Hard mask composition, hard mask layer, and method of forming pattern
By using a hard mask layer of a specific hard mask composition and solvent, the problem of insufficient etching resistance after pattern miniaturization in photolithography technology is solved, and fine etching and efficient pattern transfer are achieved.
Patent Information
- Application Number
- CN202410324218.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to form fine patterns with excellent contours using existing photolithography technology. Especially when patterns are miniaturized, the etching resistance of the hard mask layer is insufficient, affecting the etching effect.
This is accomplished by using a hard mask composition containing a specific compound and solvent, forming a hard mask layer through heat treatment, and exposing and developing the photoresist layer to selectively remove the hard mask layer to expose the material layer. Finely etched.
The etching resistance and heat resistance of the hard mask layer are improved, ensuring fine transfer of patterns and efficient etching, and solving the problems of insufficient photoresist pattern line width and etching resistance.
Smart Images

Figure CN118732399A_ABST
Abstract
Description
[0001] [CROSS-REFERENCE TO RELATED APPLICATIONS]
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2023-0040766 filed in the Korean Intellectual Property Office on March 28, 2023, the entire contents of which are incorporated herein by reference. Technical Field
[0003] Embodiments relate to a hard mask composition, a hard mask layer, and a method of forming a pattern. Background Art
[0004] Recently, the semiconductor industry has developed ultra-fine technology with patterns ranging from several nanometers to tens of nanometers in size. This ultra-fine technology can utilize photolithography technology.
[0005] Some photolithography techniques may include: providing a material layer on a semiconductor substrate; coating a photoresist layer on the material layer; exposing and developing the photoresist layer to provide a photoresist pattern; and etching the material layer using the photoresist pattern as a mask.
[0006] As the pattern to be formed is miniaturized, it may be difficult to provide a fine pattern with an excellent profile using only some photolithography techniques. Therefore, an auxiliary layer called a hard mask layer may be formed between the material layer and the photoresist layer to provide a fine pattern. Summary of the invention
[0007] The embodiment may be implemented by providing a hard mask composition, the hard mask composition including: a compound represented by Chemical Formula 1; and a solvent,
[0008] [Chemical formula 1]
[0009]
[0010] Wherein, in Chemical Formula 1, A 1 and A 2 are each independently a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a group in which a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group is linked via a single bond, a substituted or unsubstituted C1 to C5 alkylene group, or a combination thereof,
[0011] R 1 is a substituted or unsubstituted monovalent C1 to C30 saturated aliphatic hydrocarbon group, a substituted or unsubstituted monovalent C2 to C30 unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted monovalent C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group,
[0012] R 2is hydrogen, deuterium or substituted or unsubstituted C1 to C20 alkyl,
[0013] n is an integer from 1 to 6, and
[0014] If n is an integer of 2 or greater, then R 1 , R 2 and A 2 Each of them is the same or different from each other.
[0015] A in chemical formula 1 1 and A 2 The substituted or unsubstituted groups which may each independently be moieties of Group 1 are:
[0016] [Group 1]
[0017]
[0018] A in chemical formula 1 1 and A 2 The substituted or unsubstituted groups which may each independently be part of Group 1-1 are:
[0019] [Group 1-1]
[0020]
[0021] A in chemical formula 1 1 Any of the substituted or unsubstituted groups which may be part of Group 1-2:
[0022] [Group 1-2]
[0023]
[0024] A in chemical formula 1 2 Any substituted or unsubstituted group that may be part of Groups 1-3:
[0025] [Group 1-3]
[0026]
[0027] R in Formula 1 1 It may be a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, or a substituted or unsubstituted C6 to C20 aryl group.
[0028] R in Formula 1 2It may be hydrogen, deuterium, substituted or unsubstituted methyl, substituted or unsubstituted ethyl, substituted or unsubstituted propyl, substituted or unsubstituted butyl, or substituted or unsubstituted pentyl.
[0029] In Chemical Formula 1, R 1 may be a substituted or unsubstituted C1 to C20 alkyl group or a substituted or unsubstituted C6 to C20 aryl group, R 2 It may be hydrogen, deuterium, a substituted or unsubstituted methyl group, or a substituted or unsubstituted ethyl group, and n may be an integer of 1 to 3.
[0030] In Chemical Formula 1, n may be 2 or 3, and R 1 , R 2 and A 2 Can all be the same.
[0031] In Chemical Formula 1, R 1 may be a substituted or unsubstituted C1 to C10 alkyl group, R 2 It can be hydrogen or deuterium, and n can be 2.
[0032] The compound represented by Chemical Formula 1 may be represented by one of Chemical Formulas 2 to 4:
[0033] [Chemical formula 2]
[0034]
[0035] [Chemical formula 3]
[0036]
[0037] [Chemical formula 4]
[0038]
[0039] In Chemical Formulae 2 to 4, R 1 may be a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, or a substituted or unsubstituted C6 to C20 aryl group,
[0040] R 2 may be hydrogen, deuterium, or a substituted or unsubstituted C1 to C10 alkyl group,
[0041] X 1 and X 2 may each independently be deuterium, a hydroxyl group, a halogen atom, a thiol group, a substituted or unsubstituted C1 to C10 alkoxy group, or a substituted or unsubstituted C1 to C10 alkyl group,
[0042] n can be an integer from 1 to 3, and
[0043] m1 and m2 may each independently be an integer from 0 to 5.
[0044] The compound represented by Chemical Formula 1 may be represented by any one of Chemical Formulas 5 to 10:
[0045] [Chemical formula 5]
[0046]
[0047] [Chemical formula 6]
[0048]
[0049] [Chemical formula 7]
[0050]
[0051] [Chemical formula 8]
[0052]
[0053] [Chemical formula 9]
[0054]
[0055] [Chemical formula 10]
[0056]
[0057] The compound may have a molecular weight of about 500 g / mol to about 10,000 g / mol.
[0058] The compound may be included in an amount of about 0.1 weight percent (wt %) to about 30 wt % based on the total weight of the hardmask composition.
[0059] The solvent may include propylene glycol, propylene glycol diacetate, methoxypropylene glycol, diethylene glycol, diethylene glycol butyl ether, triethylene glycol monomethyl ether, propylene glycol monomethyl ether (PGME), propylene glycol monomethylether acetate (PGMEA), cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, acetylacetone or ethyl 3-ethoxypropionate.
[0060] Embodiments may be implemented by providing a hard mask layer including a cured product of the hard mask composition according to embodiments.
[0061] An embodiment can be implemented by providing a method for forming a pattern, the method comprising: providing a material layer on a substrate; applying a hard mask composition according to an embodiment to the material layer to form a hard mask layer; thermally treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer; and etching the exposed part of the material layer.
[0062] Forming the hard mask layer may include performing a heat treatment at about 100° C. to about 1,000° C. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] Various features will become apparent to those skilled in the art by describing in detail exemplary embodiments with reference to the accompanying drawings, in which:
[0064] Figure 1 Reference graphs illustrating a level difference of a hard mask layer are shown to explain a method of evaluating a planarization characteristic and a calculation formula for evaluating the planarization characteristic. DETAILED DESCRIPTION
[0065] Exemplary embodiments will now be described more fully hereinafter with reference to the accompanying drawings; however, the embodiments may be implemented in different forms and should not be construed as limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete and will fully convey exemplary implementations to those skilled in the art.
[0066] In the figures, the dimensions of layers and regions may be exaggerated for clarity of illustration. It is also understood that when a layer or substrate is referred to as being "on" another layer or substrate, the layer or substrate may be directly on the other layer or substrate, or there may be intervening layers. Furthermore, it is understood that when a layer is referred to as being "below" another layer, the layer may be directly below the other layer, and there may also be one or more intervening layers. In addition, it is also understood that when a layer is referred to as being "between" two layers, the layer may be the only layer between the two layers, or there may also be one or more intervening layers. The same reference numbers refer to the same elements throughout.
[0067] When no definition is otherwise provided, "substituted" as used herein may refer to a hydrogen atom of a compound being replaced by a substituent selected from the group consisting of a halogen atom (F, Br, Cl, or I), a hydroxyl group, an alkoxy group, a nitro group, a cyano group, an amino group, an azido group, an amidino group, a hydrazine group, a hydrazo group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphate group or a salt thereof, a vinyl group, a C1 to C20 alkyl group, a C2 to C20 alkenyl group, a C2 to C20 alkynyl group, a C6 to C30 aryl group, a C7 to C30 arylalkyl group, a C9 to C30 allylaryl group, a C1 to C30 alkoxy group, a C1 to C20 heteroalkyl group, a C3 to C20 heteroarylalkyl group, a C3 to C30 cycloalkyl group, a C3 to C15 cycloalkenyl group, a C6 to C15 cycloalkynyl group, a C3 to C30 heterocycloalkyl group, or a combination thereof. As used herein, hydrogen substitution (—H) may include deuterium substitution (—D) or tritium substitution (—T). For example, any hydrogen in any compound described herein may be protium, deuterium, or tritium (e.g., based on natural substitution or artificial substitution). As used herein, the term “or” is not necessarily an exclusive term, for example, “A or B” will include A, B, or A and B.
[0068] In addition, two adjacent substituents among a substituted halogen atom (F, Br, Cl, or I), a hydroxyl group, a nitro group, a cyano group, an amino group, an azido group, an amidino group, a hydrazine group, a hydrazone group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphoric acid group or a salt thereof, a C1 to C30 alkyl group, a C2 to C30 alkenyl group, a C2 to C30 alkynyl group, a C6 to C30 aryl group, a C7 to C30 arylalkyl group, a C1 to C30 alkoxy group, a C1 to C20 heteroalkyl group, a C3 to C20 heteroarylalkyl group, a C3 to C30 cycloalkyl group, a C3 to C15 cycloalkenyl group, a C6 to C15 cycloalkynyl group, a C2 to C30 heterocyclyl group may be condensed to form a ring.
[0069] When no definition is otherwise provided, the "aromatic hydrocarbon" used herein refers to a group having one or more hydrocarbon aromatic moieties (including a form in which the hydrocarbon aromatic moieties are linked by a single bond, a non-aromatic fused ring form in which the hydrocarbon aromatic moieties are directly or indirectly fused, or a combination thereof) as well as a non-fused aromatic hydrocarbon ring, a fused aromatic hydrocarbon ring.
[0070] More specifically, the substituted or unsubstituted aromatic hydrocarbon group may be a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthrenyl group, a substituted or unsubstituted fused tetraphenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted terphenyl group, a substituted or unsubstituted quaterphenyl group, a substituted or unsubstituted chrysenyl group, a substituted or unsubstituted triphenylenyl group, a substituted or unsubstituted peryl group, a substituted or unsubstituted indenyl group, a combination thereof, or a fused ring of a combination of the foregoing groups.
[0071] The polymer used herein may include both oligomers and polymers.
[0072] Unless otherwise specified in this specification, the “molecular weight” is measured by dissolving a powder sample in tetrahydrofuran (THF) and then using Agilent Technologies' 1200 series Gel Permeation Chromatography (GPC) (column is Shodex Company LF-804, standard sample is Showa Company polystyrene).
[0073] The hard mask composition according to some embodiments may include, for example, a compound represented by Chemical Formula 1 and a solvent.
[0074] [Chemical formula 1]
[0075]
[0076] In chemical formula 1, A 1 and A 2 Each may independently be or include, for example, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a group in which a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group may be linked via a single bond, a substituted or unsubstituted C1 to C5 alkylene group, or a combination thereof.
[0077] R 1 It may be or may include, for example, a substituted or unsubstituted monovalent C1 to C30 saturated aliphatic hydrocarbon group, a substituted or unsubstituted monovalent C2 to C30 unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted monovalent C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group.
[0078] R 2 It may be or may include, for example, hydrogen, deuterium, or a substituted or unsubstituted C1 to C20 alkyl group.
[0079] n can be an integer from 1 to 6.
[0080] In an embodiment, if n is an integer of 2 or greater, then R 1 , R 2 and A 2 Each of can be the same as or different from each other.
[0081] As shown in Chemical Formula 1, the compound according to the embodiment may include a quaternary carbon and an aromatic hydrocarbon group, a saturated or unsaturated aliphatic hydrocarbon group, or a saturated or unsaturated alicyclic hydrocarbon group or the like directly linked to the quaternary carbon, thereby increasing the carbon content in the compound, and thus increasing the carbon content in the hard mask composition and helping to improve the etching resistance of the hard mask layer formed therefrom.
[0082] In addition, the compound according to the embodiment may include a quaternary carbon, and a hydroxyl group or an alkoxy group may be linked to the quaternary carbon, so that the solubility of the compound in a solvent can be improved, and a hard mask composition including the compound can be effectively applied to a spin-on coating process. In addition, the hydroxyl group or the alkoxy group may contribute to the cross-linking between the compounds, and thus the composition including the compound may exhibit excellent cross-linking characteristics. In addition, since the compound may be cross-linked into a high molecular weight polymer form in a short period of time during heat treatment, a hard mask layer formed therefrom may have excellent heat resistance and excellent etching resistance.
[0083] In an embodiment, A of Chemical Formula 1 1 and A 2 Each may independently be a substituted or unsubstituted group such as a part of Group 1.
[0084] [Group 1]
[0085]
[0086] In an embodiment, A in Chemical Formula 1 1 and A 2 Each may independently be a substituted or unsubstituted group such as a part of Group 1-1.
[0087] [Group 1-1]
[0088]
[0089] In an embodiment, A in Chemical Formula 1 1 A may be a substituted or unsubstituted group such as a moiety of Group 1-2 (such as benzene, naphthalene, anthracene, phenanthrene, pyrene, or coronene). 1It may be, for example, benzene, pyrene or coronene.
[0090] [Group 1-2]
[0091]
[0092] In an embodiment, A of Chemical Formula 1 2 A may be a substituted or unsubstituted group such as a moiety of Groups 1-3 (such as benzene, naphthalene, anthracene, phenanthrene, or pyrene). 2 It may be, for example, benzene or pyrene.
[0093] [Group 1-3]
[0094]
[0095] In an embodiment, R in Chemical Formula 1 1 It may be, for example, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, or a substituted or unsubstituted C6 to C20 aryl group. In an embodiment, Chemical Formula 1 may be, for example, a substituted or unsubstituted C1 to C20 alkyl group or a substituted or unsubstituted C6 to C20 aryl group. In an embodiment, Chemical Formula 1 may be, for example, a substituted or unsubstituted C1 to C10 alkyl group.
[0096] In an embodiment, if R in Chemical Formula 1 1 With the substituents listed above instead of hydrogen, the carbon content of compounds according to some embodiments can be maximized.
[0097] R in Formula 1 2 It may be, for example, hydrogen, deuterium, or a substituted or unsubstituted C1 to C10 alkyl group. 2 It may be, for example, hydrogen, deuterium, substituted or unsubstituted methyl, substituted or unsubstituted ethyl, substituted or unsubstituted propyl, substituted or unsubstituted butyl, or substituted or unsubstituted pentyl, such as hydrogen, deuterium, substituted or unsubstituted methyl, or substituted or unsubstituted ethyl. In an embodiment, R in Formula 1 2 It may be, for example, hydrogen or deuterium.
[0098] In Chemical Formula 1, n may be an integer of 1 to 6, for example, an integer of 1 to 3. In an embodiment, n may be 2 or 3, for example, n may be 2. If n in Chemical Formula 1 is 2, the solubility of the compound according to some embodiments in a solvent may be optimized, and the etching resistance of a hard mask layer formed from a hard mask composition including the compound may be maximized.
[0099] In an embodiment, if n in Chemical Formula 1 is an integer of 2 or greater, R 1 , R 2 and A 2 Each of R may be the same as or different from each other. In an embodiment, if n is 2 or greater, two or more R 1 Each of R may be the same or different from each other, and two or more R 2 Each of A may be the same or different from each other, and two or more A 2 Each of can be the same as or different from each other.
[0100] In an embodiment, the compound represented by Chemical Formula 1 may be represented by one of Chemical Formulas 2 to 4, for example.
[0101] [Chemical formula 2]
[0102]
[0103] [Chemical formula 3]
[0104]
[0105] [Chemical formula 4]
[0106]
[0107] In Chemical Formulae 2 to 4, R 1 For example, it may be a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, or a substituted or unsubstituted C6 to C20 aryl group.
[0108] R 2 It may be, for example, hydrogen, deuterium, or a substituted or unsubstituted C1 to C10 alkyl group.
[0109] X 1 and X 2 Each independently may be, for example, deuterium, a hydroxyl group, a halogen atom, a thiol group, a substituted or unsubstituted C1-C10 alkoxy group, or a substituted or unsubstituted C1-C10 alkyl group.
[0110] n can be an integer from 1 to 3.
[0111] m1 and m2 may each independently be an integer from 0 to 5.
[0112] In an embodiment, the compound represented by Chemical Formula 1 may be represented by, for example, one of Chemical Formulas 5 to 10.
[0113] [Chemical formula 5]
[0114]
[0115] [Chemical formula 6]
[0116]
[0117] [Chemical formula 7]
[0118]
[0119] [Chemical formula 8]
[0120]
[0121] [Chemical formula 9]
[0122]
[0123] [Chemical formula 10]
[0124]
[0125] The compound may have a molecular weight of, for example, about 500 g / mol to about 10,000 g / mol. In an embodiment, the compound may have a molecular weight of about 500 g / mol to about 9,500 g / mol, about 500 g / mol to about 9,000 g / mol, about 600 g / mol to about 8,500 g / mol, about 600 g / mol to about 8,000 g / mol, about 700 g / mol to about 7,500 g / mol, about 700 g / mol to about 7,000 g / mol. By having a molecular weight within the above range, the carbon content and solubility in a solvent of a hard mask composition including the above compound may be adjusted and optimized.
[0126] The compound may be included in an amount of about 0.1 wt % to about 30 wt % based on the total weight of the hard mask composition. In an embodiment, the compound may be included in an amount of about 0.2 wt % to about 30 wt %, about 0.5 wt % to about 30 wt %, about 1 wt % to about 30 wt %, about 1 wt % to about 25 wt %, or about 1 wt % to about 20 wt %. By including the compound within the above range, the thickness, surface roughness, and planarization degree of the hard mask may be easily adjusted.
[0127] The hard mask composition may include a solvent. In an embodiment, the solvent may include propylene glycol, propylene glycol diacetate, methoxypropylene glycol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methyl pyrrolidone, acetylacetone, ethyl 3-ethoxypropionate, or a similar solvent. In an embodiment, the solvent may include a suitable solvent having sufficient solubility or dispersibility for the compound.
[0128] The hard mask composition may further include additives such as a surfactant, a cross-linking agent, a thermal acid generator, or a plasticizer.
[0129] The surfactant may include, for example, a fluoroalkyl compound, an alkylbenzenesulfonate, an alkylpyridinium salt, polyethylene glycol, a quaternary ammonium salt, or the like.
[0130] The crosslinking agent may include, for example, melamine, substituted urea or a polymer crosslinking agent. In an embodiment, the crosslinking agent may be a crosslinking agent having at least two crosslinking substituents, such as methoxymethylated glycouryl, butoxymethylated glycoluryl, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea or butoxymethylated thiourea.
[0131] In an embodiment, as the crosslinking agent, a crosslinking agent having high heat resistance may be used. The crosslinking agent having high heat resistance may include a compound having a crosslinking substituent having an aromatic ring (eg, a benzene ring or a naphthalene ring) in a molecule.
[0132] The thermal acid generator may include, for example, acid compounds (e.g., p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonic acid, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, hydroxybenzoic acid, naphthoic acid) or 2,4,4,6-tetrabromocyclohexadienonone, benzoin tosylate, 2-nitrobenzyl tosylate and other organic sulfonic acid alkyl esters.
[0133] According to some embodiments, a hard mask layer including a cured product of the aforementioned hard mask composition may be provided.
[0134] Hereinafter, a method of forming a pattern using the aforementioned hard mask composition is described.
[0135] According to some embodiments, the method of forming a pattern may include: providing a material layer on a substrate; applying a hard mask composition comprising the aforementioned compound and a solvent to the material layer; thermally treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer; and etching the exposed portion of the material layer.
[0136] The substrate may be, for example, a silicon wafer, a glass substrate, or a polymer substrate. The material layer may be a material to be finally patterned, such as a metal layer (e.g., an aluminum layer or a copper layer), a semiconductor layer (e.g., a silicon layer), or an insulating layer (e.g., a silicon oxide layer or a silicon nitride layer). The material layer may be formed by a method such as a chemical vapor deposition (CVD) process.
[0137] The hard mask composition may be the same as described above and may be applied by spin coating in the form of a solution. In an embodiment, the hard mask composition may be applied to a thickness of, for example, about To date
[0138] The hard mask composition may be thermally treated at, for example, about 100° C. to about 1,000° C. for about 10 seconds to about 1 hour. In an embodiment, the thermal treatment of the hard mask composition may include a plurality of thermal treatment processes, such as a first thermal treatment process and a second thermal treatment process.
[0139] In an embodiment, the heat treatment of the hard mask composition may include, for example, performing a heat treatment process at about 100° C. to about 1,000° C. for about 10 seconds to about 1 hour. In an implementation, the heat treatment may be performed in an air or nitrogen atmosphere or in an atmosphere having an oxygen concentration of 1 wt % or less.
[0140] In an embodiment, the heat treatment of the hard mask composition may include, for example, a first heat treatment process, which is performed at about 100°C to about 1,000°C, about 100°C to about 800°C, about 100°C to about 500°C, or about 150°C to about 400°C for, for example, about 30 seconds to about 1 hour, about 30 seconds to about 30 minutes, about 30 seconds to about 10 minutes, or about 30 seconds to about 5 minutes.
[0141] In an embodiment, the heat treatment of the hard mask composition may include, for example, a second heat treatment process, which is continuously performed at about 100° C. to 1,000° C., about 300° C. to about 1,000° C., about 500° C. to about 1,000° C., about 500° C. to about 600° C. for, for example, about 30 seconds to about 1 hour, about 30 seconds to about 30 minutes, about 30 seconds to about 10 minutes, about 30 seconds to about 5 minutes. In an embodiment, the first heat treatment process and the second heat treatment process may be performed in an air or nitrogen atmosphere, or may be performed in an atmosphere having an oxygen concentration of 1 wt % or less.
[0142] By performing at least one of the steps of heat-treating the hard mask composition at a high temperature, for example, 200° C. or higher, high etching resistance capable of withstanding etching gas and chemical liquid exposed in subsequent processes including an etching process may be exhibited.
[0143] In an embodiment, the formation of the hard mask layer may include an ultraviolet (UV) / visible light (Vis) curing process or a near infrared ray (IR) curing process.
[0144] In an implementation, the formation of the hard mask layer may include a first heat treatment process, a second heat treatment process, a UV / Vis curing process, or a near IR curing process, or may include two or more processes in succession.
[0145] In an embodiment, the method may further include forming a silicon-containing thin layer on the hard mask layer. The silicon-containing thin layer may be formed of, for example, SiCN, SiOC, SiON, SiOCN, SiC, SiO, SiN, or similar materials.
[0146] In an embodiment, the method may further include: before forming the photoresist layer, forming a bottom antireflective coating (BARC) on the silicon-containing thin layer or on the hard mask layer.
[0147] In an embodiment, the exposure of the photoresist layer may be performed using, for example, ArF, KrF, or extreme ultraviolet (EUV). After the exposure, a heat treatment may be performed at about 100° C. to about 700° C.
[0148] In an embodiment, the etching process of the exposed portion of the material layer may be performed by a dry etching process using an etching gas, and the etching gas may be, for example, N2 / O2, CHF3, CF4, Cl2, BCl3 or a mixed gas thereof.
[0149] The etched material layer may be formed into a plurality of patterns, and the plurality of patterns may include metal patterns, semiconductor patterns, insulating patterns, or the like, such as various patterns of semiconductor integrated circuit devices.
[0150] The following examples and comparative examples are provided to highlight the characteristics of one or more embodiments, but it should be understood that the examples and comparative examples should not be interpreted as limiting the scope of the embodiments, and the comparative examples should not be interpreted as exceeding the scope of the embodiments. In addition, it should be understood that the embodiments are not limited to the specific details set forth in the examples and comparative examples.
[0151] Synthesis of compounds
[0152] Synthesis example 1
[0153] First process: Friedel-Craft Acylation Reaction
[0154] 9.48 g (0.05 mol) of pyrene, 25.00 g (0.09 mol) of pyrene carboxylic acid chloride and 237.92 g of 1,2-dichloroethane were added to a flask to prepare a solution. 25.00 g (0.19 mol) of aluminum chloride was slowly added to the solution, and then stirred at ambient temperature for 10 hours. When the reaction was completed, methanol was added thereto, and the precipitate formed therein was filtered to obtain bis (pyrenylcarbonyl) pyrene.
[0155] Second process: Grignard reaction
[0156] 30.00 g (0.05 mol) of the obtained bis (pyrenylcarbonyl) pyrene and 235.73 g of tetrahydrofuran were added to a flask to prepare a solution. Subsequently, 21.74 g (0.18 mol) of methylmagnesium bromide was slowly added to the solution at ambient temperature, and then stirred at 60° C. for 4 hours. When the reaction was completed, the resultant was neutralized to about pH 7 using a 1% aqueous hydrogen chloride solution. Subsequently, compound A represented by Chemical Formula 5 was obtained by extraction with ethyl acetate.
[0157] [Chemical formula 5]
[0158]
[0159] Synthesis example 2
[0160] Compound B represented by Chemical Formula 6 was obtained in the same manner as in Synthesis Example 1, except that 26.83 g (0.18 mol) of propylmagnesium bromide was used instead of 21.74 g (0.18 mol) of methylmagnesium bromide in the second process.
[0161] [Chemical formula 6]
[0162]
[0163] Synthesis example 3
[0164] First process: Friedel-Crafts acylation
[0165] 10.73 g (0.05 mol) of 4-methoxypyrene, 24.76 g (0.09 mol) of pyrenecarbonyl chloride and 239.88 g of 1,2-dichloroethane were added to a flask to prepare a solution. 24.63 g (0.18 mol) of aluminum chloride was slowly added to the solution, and then stirred at ambient temperature for 4 hours. When the reaction was completed, methanol was added thereto, and the precipitate formed therein was filtered to obtain bis (pyrenylcarbonyl) methoxypyrene.
[0166] Second process: Demethylation Reaction
[0167] 28.00 g (0.04 mol) of the obtained bis(pyrenylcarbonyl)methoxypyrene, 24.68 g (0.12 mol) of 1-dodecanethiol, 9.12 g (0.16 mol) of potassium hydroxide and 247.20 g of N,N-dimethylformamide were added to a flask, and then stirred at 90° C. for 6 hours. After stirring, the resultant was cooled, and then neutralized to about pH 7 with a 1% aqueous hydrogen chloride solution, and the precipitate formed therein was filtered to obtain bis(pyrenylcarbonyl)hydroxypyrene.
[0168] The third process: Grignard reaction
[0169] 26.02 g (0.04 mol) of the obtained bis (pyrenylcarbonyl) hydroxypyrene and 240.00 g of tetrahydrofuran were added to a flask to prepare a solution. 33.96 g (0.23 mol) of propylmagnesium bromide were slowly added thereto at ambient temperature, and then heated to 60° C. and stirred for 12 hours. When the reaction was completed, the resultant was neutralized to about pH 7 using a 1% aqueous solution of hydrogen chloride. Subsequently, compound C represented by chemical formula 7 was obtained by extraction with ethyl acetate.
[0170] [Chemical formula 7]
[0171]
[0172] Synthesis example 4
[0173] Compound D represented by Chemical Formula 8 was obtained in the same manner as in Synthesis Example 1, except that 26.83 g (0.18 mol) of isopropylmagnesium bromide was used instead of 21.74 g (0.18 mol) of methylmagnesium bromide in the second process.
[0174] [Chemical formula 8]
[0175]
[0176] Synthesis example 5
[0177] First process: Friedel-Crafts acylation
[0178] 20.60 g (0.10 mol) of terephthaloyl chloride, 47.00 g (0.20 mol) of 4-methoxypyrene and 221.00 g of 1,2-dichloroethane were added to a flask to prepare a solution. 27.00 g (0.20 mol) of aluminum chloride was slowly added thereto, and then stirred at an ambient temperature of 60° C. for 8 hours. When the reaction was completed, methanol was added to the solution, and the precipitate formed therein was filtered to obtain bis (methoxypyrenylcarbonyl) benzene.
[0179] Second process: demethylation reaction
[0180] 53.50 g (0.09 mol) of bis(methoxypyrenylcarbonyl)benzene, 91.10 g (0.45 mol) of 1-dodecanethiol, 30.30 g (0.54 mol) of potassium hydroxide and 262.00 g of N,N-dimethylformamide were added to a flask, and then stirred at 120° C. for 8 hours. After stirring, the resultant was cooled, and then neutralized to about pH 7 using a 1% aqueous hydrogen chloride solution, and the precipitate formed therein was filtered to obtain bis(hydroxypyrenylcarbonyl)benzene.
[0181] The third process: Grignard reaction
[0182] 18.44 g (0.03 mol) of the obtained bis (hydroxypyrenylcarbonyl) benzene and 258.87 g of tetrahydrofuran were added to a flask to prepare a solution. 38.89 g (0.26 mol) of propylmagnesium bromide was slowly added thereto at ambient temperature, and then heated to 60° C. and stirred for 12 hours. When the reaction was completed, the resultant was neutralized to about pH 7 using a 1% aqueous solution of hydrogen chloride, and compound E represented by chemical formula 9-1 was obtained by extraction with ethyl acetate.
[0183] [Chemical formula 9-1]
[0184]
[0185] Synthesis example 6
[0186] First process: Friedel-Crafts acylation
[0187] 50.00 g (0.17 mol) of coronene, 56.80 g (0.34 mol) of 4-methoxybenzoyl chloride and 353.00 g of 1,2-dichloroethane were added to a flask to prepare a solution. 44.4 g (0.34 mol) of aluminum chloride was slowly added to the solution at ambient temperature, and then heated to 60° C. and stirred for 8 hours. When the reaction was completed, methanol was added thereto, and the precipitate formed therein was filtered to obtain bis (methoxybenzoyl) coronene.
[0188] Second process: demethylation reaction
[0189] 50.00 g (0.88 mol) of the obtained bis (methoxybenzoyl) coronene, 89.00 g (0.44 mol) of 1-dodecanethiol, 29.60 g (0.53 mol) of potassium hydroxide and 253.00 g of N, N-dimethylformamide were added to a flask, and then stirred at 120° C. for 8 hours. After stirring, the resultant was cooled, and then neutralized to about pH 7 with a 1% aqueous hydrogen chloride solution, and the precipitate formed therein was filtered to obtain bis (hydroxybenzoyl) coronene.
[0190] The third process: Grignard reaction
[0191] 17.86 g (0.03 mol) of the obtained bis (hydroxybenzoyl) coronene and 258.87 g of tetrahydrofuran were added to a flask to prepare a solution. 38.97 g (0.26 mol) of propylmagnesium bromide was slowly added thereto at ambient temperature, and then heated to 60° C. for 12 hours. When the reaction was completed, the resultant was neutralized to about pH 7 using a 1% aqueous hydrogen chloride solution, and compound F represented by Chemical Formula 10-1 was obtained by extraction with ethyl acetate.
[0192] [Chemical formula 10-1]
[0193]
[0194] Comparative Synthesis Example
[0195] First process: Friedel-Crafts acylation
[0196] 50.0 g (0.166 mol) of coronene, 56.8 g (0.333 mol) of 4-methoxybenzoyl chloride and 353 g of 1,2-dichloroethane were added to a flask to prepare a solution. 44.4 g (0.333 mol) of aluminum chloride was slowly added to the solution at ambient temperature, and then stirred at 60° C. for 8 hours. When the reaction was completed, methanol was added thereto, and the precipitate formed therein was filtered to obtain disubstituted 4-methoxybenzoyl coronene.
[0197] Second process: demethylation reaction
[0198] 50.0 g (0.880 mol) of the obtained disubstituted 4-methoxybenzoyl coronene, 89.0 g (0.440 mol) of 1-dodecanethiol, 29.6 g (0.528 mol) of potassium hydroxide and 53 g of N,N-dimethylformamide were added to a flask, and then stirred at 120° C. for 8 hours. After stirring, the resultant was cooled, neutralized to about pH 7 using a 10% aqueous hydrogen chloride solution, and then extracted with ethyl acetate to obtain disubstituted 4-hydroxybenzoyl coronene.
[0199] The third process: reduction reaction
[0200] 25.0 g (0.0463 mol) of the obtained disubstituted 4-hydroxybenzoyl coronene and 170 g of tetrahydrofuran were added to a flask to prepare a solution. 17.5 g (0.463 mol) of a sodium borohydride aqueous solution was slowly added thereto, and then stirred at ambient temperature for 24 hours. When the reaction was completed, the resultant was neutralized to about pH 7 using a 10% aqueous hydrogen chloride solution, and then extracted with ethyl acetate to obtain a compound G represented by Chemical Formula 11.
[0201] [Chemical formula 11]
[0202]
[0203] Preparation of hard mask composition
[0204] Examples and Comparative Examples
[0205] Each of Compounds A to G according to Synthesis Examples 1 to 6 and Comparative Synthesis Examples was uniformly dissolved in a mixed solvent of propylene glycol monomethyl ether acetate (PGMEA) and cyclohexanone at a volume ratio of 3:7 to prepare a hard mask composition having a compound content of 10.0 wt %.
[0206] Evaluation 1: Heat resistance evaluation
[0207] Each of the hard mask compositions of Examples 1 to 6 and the comparative examples was spin-coated on a silicon wafer and then heat-treated on a hot plate at 160°C for 1 minute to form a hard mask layer. The thickness of the hard mask layer was measured using a film thickness meter made by K-MAC Co., Ltd. Subsequently, the hard mask layer was reheat-treated at 400°C for 2 minutes to remeasure the thickness of the hard mask layer. When the thickness change rate of the hard mask layer before and after reheat treatment at 400°C for 2 minutes is less than 5%, "A" (very good) is given, when the thickness change rate is greater than or equal to 5% and less than 10%, "B" (good) is given, and when the thickness change rate is greater than or equal to 10%, "C" (poor) is given. The results are shown in Table 1.
[0208] [Table 1]
[0209] Heat resistance Example 1 A Example 2 A Example 3 A Example 4 A Example 5 A Example 6 A Comparative Example C
[0210] Referring to Table 1, the hard mask layers formed from the compositions of Examples 1 to 6 exhibited a thickness change rate of less than 5% before and after the reheat treatment, and the hard mask layers formed from the compositions according to the comparative examples exhibited a thickness change rate of greater than or equal to 10% before and after the reheat treatment. In other words, the hard mask layers formed from the compositions of Examples 1 to 6 exhibited excellent heat resistance compared to the hard mask layers formed from the compositions according to the comparative examples.
[0211] Evaluation 2: Gap-fill characteristics
[0212] Each of the hard mask compositions of Examples 1 to 6 and the comparative example was spin-coated on a patterned silicon wafer and then heat-treated at 400° C. for 60 seconds to form a hard mask layer. A pattern cross-sectional image of the hard mask layer was examined using a field emission scanning electron microscope (FE-SEM) to check whether voids occurred. The results are shown in Table 2.
[0213] [Table 2]
[0214] Is there a gap? Example 1 No gaps appear Example 2 No gaps appear Example 3 No gaps appear Example 4 No gaps appear Example 5 No gaps appear Example 6 No gaps appear Comparative Example A gap appeared
[0215] Referring to Table 2, the hard mask layers formed from the hard mask compositions of Examples 1 to 6 did not exhibit voids, but the hard mask layers formed from the hard mask compositions of the comparative examples exhibited voids. Therefore, the hard mask layers formed from the hard mask compositions of Examples 1 to 6 exhibited more excellent gap filling properties than the hard mask layers formed from the hard mask compositions of the comparative examples.
[0216] Evaluation 3: Planarization characteristics
[0217] Each of the hard mask compositions of Examples 1 to 6 and the comparative example was spin-coated on a patterned silicon wafer, and heat-treated at 400° C. for 60 seconds, and its pattern cross-sectional image was examined by a field emission scanning electron microscope (FE-SEM). The thickness h1 and the thickness h2 of the hard mask layer shown in the pattern cross-sectional image were measured, and the thickness was used to calculate the thickness according to Figure 1 The calculation equation 1 of digitizes the planarization degree. The ratio of the planarization degree of the hard mask layer formed by each of the compositions according to Examples 1 to 6 to the planarization degree of the hard mask layer formed by the composition according to the comparative example was calculated to evaluate the planarization characteristics. If the ratio is less than 5%, "A" (very good) is given, if the ratio is greater than or equal to 5% and less than 10%, "B" (good) is given, and if the ratio is greater than or equal to 10%, "C" (poor) is given. The results are shown in Table 3.
[0218] [Table 3]
[0219] Planarization characteristics Example 1 A Example 2 A Example 3 A Example 4 A Example 5 A Example 6 A Comparative Example -
[0220] Evaluation 4: Etching resistance
[0221] Each of the hard mask compositions of Examples 1 to 6 and the comparative example was spin-coated on a silicon wafer, and then heat-treated on a hot plate at 160° C. for 1 minute to form a hard mask layer. The hard mask layer was dry-etched for 30 seconds using a CF4 / Ar mixed gas, and then the hard mask thickness before and after etching was measured using a film thickness meter made by Komei Co., Ltd. to calculate the etching rate. Herein, the etching resistance is evaluated using the ratio of the etching rate of the hard mask layer formed by each of the compositions of Examples 1 to 6 to the etching rate of the hard mask layer formed by the composition of the comparative example. If the ratio is less than 0.95, "A" (very good) is given, if the ratio is greater than or equal to 0.95 and less than 1.00, "B" (good) is given, and if the ratio is greater than or equal to 1.00, "C" (poor) is given. The results are shown in Table 4.
[0222] [Table 4]
[0223] Etching resistance Example 1 A Example 2 A Example 3 A Example 4 A Example 5 A Example 6 A Comparative Example -
[0224] Referring to Table 4, the hard mask layer formed from the composition of the comparative example exhibited an etching rate of 0.95 compared to the etching rate of the hard mask layer formed from each of the compositions of Examples 1 to 6. Therefore, the hard mask layer formed from the compositions of Examples 1 to 6 exhibited excellent etching resistance compared to the hard mask layer formed from the composition of the comparative example.
[0225] In summary, there is a continuous trend to reduce chip size in the semiconductor industry. For this reason, the line width of the photoresist pattern in the photolithography technology must have a size of tens of nanometers. Therefore, the height of the line width that can withstand the photoresist pattern may be limited, and there are situations where the photoresist does not have sufficient resistance in the etching step. In order to compensate for this, an auxiliary layer that can be called a hard mask layer can be used between the material layer to be etched and the photoresist layer. Such a hard mask layer can be used as an interlayer (interlayer) for transferring the fine pattern of the photoresist layer by selective etching. Therefore, the hard mask layer may need to have sufficient etching resistance to withstand the etching process during the pattern transfer.
[0226] Some hard mask layers can be formed by chemical or physical deposition methods, and may have low economic efficiency due to large-scale equipment and high process costs. Therefore, spin coating techniques for forming hard mask layers have recently been developed. Spin coating techniques may be a process that is easier to perform than some other methods, and a hard mask layer formed according to the spin coating technique may exhibit excellent gap filling properties and planarization properties. However, in a hard mask layer formed using the spin coating technique, the required etch resistance may be reduced. Therefore, a hard mask composition may be applied using a spin coating technique to ensure an etch resistance equivalent to that of a hard mask layer formed in a chemical or physical deposition method.
[0227] Therefore, in order to improve the etching resistance of the hard mask layer, research on maximizing the carbon content of the hard mask composition is being conducted. However, as the carbon content of the compound contained in the hard mask composition is maximized, the solubility of the compound in the solvent may decrease. Therefore, the carbon content of the compound contained in the hard mask composition should be maximized to improve the etching resistance of the hard mask layer formed from the hard mask composition, and the compound must be soluble in the solvent.
[0228] The hard mask composition according to some embodiments may include a compound having an aromatic hydrocarbon ring, thereby increasing the carbon content in the composition. Therefore, the hard mask layer obtained from the composition can ensure excellent etching resistance. In addition, the compound may include a specific functional group, thereby having a high carbon content and excellent solubility in a solvent.
[0229] One or more embodiments may provide a hard mask composition that may be effectively applied to a hard mask layer.
[0230] One or more embodiments may provide a hard mask layer including a cured product of the hard mask composition.
[0231] One or more embodiments may provide a method of forming a pattern using the hard mask composition.
[0232] The hard mask composition according to some embodiments has excellent solubility in a solvent and may be effectively applied to a hard mask layer.
[0233] A hard mask layer formed from the hard mask composition according to some embodiments may ensure excellent heat resistance and excellent etching resistance.
[0234] A hard mask layer formed from the hard mask composition according to some embodiments may ensure excellent planarization characteristics.
[0235] The hard mask composition according to some embodiments may have excellent solubility in a solvent and may be effectively applied to a hard mask layer.
[0236] A hard mask layer formed from the hard mask composition according to some embodiments may ensure excellent heat resistance and excellent etching resistance.
[0237] A hard mask layer formed from the hard mask composition according to some embodiments may ensure excellent planarization characteristics.
[0238] Exemplary embodiments have been disclosed herein, and although specific terms are employed, they are used and should be interpreted in a general and illustrative sense only and not for purposes of limitation. In some cases, it will be apparent to one of ordinary skill in the art at the time this application is filed that features, characteristics, and / or elements described in connection with a particular embodiment may be used alone or in combination with features, characteristics, and / or elements described in connection with other embodiments, unless otherwise specifically stated. Therefore, it will be understood by one of ordinary skill in the art that various changes in form and detail may be made without departing from the spirit and scope of the invention as set forth in the claims above.
Claims
1. A hard mask composition comprising: A compound represented by Chemical Formula 1; and solvents, [Chemical formula 1] Wherein, in Chemical Formula 1, A 1 and A 2 are each independently a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a group in which a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group is linked via a single bond, a substituted or unsubstituted C1 to C5 alkylene group, or a combination thereof, R 1 is a substituted or unsubstituted monovalent C1 to C30 saturated aliphatic hydrocarbon group, a substituted or unsubstituted monovalent C2 to C30 unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted monovalent C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, R 2 is hydrogen, deuterium or substituted or unsubstituted C1 to C20 alkyl, n is an integer from 1 to 6, and If n is an integer of 2 or greater, then R 1 , R 2 and A 2 Each of them is the same or different from each other.
2. The hard mask composition according to claim 1, wherein A of Chemical Formula 1 1 and A 2 Substituted or unsubstituted groups each independently being part of Group 1: [Group 1] 3. The hard mask composition according to claim 1, wherein A of Chemical Formula 1 1 and A 2 Each independently a substituted or unsubstituted group that is part of Group 1-1: [Group 1-1] 4. The hard mask composition according to claim 1, wherein A in Chemical Formula 1 1 A substituted or unsubstituted group which is part of Group 1-2: [Group 1-2] 5. The hard mask composition according to claim 1, wherein A of Chemical Formula 1 2 A substituted or unsubstituted group which is part of Groups 1-3: [Group 1-3] 6. The hard mask composition according to claim 1, wherein R in Chemical Formula 1 1 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, or a substituted or unsubstituted C6 to C20 aryl group.
7. The hard mask composition according to claim 1, wherein R in Chemical Formula 1 2is hydrogen, deuterium, substituted or unsubstituted methyl, substituted or unsubstituted ethyl, substituted or unsubstituted propyl, substituted or unsubstituted butyl, or substituted or unsubstituted pentyl.
8. The hard mask composition according to claim 1, wherein In Chemical Formula 1, R 1 is a substituted or unsubstituted C1 to C20 alkyl group or a substituted or unsubstituted C6 to C20 aryl group, R 2 is hydrogen, deuterium, substituted or unsubstituted methyl, or substituted or unsubstituted ethyl, and n is an integer from 1 to 3.
9. The hard mask composition according to claim 7, wherein: In Chemical Formula 1, n is 2 or 3, and R 1 , R 2 and A 2 same.
10. The hard mask composition according to claim 1, wherein In Chemical Formula 1, R 1 is a substituted or unsubstituted C1 to C10 alkyl group, R 2 is hydrogen or deuterium, and n is 2.
11. The hard mask composition according to claim 1, wherein: The compound represented by Chemical Formula 1 is represented by one of Chemical Formulas 2 to 4: [Chemical formula 2] [Chemical formula 3] [Chemical formula 4] In Chemical Formula 2 to Chemical Formula 4, R 1 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, or a substituted or unsubstituted C6 to C20 aryl group, R 2 is hydrogen, deuterium or substituted or unsubstituted C1 to C10 alkyl, X 1 and X 2 are each independently deuterium, a hydroxyl group, a halogen atom, a thiol group, a substituted or unsubstituted C1 to C10 alkoxy group, or a substituted or unsubstituted C1 to C10 alkyl group, n is an integer from 1 to 3, and m1 and m2 are each independently an integer from 0 to 5.
12. The hard mask composition according to claim 1, wherein: The compound represented by Chemical Formula 1 is represented by one of Chemical Formulas 5 to 10, [Chemical formula 5] [Chemical formula 6] [Chemical formula 7] [Chemical formula 8] [Chemical formula 9] [Chemical formula 10] 13 . The hardmask composition of claim 1 , wherein the compound has a molecular weight of 500 g / mol to 10,000 g / mol. 14 . The hardmask composition of claim 1 , wherein the compound is included in an amount of 0.1 wt % to 30 wt % based on the total weight of the hardmask composition.
15. The hardmask composition according to claim 1, wherein the solvent comprises propylene glycol, propylene glycol diacetate, methoxypropylene glycol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, acetylacetone or ethyl 3-ethoxypropionate. 16 . A hard mask layer comprising a cured product of the hard mask composition of claim 1 .
17. A method for forming a pattern, the method comprising: providing a material layer on a substrate; applying the hard mask composition of claim 1 to the material layer; thermally treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer; as well as The exposed portion of the material layer is etched. 18 . The method of claim 17 , wherein forming the hard mask layer comprises performing a heat treatment at 100° C. to 1,000° C.
Citation Information
Patent Citations
Spade studs soccer shoes
KR1020230040766A