Preparation method of EBSD metal composite sample, EBSD metal composite sample, characterization method and application

By using the first ion beam processing and the second ion beam thinning methods in the EBSD test, the EBSD metal composite sample is formed, which solves the problem that the electrolyte cannot treat multi-metal interfaces at the same time, and achieves effective characterization and analysis of composite metal samples. Performance evaluation.

CN118731075APending Publication Date: 2024-10-01YANGJIANG ALLOY MATERIALS LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410795471.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When the existing EBSD testing method is used to process composite metal samples, due to the different applicability of different metal interfaces to the electrolyte and the soft and hard matching problems, the commonly used electrolyte cannot simultaneously test composite metal samples containing more than two metals and corresponding The interface is effectively electropolished.

Method used

The first ion beam is used to treat the surface of the original sample, and the hardness pits are set to mark the interface, and then the second ion beam is used for thinning processing to form an EBSD metal composite sample, which avoids the use of electrolyte and solves the problem of the suitability of the metal interface for electrolyte. Sexually different issues.

Benefits of technology

It achieves effective EBSD characterization of composite metal samples, clarifies the interface position and metal matrix distribution, improves the evaluation of mechanical properties and corrosion properties, and avoids the limitations of electrolyte treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731075A_ABST
    Figure CN118731075A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of metal interface characterization, and particularly relates to a preparation method of an EBSD metal composite sample, the EBSD metal composite sample, a characterization method and application. The preparation method comprises the following steps: obtaining a plurality of original samples from a metal composite material containing a first metal and a second metal; after the original sample is pretreated, a plurality of hardness pits are formed in the surface of the original sample; and after the surface of the original sample is treated through a first ion beam, the characterization surface is subjected to first thinning treatment through a second ion beam, and the EBSD metal composite sample is obtained. According to the preparation method, the problems that different metal interfaces have different applicability to different electrolytes and different metals have soft and hard matching when the composite metal is treated by the electrolytes are fundamentally solved; therefore, a common electrolyte cannot simultaneously finish electrolytic polishing on a composite metal sample containing more than two metals and a corresponding interface at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal interface characterization, and specifically relates to a method for preparing an EBSD metal composite sample, an EBSD metal composite sample, a characterization method and an application. Background Art

[0002] Titanium and titanium alloys are widely used in military, aerospace and people's livelihood fields as high-end metal materials due to their excellent corrosion resistance, low density and high specific strength. Titanium has good application prospects in the field of high-end knives due to special requirements such as light weight and high corrosion resistance for military bayonets and field daggers. However, the low hardness and insufficient sharpness of titanium have severely restricted its application in the field of high-end metal materials for knives and scissors. Martensitic stainless steel has good corrosion resistance, high hardness and high sharpness, but pure martensitic stainless steel knives are heavy and not conducive to carrying in the field. Therefore, the development of "martensitic stainless steel / titanium" composite materials, the comprehensive use of the high corrosion resistance and light weight of titanium and the high hardness and high sharpness of martensitic stainless steel, is an important way to solve the problem of lightweight and corrosion-resistant high-end knife materials. The interface metallurgical bonding mechanism of the "steel / titanium" composite plate is studied, and EBSD can well reveal the grain distribution at its interface position. Therefore, it is necessary to explore a preparation method suitable for EBSD characterization of steel-titanium composite interfaces.

[0003] Generally, EBSD testing and research use electrolytic polishing to process samples. However, due to the different applicability of different metal interfaces to different electrolytes and the problem of soft-hard matching of different metals, commonly used electrolytes cannot simultaneously complete electrolytic polishing of composite metal samples containing more than two metals and the corresponding interfaces. Summary of the invention

[0004] To solve the above problems, the present invention proposes a method for preparing an EBSD metal composite sample. The preparation method can prepare a composite metal sample that can be used for EBSD characterization without using an electrolyte, which solves the problem that different metal interfaces have different applicability to different electrolytes and different metals have soft-hard matching problems, resulting in the inability of commonly used electrolytes to simultaneously complete electrolytic polishing of composite metal samples containing more than two metals and the corresponding interfaces.

[0005] The present invention is achieved through the following technical solutions:

[0006] One of the purposes of the present invention is to provide a method for preparing an EBSD metal composite sample, the preparation method comprising the following steps:

[0007] Obtaining a plurality of original samples from a metal composite material comprising a first metal and a second metal; the characterization surface of the original samples comprising a characterization surface of the first metal, a characterization surface of the second metal, and a first cross section of an interface between the first metal and the second metal;

[0008] After pre-treating the original sample, a plurality of hardness pits are set on the surface of the original sample; the surface of the original sample is perpendicular to the characterization surface and includes a second cross section of the interface, a surface of the first metal, and a surface of the second metal;

[0009] After the original sample surface is treated by a first ion beam, a second ion beam is used to perform a first thinning treatment on the characterization surface to obtain an EBSD metal composite sample.

[0010] In the preparation method of EBSD metal composite samples provided by the present invention, the hardness pits are used to mark or identify the original sample surface, and play a marking role in EBSD characterization; the first ion beam is used to process the original sample surface containing a number of hardness pits, so as to preliminarily determine the distribution of the metal matrix on both sides of the interface (crystal orientation distribution, grain size and shape, phase distribution, etc.); and then the second ion beam is used to perform a first thinning treatment on the characterization surface to determine the state of the metal matrix on both sides of the interface, and to determine whether it will become a weak position of the metal composite material, and affect the mechanical properties / corrosion properties of the metal composite material. It fundamentally solves the problem that the commonly used electrolyte cannot simultaneously complete electrolytic polishing of the composite metal sample containing more than two metals and the corresponding interface due to the different applicability of different metal interfaces to different electrolytes and the soft-hard matching problem of different metals when using electrolyte to treat composite metals.

[0011] In some possible implementations, the first metal and the second metal are made of different materials, and the first metal includes one or more of steel, titanium, 430 stainless steel, 304 stainless steel, and high entropy alloy. These metal materials have excellent properties in mechanical properties, corrosion properties, etc., and have good application prospects in engineering and civil fields. Therefore, it is necessary to study their grain distribution.

[0012] In some possible implementations, the second metal is made of a material different from that of the first metal, and the material of the second metal includes one or more of steel, titanium, 430 stainless steel, 304 stainless steel, and a high entropy alloy.

[0013] In some possible implementations, the method of obtaining the plurality of original samples includes wire cutting.

[0014] In some possible implementations, the angle between the interface and the original sample surface is 30° to 60°. Within this angle range, during the ion thinning process, it is ensured that there is no difference in the direction of thinning thickness on both sides of the interface due to the mismatch between the soft and hard phases of the two metals. In the case of a certain angle, the ion beam will first thin the soft phase metal or the hard metal, then thin the interface position, and then thin the other phase.

[0015] In some possible implementations, the energy of the first ion beam is 20 kV to 30 kV, the intensity is 60 nA to 200 nA, and the penetration depth is 0.2 μm to 2 μm. Under this ion beam parameter range, the first ion beam can eliminate part of the stress state on the surface of the original sample containing several hardness pits, preliminarily display the grain size and distribution of the interface, and provide a reference for the thinning process during the subsequent EBSD characterization.

[0016] In some possible implementations, the ion types of the first ion beam include at least one of a xenon ion beam and a gallium ion beam. Among these ion beam types, the xenon ion beam has a higher energy, so it can be processed and analyzed deeply inside the material, and the xenon ion beam has a strong focusing ability, which can achieve high-resolution processing and imaging, and is suitable for micro-scale preparation and analysis; the gallium ion beam has the advantages of fast speed, high processing accuracy and low damage, and the mass of the gallium ion beam is small, so it can achieve higher-precision processing, especially suitable for nano-scale processing and preparation, and the gallium ion beam generates less heat and radiation during processing, and causes less damage to the material, which is conducive to maintaining the original performance of the material.

[0017] In some possible implementations, the first ion beam is used to process the surface of the original sample for a period of 2 seconds to 20 seconds. Within this time range, the smoothness of the surface of the original sample is improved, the friction coefficient of the surface is reduced, and part of the stress state on the surface is eliminated while maintaining the original performance of the original sample.

[0018] In some possible implementations, the energy of the second ion beam is 20kV to 30kV, the intensity is 0.1nA to 60nA, and the thinning thickness is 10μm to 500μm. In this case, when the second ion beam thins the characterization surface, the thinning thickness is related to the intensity and time. Under the premise of the same thinning thickness, the smaller the current intensity of the second ion beam, the longer the time required; the surface atoms are stripped with a high current ion beam to complete micro- and nano-scale surface morphology processing; a high-intensity focused ion beam (FIB) is used to process the material at nanoscale, combined with real-time observation and fixed-point processing under a scanning electron microscope (SEM).

[0019] In some possible implementations, the ion type of the second ion beam includes at least one of a xenon ion beam and a gallium ion beam. Among these ion beam types, the energy of the xenon ion beam is relatively high, so it can be processed and analyzed deeply inside the material, and the xenon ion beam has a strong focusing ability, which can achieve high-resolution processing and imaging, and is suitable for micro-scale preparation and analysis; the gallium ion beam has the advantages of fast speed, high processing accuracy and low damage, and the mass of the gallium ion beam is relatively small, so it can achieve higher-precision processing, especially suitable for nano-scale processing and preparation, and the heat and radiation generated during the gallium ion beam processing are relatively small, and the damage to the material is relatively small, which is conducive to maintaining the original performance of the material.

[0020] In some possible implementations, the first thinning treatment lasts for 30 seconds to 60 minutes. Within this time range, the surface smoothness of the original sample is improved, the surface friction coefficient is reduced, and some stress states on the surface are eliminated while maintaining the original performance of the original sample.

[0021] The second object of the present invention is to provide an EBSD metal composite sample prepared by the method for preparing an EBSD metal composite sample provided by the present invention, wherein the EBSD metal composite sample comprises at least one characterization surface and at least one original sample surface;

[0022] At least one of the original samples comprises a plurality of hardness pits on its surface.

[0023] The EBSD metal composite sample provided by the present invention, the characterization surface is used for subsequent detection of EBSD data of the EBSD metal composite sample, and the original sample surface is used to set a plurality of hardness pits. The EBSD metal composite sample adopts a physical treatment method to form the characterization surface and surface, avoiding the problem that the commonly used electrolyte cannot simultaneously complete electrolytic polishing of the composite metal sample containing more than two metals and the corresponding interface due to the different applicability of different metal interfaces to different electrolytes and the soft-hard matching problem of different metals when using electrolyte to treat the composite metal.

[0024] In some possible implementations, the hardness pits are arranged in a direction parallel to the second cross section. In this case, the hardness pits can clearly identify the location of the interface and provide a reference for the thinning process.

[0025] In some possible implementations, the interface includes one or more of a steel-titanium interface, a 430 stainless steel-304 stainless steel interface, a steel-high entropy alloy interface, and a high entropy alloy-steel-titanium interface.

[0026] In some possible implementations, the spacing between adjacent hardness pits is 10 μm to 500 μm. In this case, the equally spaced distribution of hardness pits can provide a basis for multiple cycles of thinning, and also provide a reference for obtaining multi-layer EBSD data and subsequent three-dimensional reconstruction processing.

[0027] In some possible implementations, the spacing between adjacent hardness pits is equal. In this case, the equally spaced hardness pits are helpful for determining the interface direction and position on the one hand, and for three-dimensional EBSD reconstruction on the other hand, that is, thinning the sample according to the hardness pit spacing, and then collecting EBSD data, and so on, so that three-dimensional data can be obtained by repeating the process.

[0028] In some possible implementations, the diameter of the hardness pit is 3μm to 6μm or 50μm to 200μm. In this case, using a common Vickers hardness tester, the diameter of the hardness pit can be in the range of 50μm to 200μm; using a nanoindenter, the size of the hardness pit can be in the range of 3μm to 6μm; the size of the hardness pit and the spacing between the hardness pits can be used as a reference for equal spacing during the thinning process.

[0029] In some possible implementations, the hardness pits are arranged in a row parallel to the second cross section, or in a matrix parallel to the second cross section. In this case, controlling the density distribution of the hardness pits can play a role in marking the position and measuring the spacing; and the arrangement parallel to the interface direction is mainly used to determine the interface position to prevent the final thinning position from not being in this area.

[0030] In some possible implementations, the plurality of hardness pits are set using a microhardness tester or a nanoindenter. In this case, the hardness pits are used to mark positions to provide a position reference for the equally spaced thinning sample.

[0031] In some possible implementations, the original sample includes at least one of a steel-titanium composite metal, a 430 stainless steel-304 stainless steel composite metal, a steel-high entropy alloy composite metal, and a high entropy alloy-steel-titanium composite metal.

[0032] A third object of the present invention is to provide a method for characterizing a metal composite sample by EBSD, the method comprising the following steps:

[0033] Obtaining an EBSD metal composite sample prepared by the method for preparing an EBSD metal composite sample provided by the present invention or an EBSD metal composite sample provided by the present invention;

[0034] Acquiring EBSD data of a characterization surface of the EBSD metal composite sample;

[0035] The EBSD data are processed to obtain the grain orientation distribution of the EBSD metal composite sample.

[0036] The present invention provides a method for characterizing an EBSD metal composite sample. The sample selected is an EBSD metal composite sample prepared by the method for preparing an EBSD metal composite sample provided by the present invention or an EBSD metal composite sample provided by the present invention. EBSD is used to characterize the EBSD metal composite sample to obtain the grain orientation distribution of the sample, further understand the information such as the grain growth direction, grain boundary distribution, and crystal orientation distribution of the material, and provide important reference and guidance for the design, processing and application of the material.

[0037] In some possible implementations, the step of obtaining EBSD data of the characterization surface of the EBSD metal composite sample includes: obtaining single-layer EBSD data of the characterization surface of the EBSD metal composite sample using electron backscatter diffraction technology. In this case, obtaining and analyzing the single-layer EBSD data can obtain the grain orientation distribution of the EBSD metal composite sample.

[0038] In some other possible implementations, the step of obtaining EBSD data of the characterization surface of the EBSD metal composite sample includes:

[0039] The first single-layer EBSD data of the characterization surface of the EBSD metal composite sample is obtained by using the electron backscatter diffraction technology; the second single-layer EBSD data is obtained after the characterization surface is subjected to a second thinning treatment by using a third ion beam; the second thinning treatment and the EBSD data acquisition steps are repeated on the characterization surface to obtain multi-layer EBSD data. In this case, it is easier to visually observe the grain orientation distribution of the interface by acquiring multi-layer EBSD data.

[0040] In some possible implementations, the characterization surface is thinned with a number of the hardness pits as marks, and then the multi-layer EBSD data of the characterization surface is obtained. In this case, due to the equally spaced hardness pits, on the one hand, it is helpful to determine the interface direction and position. On the other hand, it is helpful to do three-dimensional EBSD reconstruction, that is, thin the sample according to the hardness pit spacing, and then collect EBSD data, so that the three-dimensional data can be obtained in a cycle (the existing EBSD characterization is mainly data information in the plane).

[0041] In some possible implementations, CHANNEL 5 is used to process the single-layer EBSD data to obtain the grain orientation distribution of the EBSD metal composite sample. In some possible implementations, reconstruction software is used to process the multi-layer EBSD data to obtain the grain orientation distribution of the EBSD metal composite sample. In this case, CHANNEL 5 processes the single-layer EBSD data, and reconstruction software is used to process the multi-layer EBSD data, and the grain orientation distribution of the EBSD metal composite sample can be obtained after processing.

[0042] In some possible implementations, the reconstruction software includes Avizo software. The Avizo software is a comprehensive set of visualization tools that help people display, process and understand engineering science data. The three-dimensional data of the EBSD metal composite sample can be processed and obtained through the powerful data processing function and easy-to-use humanized graphical interface provided by Avizo.

[0043] In some possible implementations, the EBSD data includes grain size, grain boundary characterization, and phase distribution of the characterization surface.

[0044] Furthermore, the ion types of the third ion beam include at least one of a xenon ion beam and a gallium ion beam. Among these ion beam types, the energy of the xenon ion beam is relatively high, so it can be processed and analyzed deeply inside the material, and the xenon ion beam has a strong focusing ability, which can achieve high-resolution processing and imaging, and is suitable for micro-scale preparation and analysis; the gallium ion beam has the advantages of high speed, high processing accuracy and low damage, and the mass of the gallium ion beam is relatively small, so it can achieve higher-precision processing, especially suitable for nano-scale processing and preparation, and the heat and radiation generated during the gallium ion beam processing are relatively small, and the damage to the material is relatively small, which is conducive to maintaining the original performance of the material.

[0045] Furthermore, the energy of the third ion beam is 20kV to 30kV, the intensity is 0.1nA to 60nA, and the thinning thickness is 10μm to 500μm. In this case, when the third ion beam thins the characterization surface, the thinning thickness is related to the intensity and time. Under the premise of the same thinning thickness, the smaller the current intensity of the third ion beam, the longer the time required.

[0046] Furthermore, the second thinning treatment takes 30 seconds to 60 minutes. Within this time range, the ion beam performs thinning treatment on the surface to be characterized to obtain a state that can be used for EBSD characterization.

[0047] Furthermore, in the second thinning process, the single thinning thickness is 10 μm to 100 μm. Within the subtracted thickness range, the single thinning thickness is the spacing between adjacent hardness pits.

[0048] In some possible implementations, the number of cycles in the step of cyclically performing the second thinning process on the characterization surface and obtaining EBSD data is 1 to 5. In this case, the multi-layer EBSD data obtained by the cycle can be processed by reconstruction software to obtain the three-dimensional data of the EBSD metal composite sample.

[0049] A fourth object of the present invention is to provide an EBSD metal composite sample characterization method, and its application in the field of metal composite material analysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 A schematic diagram of a process for preparing an EBSD metal composite sample according to an embodiment of the present invention;

[0051] Figure 2a It is a schematic diagram of the relative positions of the characterization surface of the first metal, the characterization surface of the second metal and the first cross section in the characterization surface of the original sample in an embodiment of the present invention;

[0052] Figure 2b It is a schematic diagram of the relative positions of the surface of the first metal, the surface of the second metal and the second cross section in the original sample surface in an embodiment of the present invention;

[0053] Figure 3 Schematic diagram of the three-dimensional structure of the EBSD metal composite sample in an embodiment of the present invention;

[0054] Figure 4 This is a schematic flow chart of a method for characterizing a metal composite sample using EBSD in an embodiment of the present invention;

[0055] Figure 5 This is a grain orientation distribution diagram of a single layer EBSD data of an EBSD metal composite sample prepared by the method for preparing an EBSD metal composite sample in Example 1 of the present invention.

[0056] Explanation of the reference numerals: 1 - characterization surface, 2 - interface, 3 - characterization surface of the first metal, 4 - characterization surface of the second metal, 5 - first cross section, 6 - second cross section, 7 - surface of the first metal, 8 - surface of the second metal, 9 - hardness pit. DETAILED DESCRIPTION

[0057] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0058] On the contrary, the present invention covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present invention as defined by the claims. Further, in order to make the public have a better understanding of the present invention, some specific details are described in detail in the detailed description of the present invention below. Those skilled in the art can fully understand the present invention without the description of these details.

[0059]

A method for preparing EBSD metal composite samples

[0060] A first aspect of an embodiment of the present invention provides a method for preparing an EBSD metal composite sample, such as Figure 1 , Figure 2a , Figure 2b and Figure 3 As shown, the preparation method comprises the following steps:

[0061] S1. Obtain several original samples from a metal composite material comprising a first metal and a second metal; a characterization surface 1 of the original sample comprises a characterization surface 3 of the first metal, a characterization surface 4 of the second metal, and a first cross section 5 of an interface 2 between the first metal and the second metal.

[0062] S2. After pre-processing the original sample, a plurality of hardness pits 9 are set on the surface of the original sample; the surface of the original sample is perpendicular to the characterization surface 1, and includes a second cross section 6 of the interface 2, a surface 7 of the first metal, and a surface 8 of the second metal.

[0063] S3. After the original sample surface is treated with the first ion beam, the characterization surface 1 is subjected to the first thinning treatment with the second ion beam to obtain an EBSD metal composite sample.

[0064] In the preparation method of EBSD metal composite samples provided by the embodiment of the present invention, hardness pits are used to mark or identify the original sample surface, which plays a marking role in EBSD characterization; the first ion beam is used to process the original sample surface containing several hardness pits, so as to preliminarily determine the distribution of the metal matrix on both sides of the interface (crystal orientation distribution, grain size and shape, phase distribution, etc.); and then the second ion beam is used to perform the first thinning treatment on the characterization surface to determine the state of the metal matrix on both sides of the interface, and to determine whether it will become a weak position of the metal composite material, and affect the mechanical properties / corrosion properties of the metal composite material. It fundamentally solves the problem that the commonly used electrolyte cannot simultaneously complete electrolytic polishing of composite metal samples containing more than two metals and the corresponding interfaces due to the different applicability of different metal interfaces to different electrolytes and the soft-hard matching problem of different metals when using electrolyte to treat composite metals.

[0065] [Step S1]

[0066] In some embodiments, in the above step S1, the materials of the first metal and the second metal are different, and the material of the first metal includes one or more of steel, titanium, 430 stainless steel, 304 stainless steel, and high entropy alloy. These metal materials have excellent performance in mechanical properties, corrosion properties, etc., and have good application prospects in engineering and civil fields. Therefore, it is necessary to study their grain distribution.

[0067] In some embodiments, in the above step S1, the second metal is made of a material different from that of the first metal, and the second metal includes one or more of steel, titanium, 430 stainless steel, 304 stainless steel, and a high entropy alloy.

[0068] In some embodiments, in the above step S1, the method of obtaining the plurality of original samples includes wire cutting. In this case, the original samples obtained by wire cutting are not deformed by force, and the cut surface (ie, the characterization surface) obtained by cutting is flat and has good roughness.

[0069] In some embodiments, in the above step S1, the angle between the interface and the original sample surface is 30° to 60°. Within this angle range, during the ion thinning process, it is ensured that there is no difference in the direction of thinning thickness on both sides of the interface due to the mismatch between the soft and hard phases of the two metals. In the case of a certain angle, the ion beam will first thin the soft phase metal or the hard metal, then thin the interface position, and then thin the other phase.

[0070] In some embodiments, in the above step S1, the size of the original sample is (5mm-30mm)×(5mm-30mm)×(2mm-10mm). Within this size range, the composite metal interface to be observed can be located in the cut sample and can also include part of the metal matrix on both sides.

[0071] [Step S2]

[0072] In some embodiments, in the above step S2, pre-treating the original sample includes the following steps: grinding the characterization surface and the surface of the original sample, mechanically polishing it, and then ultrasonically cleaning it. In this case, after pre-treatment, the original sample can preliminarily distinguish the grain distribution state of the matrix on both sides of the interface, which is conducive to confirming the interface position and preparing for the next step of thinning. For example, the original sample is a steel / titanium two-phase. After pre-treatment, the steel / titanium two-phase can be preliminarily distinguished, which side is steel and which side is titanium (generally, the crystal structure of the composite metal is different, such as one side is BCC and the other side is FCC structure. After pre-treatment, the metal grains with FCC structure are much larger than BCC, so it is easy to distinguish the difference between the two phases).

[0073] In some specific embodiments, the grinding time for grinding the characterization surface of the original sample is 3min to 15min, and in the exemplary examples, it can be 3min, 5min, 7min, 9min, 11min, 13min, 15min, etc. typical but non-limiting time or the range between any two times; in some specific embodiments, the grinding time for grinding the surface of the original sample is 3min to 15min, and in the exemplary examples, it can be 3min, 5min, 7min, 9min, 11min, 13min, 15min, etc. typical but non-limiting time or the range between any two times. Within this grinding time range, defects (such as wire cutting marks) on the characterization surface and the surface can be removed, and the surface roughness is significantly reduced.

[0074] In some embodiments, the surface and the surface are polished using sandpaper or a pre-grinder.

[0075] Pre-grinding machine is a kind of equipment used for rough grinding and primary grinding, which is usually used in metal processing, ceramic processing and other fields. The main features of pre-grinding machine include: 1. Strong rough grinding ability: pre-grinding machine can remove rough materials and shape trimming, with a high material removal rate; this is conducive to quickly completing the rough forming of blanks; 2. Simple structure: pre-grinding machine is usually composed of basic components such as motor, spindle, grinding disc, etc., and the structure is relatively simple. This is conducive to the manufacture and maintenance of equipment; 3. Wide selection of abrasives: pre-grinding machine can use various coarse-grained abrasives, such as silicon carbide, aluminum oxide, etc.; select appropriate abrasives according to different processing materials; 4. Suitable for a variety of workpieces: pre-grinding machine can process blanks of various hard materials such as metal, ceramic, glass, etc.

[0076] In some specific embodiments, the surface and the surface are polished with sandpaper of No. 400 to No. 1200, and in the exemplary examples, the typical but non-limiting types may be No. 40, No. 60, No. 80, No. 100, No. 120, No. 150, No. 180, No. 240, No. 320, No. 400, No. 600, No. 800, No. 1000, No. 1200, etc. In this case, the defects of the surface can be effectively removed by polishing the surface with sandpaper of No. 400 to No. 1200, so as to obtain a smoother surface.

[0077] In some specific embodiments, the characterization surface and the surface are mechanically polished after grinding, and the mechanical polishing is performed until the characterization surface and the surface of the original sample are smooth without obvious scratches. The mechanical polishing time is 3 minutes to 10 minutes. In the exemplary examples, it can be 3 minutes, 5 minutes, 7 minutes, 9 minutes, 10 minutes, etc., which are typical but non-limiting times, or a range between any two times.

[0078] In some specific embodiments, the original sample is ultrasonically cleaned with anhydrous ethanol, the ultrasonic frequency is 20kHz to 60kHz, and the ultrasonic time is 1min to 5min. In this case, surface attachments caused by grinding and polishing on the surface of the original sample and the characterization surface can be removed to ensure that the characterization surface and the surface are clean.

[0079] In some embodiments, in the above step S2, a plurality of hardness pits are set using a microhardness tester or a nanoindenter. In this case, the hardness pits are used to mark the positions to provide a position reference for the equally spaced thinning sample.

[0080] A microhardness tester uses a microscope to observe the marks or indentations on the surface of a material, and detects the hardness of the material based on the shape, size, and distribution of these marks or indentations.

[0081] Nanoindenter is an instrument used to measure the mechanical properties of materials, especially mechanical properties at the nanoscale. It determines the mechanical properties of materials such as hardness, elastic modulus, and plastic deformation behavior by applying a controlled force or load at the nanoscale and measuring the deformation response of the material.

[0082] [Step S3]

[0083] In some embodiments, in the above step S3, the energy of the first ion beam is 20kV to 30kV, the intensity is 60nA to 200nA, and the penetration depth is 0.2μm to 2μm; in the exemplary embodiment, the energy of the first ion beam can be 20kV, 25kV, 30kV and other typical but non-limiting energies or the range between any two energies, the intensity can be 60nA, 80nA, 100nA, 120nA, 140nA, 160nA, 180nA, 200nA and other typical but non-limiting intensities or the range between any two intensities, and the penetration depth can be 0.2μm, 0.8μm, 1.2μm, 1.8μm, 2μm and other typical but non-limiting penetration depths or the range between any two penetration depths. Under this ion beam parameter range, the first ion beam can eliminate part of the stress state of the original sample surface containing several hardness pits, preliminarily display the grain size and distribution of the interface, and provide a reference for the subsequent thinning process during EBSD characterization.

[0084] In some embodiments, in the above step S3, the ion type of the first ion beam includes at least one of a xenon ion beam and a gallium ion beam. Among these ion beam types, the energy of the xenon ion beam is relatively high, so it can be processed and analyzed deeply inside the material, and the xenon ion beam has a strong focusing ability, which can achieve high-resolution processing and imaging, and is suitable for micro-scale preparation and analysis; the gallium ion beam has the advantages of fast speed, high processing accuracy and low damage, and the mass of the gallium ion beam is relatively small, so it can achieve higher-precision processing, especially suitable for nano-scale processing and preparation, and the heat and radiation generated during the gallium ion beam processing are relatively small, and the damage to the material is relatively small, which is conducive to maintaining the original performance of the material.

[0085] In some embodiments, in the above step S3, the time for treating the surface of the original sample with the first ion beam is 2s to 20s. In the exemplary embodiment, it can be a typical but non-limiting time such as 2s, 5s, 10s, 15s, 20s, or a range between any two times. Within this time range, under the premise of maintaining the original performance of the original sample, the smoothness of the surface of the original sample is improved, the friction coefficient of the surface is reduced, and the partial stress state of the surface of the original sample containing a number of hardness pits can be eliminated.

[0086] In some embodiments, in the above step S3, the energy of the second ion beam is 20kV~30kV, the intensity is 0.1nA~60nA, and the thinning thickness is 10μm~500μm; in the exemplary embodiment, the energy of the second ion beam can be typical but non-limiting energies such as 20kV, 25kV, 30kV, or a range between any two energies, the intensity can be typical but non-limiting intensities such as 0.1nA, 1nA, 4nA, 15nA, 30nA, 60nA, or a range between any two intensities, and the single thinning thickness can be typical but non-limiting thicknesses such as 10μm, 50μm, 100μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, 450μm, 500μm, or a range between any two thicknesses. In this case, when the second ion beam performs thinning processing on the characterization surface, the thinning thickness is related to the intensity and time, that is, under the premise of the same thinning thickness, the smaller the current intensity of the second ion beam, the longer the time required.

[0087] In some specific embodiments, a second ion beam with an energy of 30 kV and an intensity gradually reduced from 60 nA to 15 nA to 4 nA to 1 nA to 0.1 nA is used to perform a first thinning treatment on the characterization surface. In this case, the second ion beam is gradually reduced to ensure the flatness and uniformity of the characterization surface and the first cross section, and to gradually eliminate the stress state of the characterization surface, thereby ensuring the subsequent EBSD characterization effect.

[0088] In some embodiments, in the above step S3, the time of the first thinning treatment is 30s to 60min, and in the exemplary embodiment, it can be 30s, 1min, 10min, 20min, 30min, 40min, 50min, 60min, etc., typical but non-limiting time or a range between any two time periods. Within this time range, under the premise of ensuring that the characterization surface is flat and uniform, the second ion beam can effectively reduce the original sample by one unit of thinning thickness.

[0089]

EBSD metal composite samples

[0090] The second purpose of the embodiment of the present invention is to provide an EBSD metal composite sample prepared by the preparation method of the EBSD metal composite sample provided by the present invention, such as Figure 2a , Figure 2b and Figure 3 As shown, the EBSD metal composite sample comprises at least one characterization surface 1 and at least one original sample surface;

[0091] At least one original sample includes a plurality of hardness pits 9 on its surface.

[0092] The EBSD metal composite sample provided in the embodiment of the present invention has a characterization surface used for subsequent detection of EBSD data of the EBSD metal composite sample, and the original sample surface is used to set a plurality of hardness pits. The EBSD metal composite sample is formed by a physical treatment method to form a characterization surface and a surface, which avoids the problem of using an electrolyte to treat the composite metal, which is caused by the different applicability of different metal interfaces to different electrolytes and the soft-hard matching problem of different metals, resulting in the inability of commonly used electrolytes to simultaneously complete electrolytic polishing of composite metal samples containing more than two metals and the corresponding interfaces.

[0093] In some embodiments, Figure 2b As shown, the arrangement direction of the plurality of hardness pits 9 is parallel to the second cross section 6. In this case, these hardness pits can clearly identify the location of the interface and provide a reference for the thinning process.

[0094] In some embodiments, Figure 3 As shown, interface 2 includes one or more of the following: steel-titanium interface, 430 stainless steel-304 stainless steel interface, steel-high entropy alloy interface, and high entropy alloy-steel-titanium interface. These interfaces of metal composite materials are widely used in practical engineering and face many practical problems. Therefore, it is necessary to analyze the data of grain size, grain boundary characterization, phase distribution, etc. of these interfaces.

[0095] In some embodiments, the spacing between adjacent hardness pits is 10 μm to 500 μm. In exemplary embodiments, the spacing may be 10 μm, 20 μm, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, or any range between any two spacings. In this case, the equally spaced distribution of hardness pits can provide a basis for multiple cycles of thinning, and also provide a reference for obtaining multi-layer EBSD data and subsequent three-dimensional reconstruction processing.

[0096] In some embodiments, the spacing between adjacent hardness pits is equal. In this case, the equally spaced hardness pits are helpful for determining the interface orientation and position on the one hand, and for three-dimensional EBSD reconstruction on the other hand, that is, thinning the sample according to the hardness pit spacing, and then collecting EBSD data, and so on, so that three-dimensional data can be obtained by repeating the process.

[0097] In some embodiments, the diameter of the hardness pit is 3μm to 6μm or 50μm to 200μm. In the exemplary embodiment, it can be a typical but non-limiting diameter such as 3μm, 4μm, 5μm, 6μm, or a range between any two diameters, or a typical but non-limiting diameter such as 50μm, 100μm, 150μm, 200μm, or a range between any two diameters. In this case, using an ordinary Vickers hardness tester can make the diameter of the hardness pit range from 50μm to 200μm; using a nano indenter, the hardness pit size can be 3μm to 6μm; the hardness pit size and the hardness pit spacing can be used as a reference for equal spacing treatment during the thinning process.

[0098] In some embodiments, the hardness pits 9 are arranged in a row parallel to the second section 6, or in a matrix parallel to the second section 6. In this case, the density distribution of the hardness pits is controlled to improve the lubrication performance of the metal surface; and the arrangement parallel to the interface direction is mainly used to determine the interface position to prevent the final thinning position from not being in this area.

[0099] In some embodiments, the number of hardness pits is at least 3. In the exemplary embodiment, it can be 3, 6, 8, 9, etc., which are typical but non-limiting numbers or a range between any two numbers. They are arranged in a row parallel to the second section, or in a matrix parallel to the second section. In this case, when the hardness of the metal on both sides of the interface is not much different (close), the hardness pits can only be arranged in a row parallel to the second interface; when the hardness of the metal on both sides of the interface is very different, in order to accurately control the thinning thickness, it is necessary to make the hardness pits parallel to the second section and set hardness pits on both sides of the second section; controlling the density distribution of the hardness pits can play the role of marking the position and also the role of measuring the spacing; and, arranging parallel to the interface direction is mainly used to determine the interface position to prevent the final thinning position from not being in this area.

[0100] In some embodiments, the original sample includes at least one of a steel-titanium composite metal, a 430 stainless steel-304 stainless steel composite metal, a steel-high entropy alloy composite metal, and a high entropy alloy-steel-titanium composite metal.

[0101]

A characterization method for metal composite samples by EBSD

[0102] The third purpose of the embodiment of the present invention is to provide a method for characterizing a metal composite sample by EBSD, such as Figure 4 As shown, the characterization method includes the following steps:

[0103] X1. Obtain an EBSD metal composite sample prepared by the method for preparing an EBSD metal composite sample provided in an embodiment of the present invention or an EBSD metal composite sample provided in an embodiment of the present invention.

[0104] X2. Obtain EBSD data of the characterization surface of the EBSD metal composite sample.

[0105] X3. Process the EBSD data to obtain the grain orientation distribution of the EBSD metal composite sample.

[0106] The EBSD metal composite sample characterization method provided in an embodiment of the present invention is a sample selected from the EBSD metal composite sample prepared by the EBSD metal composite sample preparation method provided in the present invention or the EBSD metal composite sample provided in the present invention. The EBSD metal composite sample is characterized by using EBSD to obtain the grain orientation distribution of the sample, and further understand the information such as the grain growth direction, grain boundary distribution, and crystal orientation distribution of the material, thereby providing important reference and guidance for the design, processing and application of the material.

[0107]

Step X2

[0108] In some embodiments, in the above step X2, the step of obtaining EBSD data of the characterization surface of the EBSD metal composite sample includes:

[0109] X201. Use electron backscatter diffraction technology to obtain single-layer EBSD data of the characterization surface of the EBSD metal composite sample. In this case, after obtaining the single-layer EBSD data and analyzing and processing it, the grain orientation distribution of the EBSD metal composite sample can be obtained.

[0110] In some other embodiments, in the above step X2, the step of obtaining EBSD data of the characterization surface of the EBSD metal composite sample includes:

[0111] X202. Use electron backscatter diffraction technology to obtain the first single layer EBSD data of the EBSD metal composite sample characterization surface.

[0112] X203. Obtaining second single-layer EBSD data after performing a second thinning treatment on the characterization surface using a third ion beam, the thinning thickness being the spacing between adjacent hardness pits;

[0113] X204. The characterization surface is subjected to a second thinning process and EBSD data acquisition step to obtain multi-layer EBSD data. In this case, the acquisition of multi-layer EBSD data can perform three-dimensional reconstruction of the grains, thus realizing three-dimensional visualization observation of the grain distribution.

[0114] In the above embodiment, if only the results such as the grain orientation distribution on the sample surface are obtained, only a single layer of EBSD is needed; in this way, only the two-dimensional (2D) cross section of the material can be observed and analyzed, and comprehensive three-dimensional (3D) microstructure information cannot be obtained. For example, the grain morphology should be similar to a polyhedron, but it is displayed as a polygon in the 2D cross-section diagram, and the exact grain size and the number of crystal interfaces cannot be obtained; if the three-dimensional distribution of grains is required, multi-layer EBSD tests are required, and then three-dimensional reconstruction is performed; to obtain a three-dimensional microstructure, the three-dimensional morphological characteristics of grains and grain boundaries and the distribution law of each characteristic parameter can be analyzed, including grain size, grain surface area, number of crystal interfaces of grains, grain boundary size and average grain boundary size of grains, and the relationship between each characteristic parameter can be statistically analyzed.

[0115] In some specific embodiments, in the above step X203, the characterization surface is thinned with a number of hardness pits as marks, and then the multi-layer EBSD data of the characterization surface is obtained. In this case, due to the equally spaced hardness pits, on the one hand, it is beneficial to determine the interface direction and position. On the other hand, it is beneficial to do three-dimensional EBSD reconstruction, that is, thin the sample according to the hardness pit spacing, and then collect EBSD data, so that the cycle is carried out, and three-dimensional data can be obtained (the existing EBSD characterization is mainly data information in the plane).

[0116] In some specific embodiments, in the above step X203, the ion type of the third ion beam includes at least one of a xenon ion beam and a gallium ion beam. Among these ion beam types, the energy of the xenon ion beam is relatively high, so it can be processed and analyzed deeply inside the material, and the xenon ion beam has a strong focusing ability, which can achieve high-resolution processing and imaging, and is suitable for micro-scale preparation and analysis; the gallium ion beam has the advantages of fast speed, high processing accuracy and low damage, and the mass of the gallium ion beam is relatively small, so it can achieve higher-precision processing, especially suitable for nano-scale processing and preparation, and the heat and radiation generated during the gallium ion beam processing are relatively small, and the damage to the material is relatively small, which is conducive to maintaining the original performance of the material.

[0117] In some specific embodiments, in the above step X203, the energy of the third ion beam is 20kV~30kV, the intensity is 0.1nA~60nA, and the thinning thickness is 10μm~500μm. In the exemplary embodiment, the energy of the third ion beam can be typical but non-limiting energies such as 20kV, 25kV, 30kV, or a range between any two energies, the intensity can be typical but non-limiting intensities such as 0.1nA, 1nA, 4nA, 15nA, 30nA, 60nA, or a range between any two intensities, and the single thinning thickness can be typical but non-limiting thicknesses such as 10μm, 50μm, 100μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, 450μm, 500μm, or a range between any two thicknesses. In this case, when the third ion beam performs thinning processing on the characterization surface, the thinning thickness is related to the intensity and time. Under the premise of the same thinning thickness, the smaller the current intensity of the third ion beam is, the longer the time required is.

[0118] In some embodiments, in the above step X203, the second thinning treatment time is 30s to 60min, preferably 10min to 30min, and in the exemplary embodiment, it can be 30s, 1min, 10min, 20min, 30min, 40min, 50min, 60min, etc. typical but non-limiting time or a range between any two time periods. Within this time range, the beam current is moderate, so that the area near the thinning position will not be damaged due to excessive beam current, and the thinning efficiency will not be too low due to too small beam current.

[0119] In some embodiments, in the above step X203, in the second thinning process, the single thinning thickness is 10 μm to 100 μm, and in an exemplary embodiment, it can be 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, etc., a typical but non-limiting thickness or a range between any two thicknesses. Within this subtracted thickness range, the single thinning thickness is the spacing between adjacent hardness pits.

[0120] In some specific embodiments, in the above step X2, the EBSD data includes grain size, grain boundary characterization and phase distribution of the characterization surface.

[0121]

Step X3

[0122] In some embodiments, in the above step X3, CHANNEL 5 is used to process the single-layer EBSD data to obtain the grain orientation distribution of the EBSD metal composite sample. In some embodiments, reconstruction software is used to process the multi-layer EBSD data to obtain the grain orientation distribution of the EBSD metal composite sample. In this case, CHANNEL 5 processes the single-layer EBSD data, and the reconstruction software is used to process the multi-layer EBSD data, and the grain orientation distribution of the EBSD metal composite sample can be obtained after processing.

[0123] CHANNEL 5 is an EBSD data processing software and a data analysis tool for electron backscatter diffraction (EBSD) technology.

[0124] In some specific embodiments, the reconstruction software includes Avizo software.

[0125] Avizo software is a comprehensive set of visualization tools that help people display, process and understand engineering science data. The powerful data processing functions and easy-to-use humanized graphical interface provided by Avizo can be used to process and obtain the three-dimensional data of EBSD metal composite samples.

[0126]

application

[0127] A fourth object of the present invention is to provide an EBSD metal composite sample characterization method, and its application in the field of metal composite material analysis.

[0128] The following describes the invention in conjunction with specific embodiments.

[0129] Example 1

[0130] This embodiment provides a method for preparing a steel-titanium composite sample, comprising the following steps:

[0131] (1) Several original samples with a size of 10 mm*10 mm*5 mm were cut from the steel-titanium composite material by wire cutting. The interface direction of the original sample was 45 degrees to the surface of the original sample.

[0132] (2) The wire cutting marks on the side of the sample were polished and mechanically polished, and then the sample was ultrasonically cleaned with anhydrous ethanol. The surface was polished for 3 minutes using 400-1200 sandpaper until the wire cutting marks were removed and the surface roughness was significantly reduced; the original sample was mechanically polished for 5 minutes using polishing paste until the surface was smooth without obvious scratches.

[0133] (3) The original sample surface was treated for 10 s using a xenon ion beam (first ion beam) with an energy of 30 kV, an intensity of 60 nA, and a penetration depth of 2 μm.

[0134] (4) A xenon ion beam (second ion beam) with an energy of 30 kV was used to thin the characterization surface for 45 minutes, and the intensity of the gallium ion beam was gradually reduced from 60 nA to 15 nA to 4 nA to 1 nA to 0.1 nA, and the thinning thickness was 20 μm. After the thinning treatment, a steel-titanium metal composite sample was obtained.

[0135] Example 2

[0136] This embodiment provides a method for preparing a steel-titanium composite sample, and the preparation steps are basically the same as those in Embodiment 1, except that:

[0137] The selected metal composite material is a 430 stainless steel-304 stainless steel composite material, and the EBSD metal composite sample prepared is a 430 stainless steel-304 stainless steel metal composite sample.

[0138] Example 3

[0139] This embodiment provides a method for preparing a steel-titanium composite sample, and the preparation steps are basically the same as those in Embodiment 1, except that:

[0140] The metal composite material selected is a titanium-steel-high entropy alloy metal composite material, and the EBSD metal composite sample prepared is a titanium-steel-high entropy alloy metal composite sample.

[0141] Comparative Example 1

[0142] In this comparative example, the steel-titanium metal composite material sample was treated with an electrolyte.

[0143] Comparative Example 2

[0144] In this comparative example, the 430 stainless steel-304 stainless steel metal composite material sample was treated with an electrolyte.

[0145] Comparative Example 3

[0146] In this comparative example, an electrolyte was used to treat a titanium-steel-high entropy alloy metal composite material sample.

[0147] In order to verify the progress of the embodiments of the present invention, the EBSD metal composite samples prepared by the preparation methods of the above embodiments 1 to 3 of the present invention and the metal composite samples obtained by electrolyte polishing in comparative examples 1 to 3 are subjected to EBSD characterization, and the characterization includes the following steps:

[0148] ① Obtain the EBSD metal composite samples prepared by the preparation methods of Examples 1 to 3 of the present invention and the metal composite samples obtained by electrolyte polishing in Comparative Examples 1 to 3 respectively.

[0149] ② Electron backscatter diffraction technology is used to obtain single-layer EBSD data of the characterization surface of the EBSD metal composite sample, as shown in Table 1 below.

[0150] ③Use CHANNEL 5 to process the single-layer EBSD data to obtain the grain orientation distribution of the EBSD metal composite sample, such as Figure 5 shown.

[0151] Table 1

[0152]

[0153]

[0154] According to Table 1 above and the instructions attached Figure 5 It can be seen that when the electrolyte is used to polish the composite metal sample in Comparative Examples 1 to 3, since the characterization surface contains at least two metals, and different metals have different applicability to different electrolytes and there is a problem of hard-soft matching between the two phases, the commonly used electrolyte cannot simultaneously complete the electrolytic polishing of the steel / titanium two phases and their interfaces. The EBSD resolution rate of the interface position of the sample to be characterized after electrolytic polishing is poor, and the EBSD resolution rate of the substrate on one side of the interface position is also poor. The composite metal sample prepared by the EBSD metal composite sample in the embodiment of the present invention adopts the method of ion thinning, which solves this problem well. The EBSD resolution rate of the interface position of the surface to be characterized of the prepared composite metal sample is good, and the EBSD resolution rate of the substrates on both sides of the interface position is also good, which more intuitively displays the grain distribution of the interface position and the substrates on both sides of the interface position.

[0155] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an EBSD metal composite sample, characterized in that: The preparation method comprises the following steps: Obtaining a plurality of original samples from a metal composite material comprising a first metal and a second metal; the characterization surface of the original samples comprising a characterization surface of the first metal, a characterization surface of the second metal, and a first cross section of an interface between the first metal and the second metal; After pre-treating the original sample, a plurality of hardness pits are set on the surface of the original sample; the surface of the original sample is perpendicular to the characterization surface and includes a second cross section of the interface, a surface of the first metal, and a surface of the second metal; After the original sample surface is treated by a first ion beam, a second ion beam is used to perform a first thinning treatment on the characterization surface to obtain an EBSD metal composite sample.

2. The method for preparing an EBSD metal composite sample according to claim 1, characterized in that: The first metal and the second metal are made of different materials, and the first metal includes one or more of steel, titanium, 430 stainless steel, 304 stainless steel, and high entropy alloy; And / or, the second metal is made of a material different from that of the first metal, and the material of the second metal includes one or more of steel, titanium, 430 stainless steel, 304 stainless steel, and a high entropy alloy.

3. The method for preparing an EBSD metal composite sample according to claim 1 or 2, characterized in that: The angle between the interface and the original sample surface is 30° to 60°; and / or, the energy of the first ion beam is 20 kV to 30 kV, the intensity is 60 nA to 200 nA, and the penetration depth is 0.2 μm to 2 μm; And / or, the ion type of the first ion beam includes at least one of a xenon ion beam and a gallium ion beam; and / or, the time for treating the surface of the original sample with the first ion beam is 2s to 20s; and / or, the energy of the second ion beam is 20 kV to 30 kV, the intensity is 0.1 nA to 60 nA, and the thinning thickness is 10 μm to 500 μm; And / or, the ion type of the second ion beam includes at least one of a xenon ion beam and a gallium ion beam; And / or, the first thinning treatment time is 30s to 60min.

4. An EBSD metal composite sample prepared by the method for preparing an EBSD metal composite sample according to any one of claims 1 to 3, characterized in that: The EBSD metal composite sample comprises at least one of the characterization surfaces and at least one of the original sample surfaces; At least one of the original samples comprises a plurality of hardness pits on its surface.

5. The EBSD metal composite sample according to claim 4, characterized in that: The arrangement direction of the plurality of hardness pits is parallel to the second cross section; and / or, the spacing between adjacent hardness pits is 10 μm to 500 μm; and / or, the spacings between adjacent hardness pits are equal; And / or, the diameter of the hardness pit is 3 μm to 6 μm or 50 μm to 200 μm.

6. The EBSD metal composite sample according to claim 5, characterized in that: The hardness pits are arranged in a row parallel to the second cross section, or in a matrix parallel to the second cross section; And / or, the original sample includes at least one of a steel-titanium composite metal, a 430 stainless steel-304 stainless steel composite metal, a steel-high entropy alloy composite metal, and a high entropy alloy-steel-titanium composite metal.

7. A method for characterizing metal composite samples by EBSD, characterized in that: The characterization method comprises the following steps: Obtaining an EBSD metal composite sample obtained by the method for preparing an EBSD metal composite sample according to any one of claims 1 to 3, or an EBSD metal composite sample according to any one of claims 5 to 6; Acquiring EBSD data of a characterization surface of the EBSD metal composite sample; The EBSD data are processed to obtain the grain orientation distribution of the EBSD metal composite sample.

8. The method for characterizing a metal composite sample by EBSD according to claim 7, characterized in that: The step of obtaining EBSD data of the characterization surface of the EBSD metal composite sample comprises: Electron backscatter diffraction technology is used to obtain single-layer EBSD data of the characterization surface of EBSD metal composite samples; Alternatively, the step of obtaining EBSD data of the characterization surface of the EBSD metal composite sample comprises: The first single-layer EBSD data of the characterization surface of the EBSD metal composite sample is obtained by using the electron backscatter diffraction technology; the second single-layer EBSD data is obtained after the characterization surface is subjected to a second thinning treatment by using a third ion beam; the second thinning treatment and the EBSD data acquisition steps are cyclically performed on the characterization surface to obtain multi-layer EBSD data.

9. The method for characterizing a metal composite sample by EBSD according to claim 7 or 8, characterized in that: Processing the single-layer EBSD data using CHANNEL 5 to obtain the grain orientation distribution of the EBSD metal composite sample; Or, using reconstruction software to process the multi-layer EBSD data to obtain the grain orientation distribution of the EBSD metal composite sample; and / or, the EBSD data includes grain size, grain boundary characterization and phase distribution of the characterization surface; And / or, the ion type of the third ion beam includes at least one of a xenon ion beam and a gallium ion beam; And / or, the energy of the third ion beam is 20 kV to 30 kV, the intensity is 0.1 nA to 60 nA, and the thinning thickness is 10 μm to 500 μm; And / or, the second thinning treatment time is 30s to 60min; and / or, in the second thinning process, the single thinning thickness is 10 μm to 100 μm; And / or, in the step of cyclically performing the second thinning treatment on the characterization surface and obtaining EBSD data, the number of cycles is 1 to 5 times.

10. Application of an EBSD metal composite sample characterization method in the field of metal composite material analysis.