispersed in a solvent to prepare a carbon nanotube dispersion (CNT dispersion). The resulting CNT dispersion is then used, for example, to produce a molded product, such as a carbon film made up of an aggregate of multiple CNTs, or an electrode for a secondary battery.

[0004] Therefore, in recent years, attempts have been made to improve the properties of molded bodies by improving CNT dispersions. For example, Patent Document 1 discloses a CNT dispersion containing CNTs, a solvent, and a dispersant, in which the CNT average outer diameter, the half-width of the peak at a diffraction angle 2θ = 25° ± 2°, and the G / D ratio are all within predetermined ranges. According to Patent Document 1, resin compositions, electrode films, and the like with excellent conductivity can be obtained by using this CNT dispersion. Furthermore, Patent Document 2 discloses a CNT dispersion containing CNTs, a dispersant, and a solvent, in which the CNT average outer diameter, BET specific surface area, and average fiber length are all within predetermined ranges. According to Patent Document 2, resin compositions, electrode films, and the like with excellent conductivity and adhesion can be obtained by using this CNT dispersion.

[0005] International Publication No. 2020 / 004095 Japanese Patent Application Laid-Open No. 2021-72279

[0006] However, in recent years, there has been a demand for further improvements in the properties of molded articles formed from CNT dispersions, and the conventional CNT dispersions described above have room for improvement in terms of further increasing the conductivity of the molded articles, as well as in terms of the stability of the dispersed state over time.

[0007] Therefore, an object of the present invention is to provide a carbon nanotube dispersion liquid that has excellent stability over time in the dispersion state and is capable of forming a molded body that has excellent electrical conductivity.

[0008] Another object of the present invention is to provide a carbon nanotube dispersion capable of forming a molded body having excellent electrical conductivity, and a method for producing the same.

[0009] The present inventors have conducted extensive research with the aim of solving the above-mentioned problems, and have focused on bundles formed by aggregating multiple CNTs in a CNT dispersion (hereinafter, sometimes referred to as "CNT bundles").

[0010] <First Invention> The present inventors then discovered that in a CNT dispersion containing a plurality of CNTs, including single-walled CNTs, a solvent, and a thickener, if the average length of the CNT bundles when observed with a scanning electron microscope (hereinafter sometimes abbreviated as "SEM") exceeds a predetermined value, the average diameter of the CNT bundles is equal to or less than a predetermined value, the proportion of CNT bundles with a diameter of more than 30.0 nm is equal to or less than a predetermined value, and the average length of the CNT bundles when observed with an optical microscope is equal to or greater than a predetermined value, then a CNT dispersion can be obtained that has excellent stability over time in the dispersed state and is capable of increasing the conductivity of a molded body, and thus completed the present invention (first invention).

[0011] <Second Invention> On the other hand, the present inventors have discovered that in a CNT dispersion containing a plurality of CNTs, including single-walled CNTs, a solvent, and a thickener, if the average length of the CNT bundles, as observed with an SEM, exceeds a predetermined value, the average diameter of the CNT bundles is equal to or less than a predetermined value, and the proportion of CNT bundles with a diameter of more than 30.0 nm is equal to or less than a predetermined value, then a CNT dispersion can be obtained that has excellent stability over time in the dispersed state and is capable of increasing the conductivity of the molded body, and have completed the present invention (second invention).

[0012] <Third Invention> On the other hand, the present inventors have discovered that the conductivity of a molded body can be increased by making the average length of the CNT bundles greater than a predetermined value, the average diameter of the CNT bundles less than a predetermined value, and the proportion of CNT bundles with a diameter of greater than 30.0 nm equal to or less than a predetermined value when observed with an SEM in a CNT dispersion containing a plurality of CNTs, including single-walled CNTs, a solvent, and a dispersant, and have completed the present invention (third invention).

[0013] That is, the present invention has an object to advantageously solve the above-mentioned problems, and provides the following CNT dispersions [1] to [9] and methods for producing CNT dispersions

[10] to

[11] . Note that [1] below corresponds to the first invention, [2] below corresponds to the second invention, [3] to [5] below correspond to the first and second inventions, and [6] to

[11] below correspond to the third invention.

[0014] [1] A carbon nanotube dispersion liquid comprising a plurality of carbon nanotubes, a solvent, and a thickener, wherein the plurality of carbon nanotubes include single-walled carbon nanotubes, at least a portion of the plurality of carbon nanotubes form carbon nanotube bundles, and when the carbon nanotube bundles are observed with a scanning electron microscope, the average length of the carbon nanotube bundles is greater than 1.50 μm, the average diameter of the carbon nanotube bundles is 18.0 nm or less, the number of carbon nanotubes with a diameter of greater than 30.0 nm is 15 or less out of 100 carbon nanotubes in the carbon nanotube bundles, and when the carbon nanotube bundles are observed with an optical microscope, the average length of the carbon nanotube bundles is 8.0 μm or more. A CNT dispersion containing a plurality of CNTs, including single-walled CNTs, a solvent, and a thickener, in which, when observed with an SEM, the average length of the CNT bundles exceeds a predetermined value, the average diameter of the CNT bundles is equal to or less than a predetermined value, and the number of CNT bundles with a diameter of greater than 30.0 nm out of 100 bundles is equal to or less than a predetermined value, and the average length of the CNT bundles is equal to or greater than a predetermined value, when observed with an optical microscope, has excellent stability over time in the dispersion state and can produce a conductive film with excellent conductivity. Note that, in the present invention, the "average length of the CNT bundles," "average diameter of the CNT bundles," and "number of CNT bundles with a diameter of greater than 30.0 nm out of 100 bundles" when observed with an SEM, and the "average length of the CNT bundles" when observed with an optical microscope can each be measured using the methods described in the Examples of this specification.

[0015] [2] A carbon nanotube dispersion comprising a plurality of carbon nanotubes, a solvent, and a thickener, wherein the plurality of carbon nanotubes include single-walled carbon nanotubes, at least some of the plurality of carbon nanotubes form carbon nanotube bundles, and wherein, when the carbon nanotube bundles are observed with a scanning electron microscope, the average length of the carbon nanotube bundles exceeds 1.50 μm, the average diameter of the carbon nanotube bundles is 16.0 nm or less, and the number of carbon nanotubes with a diameter of greater than 30.0 nm is 15 or less out of 100 carbon nanotube bundles. A CNT dispersion comprising a plurality of CNTs including single-walled CNTs, a solvent, and a thickener, wherein, when observed with an SEM, the average length of the CNT bundles exceeds a predetermined value, the average diameter of the CNT bundles is a predetermined value or less, and the number of CNT bundles with a diameter of greater than 30.0 nm is a predetermined value or less, has excellent stability over time in the dispersion state and can enable a conductive film to exhibit excellent conductivity.

[0016] [3] The carbon nanotube dispersion according to [1] or [2] above, wherein the carbon nanotube bundles have an average aspect ratio of more than 100. If the average aspect ratio of the CNT bundles is more than 100, the stability of the dispersion state of the CNT dispersion over time can be further improved, and the conductivity of the molded body can be further increased. In the present invention, the "average aspect ratio" of the CNT bundles can be determined by calculating the ratio of the average length to the average diameter (average length / average diameter) of the CNT bundles when observed with an SEM.

[0017] [4] The carbon nanotube dispersion according to any one of [1] to [3] above, wherein the G / D ratio of the carbon nanotubes is 0.5 or more and 120 or less. When the G / D ratio of the CNTs is within the above range, the stability of the dispersion state of the CNT dispersion over time can be further improved, and the conductivity of the molded body can be further increased. In the present invention, the "G / D ratio" refers to the ratio of the G-band peak intensity to the D-band peak intensity in a Raman spectrum, and can be measured using the method described in the examples of this specification.

[0018] [5] The carbon nanotube dispersion liquid according to any one of [1] to [4] above, wherein the thickener comprises at least one selected from the group consisting of a cellulose-based polymer, a polycarboxylic acid, and polyvinylpyrrolidone. When the thickener comprises at least one selected from the group consisting of a cellulose-based polymer, a polycarboxylic acid, and polyvinylpyrrolidone, the stability of the dispersion state of the CNT dispersion liquid over time can be further improved, and the conductivity of the molded body can be further increased.

[0019] [6] A carbon nanotube dispersion comprising a plurality of carbon nanotubes, a solvent, and a dispersant, wherein the plurality of carbon nanotubes include single-walled carbon nanotubes, at least some of the plurality of carbon nanotubes form carbon nanotube bundles, and wherein, when the carbon nanotube bundles are observed with a scanning electron microscope, the average length of the carbon nanotube bundles is greater than 1.5 μm, the average diameter of the carbon nanotube bundles is less than 15.0 nm, and the number of carbon nanotubes with a diameter of greater than 30.0 nm is 10 or less out of 100 carbon nanotube bundles. A CNT dispersion comprising a plurality of CNTs including single-walled CNTs, a solvent, and a dispersant, wherein, when observed with an SEM, the average length of the CNT bundles is greater than a predetermined value, the average diameter of the CNT bundles is less than a predetermined value, and the number of CNT bundles with a diameter of greater than 30.0 nm is the predetermined value or less, can provide a conductive film with excellent conductivity.

[0020] [7] The carbon nanotube dispersion according to [6] above, wherein the carbon nanotube bundles have an average aspect ratio of more than 120. If the average aspect ratio of the CNT bundles is more than 120, the conductivity of the molded body can be further increased. In the present invention, the "average aspect ratio" of the CNT bundles can be determined by calculating the ratio of the average length to the average diameter of the CNT bundles (average length / average diameter).

[0021] [8] The carbon nanotube dispersion liquid according to [6] or [7] above, wherein the G / D ratio of the carbon nanotubes is 0.5 or more and 20 or less. If the G / D ratio of the CNTs is within the above range, the conductivity of the molded body can be further increased. In the present invention, the "G / D ratio" refers to the ratio of the G-band peak intensity to the D-band peak intensity in a Raman spectrum, and can be measured using the method described in the examples of this specification.

[0022] [9] The carbon nanotube dispersion according to any one of [6] to [8], wherein the harmonic mean diameter of the carbon nanotubes exceeds 500 nm. When the harmonic mean diameter of the CNTs exceeds 500 nm, the conductivity of the molded article can be further increased. In the present invention, the "harmonic mean diameter" refers to the z-average diameter measured by dynamic light scattering (DLS), and can be measured using the method described in the examples of this specification.

[0023]

[10] A method for producing a carbon nanotube dispersion liquid according to any one of [6] to [9] above, comprising a step of dispersing a mixed liquid containing the plurality of carbon nanotubes, the solvent, and the dispersant using a wet jet mill. According to the method for producing a CNT dispersion liquid including the steps described above, a CNT dispersion liquid capable of forming a molded body having excellent electrical conductivity can be produced.

[0024]

[11] The method for producing a carbon nanotube dispersion liquid according to

[10] above, wherein the pressure applied to the mixed liquid during the dispersion treatment is 50 MPa or less, and the number of passes during the dispersion treatment is 10 or more. If the dispersion treatment using a wet jet mill is performed under conditions of a pressure of 50 MPa or less and a number of passes of 10 or more, the conductivity of the resulting molded body can be further increased. In the present invention, the "number of passes" refers to the number of times the entire mixed liquid passes through the wet jet mill.

[0025] According to the present invention (first invention and second invention), it is possible to provide a carbon nanotube dispersion liquid that has excellent stability of the dispersion state over time and that can form a molded product with excellent electrical conductivity. Also, according to the present invention (third invention), it is possible to provide a carbon nanotube dispersion liquid that can form a molded product with excellent electrical conductivity and a method for producing the same.

[0026] (First Invention) Hereinafter, an embodiment of the first invention (CNT dispersion liquid) will be described in detail.

[0027] The CNT dispersion of the present invention is not particularly limited and can be used, for example, as a material for forming molded articles such as carbon films and elastomer molded articles, electrodes for secondary batteries, and the like.

[0028] (Carbon Nanotube Dispersion) The CNT dispersion of the present invention contains at least CNTs, a solvent, and a thickener, and optionally contains components other than the CNTs, solvent, and thickener (other components). At least a portion of the CNTs are single-walled CNTs, forming CNT bundles in the CNT dispersion. The CNT dispersion of the present invention is characterized in that, when observed with an SEM, the average length of the CNT bundles exceeds 1.50 μm, the average diameter of the CNT bundles is 18.0 nm or less, the number of CNT bundles with a diameter of more than 30.0 nm is 15 or less out of 100, and the average length of the CNT bundles is 8.0 μm when observed with an optical microscope. The CNT bundles are formed by assembling multiple CNTs into bundles (bundles) along the longitudinal axis direction of the CNTs.

[0029] Furthermore, in the CNT dispersion of the present invention, the average length of the CNT bundles exceeds a predetermined value when observed with an SEM, the average diameter of the CNT bundles is equal to or less than a predetermined value, the number of CNT bundles with a diameter of more than 30.0 nm out of 100 bundles is equal to or less than a predetermined value, and the average length of the CNT bundles is equal to or greater than a predetermined value when observed with an optical microscope, so that the CNT dispersion not only has excellent stability over time in the dispersed state but can also produce molded articles that exhibit excellent conductivity. The reason why the above effects are obtained by using the CNT dispersion of the present invention is not clear, but is presumed to be as follows.

[0030] The present inventors focused on CNT bundles composed of multiple CNTs in a CNT dispersion in order to improve the dispersibility of the CNT dispersion. The smaller the average diameter of the CNT bundles, the fewer the number of CNTs comprising each bundle. Furthermore, the fewer the number of CNTs with a diameter greater than 30.0 nm among 100 CNT bundles, the greater the number of CNT bundles present in the CNT dispersion. In the CNT dispersion of the present invention, the average diameter of the CNT bundles is set to 18.0 nm or less, and the number of CNT bundles with a diameter greater than 30.0 nm among 100 CNT bundles is set to 15 or less, thereby ensuring a sufficient number of CNT bundles present in the CNT dispersion. Additionally, the dispersion of the present invention ensures a sufficient length of the CNT bundles present in the CNT dispersion by having an average length of greater than 1.50 μm when observed with an SEM and an average length of 8.0 μm or more when observed with an optical microscope. The reason why the average length of CNT bundles usually differs between observations with an SEM and an optical microscope is believed to be due to the following: While CNT bundles with small diameters can be observed with an SEM, which has high resolution, they cannot be observed with an optical microscope, which has lower resolution than an SEM. Therefore, optical microscopes tend to selectively observe CNT bundles with large diameters and lengths composed of a large number of CNTs, which is thought to be the reason why the average length of CNT bundles differs between observations with an SEM and an optical microscope. Furthermore, in a CNT dispersion in which the number and length of CNT bundles are sufficiently ensured as described above, CNTs are stably dispersed over time. Furthermore, using such a CNT dispersion allows CNT bundles of sufficient length to be distributed in a molded body, thereby forming a good conductive path. For the above reasons, the CNT dispersion of the present invention is believed to have excellent stability of the dispersion state over time, and its use is believed to enable a conductive film to exhibit excellent conductivity.

[0031] <CNT> The CNT is not particularly limited as long as it contains single-walled CNT. As the CNT, only single-walled CNT may be used, or a combination of single-walled CNT and multi-walled CNT may be used.

[0032] <<Properties>> [Average length when observed with SEM] The average length of the CNT bundles when observed with SEM needs to be more than 1.50 μm, preferably 1.60 μm or more, more preferably 1.70 μm or more, even more preferably 1.80 μm or more, even more preferably 1.90 μm or more, and particularly preferably 2.00 μm or more. If the average length of the CNT bundles when observed with SEM is 1.50 μm or less, the conductivity of the molded body decreases. Furthermore, the upper limit of the average length of the CNT bundles when observed with SEM is not particularly limited, and can be, for example, 3.50 μm or less, or 3.00 μm or less.

[0033] [Average Length When Observed with an Optical Microscope] The average length of the CNT bundles when observed with an optical microscope must be 8.0 μm or more, preferably 10.0 μm or more, more preferably 12.0 μm or more, and even more preferably 15.0 μm or more. If the average length of the CNT bundles when observed with an optical microscope is less than 8.0 μm, the conductivity of the molded body will decrease. Furthermore, the upper limit of the average length of the CNT bundles when observed with an optical microscope is not particularly limited, and can be, for example, 30.0 μm or less, 25.0 μm or less, or 20.0 μm or less.

[0034] Note that the average length of CNT bundles observed with an optical microscope is usually longer than the average length of CNT bundles observed with an SEM. The average length of CNT bundles in a CNT dispersion can be adjusted, for example, by changing the length of the raw CNTs (CNTs used as raw materials when preparing the CNT dispersion) and the conditions of the dispersion treatment. For example, when a wet jet mill is used for dispersion treatment, increasing the pressure applied to the mixed liquid passing through the jet mill reduces the average length of the CNT bundles, while decreasing the pressure increases the average length. Furthermore, increasing the number of passes of the dispersion treatment using the wet jet mill (the number of times the entire mixed liquid passes through the wet jet mill) reduces the average length of the CNT bundles in the CNT dispersion, while decreasing the pressure increases the average length.

[0035] [Average Diameter] The average diameter of the CNT bundles must be 18.0 nm or less, preferably 17.5 nm or less, more preferably 17.0 nm or less, even more preferably 16.5 nm or less, even more preferably 16.0 nm or less, and particularly preferably 15.5 nm or less. If the average diameter of the CNT bundles exceeds 18.0 nm, the stability of the dispersion state of the CNT dispersion over time decreases, and the conductivity of the resulting molded body decreases. The lower limit of the average diameter of the CNT bundles is not particularly limited, and can be, for example, 13.5 nm or more, or 14.0 nm or more. The average diameter of the CNT bundles in the CNT dispersion can be adjusted, for example, by changing the diameter of the raw CNTs and the dispersion treatment conditions. For example, when a wet jet mill is used for dispersion treatment, increasing the pressure applied to the mixed liquid passing through the wet jet mill reduces the average diameter of the CNT bundles, while decreasing the pressure increases the average diameter. Furthermore, increasing the number of passes of the dispersion treatment using a wet jet mill reduces the average diameter of the CNT bundles in the CNT dispersion, while decreasing the number of passes increases the average diameter.

[0036] [Number of CNT bundles with a diameter greater than 30.0 nm] The number of CNT bundles with a diameter greater than 30.0 nm must be 15 or less, preferably 14 or less, more preferably 13 or less, even more preferably 12 or less, even more preferably 11 or less, and particularly preferably 10 or less. If the number of CNT bundles with a diameter greater than 30.0 nm is greater than 15, the stability of the dispersion state of the CNT dispersion over time decreases, and the conductivity of the resulting molded body decreases. Furthermore, the lower limit of the number of CNT bundles with a diameter greater than 30.0 nm is not particularly limited, and can be, for example, one or more, or two or more. The number of CNT bundles with a diameter greater than 30.0 nm can be adjusted, for example, by changing the length or diameter of the raw CNTs and the dispersion treatment conditions. For example, when a wet jet mill is used for dispersion treatment, increasing the pressure applied to the mixed liquid passing through the wet jet mill reduces the number of CNT bundles with diameters exceeding 30.0 nm, while decreasing the pressure increases the number. Furthermore, increasing the number of passes of dispersion treatment using the wet jet mill reduces the number of CNT bundles with diameters exceeding 30.0 nm, while decreasing the number increases the number.

[0037] [Average Aspect Ratio] The average aspect ratio of the CNT bundles is preferably greater than 100, more preferably greater than 110, even more preferably greater than 120, even more preferably greater than 130, and particularly preferably greater than 135. If the average aspect ratio of the CNT bundles is greater than 100, the stability of the dispersion state of the CNT dispersion over time can be further improved, and the conductivity of the molded body can be further increased. Furthermore, the upper limit of the average aspect ratio of the CNT bundles is not particularly limited, and can be, for example, 250 or less, 225 or less, or 200 or less.

[0038] [G / D ratio] The G / D ratio of the CNT is preferably 0.5 or more, more preferably 1 or more, and is preferably 120 or less, more preferably 110 or less, even more preferably 95 or less, still more preferably 70 or less, still more preferably 45 or less, and particularly preferably 20 or less. If the G / D ratio of the CNT is within the above range, the stability over time of the dispersed state of the CNT dispersion can be further improved, and the conductivity of the molded body can be further increased.

[0039] <<Content Ratio>> The content ratio of CNTs in the CNT dispersion is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more, and preferably 2% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less, based on the total amount of the CNT dispersion being 100% by mass. If the ratio of CNTs in the CNT dispersion is 0.01% by mass or more, the conductivity of the molded body can be further increased and the productivity of the molded body can be improved. On the other hand, if the ratio of CNTs in the CNT dispersion is 2% by mass or less, the stability of the dispersion state of the CNT dispersion over time can be further improved.

[0040] <Solvent> The CNT dispersion of the present invention may contain only water as the solvent, or may contain only an organic solvent (e.g., esters, ketones, alcohols) as the solvent, or the solvent may be a mixture of water and an organic solvent. From the viewpoint of further improving the stability of the dispersion state of the CNT dispersion over time while further increasing the conductivity of the molded body, it is preferable that the CNT dispersion of the present invention contains water as the solvent. Note that the CNT dispersion of the present invention may contain one type of organic solvent, or may contain two or more types of organic solvents.

[0041] Here, in the CNT dispersion of the present invention, the proportion of water in the solvent is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass (i.e., the CNT dispersion of the present invention contains only water as the solvent), with the total amount of solvent being 100% by mass. If the proportion of water in the solvent in the CNT dispersion is equal to or greater than the above lower limit, the stability of the dispersed state of the CNT dispersion over time can be further improved, and the conductivity of the molded body can be further increased.

[0042] <Thickener> The thickener is not particularly limited, and known thickeners can be used. Examples of the thickener include water-soluble polymers such as cellulose polymers, polycarboxylic acids, and water-soluble vinyl polymers. In the present invention, a polymer being "water-soluble" means that when 0.5 g of the polymer (in terms of solid content) is dissolved in 100 g of water at 25° C., the amount of insoluble matter is less than 10.0 mass %.

[0043] Examples of cellulose-based polymers include carboxymethyl cellulose, methyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, and salts and derivatives thereof. Examples of polycarboxylic acids include polyacrylic acid, polymethacrylic acid, alginic acid, and salts and derivatives thereof. Examples of water-soluble vinyl polymers include polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl methyl ether, poly N-vinylacetamide, polyacrylamide, and polyimide. Examples of the salts include alkali metal salts such as sodium salts, and ammonium salts. Examples of the derivatives include esters such as alkyl esters, and ethers.

[0044] The above-mentioned thickeners may be used alone or in combination of two or more in any ratio. Among these, from the viewpoint of further improving the stability over time of the dispersion state of the CNT dispersion and further increasing the conductivity of the molded body, cellulose-based polymers, polycarboxylic acids, and polyvinylpyrrolidone are preferred as thickeners, and carboxymethylcellulose and its salts, polyacrylic acid and its salts, and polyvinylpyrrolidone are more preferred.

[0045] <<Weight Average Molecular Weight>> The weight average molecular weight of the thickener is preferably 5,000 or more, more preferably 10,000 or more, and preferably 1,000,000 or less, and more preferably 500,000 or less. If the weight average molecular weight of the thickener is 5,000 or more, the dispersibility of CNTs in the CNT dispersion can be improved. Furthermore, if the weight average molecular weight of the thickener is 1,000,000 or less, an increase in the viscosity of the CNT dispersion can be suppressed. In the present invention, the "weight average molecular weight" can be measured using gel permeation chromatography as a standard polystyrene equivalent value.

[0046] <<Content Ratio>> The ratio of the thickener contained in the CNT dispersion is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less, where the total amount of the CNT dispersion is 100% by mass. If the ratio of the thickener in the CNT dispersion is within the above-mentioned range, the stability over time of the dispersed state of the CNT dispersion can be further improved, and the conductivity of the molded body can be further increased.

[0047] The content of the thickener in the CNT dispersion is preferably 50 parts by mass or more, more preferably 100 parts by mass or more, and preferably 500 parts by mass or less, more preferably 400 parts by mass or less, and even more preferably 300 parts by mass or less, per 100 parts by mass of CNT. If the ratio of the thickener to the CNT in the CNT dispersion is within the above range, the stability of the dispersion state of the CNT dispersion over time can be further improved, and the conductivity of the molded body can be further increased.

[0048] <Other Components> Examples of other components that the CNT dispersion may optionally contain include conductive materials other than CNTs, polymer components other than the above-mentioned thickeners, antioxidants, resins, etc. The CNT dispersion may contain only one type of other component, or may contain two or more types. The proportion of other components contained in the CNT dispersion is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0% by mass (i.e., the CNT dispersion of the present invention does not contain other components), based on the total amount of the CNT dispersion being 100% by mass.

[0049] <Preparation of CNT Dispersion> The CNT dispersion of the present invention can be prepared, for example, by subjecting a mixture containing the above-described CNTs, solvent, thickener, and any other components to a dispersion treatment. The dispersion treatment is not particularly limited, and can be carried out using a mixer such as a wet jet mill, bead mill, ball mill, sand mill, pigment disperser, crusher, ultrasonic disperser, homogenizer, planetary mixer, or Filmix. Among these, a wet jet mill is preferred from the viewpoint of further improving the stability of the dispersion state of the CNT dispersion over time while further increasing the conductivity of the molded body. Examples of wet jet mills include "NanoVeita (registered trademark)" (manufactured by Yoshida Kikai Kogyo Co., Ltd.), "BERYU SYSTEM PRO" (manufactured by Biryu Co., Ltd.), an ultra-high pressure wet atomizer (manufactured by Yoshida Kogyo Co., Ltd.), "Nanomizer (registered trademark)" (manufactured by Nanomizer Co., Ltd.), and "Starburst (registered trademark)" (manufactured by Sugino Machine Co., Ltd.).

[0050] Here, examples of nozzles provided in the wet jet mill include a straight nozzle and a cross nozzle. A straight nozzle has an I-shaped nozzle cross section and requires relatively small processing energy. On the other hand, a cross nozzle has an X-shaped nozzle cross section and requires larger processing energy than a straight nozzle. From the viewpoint of further improving the stability of the dispersion state of the CNT dispersion over time while further increasing the conductivity of the molded body, it is preferable to use a straight nozzle as the nozzle provided in the wet jet mill.

[0051] Here, the pressure applied during the dispersion treatment of the mixed solution using a wet jet mill is preferably 10 MPa or more, more preferably 20 MPa or more, even more preferably 40 MPa or more, and preferably 200 MPa or less, more preferably 150 MPa or less. If the pressure applied to the mixed solution is 10 MPa or more, the stability of the dispersion state of the CNT dispersion over time can be further improved and the conductivity of the resulting molded body can be further increased. Furthermore, if the pressure applied to the mixed solution is 200 MPa or less, the breakage of CNTs during the dispersion treatment can be suppressed, thereby further increasing the conductivity of the resulting molded body.

[0052] Furthermore, the number of passes in the dispersion treatment using a wet jet mill is preferably 10 or more, more preferably 15 or more, and preferably 100 or less, more preferably 80 or less, and even more preferably 60 or less. If the number of passes in the dispersion treatment using a wet jet mill is 10 or more, the stability of the dispersion state of the CNT dispersion over time can be further improved and the conductivity of the resulting molded body can be further increased. Furthermore, if the number of passes in the dispersion treatment using a wet jet mill is 100 or less, shearing of the CNTs during the dispersion treatment can be suppressed, thereby further increasing the conductivity of the resulting molded body and ensuring sufficient production efficiency of the CNT dispersion.

[0053] (Second Invention) Hereinafter, an embodiment of the second invention (CNT dispersion liquid) will be described in detail.

[0054] The CNT dispersion of the present invention is not particularly limited and can be used, for example, as a material for forming molded articles such as carbon films and elastomer molded articles, electrodes for secondary batteries, and the like.

[0055] (Carbon Nanotube Dispersion) The CNT dispersion of the present invention contains at least CNTs, a solvent, and a thickener, and optionally contains components other than the CNTs, solvent, and thickener (other components). At least a portion of the multiple CNTs are single-walled CNTs, forming CNT bundles in the CNT dispersion. The CNT dispersion of the present invention is characterized in that the average length of the CNT bundles is greater than 1.50 μm, the average diameter of the CNT bundles is 16.0 nm or less, and the number of CNT bundles with a diameter of greater than 30.0 nm is 15 or less out of 100 CNT bundles. The CNT bundles are formed by assembling multiple CNTs into a bundle (bundle) along the longitudinal axis direction of the CNTs.

[0056] Furthermore, in the CNT dispersion of the present invention, the average length of the CNT bundles exceeds a predetermined value, the average diameter of the CNT bundles is equal to or less than a predetermined value, and the number of CNT bundles with a diameter of more than 30.0 nm per 100 bundles is equal to or less than a predetermined value, so the CNT dispersion has excellent stability over time in the dispersed state and can produce molded articles that exhibit excellent electrical conductivity. The reason why the above effects are obtained by using the CNT dispersion of the present invention is not clear, but it is presumed to be as follows.

[0057] The present inventors focused on CNT bundles composed of multiple CNTs in a CNT dispersion in order to improve the dispersibility of the CNT dispersion. The smaller the average diameter of the CNT bundles, the fewer the number of CNTs comprising each bundle. Furthermore, the fewer the number of CNTs with a diameter greater than 30.0 nm among 100 CNT bundles, the greater the number of CNT bundles present in the CNT dispersion. In the CNT dispersion of the present invention, the average diameter of the CNT bundles is set to 16.0 nm or less, and the number of CNT bundles with a diameter greater than 30.0 nm among 100 CNT bundles is set to 15 or less, thereby ensuring a sufficient number of CNT bundles present in the CNT dispersion. Additionally, in the dispersion of the present invention, the average length of the CNT bundles exceeds 1.50 μm, thereby ensuring a sufficient length of the CNT bundles present in the CNT dispersion. In a CNT dispersion in which the number and length of CNT bundles are sufficiently ensured, the CNTs are dispersed stably over time, and furthermore, by using such a CNT dispersion, CNT bundles of sufficient length can be distributed in the molded product, thereby forming good conductive paths. For the reasons described above, the CNT dispersion of the present invention has excellent stability of the dispersed state over time, and it is believed that the use of this CNT dispersion can enable the conductive film to exhibit excellent conductivity.

[0058] <CNT> The CNT is not particularly limited as long as it contains single-walled CNT. As the CNT, only single-walled CNT may be used, or a combination of single-walled CNT and multi-walled CNT may be used.

[0059] <<Properties>> [Average Length of CNT Bundles] The average length of the CNT bundles must be greater than 1.50 μm, preferably 1.60 μm or greater, more preferably 1.70 μm or greater, even more preferably 1.80 μm or greater, and particularly preferably 1.90 μm or greater. If the average length of the CNT bundles is 1.50 μm or less, the conductivity of the molded body decreases. The upper limit of the average length of the CNT bundles is not particularly limited, and can be, for example, 3.50 μm or less, or 3.00 μm or less. The average length of the CNT bundles in the CNT dispersion can be adjusted, for example, by changing the length of the raw CNTs (CNTs used as raw materials when preparing the CNT dispersion) and the dispersion treatment conditions. For example, when a wet jet mill is used for dispersion treatment, increasing the pressure applied to the mixed liquid passing through the jet mill reduces the average length of the CNT bundles, while decreasing the pressure increases the average length. Furthermore, increasing the number of passes in the dispersion treatment using a wet jet mill (the number of times the entire amount of the mixed liquid passes through the wet jet mill) decreases the average length of the CNT bundles in the CNT dispersion, and decreasing it increases the average length.

[0060] [Average Diameter of CNT Bundles] The average diameter of the CNT bundles must be 16.0 nm or less, preferably 15.9 nm or less, more preferably 15.8 nm or less, and even more preferably 15.7 nm or less. If the average diameter of the CNT bundles exceeds 16.0 nm, the stability of the dispersion state of the CNT dispersion over time decreases, and the conductivity of the resulting molded body decreases. The lower limit of the average diameter of the CNT bundles is not particularly limited, and can be, for example, 13.5 nm or more, or 14.0 nm or more. The average diameter of the CNT bundles in the CNT dispersion can be adjusted, for example, by changing the diameter of the raw CNTs and the dispersion treatment conditions. For example, when a wet jet mill is used for dispersion treatment, increasing the pressure applied to the mixed liquid passing through the wet jet mill reduces the average diameter of the CNT bundles, while decreasing the pressure increases the average diameter. Furthermore, increasing the number of passes of the dispersion treatment using a wet jet mill reduces the average diameter of the CNT bundles in the CNT dispersion, while decreasing the number of passes increases the average diameter.

[0061] [Number of CNT bundles with a diameter greater than 30.0 nm] The number of CNT bundles with a diameter greater than 30.0 nm must be 15 or less, preferably 14 or less, more preferably 13 or less, even more preferably 12 or less, even more preferably 11 or less, and particularly preferably 10 or less. If the number of CNT bundles with a diameter greater than 30.0 nm is greater than 15, the stability of the dispersion state of the CNT dispersion over time decreases, and the conductivity of the resulting molded body decreases. Furthermore, the lower limit of the number of CNT bundles with a diameter greater than 30.0 nm is not particularly limited, and can be, for example, one or more, or two or more. The number of CNT bundles with a diameter greater than 30.0 nm can be adjusted, for example, by changing the length or diameter of the raw CNTs and the dispersion treatment conditions. For example, when a wet jet mill is used for dispersion treatment, increasing the pressure applied to the mixed liquid passing through the wet jet mill reduces the number of CNT bundles with diameters exceeding 30.0 nm, while decreasing the pressure increases the number. Furthermore, increasing the number of passes of dispersion treatment using the wet jet mill reduces the number of CNT bundles with diameters exceeding 30.0 nm, while decreasing the number increases the number.

[0062] [Average Aspect Ratio of CNT Bundles] The average aspect ratio of the CNT bundles is preferably greater than 100, more preferably greater than 110, even more preferably greater than 120, and particularly preferably greater than 125. If the average aspect ratio of the CNT bundles is greater than 100, the stability of the dispersion state of the CNT dispersion over time can be further improved, and the conductivity of the molded body can be further increased. Furthermore, the upper limit of the average aspect ratio of the CNT bundles is not particularly limited, and can be, for example, 250 or less, 225 or less, or 200 or less.

[0063] [G / D ratio] The G / D ratio of the CNT is preferably 0.5 or more, more preferably 1 or more, and is preferably 120 or less, more preferably 110 or less, even more preferably 95 or less, still more preferably 70 or less, still more preferably 45 or less, and particularly preferably 20 or less. If the G / D ratio of the CNT is within the above range, the stability over time of the dispersed state of the CNT dispersion can be further improved, and the conductivity of the molded body can be further increased.

[0064] <<Content Ratio>> The content ratio of CNTs in the CNT dispersion is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, preferably 2% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less, with the total amount of the CNT dispersion being 100% by mass. If the ratio of CNTs in the CNT dispersion is 0.01% by mass or more, the conductivity of the molded body can be further increased and the productivity of the molded body can be improved. On the other hand, if the ratio of CNTs in the CNT dispersion is 2% by mass or less, the stability of the dispersion state of the CNT dispersion over time can be further improved.

[0065] <Solvent> The CNT dispersion of the present invention may contain only water as the solvent, or may contain only an organic solvent (e.g., esters, ketones, alcohols) as the solvent, or the solvent may be a mixture of water and an organic solvent. From the viewpoint of further improving the stability of the dispersion state of the CNT dispersion over time while further increasing the conductivity of the molded body, it is preferable that the CNT dispersion of the present invention contains water as the solvent. Note that the CNT dispersion of the present invention may contain one type of organic solvent, or may contain two or more types of organic solvents.

[0066] Here, in the CNT dispersion of the present invention, the proportion of water in the solvent is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass (i.e., the CNT dispersion of the present invention contains only water as the solvent), with the total amount of solvent being 100% by mass. If the proportion of water in the solvent in the CNT dispersion is equal to or greater than the above lower limit, the stability of the dispersed state of the CNT dispersion over time can be further improved, and the conductivity of the molded body can be further increased.

[0067] <Thickener> The thickener is not particularly limited, and known thickeners can be used. Examples of the thickener include water-soluble polymers such as cellulose polymers, polycarboxylic acids, polyvinylpyrrolidone, polyvinyl alcohol, polyacrylamide, and polyimides. In the present invention, a polymer being "water-soluble" means that when 0.5 g of the polymer (in terms of solid content) is dissolved in 100 g of water at 25° C., the amount of insoluble matter is less than 10.0 mass %.

[0068] Examples of cellulose-based polymers include carboxymethyl cellulose, methyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, and salts and derivatives thereof. Examples of polycarboxylic acids include polyacrylic acid, polymethacrylic acid, alginic acid, and salts and derivatives thereof. Examples of water-soluble vinyl polymers include polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl methyl ether, poly N-vinylacetamide, polyacrylamide, and polyimide. Examples of the salts include alkali metal salts such as sodium salts, and ammonium salts. Examples of the derivatives include esters such as alkyl esters, and ethers.

[0069] The above-mentioned thickeners may be used alone or in combination of two or more in any ratio. Among these, from the viewpoint of further improving the stability over time of the dispersion state of the CNT dispersion and further increasing the conductivity of the molded body, cellulose-based polymers, polycarboxylic acids, and polyvinylpyrrolidone are preferred as thickeners, and carboxymethylcellulose and its salts, polyacrylic acid and its salts, and polyvinylpyrrolidone are more preferred.

[0070] <<Weight Average Molecular Weight>> The weight average molecular weight of the thickener is preferably 5,000 or more, more preferably 10,000 or more, and preferably 1,000,000 or less, and more preferably 500,000 or less. If the weight average molecular weight of the thickener is 5,000 or more, the dispersibility of CNTs in the CNT dispersion can be improved. Furthermore, if the weight average molecular weight of the thickener is 1,000,000 or less, an increase in the viscosity of the CNT dispersion can be suppressed. In the present invention, the "weight average molecular weight" can be measured using gel permeation chromatography as a standard polystyrene equivalent value.

[0071] <<Content Ratio>> The ratio of the thickener contained in the CNT dispersion is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less, based on the total amount of the CNT dispersion being 100% by mass. If the ratio of the thickener in the CNT dispersion is within the above-mentioned range, the stability over time of the dispersion state of the CNT dispersion can be further improved, and the conductivity of the molded body can be further increased.

[0072] The content of the thickener in the CNT dispersion is preferably 100 parts by mass or more, more preferably 200 parts by mass or more, and even more preferably 300 parts by mass or more, and preferably 500 parts by mass or less, and more preferably 450 parts by mass or less, per 100 parts by mass of CNT. If the ratio of the thickener to the CNT in the CNT dispersion is within the above range, the stability of the dispersion state of the CNT dispersion over time can be further improved, and the conductivity of the molded body can be further increased.

[0073] <Other Components> Examples of other components that the CNT dispersion may optionally contain include conductive materials other than CNTs, polymer components other than the above-mentioned thickeners, antioxidants, resins, etc. The CNT dispersion may contain only one type of other component, or may contain two or more types. The proportion of other components contained in the CNT dispersion is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0% by mass (i.e., the CNT dispersion of the present invention does not contain other components), based on the total amount of the CNT dispersion being 100% by mass.

[0074] <Preparation of CNT Dispersion> The CNT dispersion of the present invention can be prepared, for example, by subjecting a mixture containing the above-described CNTs, solvent, thickener, and any other components to a dispersion treatment. The dispersion treatment is not particularly limited, and can be carried out using a mixer such as a wet jet mill, bead mill, ball mill, sand mill, pigment disperser, crusher, ultrasonic disperser, homogenizer, planetary mixer, or Filmix. Among these, a wet jet mill is preferred from the viewpoint of further improving the stability of the dispersion state of the CNT dispersion over time while further increasing the conductivity of the molded body. Examples of wet jet mills include "NanoVeita (registered trademark)" (manufactured by Yoshida Kikai Kogyo Co., Ltd.), "BERYU SYSTEM PRO" (manufactured by Biryu Co., Ltd.), an ultra-high pressure wet atomizer (manufactured by Yoshida Kogyo Co., Ltd.), "Nanomizer (registered trademark)" (manufactured by Nanomizer Co., Ltd.), and "Starburst (registered trademark)" (manufactured by Sugino Machine Co., Ltd.).

[0075] Here, examples of nozzles provided in the wet jet mill include a straight nozzle and a cross nozzle. A straight nozzle has an I-shaped nozzle cross section and requires relatively small processing energy. On the other hand, a cross nozzle has an X-shaped nozzle cross section and requires larger processing energy than a straight nozzle. From the viewpoint of further improving the stability of the dispersion state of the CNT dispersion over time while further increasing the conductivity of the molded body, it is preferable to use a straight nozzle as the nozzle provided in the wet jet mill.

[0076] Here, the pressure applied during the dispersion treatment of the mixed solution using a wet jet mill is preferably 10 MPa or more, more preferably 15 MPa or more, even more preferably 20 MPa or more, and preferably 200 MPa or less, more preferably 150 MPa or less, and even more preferably 100 MPa or less. If the pressure applied to the mixed solution is 10 MPa or more, the stability of the dispersion state of the CNT dispersion over time can be further improved and the conductivity of the resulting molded body can be further increased. Furthermore, if the pressure applied to the mixed solution is 200 MPa or less, the breakage of CNTs during the dispersion treatment can be suppressed, thereby further increasing the conductivity of the resulting molded body.

[0077] Furthermore, the number of passes in the dispersion treatment using a wet jet mill is preferably 10 or more, more preferably 15 or more, even more preferably 20 or more, and preferably 100 or less, more preferably 80 or less, and even more preferably 60 or less. If the number of passes in the dispersion treatment using a wet jet mill is 10 or more, the stability of the dispersion state of the CNT dispersion over time can be further improved and the conductivity of the resulting molded body can be further increased. Furthermore, if the number of passes in the dispersion treatment using a wet jet mill is 100 or less, shearing of the CNTs during the dispersion treatment can be suppressed, thereby further increasing the conductivity of the resulting molded body and ensuring sufficient production efficiency of the CNT dispersion.

[0078] (Third Invention) Hereinafter, an embodiment of the third invention (CNT dispersion liquid and its manufacturing method) will be described in detail.

[0079] The CNT dispersion of the present invention is not particularly limited and can be used, for example, as a material for producing molded articles such as carbon films and elastomer molded articles. The CNT dispersion of the present invention can be produced using the CNT dispersion production method of the present invention.

[0080] (Carbon Nanotube Dispersion) The CNT dispersion of the present invention contains at least CNTs, a solvent, and a dispersant, and optionally contains components other than the CNTs, solvent, and dispersant (other components). At least a portion of the multiple CNTs are single-walled CNTs, forming CNT bundles in the CNT dispersion. The CNT dispersion of the present invention is characterized in that the average length of the CNT bundles is greater than 1.5 μm, the average diameter of the CNT bundles is less than 15.0 nm, and the number of CNTs with a diameter greater than 30.0 nm is 10 or less out of 100 CNT bundles. The CNT bundle is formed by assembling multiple CNTs into a bundle (bundle) along the longitudinal axis direction of the CNTs.

[0081] Furthermore, in the CNT dispersion of the present invention, the average length of the CNT bundles exceeds a predetermined value, the average diameter of the CNT bundles is less than a predetermined value, and the number of CNT bundles with a diameter of more than 30.0 nm per 100 bundles is equal to or less than a predetermined value, so that use of this CNT dispersion can enable a molded article to exhibit excellent electrical conductivity. The reason why the above effects are obtained by using such a CNT dispersion of the present invention is not clear, but it is presumed to be as follows.

[0082] The present inventors focused on CNT bundles composed of multiple CNTs in a CNT dispersion in order to improve the dispersibility of the CNT dispersion. The smaller the average diameter of the CNT bundles, the fewer the number of CNTs comprising each bundle. Furthermore, the fewer the number of CNTs with a diameter greater than 30.0 nm among 100 CNT bundles, the greater the number of CNT bundles present in the CNT dispersion. In the CNT dispersion of the present invention, the average diameter of the CNT bundles is less than 15.0 nm, and the number of CNT bundles with a diameter greater than 30.0 nm among 100 CNT bundles is 10 or less, thereby ensuring a sufficient number of CNT bundles present in the CNT dispersion. Additionally, in the dispersion of the present invention, the average length of the CNT bundles exceeds 1.5 μm, thereby ensuring a sufficient length of the CNT bundles present in the CNT dispersion. Using such a CNT dispersion, CNT bundles of sufficient length are distributed in the molded body, thereby enabling the formation of good conductive paths. For the above reasons, it is believed that the use of the CNT dispersion of the present invention allows the conductive film to exhibit excellent conductivity.

[0083] <CNT> The CNT is not particularly limited as long as it contains single-walled CNT. As the CNT, only single-walled CNT may be used, or a combination of single-walled CNT and multi-walled CNT may be used.

[0084] <<Properties>> [Average Length of CNT Bundles] The average length of the CNT bundles must be greater than 1.5 μm, preferably 1.6 μm or greater, more preferably 1.7 μm or greater, even more preferably 1.8 μm or greater, even more preferably 1.9 μm or greater, and particularly preferably 2.0 μm or greater. If the average length of the CNT bundles is 1.5 μm or less, the conductivity of the molded body decreases. The upper limit of the average length of the CNT bundles is not particularly limited, and can be, for example, 3.5 μm or less, or 3.0 μm or less. The average length of the CNT bundles in the CNT dispersion can be adjusted, for example, by changing the length of the raw CNTs (CNTs used as raw materials in preparing the CNT dispersion), the type and amount of dispersant, and the dispersion treatment conditions. Specifically, in the dispersion step of the CNT dispersion production method of the present invention, described below, increasing the pressure applied to the mixed liquid reduces the average length of the CNT bundles, while decreasing the pressure increases the average length. Furthermore, increasing the number of passes of the dispersion treatment using a wet jet mill reduces the average length of the CNT bundles in the CNT dispersion, while decreasing the number of passes increases the average length.

[0085] [Average Diameter of CNT Bundles] The average diameter of the CNT bundles must be less than 15.0 nm, preferably 14.5 nm or less, and more preferably 14.0 nm or less. If the average diameter of the CNT bundles is 15.0 nm or more, the conductivity of the resulting molded body will decrease. The lower limit of the average diameter of the CNT bundles is not particularly limited, and can be, for example, 12.0 nm or more, or 12.5 nm or more. The average diameter of the CNT bundles in the CNT dispersion can be adjusted, for example, by changing the diameter of the raw CNTs, the type and amount of dispersant, and the dispersion treatment conditions. Specifically, in the CNT dispersion production method of the present invention described below, increasing the pressure (pressure applied to the mixed liquid) during dispersion treatment using a wet jet mill reduces the average diameter of the CNT bundles, while decreasing it increases the average diameter. Furthermore, increasing the number of passes of dispersion treatment using a wet jet mill reduces the average diameter of the CNT bundles in the CNT dispersion, while decreasing it increases the average diameter.

[0086] [Number of Bundles with a Diameter Exceeding 30.0 nm] The number of bundles with a diameter exceeding 30.0 nm must be 10 or less, preferably 9 or less, more preferably 8 or less, even more preferably 7 or less, even more preferably 6 or less, and particularly preferably 5 or less. If the number of bundles with a diameter exceeding 30.0 nm is more than 10, the conductivity of the molded body decreases. Furthermore, the lower limit of the number of bundles with a diameter exceeding 30.0 nm is not particularly limited, and can be, for example, 1 or more, or 2 or more. The number of bundles with a diameter exceeding 30.0 nm can be adjusted, for example, by changing the diameter of the raw CNTs, the type and amount of dispersant, and the dispersion treatment conditions. Specifically, in the dispersion step of the CNT dispersion manufacturing method of the present invention described below, increasing the pressure applied to the mixed liquid reduces the number of bundles with a diameter exceeding 30.0 nm, and decreasing the pressure increases the number. Furthermore, by increasing the number of passes of the dispersion treatment using a wet jet mill, the number of bundles having a diameter of more than 30.0 nm decreases, and by decreasing the number, the number increases.

[0087] [Average Aspect Ratio of CNT Bundles] The average aspect ratio of the CNT bundles is preferably greater than 120, more preferably greater than 130, even more preferably greater than 140, and particularly preferably greater than 150. If the average aspect ratio of the CNT bundles is greater than 120, the conductivity of the molded body can be further increased. There are no particular limitations on the upper limit of the average aspect ratio of the CNT bundles, and it can be, for example, 250 or less, 225 or less, or 200 or less.

[0088] [G / D ratio] The G / D ratio of the CNT is preferably 0.5 or more, more preferably 1 or more, and is preferably 20 or less, more preferably 10 or less. If the G / D ratio of the CNT is within the above range, the conductivity of the molded body can be further increased.

[0089] [Harmonic Mean Diameter] The harmonic mean diameter of the CNTs is preferably greater than 500 nm, more preferably greater than 550 nm, and even more preferably greater than 600 nm. If the harmonic mean diameter of the CNTs exceeds 500 nm, the conductivity of the molded body can be further increased. The upper limit of the harmonic mean diameter of the CNTs is not particularly limited, and can be, for example, 1500 nm or less, 1250 nm or less, or 1000 nm or less. The harmonic mean diameter of the CNTs can be adjusted, for example, by changing the length and diameter of the raw CNTs, the type and amount of dispersant, and the dispersion treatment conditions. Specifically, in the dispersion step of the CNT dispersion liquid manufacturing method of the present invention, described below, increasing the pressure applied to the mixed liquid reduces the harmonic mean diameter of the CNTs, while decreasing the pressure increases the harmonic mean diameter. Furthermore, increasing the number of passes of the dispersion treatment using a wet jet mill reduces the harmonic mean diameter of the CNTs, while decreasing the pressure increases the harmonic mean diameter.

[0090] <<Content Ratio>> The content ratio of CNTs in the CNT dispersion is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.05% by mass or more, and is preferably 2% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less, where the total amount of the CNT dispersion is 100% by mass. If the ratio of CNTs in the CNT dispersion is within the above-mentioned range, the conductivity of the molded body can be further increased.

[0091] <Solvent> The CNT dispersion of the present invention may contain only water as the solvent, or may contain only an organic solvent (e.g., esters, ketones, alcohols) as the solvent, or the solvent may be a mixture of water and an organic solvent. From the viewpoint of improving the dispersibility of the CNT dispersion and further increasing the conductivity of the molded body, it is preferable that the CNT dispersion of the present invention contains water as the solvent. Note that the CNT dispersion of the present invention may contain one type of organic solvent, or may contain two or more types of organic solvents.

[0092] Here, in the CNT dispersion of the present invention, the proportion of water in the solvent is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass (i.e., the CNT dispersion of the present invention contains only water as the solvent), with the total amount of solvent being 100% by mass. If the proportion of water in the solvent in the CNT dispersion is equal to or greater than the above lower limit, the conductivity of the molded body can be further increased.

[0093] <Dispersant> The dispersant is not particularly limited, and any known dispersant capable of assisting the dispersion of CNTs can be used. Examples of the dispersant include surfactants and polymers having carboxylic acid groups. Note that one type of dispersant may be used alone, or two or more types may be used in combination at any ratio.

[0094] Here, examples of surfactants include ionic (cationic, anionic) surfactants and nonionic (nonionic) surfactants. Examples of cationic surfactants include quaternary ammonium salts such as dodecyltrimethylammonium bromide, cetyltrimethylammonium bromide, and distearyldimethylammonium chloride; and quaternary phosphonium salts such as tetrabutylphosphonium chloride, tetrapentylphosphonium chloride, trioctylmethylphosphonium chloride, and pentyltriphenylphosphonium chloride. Examples of anionic surfactants include sodium dodecyl sulfate, sodium deoxycholate, sodium cholate, sodium dodecylbenzenesulfonate, sodium dodecylbenzenesulfonate, and sodium dodecyldiphenyloxide disulfonate. Examples of nonionic surfactants include ether-type nonionic surfactants such as polyoxyethylene alkyl ethers; ether ester-type nonionic surfactants such as polyoxyethylene ethers of glycerin esters; polyethylene glycol fatty acid esters; and glycerin esters. Among the surfactants mentioned above, anionic surfactants are preferred, and sodium cholate and sodium dodecylbenzene sulfate are more preferred, from the viewpoint of further increasing the conductivity of the molded article.

[0095] Examples of polymers having a carboxylic acid group include carboxymethyl cellulose and its salts, copolymers containing carboxylic acid group-containing monomer units, etc. In the present invention, when a polymer "contains a monomer unit," it means that "a polymer obtained using that monomer contains a repeating unit derived from the monomer."

[0096] The copolymer containing a carboxylic acid group-containing monomer unit is a copolymer containing a carboxylic acid group-containing monomer unit and other repeating units. The carboxylic acid group of the carboxylic acid group-containing monomer unit may form a salt with an alkali metal, ammonia, or the like.

[0097] Here, examples of carboxylic acid group-containing monomers capable of forming carboxylic acid group-containing monomer units include monocarboxylic acids and their derivatives, dicarboxylic acids and their acid anhydrides, and their derivatives. Examples of monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of monocarboxylic acid derivatives include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, and α-chloro-β-E-methoxyacrylic acid. Examples of dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of dicarboxylic acid derivatives include methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, and maleic acid monoesters such as butyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleates. Examples of dicarboxylic acid anhydrides include maleic anhydride, acrylic anhydride, methyl maleic anhydride, dimethyl maleic anhydride, and citraconic anhydride. Furthermore, acid anhydrides that generate carboxylic acid groups upon hydrolysis can also be used as carboxylic acid group-containing monomers. Furthermore, examples of carboxylic acid group-containing monomers that can be used include ethylenically unsaturated polycarboxylic acids such as butenetricarboxylic acid, and partial esters of ethylenically unsaturated polycarboxylic acids such as monobutyl fumarate and mono-2-hydroxypropyl maleate. The above-mentioned carboxylic acid group-containing monomers may be used alone or in combination of two or more.

[0098] The other repeating units contained in the copolymer are not particularly limited, and examples thereof include conjugated diene monomer units such as 1,3-butadiene and isoprene (2-methyl-1,3-butadiene); nitrile group-containing monomer units such as acrylonitrile units and methacrylonitrile units; and (meth)acrylic acid ester monomer units such as acrylic acid alkyl ester units and methacrylic acid alkyl ester units. The copolymer may contain one type of other repeating unit, or two or more types. In the present invention, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid.

[0099] <<Content Ratio>> The ratio of the dispersant contained in the CNT dispersion is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and even more preferably 0.5% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less, based on the total amount of the CNT dispersion being 100% by mass. If the ratio of the dispersant in the CNT dispersion is within the above-mentioned range, the conductivity of the molded body can be further increased.

[0100] <Other Components> Examples of other components that the CNT dispersion may optionally contain include conductive materials other than CNTs, polymer components other than the dispersants described above, antioxidants, resins, etc. The CNT dispersion may contain only one type of other component, or may contain two or more types.

[0101] The proportion of other components contained in the CNT dispersion is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, still more preferably 0.1% by mass or less, and particularly preferably 0% by mass (i.e., the CNT dispersion of the present invention does not contain other components), with the total amount of the CNT dispersion being 100% by mass.

[0102] (Method for producing CNT dispersion) The above-mentioned CNT dispersion of the present invention can be prepared, for example, using the method for producing a CNT dispersion of the present invention. The method for producing a CNT dispersion of the present invention includes a step (dispersion step) of subjecting a mixed liquid containing a plurality of CNTs, a solvent, and a dispersant to a dispersion treatment using a wet jet mill. Note that the method for producing a CNT dispersion of the present invention may include steps (other steps) other than the above-mentioned dispersion step.

[0103] Furthermore, according to the method for producing a CNT dispersion of the present invention, it is possible to obtain a CNT dispersion of the present invention that can form a molded product with excellent electrical conductivity.

[0104] <Dispersion Step> In the dispersion step, a mixture containing a plurality of CNTs, a solvent, and a dispersant is subjected to dispersion treatment using a wet jet mill. Note that the CNTs, solvent, and dispersant may be those described above in the "CNT Dispersion" section of this invention.

[0105] <<Wet Jet Mill>> Examples of wet jet mills that can be used for the dispersion treatment in the dispersion step include "Nanovata (registered trademark)" (manufactured by Yoshida Kikai Kogyo Co., Ltd.), "BERYU SYSTEM PRO" (manufactured by Biryu Co., Ltd.), ultra-high pressure wet atomization device (manufactured by Yoshida Kogyo Co., Ltd.), "Nanomizer (registered trademark)" (manufactured by Nanomizer Co., Ltd.), and "Starburst (registered trademark)" (manufactured by Sugino Machine Ltd.).

[0106] Here, examples of nozzles provided in wet jet mills include straight nozzles and cross nozzles. Straight nozzles have an I-shaped nozzle cross section and require relatively small processing energy. On the other hand, cross nozzles have an X-shaped nozzle cross section and require larger processing energy than straight nozzles. From the viewpoint of further increasing the conductivity of the compact, it is preferable to use straight nozzles as nozzles provided in wet jet mills.

[0107] [Pressure] Here, the pressure applied during the dispersion treatment of the mixed solution using a wet jet mill is preferably 10 MPa or more, more preferably 15 MPa or more, even more preferably 20 MPa or more, and preferably 50 MPa or less, more preferably 40 MPa or less, and even more preferably 30 MPa or less. If the pressure applied to the mixed solution is 10 MPa or more, the dispersibility of the CNT dispersion can be improved and the conductivity of the obtained molded body can be further increased. Furthermore, if the pressure applied to the mixed solution is 50 MPa or less, the breakage of CNTs during the dispersion treatment can be suppressed, thereby further increasing the conductivity of the obtained molded body.

[0108] [Number of Passes] The number of passes in the dispersion treatment using a wet jet mill is preferably 10 or more, more preferably 15 or more, even more preferably 20 or more, even more preferably 25 or more, particularly preferably 30 or more, and preferably 50 or less, and more preferably 45 or less. If the number of passes in the dispersion treatment using a wet jet mill is 10 or more, the dispersibility of the CNT dispersion can be improved and the conductivity of the resulting molded body can be further increased. If the number of passes in the dispersion treatment using a wet jet mill is 50 or less, the breakage of CNTs during the dispersion treatment can be suppressed, thereby further increasing the conductivity of the resulting molded body and sufficiently ensuring the production efficiency of the CNT dispersion.

[0109] <Other Steps> Examples of other steps include a step (mixing step) of mixing a plurality of CNTs, a solvent, and a dispersant to obtain a mixed liquid before the above-described dispersion step.

[0110] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified.

[0111] Examples and comparative examples of the first invention (Examples A1 to A21, Comparative Examples A1 to A7) are described below. In the examples and comparative examples of the first invention, various measurements and evaluations were carried out using the following methods.

[0112] <Average Length, Average Diameter, and Average Aspect Ratio (SEM)> The CNT dispersions prepared in the Examples and Comparative Examples were diluted with pure water to a CNT concentration of 25 ppm by mass. A drop of the resulting diluted solution was dispensed onto a wafer using a dropper, and the wafer was then placed on a hot plate heated to 90°C and baked for 1 minute. The resulting CNT-coated wafers were observed using a scanning electron microscope (SEM, Hitachi High-Tech Corporation, product name "SU8200") at a working distance of 3 mm, an acceleration voltage of 1.0 kV, and a magnification of 10,000x, to obtain multiple SEM images containing 10 or more CNT bundles within the field of view. The diameter (outer diameter) and length of 100 CNT bundles randomly extracted from the obtained SEM images were measured. The arithmetic mean value of the diameters of the 100 measured CNT bundles was then used as the average diameter (nm) of the CNT bundles in the CNT dispersion. The arithmetic mean value of the measured lengths of 100 CNT bundles was taken as the average length (μm) of the CNT bundles in the CNT dispersion. The average aspect ratio was calculated by dividing the average length (nm) by the average diameter (nm). <Number of CNT bundles with a diameter greater than 30.0 nm> The diameters (outer diameters) of 100 CNT bundles were measured using an SEM as described above, and evaluated according to the following criteria. A: The number of CNT bundles with a diameter greater than 30.0 nm was 10 or less. B: The number of CNT bundles with a diameter greater than 30.0 nm was 11 to 15. C: The number of CNT bundles with a diameter greater than 30.0 nm was 16 or more. <Average length (optical microscope)> The CNT dispersions prepared in the examples and comparative examples were diluted to 0.02% with pure water. A drop of the resulting diluted solution was placed on a glass slide using a dropper, and the glass slide was then sandwiched between the slides and observed at a magnification of 700x using a digital microscope (Keyence Corporation, product name "VHX-7000") The lengths of all CNT bundles observed in one field of view were measured, and the arithmetic mean value was taken as the average length (μm) of the CNT bundles, which was evaluated according to the following criteria.A: Average length is 15.0 μm or more B: Average length is 8.0 μm or more and less than 15.0 μm C: Average length is less than 8.0 μm <G / D ratio> Using a microscopic laser Raman spectrophotometer (manufactured by Thermo Fisher Scientific, product name "Nicolet Almega XR"), the Raman spectra of the CNTs used in the examples and comparative examples were measured. Then, for the obtained Raman spectra, the peak at 1590 cm was measured. -1 The intensity of the G band peak observed near 1340 cm -1 The intensity of the D-band peak observed near the CNT dispersion was determined, and the G / D ratio was calculated. <Temporal Stability of Dispersion State> If both the "particle diameter change rate" and the "viscosity change rate" shown below were rated A or B, it means that the CNT dispersion has excellent temporal stability of the dispersion state. [Particle diameter change rate] For the CNT dispersions obtained in the Examples and Comparative Examples, the average particle diameter (D50) immediately after preparation and the average particle diameter (D50) 10 days after preparation were measured. The average particle diameter (D50) was measured using a laser diffraction / scattering particle size distribution analyzer (manufactured by HORIBA, product name "Partica LA-960V2") on an aqueous dispersion diluted with water to a CNT concentration of 0.04%, and the particle diameter at which the cumulative volume calculated from the smallest diameter side in the obtained particle size distribution (volume basis) reached 50% was taken as the average particle diameter (μm). The measurement conditions were as follows: Circulation speed: 3, ultrasonic intensity: 7, ultrasonic time: 1 minute, stirring speed: 1, stirring mode: continuous (circulation / ultrasonic operation conditions) Ultrasonic intensity: 7, ultrasonic time: 5 seconds (ultrasonic operation during air evacuation) Refractive index of water: 1.333 Refractive index of carbon material: 1.92 Then, the value of the average particle diameter (D50) immediately after preparation was determined as d 0 (μm), and the average particle diameter (D50) 10 days after preparation was taken as d 1 (μm), the particle size change rate (%) = [(d 1 -d 0 ) / d 0] × 100, the particle diameter change rate (%) was calculated and evaluated according to the following criteria. The smaller the particle diameter change rate value, the less likely the CNT dispersion state to change, i.e., the more excellent the stability of the dispersion state over time. A: Particle diameter change rate less than 1% B: Particle diameter change rate 1% or more but less than 30% C: Particle diameter change rate 30% or more [Viscosity Change Rate] For the CNT dispersions obtained in the Examples and Comparative Examples, the viscosity values ​​immediately after preparation and the viscosity values ​​10 days after preparation were measured. Each viscosity was measured using a rheometer (manufactured by Antonpaar, product name "MCR-102") at a temperature of 20°C. Specifically, a cone-plate was used as a measuring jig to measure the shear rate range of 100 to 9000 (1 / s), and the viscosity (mPa·s) at a shear rate of 1000 (1 / s) was determined. The viscosity value immediately after preparation was then expressed as η 0 (mPa·s), and the viscosity value 10 days after preparation was expressed as η 1 (mPa·s), viscosity change rate (%) = [(η 1 -η 0 ) / η 0 ] × 100, and evaluated according to the following criteria. A smaller viscosity change rate value means that the CNT dispersion is less likely to thicken over time, i.e., the stability of the dispersion state over time is superior. A: Viscosity change rate is less than 10% B: Viscosity change rate is 10% or more and less than 20% C: Viscosity change rate is 20% or more <Volume Conductivity> The volume conductivity (S / cm) of the carbon films (molded products) produced in the examples and comparative examples was measured in accordance with JIS K 7194 using a low resistivity meter (manufactured by Mitsubishi Chemical Analytech Co., Ltd., product name "Loresta GX") and evaluated according to the following criteria. The higher this volume conductivity value, the more excellent the conductivity of the carbon film (molded product). A: Volume conductivity value is 100 S / cm or more B: Volume conductivity value is 50 S / cm or more and less than 100 S / cm C: Volume conductivity value is less than 50 S / cm

[0113] (Example A1) <Preparation of CNT Dispersion> [Synthesis of CNT] Single-walled CNTs (hereinafter referred to as "CNT-a") were produced according to the method disclosed in Example 4 of WO 2022 / 114237. The properties of the obtained CNT-a were G / D ratio: 1.2, tapped bulk density: 0.02 g / cm3 , CNT average length: 150 μm, BET specific surface area: 600 m 2 The carbon content was 99.0% by mass, with a mean outer diameter of 4.0 nm. [Preparation of CNT Dispersion] 1.2 g of the CNT-a (G / D ratio: 1.2) single-walled CNT obtained above was added to 300 mL of an aqueous solution (concentration of sodium carboxymethylcellulose: 0.4%) containing sodium carboxymethylcellulose (manufactured by Tokyo Chemical Industry Co., Ltd., product code "C0045"; average degree of polymerization: 500) as a thickener in water as a solvent, to obtain a mixed solution (concentration of single-walled CNT: 0.4%). This mixed solution was subjected to a dispersion treatment using a wet jet mill (manufactured by Yoshida Kikai Kogyo Co., Ltd., model number "NVL-ES008A-D10", product name "NanoVata (registered trademark)") at a pressure of 50 MPa and 40 passes. Specifically, a shear force was applied to the mixed solution while applying back pressure to disperse the single-walled CNT, obtaining a CNT dispersion. The resulting CNT dispersion was measured for the average length, average diameter, average aspect ratio, and number of CNT bundles with a diameter greater than 30.0 nm when observed with an SEM. The average length of the CNT bundles, as well as the rate of change in particle size and viscosity, were also measured when observed with an optical microscope. The results are shown in Table 1. <Preparation of Carbon Film (Molded Product)> The CNT dispersion prepared above was filtered under a pressure of 0.09 MPa using a vacuum filtration device equipped with a membrane filter. After filtration, the carbon film formed on the membrane filter was washed by passing isopropyl alcohol and water through the vacuum filtration device, followed by passing air through the device for 15 minutes. The carbon film / membrane filter was then immersed in ethanol, and the carbon film was peeled off from the membrane filter to obtain a molded carbon film. The resulting carbon film was comparable in size to the membrane filter, possessed excellent film-forming properties, maintained its film state even after peeling from the filter, and exhibited excellent self-supporting properties. The volume conductivity of this carbon film was measured. The results are shown in Table 1.

[0114] (Examples A2 to A8, Comparative Examples A1 to A6) CNT dispersions were prepared and carbon films were fabricated in the same manner as in Example 1A, except that the pressure and number of passes in the dispersion treatment using a wet jet mill during preparation of the CNT dispersions were changed as shown in Tables 1 and 3. Evaluations were then performed in the same manner as in Example 1A. The results are shown in Tables 1 and 3.

[0115] (Examples A9 to A11) CNT synthesis, preparation of CNT dispersions, and production of carbon films were carried out in the same manner as in Example 1A, except that during preparation of the CNT dispersion, the concentration of the aqueous carboxymethyl cellulose sodium solution was changed from 0.4% to 0.8%, and the pressure and number of passes in the dispersion treatment using a wet jet mill were changed as shown in Table 1. Evaluations were then carried out in the same manner as in Example 1A. The results are shown in Table 1.

[0116] (Examples A12 to A14) CNT synthesis, preparation of CNT dispersions, and production of carbon films were carried out in the same manner as in Example 1A, except that during preparation of the CNT dispersion, the concentration of the aqueous carboxymethyl cellulose sodium solution was changed from 0.4% to 1.2%, and the pressure and number of passes in the dispersion treatment using a wet jet mill were changed as shown in Table 2. Evaluations were then carried out in the same manner as in Example 1A. The results are shown in Table 2.

[0117] (Example A15) CNT synthesis, preparation of a CNT dispersion, and production of a carbon film were carried out in the same manner as in Example 1A, except that sodium polyacrylate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product code "196-02955"; degree of polymerization: 22,000 to 70,000) was used instead of sodium carboxymethyl cellulose as the thickener when preparing the CNT dispersion. Evaluations were then carried out in the same manner as in Example 1A. The results are shown in Table 2.

[0118] (Example A16) CNT synthesis, preparation of a CNT dispersion, and production of a carbon film were carried out in the same manner as in Example 1A, except that polyvinylpyrrolidone (manufactured by Nippon Shokubai Co., Ltd., product name "Polyvinylpyrrolidone-K30"; HLB value: 15) was used instead of sodium carboxymethyl cellulose as the thickener when preparing the CNT dispersion. Evaluations were then carried out in the same manner as in Example 1A. The results are shown in Table 2.

[0119] (Example A17) A CNT dispersion was prepared and a carbon film was produced in the same manner as in Example 1A, except that CNT-b (manufactured by Zeon Corporation, product name "ZEONANO (registered trademark) SG101"; G / D ratio: 5.0) was used instead of CNT-a as the single-walled CNT when preparing the CNT dispersion, and the pressure and number of passes in the dispersion treatment using a wet jet mill were changed as shown in Table 2. Then, evaluation was performed in the same manner as in Example 1A. The results are shown in Table 2.

[0120] (Examples A18 to A19) Preparation of CNT dispersions and production of carbon films were carried out in the same manner as in Example 1A, except that, when preparing the CNT dispersions, CNT-c (manufactured by OCSiAl Corporation, product name "Tuball (registered trademark)"; G / D ratio: 109) was used instead of CNT-a as the single-walled CNTs, and the pressure and number of passes in the dispersion treatment using a wet jet mill were changed as shown in Table 2. Evaluations were then carried out in the same manner as in Example 1A. The results are shown in Table 2.

[0121] (Examples A20 to A21) Preparation of CNT dispersions and production of carbon films were carried out in the same manner as in Example 1A, except that, when preparing the CNT dispersions, CNT-d (manufactured by Meijo Nanocarbon Co., Ltd., product name "MEIJO eDIPS (registered trademark)"; G / D ratio: 119) was used instead of CNT-a as the single-walled CNTs, and the pressure and number of passes in the dispersion treatment using the wet jet mill were changed as shown in Table 2. Then, evaluations were carried out in the same manner as in Example 1A. The results are shown in Table 2.

[0122] (Comparative Example A7) CNT synthesis, preparation of a CNT dispersion, and production of a carbon film were carried out in the same manner as in Example 1A, except that the amount of CNT-a used during preparation of the CNT dispersion was changed from 1.2 g to 0.3 g. Evaluations were then carried out in the same manner as in Example 1A. The results are shown in Table 3. Note that the dispersibility of the CNTs in the CNT dispersion was extremely low, and it was not possible to measure the average length and average diameter of the CNT bundles when observed with an SEM.

[0123] Examples and comparative examples of the second invention (Examples B1 to B19, Comparative Examples B1 to B8) are described below. In the examples and comparative examples of the second invention, various measurements and evaluations were carried out using the following methods.

[0124] <Average Length, Average Diameter, Average Aspect Ratio> The CNT dispersions prepared in the Examples and Comparative Examples were diluted with pure water to a CNT concentration of 25 ppm by mass. A drop of the resulting diluted solution was dispensed onto a wafer using a dropper, and the wafer was then placed on a hot plate heated to 90°C and baked for 1 minute. The resulting CNT-coated wafers were observed using a scanning electron microscope (SEM, Hitachi High-Tech Corporation, product name "SU8200") at a working distance of 3 mm, an acceleration voltage of 1.0 kV, and a magnification of 10,000x, to obtain multiple SEM images containing 10 or more CNT bundles within the field of view. The diameter (outer diameter) and length of 100 CNT bundles randomly extracted from the obtained SEM images were measured. The arithmetic mean value of the diameters of the 100 measured CNT bundles was then used as the average diameter (nm) of the CNT bundles in the CNT dispersion. The arithmetic mean value of the measured lengths of 100 CNT bundles was taken as the average length (μm) of the CNT bundles in the CNT dispersion. The average aspect ratio was calculated by dividing the average length (nm) by the average diameter (nm). <Number of CNT bundles with a diameter of more than 30.0 nm> The diameters (outer diameters) of 100 CNT bundles were measured as described above and evaluated according to the following criteria. A: The number of CNT bundles with a diameter of more than 30.0 nm was 10 or less B: The number of CNT bundles with a diameter of more than 30.0 nm was 11 to 15 C: The number of CNT bundles with a diameter of more than 30.0 nm was 16 or more <G / D ratio> The Raman spectra of the CNTs used in the examples and comparative examples were measured using a microscopic laser Raman spectrophotometer (manufactured by Thermo Fisher Scientific, product name "Nicolet Almega XR"). The Raman spectra obtained were analyzed using a Raman spectrum of 1590 cm -1 The intensity of the G band peak observed near 1340 cm -1The intensity of the D-band peak observed near the CNT dispersion was determined, and the G / D ratio was calculated. <Temporal Stability of Dispersion State> If both the "particle diameter change rate" and the "viscosity change rate" shown below were rated A or B, it means that the CNT dispersion has excellent temporal stability of the dispersion state. [Particle diameter change rate] For the CNT dispersions obtained in the Examples and Comparative Examples, the average particle diameter (D50) immediately after preparation and the average particle diameter (D50) 10 days after preparation were measured. The average particle diameter (D50) was measured using a laser diffraction / scattering particle size distribution analyzer (manufactured by HORIBA, product name "Partica LA-960V2") on an aqueous dispersion diluted with water to a CNT concentration of 0.04%, and the particle diameter at which the cumulative volume calculated from the smallest diameter side in the obtained particle size distribution (volume basis) reached 50% was taken as the average particle diameter (μm). The measurement conditions were as follows: Circulation speed: 3, ultrasonic intensity: 7, ultrasonic time: 1 minute, stirring speed: 1, stirring mode: continuous (circulation / ultrasonic operation conditions) Ultrasonic intensity: 7, ultrasonic time: 5 seconds (ultrasonic operation during air evacuation) Refractive index of water: 1.333 Refractive index of carbon material: 1.92 Then, the value of the average particle diameter (D50) immediately after preparation was determined as d 0 (μm), and the average particle diameter (D50) 10 days after preparation was taken as d 1 (μm), the particle size change rate (%) = [(d 1 -d 0 ) / d 0 ] × 100, the particle diameter change rate (%) was calculated and evaluated according to the following criteria. The smaller the particle diameter change rate value, the less likely the CNT dispersion state to change, i.e., the more excellent the stability of the dispersion state over time. A: Particle diameter change rate less than 1% B: Particle diameter change rate 1% or more but less than 30% C: Particle diameter change rate 30% or more [Viscosity Change Rate] For the CNT dispersions obtained in the Examples and Comparative Examples, the viscosity values ​​immediately after preparation and the viscosity values ​​10 days after preparation were measured. Each viscosity was measured using a rheometer (manufactured by Antonpaar, product name "MCR-102") at a temperature of 20°C. Specifically, a cone-plate was used as a measuring jig to measure the shear rate range of 100 to 9000 (1 / s), and the viscosity (mPa·s) at a shear rate of 1000 (1 / s) was determined. The viscosity value immediately after preparation was then expressed as η0 (mPa·s), and the viscosity value 10 days after preparation was expressed as η 1 (mPa·s), viscosity change rate (%) = [(η 1 -η 0 ) / η 0 ] × 100, and evaluated according to the following criteria. A smaller viscosity change rate value means that the CNT dispersion is less likely to thicken over time, i.e., the stability of the dispersion state over time is superior. A: Viscosity change rate is less than 10% B: Viscosity change rate is 10% or more and less than 20% C: Viscosity change rate is 20% or more <Volume Conductivity> The volume conductivity (S / cm) of the carbon films (molded products) produced in the examples and comparative examples was measured in accordance with JIS K 7194 using a low resistivity meter (manufactured by Mitsubishi Chemical Analytech Co., Ltd., product name "Loresta GX") and evaluated according to the following criteria. The higher this volume conductivity value, the more excellent the conductivity of the carbon film (molded product). A: Volume conductivity value is 100 S / cm or more B: Volume conductivity value is 50 S / cm or more and less than 100 S / cm C: Volume conductivity value is less than 50 S / cm

[0125] (Example B1) <Preparation of CNT Dispersion> [Synthesis of CNT] Single-walled CNTs (hereinafter referred to as "CNT-a") were produced according to the method disclosed in Example 4 of WO 2022 / 114237. The properties of the obtained CNT-a were G / D ratio: 1.2, tapped bulk density: 0.02 g / cm 3 , CNT average length: 150 μm, BET specific surface area: 600 m 2The results were: 1 / g, average outer diameter: 4.0 nm, and carbon purity: 99.0% by mass. [Preparation of CNT Dispersion] 0.3 g of the CNT-a (G / D ratio: 1.2) as the single-walled CNT obtained above was added to 300 mL of an aqueous solution (concentration of sodium carboxymethylcellulose: 0.4%) containing sodium carboxymethylcellulose (manufactured by Tokyo Chemical Industry Co., Ltd., product code "C0045"; average degree of polymerization: 500) as a thickener in water as a solvent, to obtain a mixed solution (concentration of single-walled CNT: 0.1%). This mixed solution was subjected to a dispersion treatment using a wet jet mill (manufactured by Yoshida Kikai Kogyo Co., Ltd., model number "NVL-ES008A-D10", product name "NanoVata (registered trademark)") at a pressure of 25 MPa and 40 passes. Specifically, a shear force was applied to the mixed solution while applying back pressure to disperse the single-walled CNT, obtaining a CNT dispersion. The resulting CNT dispersion was measured for the average length, average diameter, and average aspect ratio of the CNT bundles, the number of CNT bundles with a diameter greater than 30.0 nm, and the rate of change in particle size and viscosity. The results are shown in Table 4. <Preparation of Carbon Film (Molded Product)> The CNT dispersion prepared above was filtered under 0.09 MPa using a vacuum filtration device equipped with a membrane filter. After filtration, the carbon film formed on the membrane filter was washed by passing isopropyl alcohol and water through the vacuum filtration device, followed by passing air through it for 15 minutes. Next, the carbon film / membrane filter was immersed in ethanol, and the carbon film was peeled off from the membrane filter to obtain a molded carbon film. The resulting carbon film was comparable in size to the membrane filter, had excellent film-forming properties, maintained its film state even after peeling off from the filter, and exhibited excellent self-supporting properties. The volume conductivity of this carbon film was measured. The results are shown in Table 4.

[0126] (Examples B2 to B11, Comparative Examples B1 to B8) CNT dispersions were prepared and carbon films were produced in the same manner as in Example B1, except that the pressure and number of passes in the dispersion treatment using a wet jet mill during the preparation of the CNT dispersion were changed as shown in Tables 4 to 6. Evaluations were then carried out in the same manner as in Example B1. The results are shown in Tables 4 to 6. In Comparative Example B8, the dispersibility of the CNTs in the CNT dispersion was extremely low, and it was not possible to measure the average length and average diameter of the CNT bundles.

[0127] (Example B12) A CNT dispersion was prepared and a carbon film was produced in the same manner as in Example B1, except that, when preparing the CNT dispersion, CNT-b (manufactured by Zeon Corporation, product name "ZEONANO (registered trademark) SG101"; G / D ratio: 5.0) was used instead of CNT-a as the single-walled CNT, and the pressure and number of passes in the dispersion treatment using a wet jet mill were changed as shown in Table 5. Then, evaluation was performed in the same manner as in Example B1. The results are shown in Table 5.

[0128] (Example B13) CNT synthesis, preparation of a CNT dispersion, and production of a carbon film were carried out in the same manner as in Example B1, except that sodium polyacrylate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product code "196-02955"; degree of polymerization: 22,000 to 70,000) was used instead of sodium carboxymethyl cellulose as the thickener when preparing the CNT dispersion, and the pressure and number of passes in the dispersion treatment using a wet jet mill were changed as shown in Table 5. Then, evaluations were carried out in the same manner as in Example B1. The results are shown in Table 5.

[0129] (Example B14) CNT synthesis, preparation of a CNT dispersion, and production of a carbon film were carried out in the same manner as in Example B1, except that polyvinylpyrrolidone (manufactured by Nippon Shokubai Co., Ltd., product name "Polyvinylpyrrolidone-K30"; HLB value: 15) was used instead of sodium carboxymethyl cellulose as the thickener when preparing the CNT dispersion, and the pressure and number of passes in the dispersion treatment using the wet jet mill were changed as shown in Table 5. Evaluations were then carried out in the same manner as in Example B1. The results are shown in Table 5.

[0130] (Examples B15 to B17) Preparation of CNT dispersions and production of carbon films were carried out in the same manner as in Example B1, except that, when preparing the CNT dispersions, CNT-c (manufactured by OCSiAl Corporation, product name "Tuball (registered trademark)"; G / D ratio: 109) was used instead of CNT-a as the single-walled CNTs, and the pressure and number of passes in the dispersion treatment using the wet jet mill were changed as shown in Table 5. Then, evaluations were carried out in the same manner as in Example B1. The results are shown in Table 5.

[0131] (Examples B18-19) Preparation of CNT dispersions and production of carbon films were carried out in the same manner as in Example B1, except that, when preparing the CNT dispersions, CNT-d (manufactured by Meijo Nanocarbon Co., Ltd., product name "MEIJO eDIPS (registered trademark)"; G / D ratio: 119) was used instead of CNT-a as the single-walled CNTs, and the pressure and number of passes in the dispersion treatment using the wet jet mill were changed as shown in Tables 5 and 6. Then, evaluations were carried out in the same manner as in Example B1. The results are shown in Tables 5 and 6.

[0132] Examples and comparative examples of the third invention (Examples C1 to C22, Comparative Examples C1 to C25) are described below. In the examples and comparative examples of the third invention, various measurements and evaluations were carried out using the following methods.

[0133] <Average Length, Average Diameter, and Average Aspect Ratio> The CNT dispersions prepared in the Examples and Comparative Examples were diluted with a 1% aqueous solution of sodium cholate to a single-walled CNT concentration of 25 ppm by mass. A drop of the resulting diluted solution was dispensed onto a wafer using a dropper, and the wafer was placed on a hot plate heated to 90°C and baked for 1 minute. The resulting CNT-coated wafers were observed using a scanning electron microscope (SEM, Hitachi High-Tech Corporation, product name "SU8200") at a working distance of 3 mm, an acceleration voltage of 1.0 kV, and a magnification of 10,000x, to obtain multiple SEM images containing 10 or more CNTs within the field of view. The diameter (outer diameter) and length of 100 CNT bundles randomly extracted from the obtained SEM images were measured. The arithmetic mean value of the diameters of the 100 measured CNT bundles was then used as the average diameter (nm) of the CNT bundles in the CNT dispersion. The arithmetic mean value of the measured lengths of 100 CNT bundles was taken as the average length (μm) of the CNT bundles in the CNT dispersion. The average aspect ratio was calculated by dividing the average length (nm) by the average diameter (nm). <Number of Bundles with a Diameter of More than 30.0 nm> The diameters (outer diameters) of 100 CNT bundles were measured as described above and evaluated according to the following criteria. A: The number of bundles with a diameter of more than 30.0 nm was 5 or less B: The number of bundles with a diameter of more than 30.0 nm was 6 to 10 C: The number of bundles with a diameter of more than 30.0 nm was 11 or more <G / D Ratio> The Raman spectra of the CNTs used in the examples and comparative examples were measured using a microscopic laser Raman spectrophotometer (manufactured by Thermo Fisher Scientific, product name "Nicolet Almega XR"). The Raman spectra obtained were analyzed using a Raman spectrum of 1590 cm -1 The intensity of the G band peak observed near 1340 cm -1The intensity of the D-band peak observed near the center was determined, and the G / D ratio was calculated. <Harmonic Mean Diameter> The CNT dispersions prepared in the Examples and Comparative Examples were diluted with a 1% aqueous solution of sodium cholate so that the concentration of single-walled CNTs was 10 ppm by mass. The resulting diluted solutions were measured using a Zetasizer Nano (manufactured by Malvern, product name "Nano ZS") at a temperature of 25°C, three scans, and a scan time of 60 seconds to determine the harmonic mean diameter (z-average diameter). <Volume Conductivity> The volume conductivity (S / cm) of the carbon films (molded products) prepared in the Examples and Comparative Examples was measured using a low resistivity meter (manufactured by Mitsubishi Chemical Analytech, product name "Loresta-GX") in accordance with JIS K 7194. The higher the volume conductivity value, the more excellent the conductivity of the carbon film (molded product).

[0134] Example C1 Preparation of CNT Dispersion 0.3 g of single-walled CNT (manufactured by Zeon Corporation, product name "ZEONANO (registered trademark) SG101", G / D ratio: 5.0, hereinafter referred to as "CNT-a") was added to 300 mL of a sodium cholate aqueous solution (concentration of sodium cholate: 1%) containing sodium cholate as a dispersant in water as a solvent, to obtain a mixed solution (concentration of single-walled CNT: 0.1%). This mixed solution was subjected to a dispersion treatment using a wet jet mill (manufactured by Yoshida Kikai Kogyo Co., Ltd., model number "NVL-ES008A-D10", product name "NanoVata (registered trademark)") at a pressure of 25 MPa and five passes. Specifically, a shear force was applied to the mixed solution while applying back pressure to disperse the single-walled CNT, thereby obtaining a CNT dispersion. The average length, average diameter, and average aspect ratio of the CNT bundles in the resulting CNT dispersion, the number of bundles with a diameter greater than 30.0 nm, and the harmonic mean diameter were measured. The results are shown in Table 7. <Preparation of Carbon Film (Molded Product)> The CNT dispersion prepared above was filtered under 0.09 MPa using a vacuum filtration device equipped with a membrane filter. After filtration, the carbon film formed on the membrane filter was washed by passing isopropyl alcohol and water through the vacuum filtration device, followed by passing air through it for 15 minutes. Next, the carbon film / membrane filter was immersed in ethanol, and the carbon film was peeled off from the membrane filter to obtain a molded carbon film. The resulting carbon film was comparable in size to the membrane filter, had excellent film-forming properties, maintained its film state even after peeling off from the filter, and exhibited excellent self-supporting properties. The conductivity of this carbon film was measured. The results are shown in Table 7.

[0135] (Examples C2 to C9) CNT dispersions were prepared and carbon films were fabricated in the same manner as in Example C1, except that the pressure and number of passes in the dispersion treatment using a wet jet mill during the preparation of the CNT dispersions were changed as shown in Table 7. Evaluations were then performed in the same manner as in Example C1. The results are shown in Table 7.

[0136] (Example C10) A CNT dispersion was prepared and a carbon film was produced in the same manner as in Example C1, except that CNT-b (single-walled CNT, G / D ratio: 1.2) was used instead of CNT-a as the single-walled CNT during the preparation of the CNT dispersion, and the number of passes in the dispersion treatment using a wet jet mill was changed from 5 to 10. Evaluations were then carried out in the same manner as in Example C1. The results are shown in Table 7.

[0137] (Examples C11 to C21) CNT dispersions were prepared and carbon films were fabricated in the same manner as in Example C10, except that the pressure and number of passes in the dispersion treatment using a wet jet mill during the preparation of the CNT dispersions were changed as shown in Tables 7 and 8. Evaluations were then performed in the same manner as in Example C1. The results are shown in Tables 7 to 8.

[0138] (Example C22) A CNT dispersion was prepared and a carbon film was produced in the same manner as in Example C10, except that sodium dodecylbenzene sulfate was used instead of sodium cholate as the dispersant when preparing the CNT dispersion, and the number of passes in the dispersion treatment using a wet jet mill was changed from 10 to 40. Then, evaluation was performed in the same manner as in Example C1. The results are shown in Table 8.

[0139] (Comparative Examples C1 to C8) CNT dispersions were prepared and carbon films were fabricated in the same manner as in Example C1, except that the pressure and number of passes in the dispersion treatment using a wet jet mill during preparation of the CNT dispersions were changed as shown in Table 7. Evaluations were then performed in the same manner as in Example C1. The results are shown in Tables 8 and 9.

[0140] (Comparative Examples C9 to C15) CNT dispersions were prepared and carbon films were fabricated in the same manner as in Example C10, except that the pressure and number of passes in the dispersion treatment using a wet jet mill during preparation of the CNT dispersions were changed as shown in Table 7. Evaluations were then performed in the same manner as in Example C1. The results are shown in Tables 9 and 10.

[0141] Comparative Example C16 A carbon film was produced in the same manner as in Example C1, except that a CNT dispersion prepared as follows was used. Evaluation was then performed in the same manner as in Example C1. The results are shown in Table 10. <Preparation of CNT Dispersion> 0.025 g of CNT-a as single-walled CNTs was added to 25 mL of a sodium cholate aqueous solution (sodium cholate concentration: 1%) containing sodium cholate as a dispersant in water as a solvent, to obtain a mixed solution (single-walled CNT concentration: 0.1%). This mixed solution was subjected to a dispersion treatment using an ultrasonic device (manufactured by Thinky Corporation, product name "Ultrasonic Nanotaro") at an output of 140 W for a treatment time of 40 minutes, to obtain a CNT dispersion.

[0142] (Comparative Examples C17 to C19) CNT dispersions were prepared and carbon films were produced in the same manner as in Comparative Example C16, except that the ultrasonic treatment time during preparation of the CNT dispersion was changed as shown in Table 10. Evaluations were then performed in the same manner as in Example C1. The results are shown in Table 10.

[0143] (Comparative Example C20) A CNT dispersion was prepared and a carbon film was produced in the same manner as in Comparative Example C16, except that CNT-b was used instead of CNT-a as the single-walled CNT when preparing the CNT dispersion. Evaluations were then carried out in the same manner as in Example C1. The results are shown in Table 10.

[0144] (Comparative Examples C21 to C23) CNT dispersions were prepared and carbon films were produced in the same manner as in Comparative Example C20, except that the ultrasonic treatment time during preparation of the CNT dispersion was changed as shown in Table 10. Evaluations were then performed in the same manner as in Example C1. The results are shown in Table 10.

[0145] (Comparative Example C24) A CNT dispersion was prepared and a carbon film was produced in the same manner as in Example C1, except that sodium cholate was not used as a dispersant when preparing the CNT dispersion and the number of passes in the dispersion treatment using a wet jet mill was changed from 5 to 40. Evaluations were then carried out in the same manner as in Example C1. The results are shown in Table 10. Note that the harmonic mean diameter of the CNTs could not be measured.

[0146] (Comparative Example C25) A CNT dispersion was prepared and a carbon film was produced in the same manner as in Example C10, except that sodium cholate was not used as a dispersant when preparing the CNT dispersion and the number of passes in the dispersion treatment using a wet jet mill was changed from 10 to 40. Evaluations were then carried out in the same manner as in Example C1. The results are shown in Table 10. Note that the harmonic mean diameter of the CNTs could not be measured.

[0147] In Tables 1 to 10 shown below, "SEM" indicates scanning electron microscope, "OM" indicates optical microscope, "single-walled" indicates single-walled CNT, "CMC" indicates sodium carboxymethylcellulose, "SC" indicates sodium cholate, "SDBS" indicates sodium dodecylbenzene sulfate, "PAA" indicates sodium polyacrylate, "PVP" indicates polyvinylpyrrolidone, "jet mill" indicates wet jet mill, "ultrasonic" indicates ultrasonic treatment, "number of CNT bundles with a diameter of more than 30 nm" indicates the number of CNT bundles with a diameter of more than 30.0 nm out of 100 CNT bundles, "A" indicates 5 or less, "B" indicates 6 to 10, and "C" indicates 11 or more. Furthermore, the "average aspect ratio of CNT bundles" is expressed as a value rounded to one decimal place.

[0148]

[0149]

[0150]

[0151]

[0152]

[0153]

[0154]

[0155]

[0156]

[0157]

[0158] <First Invention> Tables 1 to 3 show that Examples A1 to A21, which used CNT dispersions containing single-walled CNTs, a solvent, and a thickener, in which the average length of the CNT bundles exceeded a predetermined value when observed with an SEM, the average diameter of the CNT bundles was equal to or less than a predetermined value, and the number of CNT bundles with a diameter of greater than 30.0 nm per 100 CNT bundles was equal to or less than a predetermined value, and the average length of the CNT bundles was equal to or greater than a predetermined value when observed with an optical microscope, enabled the production of CNT dispersions with excellent stability over time of the dispersion state and carbon films with excellent electrical conductivity. On the other hand, Comparative Examples A1 to A4, in which the average diameter and the number of CNT bundles with a diameter of greater than 30.0 nm exceeded the predetermined values, and Comparative Example A7, in which the number of CNT bundles with a diameter of greater than 30.0 nm exceeded the predetermined value, showed reduced stability over time of the CNT dispersion and reduced electrical conductivity of the carbon film compared to Examples A1 to A21. Furthermore, it can be seen that the conductivity of the carbon film is lower in Comparative Example A3, in which the average length when observed with an optical microscope is less than a predetermined value, and in Comparative Examples A5 and A6, in which the average length when observed with an SEM is equal to or less than a predetermined value, compared to Examples A1 to A21.

[0159] <Second Invention> Tables 4 to 6 show that in Examples B1 to B19, which used CNT dispersions containing single-walled CNTs, a solvent, and a thickener, in which the average length of the CNT bundles exceeded a predetermined value, the average diameter of the CNT bundles was equal to or less than a predetermined value, and the number of CNT bundles with a diameter of greater than 30.0 nm per 100 CNT bundles was equal to or less than a predetermined value, CNT dispersions with excellent stability over time of the dispersed state and carbon films with excellent electrical conductivity were produced. On the other hand, in Comparative Examples B1 to B3, in which the average diameter of the CNT bundles exceeded the predetermined value, and Comparative Examples B4 to B6, in which the average length of the CNT bundles was equal to or less than the predetermined value, the electrical conductivity of the carbon films was reduced compared to Examples B1 to B19. Furthermore, in Comparative Example B7, in which the average diameter of the CNT bundles exceeds a predetermined value and the number of CNT bundles with a diameter of more than 30.0 nm out of 100 CNT bundles exceeds a predetermined value, it is clear that the stability of the dispersion state of the CNT dispersion over time and the conductivity of the carbon film are reduced compared to Examples B1 to 19. Furthermore, in Comparative Example B8, in which the number of CNT bundles with a diameter of more than 30.0 nm out of 100 CNT bundles exceeds a predetermined value, it is clear that the stability of the dispersion state of the CNT dispersion over time and the conductivity of the carbon film are reduced compared to Examples B1 to 19.

[0160] <Third Invention> Tables 7 to 10 show that carbon films with excellent conductivity were produced in Examples C1 to C22, which used CNT dispersions containing single-walled CNTs, a solvent, and a dispersant, in which the average length of the CNT bundles exceeded a predetermined value, the average diameter of the CNT bundles was less than a predetermined value, and the number of CNT bundles with a diameter of more than 30.0 nm per 100 CNT bundles was equal to or less than a predetermined value. On the other hand, Comparative Examples C1 to C23, which used CNT dispersions in which at least one of the average length of the CNT bundles, the average diameter of the CNT bundles, and the number of CNT bundles with a diameter of more than 30.0 nm per 100 CNT bundles was outside the predetermined range, showed reduced conductivity of the carbon films compared to Examples C1 to C22. Furthermore, Comparative Examples C24 and C25, which used CNT dispersions that did not contain a dispersant, also showed reduced conductivity of the carbon films compared to Examples C1 to C22.

[0161] According to the present invention (first invention and second invention), it is possible to provide a carbon nanotube dispersion liquid that has excellent stability of the dispersion state over time and that can form a molded product with excellent electrical conductivity. Also, according to the present invention (third invention), it is possible to provide a carbon nanotube dispersion liquid that can form a molded product with excellent electrical conductivity and a method for producing the same.

Claims

1. A carbon nanotube dispersion comprising a plurality of carbon nanotubes, a solvent, and a thickener, wherein the plurality of carbon nanotubes include single-walled carbon nanotubes, at least a portion of the plurality of carbon nanotubes form carbon nanotube bundles, and when the carbon nanotube bundles are observed with a scanning electron microscope, the average length of the carbon nanotube bundles is greater than 1.50 μm, the average diameter of the carbon nanotube bundles is 18.0 nm or less, and out of 100 carbon nanotubes in the carbon nanotube bundles, 15 or less carbon nanotubes have a diameter greater than 30.0 nm, and when the carbon nanotube bundles are observed with an optical microscope, the average length of the carbon nanotube bundles is 8.0 μm or more.

2. A carbon nanotube dispersion comprising a plurality of carbon nanotubes, a solvent, and a thickener, wherein the plurality of carbon nanotubes include single-walled carbon nanotubes, at least a portion of the plurality of carbon nanotubes form carbon nanotube bundles, and when the carbon nanotube bundles are observed with a scanning electron microscope, the average length of the carbon nanotube bundles is greater than 1.50 μm, the average diameter of the carbon nanotube bundles is 16.0 nm or less, and the number of carbon nanotubes having a diameter of greater than 30.0 nm is 15 or less out of 100 carbon nanotubes in the carbon nanotube bundles.

3. The carbon nanotube dispersion according to claim 1 or 2, wherein the carbon nanotube bundles have an average aspect ratio of more than 100.

4. The carbon nanotube dispersion according to claim 1 or 2, wherein the G / D ratio of the carbon nanotubes is 0.5 or more and 120 or less.

5. The carbon nanotube dispersion liquid according to claim 1 or 2, wherein the thickener comprises at least one selected from the group consisting of cellulose-based polymers, polycarboxylic acids and polyvinylpyrrolidone.

6. A carbon nanotube dispersion comprising a plurality of carbon nanotubes, a solvent, and a dispersant, wherein the plurality of carbon nanotubes include single-walled carbon nanotubes, at least a portion of the plurality of carbon nanotubes form carbon nanotube bundles, and when the carbon nanotube bundles are observed with a scanning electron microscope, the average length of the carbon nanotube bundles is greater than 1.5 μm, the average diameter of the carbon nanotube bundles is less than 15.0 nm, and the number of carbon nanotubes having a diameter of greater than 30.0 nm is 10 or less out of 100 carbon nanotubes in the carbon nanotube bundles.

7. The carbon nanotube dispersion of claim 6, wherein the carbon nanotube bundles have an average aspect ratio of greater than 120.

8. The carbon nanotube dispersion according to claim 6, wherein the G / D ratio of the carbon nanotubes is 0.5 or more and 20 or less.

9. The carbon nanotube dispersion according to claim 6, wherein the harmonic mean diameter of the carbon nanotubes is greater than 500 nm.

10. A method for producing a carbon nanotube dispersion liquid according to any one of claims 6 to 9, comprising a step of subjecting a mixture containing the plurality of carbon nanotubes, the solvent, and the dispersant to a dispersion treatment using a wet jet mill.

11. The method for producing a carbon nanotube dispersion liquid according to claim 10, wherein the pressure applied to the mixed liquid in the dispersion treatment is 50 MPa or less, and the number of passes in the dispersion treatment is 10 or more.

Citation Information

Patent Citations

  • Carbon nanotube dispersion liquid for non-aqueous electrolyte secondary battery, resin composition using the same, mixture slurry, electrode film, and non-aqueous electrolyte secondary battery

    JP2021072279A

  • Carbon nanotube dispersion and usage therefor

    WO2020004095A1

  • Carbon film

    WO2022114237A1

  • Method for producing carboxymethylcellulose, dispersant of carboxymethylcellulose and carbone nanotube-containing composition

    JP2014028935A

  • Carbon nanotube dispersion

    JP2017206412A

Cited By

  • Carbon nanotube slurry, carbon nanotube slurry for electrodes, and electrode film

    WO2026075047A1