Semiconductor device and method for manufacturing semiconductor device

By using a polycrystalline oxide semiconductor layer and etching technology in semiconductor devices, the problems of poor etching resistance and difficult shape control of the oxide semiconductor layer are solved, and stable electrical characteristics and high yields are achieved.

CN118738138APending Publication Date: 2024-10-01JAPAN DISPLAY INC +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410326788.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-21
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing oxide semiconductor layers in semiconductor devices have poor etching resistance and are difficult to control the shape, resulting in in-plane variations in electrical characteristics and reduced yields. Especially in the manufacturing of large-area substrates, electrical characteristics problems caused by shape variation are serious.

Method used

Use an oxide semiconductor layer with a polycrystalline structure, and use etching technology to form the area overlapping the source electrode or drain electrode and the area in contact with the interlayer insulating layer, ensuring that the film thickness difference is less than 5nm, using metal oxide layer covering and etching technology Control the thickness of the channel region to improve the etching resistance of the oxide semiconductor layer.

Benefits of technology

A semiconductor device with less shape deviation and stable electrical characteristics has been realized, improving the yield, and through the combination of polycrystalline structure and etching technology, the etching resistance of the oxide semiconductor layer has been significantly improved, ensuring high mobility and stable electrical properties. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738138A_ABST
    Figure CN118738138A_ABST
Patent Text Reader

Abstract

The invention relates to a semiconductor device and a manufacturing method of the semiconductor device. The present invention addresses the problem of providing a semiconductor device having little variation in shape and stable electrical characteristics. The semiconductor device includes: a gate electrode; a gate insulating layer over the gate electrode; a metal oxide layer over the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure over the metal oxide layer; a source electrode and a drain electrode over the oxide semiconductor layer; and an interlayer insulating layer covering the source electrode and the drain electrode and in contact with the oxide semiconductor layer, the oxide semiconductor layer includes a first region overlapping the source electrode or the drain electrode and a second region in contact with the interlayer insulating layer, and the difference between the film thickness of the first region and the film thickness of the second region is 5 nm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a semiconductor device. In particular, one embodiment of the present invention relates to a semiconductor device using an oxide semiconductor as a channel. In addition, one embodiment of the present invention relates to a method for manufacturing a semiconductor device. Background Art

[0002] In recent years, the development of semiconductor devices that use oxide semiconductors for channels instead of amorphous silicon, low-temperature polycrystalline silicon, and single-crystal silicon has been progressing (for example, Patent Documents 1 to 6). Semiconductor devices that use oxide semiconductors for channels can be formed by simple structures and low-temperature processes, just like semiconductor devices that use amorphous silicon for channels. It is known that semiconductor devices that use oxide semiconductors for channels have higher mobility than semiconductor devices that use amorphous silicon for channels.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2021-141338

[0006] Patent Document 2: Japanese Patent Application Publication No. 2014-099601

[0007] Patent Document 3: Japanese Patent Application Publication No. 2021-153196

[0008] Patent Document 4: Japanese Patent Application Publication No. 2018-006730

[0009] Patent Document 5: Japanese Patent Application Publication No. 2016-184771

[0010] Patent Document 6: Japanese Patent Application Publication No. 2021-108405 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, in the existing semiconductor devices including oxide semiconductor layers, the oxide semiconductor layers have low etching resistance, and it is difficult to control the shape of the oxide semiconductor layers. In particular, in semiconductor devices manufactured using large-area substrates, the deviation in the shape of the oxide semiconductor layers will cause in-plane deviations in the electrical characteristics of the semiconductor devices, which is the main reason for the reduction in yield.

[0013] One object of one embodiment of the present invention is to provide a semiconductor device with less shape variation and stable electrical characteristics. Another object of one embodiment of the present invention is to provide a method for manufacturing a semiconductor device with reduced manufacturing variation and improved yield.

[0014] Means for solving problems

[0015] A semiconductor device involved in one embodiment of the present invention includes: a gate electrode; a gate insulating layer above the gate electrode; a metal oxide layer above the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure above the metal oxide layer; a source electrode and a drain electrode above the oxide semiconductor layer; and an interlayer insulating layer covering the source electrode and the drain electrode and connected to the oxide semiconductor layer, the oxide semiconductor layer including a first region overlapping with the source electrode or the drain electrode and a second region connected to the interlayer insulating layer, and the difference between the film thickness of the first region and the film thickness of the second region is less than 5nm.

[0016] A method for manufacturing a semiconductor device involved in one embodiment of the present invention includes: forming a gate electrode; forming a gate insulating layer on the gate electrode; forming a metal oxide film on the gate insulating layer; forming an oxide semiconductor layer having a polycrystalline structure on the metal oxide film; etching the metal oxide film using the oxide semiconductor layer as a mask to form the metal oxide layer; forming a conductive film on the oxide semiconductor layer; patterning the conductive film by etching to form a source electrode and a drain electrode; and forming an interlayer insulating layer covering the source electrode and the drain electrode and connected to the oxide semiconductor layer, wherein the oxide semiconductor layer includes a first region overlapping with the source electrode or the drain electrode and a second region connected to the interlayer insulating layer, and the difference between the film thickness of the first region and the film thickness of the second region is less than 5nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a cross-sectional view schematically showing a semiconductor device according to an embodiment of the present invention.

[0018] Figure 2 It is a plan view schematically showing a semiconductor device according to an embodiment of the present invention.

[0019] Figure 3 This is a flowchart showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0020] Figure 4 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0021] Figure 5 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0022] Figure 6 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0023] Figure 7It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0024] Figure 8 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0025] Fig. 9 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0026] Fig.10 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0027] Fig.11 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0028] Fig.12 It is a plan view schematically showing a display device according to one embodiment of the present invention.

[0029] Fig.13 This is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention.

[0030] Fig.14 : is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention.

[0031] Fig.15 It is a cross-sectional view schematically showing a display device according to an embodiment of the present invention.

[0032] Fig.16 : is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention.

[0033] Fig.17 It is a cross-sectional view schematically showing a display device according to an embodiment of the present invention.

[0034] Fig.18 It is a graph showing the electrical characteristics of sample A, sample B, and sample C.

[0035] Fig.19 It is a graph showing the electrical characteristics of sample D and sample F.

[0036] Fig. 20 Graphs showing the electrical characteristics of sample G, sample E, and sample H.

[0037] Fig.21 This is a graph showing the electrical characteristics of sample I.

[0038] Fig. 22 Graph showing the electrical characteristics of sample J.

[0039] Description of Reference Numerals

[0040] 10: semiconductor device, 11: substrate, 12C: wiring, 12GE: gate electrode, 12W: wiring, 14: gate insulating layer, 15: contact hole, 16: gate insulating layer, 18: metal oxide film, 20: display device, 22: oxide semiconductor film, 24: oxide semiconductor layer, 26: oxide semiconductor layer, 28: metal oxide layer, 32: source electrode and drain electrode, 32C: wiring, 32D: drain electrode, 32S: source electrode, 32W: wiring, 34: interlayer insulating layer, 36: metal oxide film, 38: interlayer insulating layer, 39: insulating layer, 42C: common electrode, 44: insulating layer, 46C: electrode, 46P: pixel electrode, 110: driving transistor, 120: selection selection transistor, 210: holding capacitor, 211: signal line, 212: gate line, 213: anode power line, 214: cathode power line, 220: liquid crystal area, 240: sealing area, 260: terminal area, 300: array substrate, 301: pixel circuit, 302: source driving circuit, 303: gate driving circuit, 304: source wiring, 305: gate wiring, 306: terminal part, 307: connection wiring, 310: sealing part, 311: liquid crystal element, 320: opposing substrate, 330: flexible printed circuit substrate, 340: chip, 350: holding capacitor, 362: insulating layer, 363: opening, 390: pixel electrode, 392: light-emitting layer, 394: common electrode DETAILED DESCRIPTION

[0041] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings. The following disclosure is only an example. The configuration that can be easily thought of by those skilled in the art by appropriately changing the configuration of the embodiment while maintaining the gist of the invention is of course included in the scope of the present invention. With respect to the accompanying drawings, in order to make the description clearer, the width, film thickness, shape, etc. of each part are sometimes schematically indicated compared to the actual method. However, the shape shown in the figure is only an example and does not limit the interpretation of the present invention. In this specification and each figure, the same figure mark is marked for the same elements as those described in the accompanying drawings that have appeared, and the detailed description is sometimes appropriately omitted.

[0042] "Semiconductor device" refers to any device that can function by utilizing semiconductor characteristics. Transistors and semiconductor circuits are a form of semiconductor devices. The semiconductor device of the embodiment shown below may also be a transistor used in an integrated circuit (IC) such as a display device, a microprocessor (MPU), or a memory circuit.

[0043] "Display device" refers to a structure that uses an electro-optical layer to display images. For example, the term display device sometimes refers to a display panel including an electro-optical layer, or sometimes refers to a structure in which other optical components (such as polarization components, backlight sources, touch panels, etc.) are assembled for the display unit. As long as no technical contradictions arise, the "electro-optical layer" can include a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer. Therefore, with respect to the embodiments described later, a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer are exemplified as display devices for explanation, and the structure in this embodiment can be applied to display devices including the above-mentioned other electro-optical layers.

[0044] In each embodiment of the present invention, the direction from the substrate toward the oxide semiconductor layer is referred to as up or above. Conversely, the direction from the oxide semiconductor layer toward the substrate is referred to as down or below. Thus, for ease of explanation, the above or below phrases are used for explanation, but, for example, the up-and-down relationship between the substrate and the oxide semiconductor layer may be configured in a manner opposite to that shown in the figure. In the following description, for example, the oxide semiconductor layer on the substrate is merely used to illustrate the up-and-down relationship between the substrate and the oxide semiconductor layer as described above, and other components may be configured between the substrate and the oxide semiconductor layer. Above or below means the stacking order in a structure having multiple layers stacked, and in the case of a pixel electrode described as above the transistor, it may also be a positional relationship in which the transistor and the pixel electrode do not overlap when viewed from above. On the other hand, in the case of a pixel electrode described as being vertically above the transistor, it means a positional relationship in which the transistor and the pixel electrode overlap when viewed from above. It should be noted that viewing from above refers to a method of observing from a direction perpendicular to the surface of the substrate.

[0045] In this specification and the like, the term "film" and the term "layer" can be used interchangeably according to circumstances.

[0046] In this specification, unless otherwise specified, expressions such as “α includes A, B, or C”, “α includes any one of A, B, and C”, and “α includes one selected from the group consisting of A, B, and C” do not exclude the case where α includes a combination of multiple elements of A to C. In addition, the above expressions do not exclude the case where α includes other elements.

[0047] It should be noted that the following embodiments can be combined with each other as long as no technical contradiction occurs.

[0048] <First Embodiment>

[0049] Reference Figures 1 to 11 A semiconductor device 10 according to an embodiment of the present invention will be described.

[0050] [Configuration of Semiconductor Device 10]

[0051] use Figure 1-2 Next, a configuration of a semiconductor device 10 according to an embodiment of the present invention will be described. Figure 1 It is a cross-sectional view schematically showing a semiconductor device 10 according to an embodiment of the present invention. Figure 2 It is a plan view schematically showing a semiconductor device 10 according to an embodiment of the present invention. Figure 1 The cross-sectional view shown is similar to the Figure 2 The cross section shown corresponds to the cross section taken along the A1-A2 line.

[0052] like Figure 1 As shown, the semiconductor device 10 is provided on the substrate 11. The semiconductor device 10 includes a gate electrode 12GE, gate insulating layers 14 and 16, a metal oxide layer 28, an oxide semiconductor layer 26, a source electrode 32S, a drain electrode 32D, and interlayer insulating layers 34 and 38. When the source electrode 32S and the drain electrode 32D are not particularly distinguished, they are sometimes collectively referred to as a source electrode and a drain electrode 32. In addition, the gate electrode 12GE, the gate insulating layers 14 and 16, the metal oxide layer 28, and the oxide semiconductor layer 26 are sometimes referred to as a transistor. In this embodiment, a bottom-gate transistor in which the gate electrode 12GE is provided below the oxide semiconductor layer 26 is described.

[0053] In this embodiment, a bottom-gate transistor is exemplified as the semiconductor device 10 , but the semiconductor device 10 is not limited to a bottom-gate transistor. For example, the semiconductor device 10 may be a dual-gate transistor in which gate electrodes are provided above and below the oxide semiconductor layer 26 .

[0054] The gate electrode 12GE is provided on the substrate 11. The gate insulating layers 14 and 16 are provided on the substrate 11 and the gate electrode 12GE. The gate insulating layers 14 and 16 have a stacked structure. The metal oxide layer 28 is provided on the gate insulating layer 16. The oxide semiconductor layer 26 is provided on the metal oxide layer 28. The source electrode 32S and the drain electrode 32D are provided on the oxide semiconductor layer 26. The interlayer insulating layers 34 and 38 are provided on the oxide semiconductor layer 26, and the source electrode 32S and the drain electrode 32D. The interlayer insulating layers 34 and 38 have a stacked structure, and the interlayer insulating layer 38 is provided on the interlayer insulating layer 34. That is, the interlayer insulating layers 34 and 38 cover the source electrode 32S and the drain electrode 32D, and the interlayer insulating layer 34 is in contact with the oxide semiconductor layer 26.

[0055] like Figure 2As shown, in a plan view, the oxide semiconductor layer 26 overlaps with the gate electrode 12GE. The D1 direction is a direction connecting the source electrode 32S and the drain electrode 32D, and the D2 direction is a direction orthogonal to the D1 direction. In the semiconductor device 10, the channel length L corresponds to the length of the region (channel region) of the oxide semiconductor layer 26 between the source electrode 32S and the drain electrode 32D in the D1 direction, and the channel width W corresponds to the width of the channel region in the D2 direction. In a plan view, the region of the oxide semiconductor layer 26 overlapping with the source electrode 32S is the source region, and the region of the oxide semiconductor layer 26 overlapping with the drain electrode 32D is the drain region. That is, the channel region is located between the source region and the drain region.

[0056] like Figure 2 As shown, in a plan view, the planar pattern of the metal oxide layer 28 is substantially the same as the planar pattern of the oxide semiconductor layer 26. In other words, the end of the metal oxide layer 28 is substantially consistent with the end of the oxide semiconductor layer 26. Figure 1 and Figure 2 The lower surface of the oxide semiconductor layer 26 is covered by the metal oxide layer 28. In particular, in the semiconductor device 10 according to the present embodiment, the lower surface of the oxide semiconductor layer 26 is entirely covered by the metal oxide layer 28.

[0057] The wiring 12W and the wiring 32W function as gate wiring. The wiring 32W is electrically connected to the wiring 12W via the contact hole 15. The wiring 12W is formed as the same layer as the gate electrode 12GE, and the details will be described later. In addition, the wiring 32W is formed as the same layer as the source electrode 32S and the drain electrode 32D. It should be noted that the wiring 32W is sometimes not provided on the wiring 12W.

[0058] The oxide semiconductor layer 26 is light-transmissive and has a polycrystalline structure including a plurality of crystal grains. The oxide semiconductor layer 26 having a polycrystalline structure can be formed by using the Poly-OS (Poly-crystalline Oxide Semiconductor) technology, and the details will be described later. Therefore, the oxide semiconductor contained in the oxide semiconductor layer 26 is sometimes described as Poly-OS below.

[0059] The crystal grain size of the crystal grains contained in the Poly-OS is 0.1 μm or more, preferably 0.3 μm or more, and more preferably 0.5 μm or more. The crystal grain size of the crystal grains can be obtained by, for example, cross-sectional SEM observation, cross-sectional TEM observation, or electron backscattered diffraction (EBSD) method.

[0060] As described above, since the crystal grain size of the crystal grains included in the Poly-OS is 0.1 μm or more, there is a region including only one crystal grain along the film thickness direction in the oxide semiconductor layer 26 having a film thickness of 10 nm to 30 nm.

[0061] Poly-OS is excellent in etching resistance. Poly-OS has excellent etching resistance to the etching solution or etching gas used in the formation of the source electrode 32S and the drain electrode 32D, and the details will be described later. Therefore, in the formation of the source electrode 32S and the drain electrode 32D, the oxide semiconductor layer 26 is hardly etched. Therefore, the film thickness of the first region (i.e., the source region or the drain region) of the oxide semiconductor layer 26 overlapping with the source electrode 32S or the drain electrode 32D and the film thickness of the second region (i.e., the channel region) of the oxide semiconductor layer 26 that does not overlap with the source electrode 32S and the drain electrode 32D are substantially the same. In other words, the difference between the film thickness of the first region and the film thickness of the second region is less than 5nm, preferably less than 3nm, and more preferably less than 1nm.

[0062] The film thickness of the channel region affects the electrical characteristics of the semiconductor device. The greater the deviation of the film thickness of the channel region, the less likely it is to provide a semiconductor device with stable electrical characteristics. That is, the yield of the semiconductor device will decrease. On the other hand, in the semiconductor device 10, since the film thickness of the channel region of the oxide semiconductor layer 26 can be controlled, the semiconductor device 10 has stable electrical characteristics. For example, in the semiconductor device 10, when the channel length L of the channel region is in the range of 2 μm to 4 μm and the channel width of the channel region is in the range of 2 μm to 25 μm, a mobility of 20 cm 2 / Vs or more, and further 30cm 2 / Vs or above field effect mobility (field effect mobility in the linear region).

[0063] [Method of Manufacturing Semiconductor Device 10]

[0064] use Figure 3 to Figure 11 A method for manufacturing the semiconductor device 10 according to an embodiment of the present invention will be described. Figure 3 1 is a flowchart illustrating a method for manufacturing the semiconductor device 10 according to an embodiment of the present invention. Figures 4 to 11 1 is a schematic cross-sectional view showing a method for manufacturing a semiconductor device 10 according to an embodiment of the present invention. Figure 3 The steps of the flowchart shown.

[0065] exist Figure 3 In step S1001 (“GE formation”), a gate electrode 12GE is formed on the substrate 11 (see Figure 4 ).

[0066] As the substrate 11, a glass substrate, a quartz substrate, a sapphire substrate, or other light-transmitting rigid substrate is used. When the substrate 11 needs to be flexible, a polyimide substrate, an acrylic substrate, a siloxane-based substrate, a fluororesin substrate, or a substrate containing resin can be used as the substrate 11. When a substrate containing resin is used as the substrate 11, in order to improve the heat resistance of the substrate 11, impurity elements can also be introduced into the above-mentioned resin. In particular, when the semiconductor device 10 is a top-emission display, the substrate 11 does not need to be transparent, so impurities that reduce the transmittance of the substrate 11 can also be used. When the semiconductor device 10 is used for an integrated circuit instead of a display device, as the substrate 11, a semiconductor substrate such as a silicon substrate, a silicon carbide substrate, a compound semiconductor substrate, or a conductive substrate such as a stainless steel substrate, which is not light-transmitting, can be used.

[0067] The gate electrode 12GE is formed by processing a conductive film formed by a sputtering method. As a metal material of the gate electrode 12GE, a common metal material is used. As the gate electrode 12GE, for example, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys thereof or compounds thereof are used. As the gate electrode 12GE, the above-mentioned metal materials can be used in the form of a single layer or in the form of a stack.

[0068] exist Figure 3 In step S1002 (“GI formation”), gate insulating layers 14 and 16 are formed on the gate electrode 12GE (see Figure 4 The gate insulating layers 14 and 16 are formed by CVD (Chemical Vapor Deposition) or sputtering. As the gate insulating layers 14 and 16, an insulating material can be used. For example, as the insulating material of the gate insulating layers 14 and 16, silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), silicon nitride (SiN x ), silicon oxynitride (SiN x O y ) and other inorganic insulating materials. The above-mentioned SiO x N y It is a silicon compound containing nitrogen (N) at a ratio (x>y) less than oxygen (O). SiN x O y It is a silicon compound containing oxygen at a ratio smaller than nitrogen (x>y).

[0069] On the substrate 11, a gate insulating layer 14 using an insulating material containing nitrogen and a gate insulating layer 16 using an insulating material containing oxygen are preferably formed in sequence. By using an insulating material containing nitrogen as the gate insulating layer 14, impurities diffusing from the substrate 11 toward the oxide semiconductor layer 26 can be blocked. In addition, by using an insulating material containing oxygen as the gate insulating layer 16, oxygen can be released under heat treatment. The temperature of the heat treatment for causing the insulating material containing oxygen to release oxygen is, for example, below 500° C., below 450° C., or below 400° C. It should be noted that the insulating material containing oxygen can also release oxygen when heated in any step of the manufacturing process of the semiconductor device 10.

[0070] The gate insulating layer 14 is preferably thicker than the gate insulating layer 16. In the present embodiment, for example, 300 nm of silicon nitride is formed as the gate insulating layer 14, and for example, 100 nm of silicon oxide is formed as the gate insulating layer 16.

[0071] exist Figure 3 In step S1003 (“MO film formation”), a metal oxide film 18 is formed on the gate insulating layers 14 and 16. The metal oxide film 18 is formed by sputtering or atomic layer deposition (ALD: Atomic Layer Deposition).

[0072] As the metal oxide film 18, a metal oxide containing aluminum as a main component is used. For example, as the metal oxide film 18, aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ), aluminum oxynitride (AlN x O y ), aluminum nitride (AlN x ) or the like. A metal oxide layer having aluminum as a main component means that the ratio of aluminum contained in the metal oxide layer is 1% or more of the entire metal oxide film 18. The ratio of aluminum contained in the metal oxide film 18 may be 5% or more and 70% or more, 10% or more and 60% or more, or 30% or more and 50% or less of the entire metal oxide film 18. The above ratio may be a mass ratio or a weight ratio.

[0073] The thickness of the metal oxide film 18 is, for example, not less than 1 nm and not more than 10 nm, preferably not less than 1 nm and not more than 5 nm. In the present embodiment, aluminum oxide is used as the metal oxide film 18. Aluminum oxide has a high barrier property to gases such as oxygen or hydrogen. In other words, the barrier property refers to the function of inhibiting the permeation of gases such as oxygen or hydrogen through aluminum oxide. That is, even if gases such as oxygen or hydrogen exist in the layer disposed under the aluminum oxide film, they will not move to the layer disposed on the aluminum oxide film. Or it means that even if gases such as oxygen or hydrogen exist from the layer disposed on the aluminum oxide film, they will not move to the layer disposed under the aluminum oxide film.

[0074] exist Figure 3 In step S1004 (“OS film formation”), an oxide semiconductor film 22 is formed on the metal oxide film 18 (see Figure 5 The oxide semiconductor film 22 is formed by sputtering or atomic layer deposition (ALD). The oxide semiconductor film 22 has a film thickness of 10 nm to 50 nm, preferably 10 nm to 40 nm, and more preferably 10 nm to 30 nm.

[0075] As the oxide semiconductor film 22, a metal oxide having semiconductor properties can be used. For example, as the oxide semiconductor film 22, an oxide semiconductor containing two or more metal elements including indium (In) can be used. In addition, the ratio of indium in the two or more metal elements is 50% or more. As the oxide semiconductor film 22, in addition to indium, gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconium (Zr) or lanthanide elements can be used. As the oxide semiconductor film 22, it is preferred to contain a Group 13 element. In addition, as the oxide semiconductor film 22, other elements other than those mentioned above can also be used.

[0076] When the oxide semiconductor film 22 is crystallized by OS annealing described later, it is preferable that the oxide semiconductor film 22 after film formation and before OS annealing is in an amorphous state (a state in which the crystal component of the oxide semiconductor is small). That is, the oxide semiconductor film 22 is preferably formed under conditions that prevent the oxide semiconductor film 22 from crystallizing as much as possible immediately after film formation. For example, when the oxide semiconductor film 22 is formed by sputtering, the oxide semiconductor film 22 is formed while controlling the temperature of the object to be formed (the substrate 11 and the structure formed thereon).

[0077] When a film is formed on an object to be formed by sputtering, ions generated in the plasma and atoms recoiled by the sputtering target collide with the object to be formed, so the temperature of the object to be formed rises as the film forming process progresses. If the temperature of the object to be formed rises during the film forming process, the oxide semiconductor film 22 contains microcrystals in the state just after the film is formed. If the oxide semiconductor film 22 contains microcrystals, the crystal grain size cannot be increased by subsequent OS annealing. In order to control the temperature of the object to be formed, for example, the film can be formed while the object to be formed is cooled. For example, the object to be formed can be cooled from the opposite side of the film forming surface in such a way that the temperature of the film forming surface of the object to be formed (hereinafter referred to as the "film forming temperature") is below 100°C, below 70°C, below 50°C, or below 30°C. In particular, it is preferred that the film forming temperature of the oxide semiconductor film 22 is below 50°C. By forming the oxide semiconductor film 22 while cooling the substrate 11 , it is possible to obtain the oxide semiconductor film 22 having a small crystal component immediately after film formation.

[0078] In the sputtering process, the oxide semiconductor film 22 having an amorphous structure is formed under the condition of an oxygen partial pressure of less than 10%. If the oxygen partial pressure is high, the oxide semiconductor film 22 immediately after film formation will contain microcrystals due to the excess oxygen contained in the oxide semiconductor film 22. Therefore, it is preferred to form the oxide semiconductor film 22 under the condition of a low oxygen partial pressure. The oxygen partial pressure is, for example, not less than 1% and not more than 5%, preferably not less than 2% and not more than 4%. Under the condition of an oxygen partial pressure of less than 1%, the distribution of oxygen in the film forming device tends to become uneven. As a result, the oxygen composition in the oxide semiconductor layer also becomes uneven, and an oxide semiconductor layer containing a large number of microcrystals is formed, or an oxide semiconductor layer that will not crystallize even if an OS annealing treatment is performed later is formed.

[0079] exist Figure 3 In step S1005 (“OS pattern formation”), a pattern of the oxide semiconductor layer 24 is formed (see Figure 6 ). The pattern of the oxide semiconductor layer 24 is formed using photolithography. For example, a resist mask (not shown) is formed on the oxide semiconductor film 22, and the oxide semiconductor film 22 is etched using the resist mask. As the etching of the oxide semiconductor film 22, wet etching or dry etching can be used. As wet etching, an acidic etching solution can be used for etching. As an etching solution, for example, oxalic acid, PAN, sulfuric acid, hydrogen peroxide or hydrofluoric acid can be used. In this way, an oxide semiconductor layer 24 having a predetermined pattern can be formed. Thereafter, the resist mask is removed.

[0080] The formation of the oxide semiconductor layer 24 having a predetermined pattern (i.e., patterning of the oxide semiconductor film 22) is preferably performed before OS annealing. The etching resistance of the Poly-OS after OS annealing is high, and it is difficult to perform patterning by etching. In addition, by performing OS annealing after the formation of the oxide semiconductor layer 24, damage generated during the formation of the oxide semiconductor layer 24 (e.g., oxygen defects in the oxide semiconductor layer 24) can be repaired by OS annealing.

[0081] exist Figure 3 In step S1006 (“OS annealing”), after the oxide semiconductor layer 24 is formed, the oxide semiconductor layer 24 is subjected to heat treatment (OS annealing), thereby forming the oxide semiconductor layer 26 (see Figure 7 ). In the OS annealing, the oxide semiconductor layer 24 is maintained at a predetermined reaching temperature for a predetermined time. The predetermined reaching temperature is 300° C. to 500° C., preferably 350° C. to 450° C. In addition, the holding time at the reaching temperature is 15 minutes to 120 minutes, preferably 30 minutes to 60 minutes. By performing the OS annealing, the oxide semiconductor layer 24 having an amorphous structure is crystallized to form an oxide semiconductor layer 26 having a polycrystalline structure. That is, by the OS annealing, the oxide semiconductor layer 26 including Poly-OS is formed.

[0082] In thin film transistors, there is a tendency to increase the number of carriers by reducing the thickness of the oxide semiconductor layer, reduce the influence of the reverse channel, and thus increase the field effect mobility. That is, the thin film transistor has a tendency that the smaller the thickness of the region of the oxide semiconductor layer that functions as a channel, the higher the field effect mobility. Therefore, the smaller the thickness of the oxide semiconductor layer, the better. However, after forming the oxide semiconductor layer with a thickness of less than 10nm, even if heat treatment is performed, the oxide semiconductor layer cannot be fully crystallized. In the case where the oxide semiconductor layer is not fully crystallized, when the oxide semiconductor layer is subsequently used as a mask for etching treatment to pattern the metal oxide layer, the oxide semiconductor layer and the metal oxide layer will disappear.

[0083] In addition, in a thin film transistor, the crystallinity of the oxide semiconductor layer 26 contributes to the improvement of field effect mobility. Therefore, the oxide semiconductor layer 26 preferably has a polycrystalline structure. However, when the oxide semiconductor film 22 is formed, if microcrystals are contained, the crystal grain size of the crystal grains in the polycrystalline structure cannot be increased even if a heat treatment is performed later. In this way, it is difficult to simultaneously achieve thin film and good crystallization of the oxide semiconductor layer.

[0084] When the oxide semiconductor film 22 is formed by sputtering, the film is formed under a low oxygen partial pressure of 3% to 5%. By forming the oxide semiconductor film 22 under the condition of low oxygen partial pressure, it is possible to suppress excessive oxygen in the oxide semiconductor film 22 and suppress the inclusion of microcrystals in the oxide semiconductor film 22 just after film formation. As a result, during the heat treatment of the oxide semiconductor layer 24, it is possible to suppress the growth of crystals from microcrystals. Therefore, even when the oxide semiconductor film 22 is formed with a thin film thickness of more than 10 nm and less than 30 nm, the crystal grain size of the crystal grains in the polycrystalline structure of the oxide semiconductor layer 26 can be increased.

[0085] like Figure 3 As shown in step S1007, the metal oxide film 18 is patterned to form a metal oxide layer 28 (see Figure 8 ). The oxide semiconductor layer 26 that has been fully crystallized by heat treatment has high etching resistance. Therefore, when the metal oxide film 18 is patterned using the crystallized oxide semiconductor layer 26 as a mask, the disappearance of the oxide semiconductor layer 26 can be suppressed. The metal oxide film 18 is etched using the oxide semiconductor layer 26 patterned in the above process as a mask. As the etching of the metal oxide film 18, wet etching or dry etching can be used. As a wet etching, for example, diluted hydrofluoric acid (DHF) can be used. By etching the metal oxide film 18 using the oxide semiconductor layer 26 as a mask, the photolithography process can be omitted.

[0086] exist Figure 3 In step S1008 (“contact hole formation”), a contact hole 15 is formed in the gate insulating layer 14, 16 (see Figure 8 ). Thus, the upper surface of the wiring 12W is exposed. It should be noted that when it is not necessary to connect the wiring 32W to the wiring 12W, the process of step S1008 may not be performed.

[0087] exist Figure 3 In step S1009 (“SD formation”), the source electrode 32S, the drain electrode 32D and the wiring 32W are formed (see Fig. 9). The source electrode 32S, the drain electrode 32D, and the wiring 32W are formed by etching a conductive film formed by a sputtering method to pattern it. In addition, the wiring 32W can be connected to the wiring 12W via the contact hole 15. As the source electrode 32S and the drain electrode 32D, the same conductive material as the gate electrode 12GE can be used. As the source electrode 32S, the drain electrode 32D, and the wiring 32W, the conductive material can be used in the form of a single layer or in the form of a stack. In this embodiment, a stacked structure of MoW alloy, Al and MoW alloy (MoW / Al / MoW structure), a single-layer structure of MoW alloy (MoW structure), a single-layer structure of Ti (Ti structure), and a stacked structure of Ti, Al and Ti (Ti / Al / Ti structure) are exemplified.

[0088] In order to form the source electrode 32S, the drain electrode 32D and the wiring 32W, wet etching or dry etching is used for patterning. In wet etching, an etching solution is used. For example, as an etching solution, a solution containing at least two selected from the group consisting of phosphoric acid, acetic acid, nitric acid, hydrofluoric acid, hydrochloric acid, sulfuric acid and oxalic acid can be used. Specifically, as an etching solution, a mixed acid etching solution with phosphoric acid, acetic acid and nitric acid as main components can be used. In addition, as an etching solution, a mixed solution of hydrogen peroxide and ammonia water (hereinafter referred to as "H2O2 / NH3 solution") can also be used. In dry etching, an etching gas is used. For example, as an etching gas, a fluorine-containing gas such as sulfur hexafluoride gas (SF6) (hereinafter referred to as "fluorine-based gas") or a chlorine-containing gas such as chlorine (Cl2) (hereinafter referred to as "chlorine-based gas") is used.

[0089] Poly-OS has excellent etching resistance. Specifically, the etching rate is very low relative to the etching solution or etching gas used in forming the source electrode 32S and the drain electrode 32D. This means that Poly-OS is hardly etched by the etching solution or etching gas. Therefore, in the semiconductor device 10, even if a conductive film is directly formed on the oxide semiconductor layer 26 and the conductive film is patterned to form the source electrode 32S and the drain electrode 32D, the channel region of the oxide semiconductor layer 26 is hardly etched.

[0090] For example, the etching rate of the oxide semiconductor layer 26 relative to the etching liquid used in the formation of the source electrode 32S and the drain electrode 32D is 0.1 nm / sec or less or 0.01 nm / sec or less. In addition, the etching rate of the oxide semiconductor layer 26 relative to the etching gas used in the formation of the source electrode 32S and the drain electrode 32D is 0.5 nm / sec or less or 0.1 nm / sec or less. For example, the etching rate of the oxide semiconductor layer 26 relative to the chlorine-based gas used in the formation of the source electrode 32S and the drain electrode 32D is 0.3 nm / sec or less. For example, the etching rate of the oxide semiconductor layer 26 relative to the fluorine-based gas used in the formation of the source electrode 32S and the drain electrode 32D is 0.1 nm / sec or less. It should be noted that the etching rate is slightly higher in the etching using the chlorine-based gas than in the etching using the etching liquid or the fluorine-based gas. In the case of etching using the chlorine-based gas, the processability of the source electrode 32S and the drain electrode 32D is good compared to etching using the etching liquid. Therefore, the etching solution or etching gas may be appropriately selected according to the structure of the conductive film for forming the source electrode 32S and the drain electrode 32D.

[0091] As an oxide semiconductor layer, in a semiconductor device using an oxide semiconductor that does not have a polycrystalline structure such as IGZO, when a source electrode and a drain electrode are formed on the oxide semiconductor, the oxide semiconductor layer will also be etched due to the etching of the source electrode and the drain electrode. Specifically, the etching rate of IGZO relative to chlorine-containing gas is 1.0nm / sec. Considering that the channel region will be etched at this etching rate, it is necessary to form the oxide semiconductor layer in advance to make it thick. For example, in the case of a semiconductor device in which the film thickness of the channel region of the oxide semiconductor layer is less than 40nm, it is necessary to form an oxide semiconductor layer with a thickness of about 65nm in advance, and in the formation of the source electrode and the drain electrode, the etching time is adjusted in a manner such that the film thickness of the channel region is less than 40nm. However, it is difficult to control the film thickness of the channel region based on the etching time. In addition, when the etching rate is large, it is difficult to precisely control the film thickness of the channel region based on the etching time. In this case, the deviation of the film thickness of the channel region becomes larger.

[0092] In addition, if the film thickness of the channel region is greatly reduced, a recess will be formed on the upper surface of the oxide semiconductor layer. Although the interlayer insulating layer provided on the oxide semiconductor layer is formed in a manner covering the recess, if the depth of the recess is large, the interlayer insulating layer cannot fully cover the recess. That is, sometimes a gap is generated between the oxide semiconductor layer and the interlayer insulating layer, or between the source electrode and the drain electrode and the interlayer insulating layer. This will become the main reason for the deviation of not only the electrical characteristics but also the reliability of the semiconductor device.

[0093] In contrast, the oxide semiconductor layer 26 having a polycrystalline structure can have an etching rate of 0.00 nm / sec to 0.1 nm / sec, preferably 0.00 nm / sec to 0.06 nm / sec, in either wet etching or dry etching. That is, the oxide semiconductor layer 26 having a polycrystalline structure has a low etching rate and high etching resistance compared to the oxide semiconductor layer using IGZO. Therefore, the film loss caused by etching can be ignored, and the controllability is good. Therefore, when the oxide semiconductor layer is formed, the film can be formed with a thin film thickness greater than 10 nm and less than 30 nm. In addition, the selectivity of the conductive material that can be used as the source electrode 32S, the drain electrode 32D and the wiring 32W is improved. For example, even when a conductive film using a stacked structure of MoW / Al / MoW or a single-layer structure of a MoW alloy is processed by wet etching to form the source electrode 32S and the drain electrode 32D, the film loss of the oxide semiconductor layer 26 can be suppressed.

[0094] As described above, the etching rate of the oxide semiconductor layer 26 relative to the etching solution used in forming the source electrode 32S and the drain electrode 32D is very small. Therefore, the film thickness of the first region (i.e., the source region or the drain region) of the oxide semiconductor layer 26 overlapping with the source electrode 32S or the drain electrode 32D and the film thickness of the second region (i.e., the channel region) of the oxide semiconductor layer 26 not overlapping with the source electrode 32S and the drain electrode 32D are substantially the same. In other words, the difference between the film thickness of the first region and the film thickness of the second region can be controlled to be 5 nm or less, preferably 3 nm or less, and more preferably 1 nm or less. That is, the variation of the film thickness of the channel region is suppressed.

[0095] exist Figure 3 In step S1010 ("SiOx formation"), an interlayer insulating layer 34 is formed on the oxide semiconductor layer 26, the source electrode 32S, and the drain electrode 32D. As the interlayer insulating layer 34, an insulating material containing oxygen is preferably used. For example, silicon oxide (SiO x ) or silicon oxynitride (SiO x N y ) etc. In addition, as the interlayer insulating layer 34, it is preferable to use an insulating layer with few defects. For example, when the composition ratio of oxygen in the interlayer insulating layer 34 is compared with the composition ratio of oxygen in an insulating layer having the same composition as the interlayer insulating layer 34 (hereinafter referred to as "other insulating layer"), the composition ratio of oxygen in the interlayer insulating layer 34 is closer to the stoichiometric ratio of the insulating layer than the composition ratio of oxygen in the other insulating layer. For example, silicon oxide (SiO x), the interlayer insulating layer 34 has a composition ratio closer to the stoichiometric ratio of silicon oxide (SiO 2 ) than the gate insulating layer 16. As the interlayer insulating layer 34, a layer in which no defects are observed when evaluated by electron spin resonance (ESR) may be used.

[0096] The interlayer insulating layer 34 can be formed by the same film forming method as the gate insulating layers 14 and 16. In order to increase the oxygen composition ratio in the interlayer insulating layer 34, the film formation can be performed at a relatively low temperature (for example, a film formation temperature of less than 350° C.). In addition, in order to form an insulating layer with fewer defects as the interlayer insulating layer 34, the interlayer insulating layer 34 can also be formed at a film formation temperature of 350° C. or more. In addition, after the interlayer insulating layer 34 is formed, a process of injecting oxygen into a part of the interlayer insulating layer 34 can be performed.

[0097] The film thickness of the interlayer insulating layer 34 is not less than 50 nm and not more than 300 nm, not less than 60 nm and not more than 200 nm, or not less than 70 nm and not more than 150 nm.

[0098] exist Figure 3 In step S1011 (“MO film formation”), a metal oxide film 36 is formed on the interlayer insulating layer 34 (see Fig.10 ). The metal oxide film 36 is formed by a sputtering method or an atomic layer deposition method (ALD: Atomic Layer Deposition).

[0099] As the metal oxide film 36, a metal oxide containing aluminum as a main component is used. For example, as the metal oxide film 36, aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ), aluminum oxynitride (AlN x O y ), aluminum nitride (AlN x ) or the like. A metal oxide layer having aluminum as a main component means that the ratio of aluminum contained in the metal oxide layer is 1% or more of the entire metal oxide film 36. The ratio of aluminum contained in the metal oxide film 36 may be 5% or more and 70% or more, 10% or more and 60% or more, or 30% or more and 50% or less of the entire metal oxide film 36. The above ratio may be a mass ratio or a weight ratio.

[0100] The thickness of the metal oxide film 36 is not less than 1 nm and not more than 50 nm, preferably not less than 1 nm and not more than 30 nm. As the metal oxide film 36, aluminum oxide is preferably used. Aluminum oxide has a high barrier property to gases such as oxygen and hydrogen. Here, the barrier property refers to the function of inhibiting the permeation of gases such as oxygen and hydrogen through aluminum oxide. That is, it means that gases such as oxygen and hydrogen in the layer below the aluminum oxide film do not move to the layer above the aluminum oxide film. Or it means that gases such as oxygen and hydrogen in the layer above the aluminum oxide film do not move to the layer below the aluminum oxide film.

[0101] Note that a metal oxide containing a metal other than aluminum as a main component may be used as the metal oxide film 36. For example, the metal oxide film 36 may be made of indium tin oxide (ITO), indium zinc oxide (IZO), or indium gallium zinc oxide (IGZO).

[0102] exist Figure 3 In step S1012 (“oxidation annealing”), a heat treatment is performed while the interlayer insulating layer 34 and the metal oxide film 36 are formed on the oxide semiconductor layer 26 (see Fig.10 Here, the oxidation annealing can be performed at, for example, 300° C. to 450° C. Thus, oxygen released from the interlayer insulating layer 34 is supplied to the oxide semiconductor layer 26. By providing the metal oxide film 36 so as to cover the substrate 11, it is possible to suppress the oxygen released from the interlayer insulating layer 34 from being released to the outside of the metal oxide film 36.

[0103] In the process from forming the oxide semiconductor layer 26 to forming the interlayer insulating layer 34 on the oxide semiconductor layer 26, a large number of oxygen defects are generated in the oxide semiconductor layer 26. However, by the oxidation annealing in step S1012, oxygen released from the interlayer insulating layer 34 is supplied to the oxide semiconductor layer 26 to repair the oxygen defects.

[0104] exist Figure 3 In step S1013 ("MO removal"), the metal oxide film 36 (see Fig.11 ). For example, the metal oxide film 36 may be removed using diluted hydrofluoric acid (DHF).

[0105] exist Figure 3 In step S1014 ("SiNx film formation"), an interlayer insulating layer 38 is formed on the interlayer insulating layer 34. As the interlayer insulating layer 38, an insulating material containing nitrogen is preferably used. For example, silicon nitride (SiN x ) or silicon oxynitride (SiN x O y) etc. The interlayer insulating layer 38 can be formed by using the same film forming method as the gate insulating layers 14 and 16 .

[0106] Through the above steps, we can produce Figure 1 A semiconductor device 10 is shown.

[0107] In the semiconductor device 10 manufactured by the above manufacturing method, a mobility of 20 cm-1 can be obtained when the channel length L of the channel region is within the range of 2 μm to 4 μm and the channel width of the channel region is within the range of 2 μm to 25 μm. 2 / Vs or more, and further 30cm 2 / Vs or above excellent electrical characteristics.

[0108] In addition, by providing the metal oxide layer 28 under the oxide semiconductor layer 26, the film thickness of the region in the oxide semiconductor layer 26 that functions as a channel can be substantially reduced by utilizing the effect of the metal oxide layer 28. As a result, the density of carriers accumulated in the channel can be increased, and thus the mobility of the semiconductor device 10 can be increased. The metal oxide film 18 has gas barrier properties for oxygen and hydrogen. However, if oxygen is not supplied to the oxide semiconductor layer 26 from the gate insulating layer 14, 16 side via the metal oxide layer 28, the oxygen defects on the back side of the oxide semiconductor layer 26 cannot be repaired. Therefore, by setting the film thickness of the metal oxide film 18 to be greater than 1 nm and less than 10 nm, preferably greater than 1 nm and less than 5 nm, the oxygen contained in the gate insulating layer 16 can be appropriately supplied to the back side of the oxide semiconductor layer 26.

[0109] Furthermore, even when the semiconductor device 10 is manufactured using a large-area substrate, it is possible to suppress shape variations in the oxide semiconductor layer 26. Therefore, it is possible to suppress in-plane variations in electrical characteristics of the semiconductor device 10, and to improve yield.

[0110] <Second Embodiment>

[0111] use Figure 12 to Figure 15 A display device 20 using the semiconductor device 10 according to one embodiment of the present invention will be described. In the following embodiment, a circuit configuration in which the semiconductor device 10 described in the first embodiment is applied to a liquid crystal display device will be described.

[0112] [Overview of Display Device 20]

[0113] Fig.12 FIG. 2 is a top view showing an overview of a display device 20 according to an embodiment of the present invention. Fig.12As shown, the display device 20 includes an array substrate 300, a sealing portion 310, an opposing substrate 320, a flexible printed circuit substrate 330 (FPC 330), and an IC chip 340. The array substrate 300 and the opposing substrate 320 are bonded together by the sealing portion 310. A plurality of pixel circuits 301 are arranged in a matrix in a liquid crystal region 220 surrounded by the sealing portion 310. The liquid crystal region 220 is a region that overlaps with a liquid crystal element 311 described later in a plan view.

[0114] The sealing region 240 provided with the sealing portion 310 is an area around the liquid crystal region 220. The FPC 330 is provided in the terminal region 260. The terminal region 260 is an area where the array substrate 300 is exposed from the counter substrate 320 and is provided outside the sealing region 240. The outside of the sealing region 240 refers to the outside of the area provided with the sealing portion 310 and the area surrounded by the sealing portion 310. The IC chip 340 is provided on the FPC 330. The IC chip 340 supplies a signal for driving each pixel circuit 301.

[0115] [Circuit Configuration of Display Device 20]

[0116] Fig.13 1 is a block diagram showing a circuit configuration of a display device 20 according to an embodiment of the present invention. Fig.13 As shown, a source driving circuit 302 is provided at a position adjacent to the liquid crystal region 220 in the second direction D2 (column direction) where the pixel circuit 301 is arranged, and a gate driving circuit 303 is provided at a position adjacent to the liquid crystal region 220 in the first direction D1 (row direction). The source driving circuit 302 and the gate driving circuit 303 are provided in the above-mentioned sealing region 240. However, the region where the source driving circuit 302 and the gate driving circuit 303 are provided is not limited to the sealing region 240, and may be any region as long as it is outside the region where the pixel circuit 301 is provided.

[0117] The source wiring 304 extends from the source driving circuit 302 along the second direction D2 and is connected to the plurality of pixel circuits 301 arranged in the second direction D2. The gate electrode 12GE extends from the gate driving circuit 303 along the first direction D1 and is connected to the plurality of pixel circuits 301 arranged in the first direction D1.

[0118] The terminal region 260 is provided with a terminal portion 306. The terminal portion 306 and the source driver circuit 302 are connected via a connection wiring 307. Similarly, the terminal portion 306 and the gate driver circuit 303 are connected via a connection wiring 307. By connecting the FPC 330 to the terminal portion 306, an external device connected to the FPC 330 is connected to the display device 20, and each pixel circuit 301 provided in the display device 20 is driven by a signal from the external device.

[0119] The semiconductor device 10 described in the first embodiment is used as a transistor included in the pixel circuit 301 , the source driver circuit 302 , and the gate driver circuit 303 .

[0120] [Pixel Circuit 301 of Display Device 20]

[0121] Fig.14 is a circuit diagram showing a pixel circuit 301 of a display device 20 according to an embodiment of the present invention. Fig.14 As shown, the pixel circuit 301 includes components such as the semiconductor device 10, the storage capacitor 350, and the liquid crystal element 311. The semiconductor device 10 has a gate electrode 12GE, an oxide semiconductor layer 26, a source electrode 32S, and a drain electrode 32D. The gate electrode 12GE is connected to the gate wiring 305. The source electrode 32S is connected to the source wiring 304. The drain electrode 32D is connected to the storage capacitor 350 and the liquid crystal element 311.

[0122] [Configuration of Display Device 20]

[0123] Fig.15 It is a cross-sectional view of a display device 20 according to an embodiment of the present invention. Fig.15 The semiconductor device 10 is applied to the display device 20 shown.

[0124] like Fig.15 As shown, a gate electrode 12GE is provided on the substrate 11. Moreover, a metal oxide layer 28 and an oxide semiconductor layer 26 are provided on the gate electrode 12GE via gate insulating layers 14 and 16. On the oxide semiconductor layer 26, a source electrode 32S and a drain electrode 32D are provided.

[0125] Interlayer insulating layers 34 and 38 are provided on the source electrode 32S and the drain electrode 32D. An insulating layer 39 is provided on the interlayer insulating layers 34 and 38. The insulating layer 39 is provided to alleviate the unevenness generated by the semiconductor device 10. Contact holes are formed in the interlayer insulating layers 34, 38 and the insulating layer 39 so as to expose the upper surface of the source electrode 32S. A common electrode 42C provided in common to a plurality of pixels is provided on the insulating layer 39. An insulating layer 44 is provided on the common electrode 42C. An insulating layer 44 is provided inside the contact hole. By forming the insulating layer 44 from a silicon nitride film, it is possible to suppress the intrusion of moisture from the contact hole through the insulating layer 44. A pixel electrode 46P is provided on the insulating layer 44 and inside the contact hole. The pixel electrode 46P is connected to the drain electrode 32D.

[0126] In addition, wiring 12C is provided on substrate 11, and wiring 12C is connected to wiring 32C via contact holes provided in gate insulating layers 14 and 16. Wiring 12C and wiring 32C function as capacitor wiring. In addition, electrode 46C is provided on insulating layer 39 and inside the opening. A holding capacitor 350 is formed by common electrode 42C, insulating layer 44 and electrode 46C.

[0127] In this embodiment, a configuration in which the semiconductor device 10 is used in the pixel circuit 301 is exemplified. However, the semiconductor device 10 may be used in peripheral circuits including the source driver circuit 302 and the gate driver circuit 303 .

[0128] <Third Embodiment>

[0129] use Fig.16 and Fig.17 A display device 20 using the semiconductor device 10 according to one embodiment of the present invention is described. In this embodiment, a circuit configuration in which the semiconductor device 10 described in the first embodiment is applied to an organic EL display device is described. The overview and circuit configuration of the display device 20 are related to Fig.12 and Fig.13 The scheme shown is the same, so the description is omitted.

[0130] [Pixel Circuit 301 of Display Device 20]

[0131] Fig.16 1 is a circuit diagram showing a pixel circuit of a display device 20 according to an embodiment of the present invention. Fig.16 As shown, the pixel circuit 301 includes components such as a driving transistor 110, a selection transistor 120, a holding capacitor 210 and a light-emitting element DO. The driving transistor 110 and the selection transistor 120 have the same structure as the semiconductor device 10. The source electrode of the selection transistor 120 is connected to the signal line 211, and the gate electrode of the selection transistor 120 is connected to the gate line 212. The source electrode of the driving transistor 110 is connected to the anode power line 213, and the drain electrode of the driving transistor 110 is connected to one end of the light-emitting element DO. The other end of the light-emitting element DO is connected to the cathode power line 214. The gate electrode of the driving transistor 110 is connected to the drain electrode of the selection transistor 120. The holding capacitor 210 is connected to the gate electrode and the drain electrode of the driving transistor 110. A grayscale signal that determines the light intensity of the light-emitting element DO is supplied to the signal line 211. A signal for selecting a pixel row to which the above-mentioned grayscale signal is to be written is supplied to the gate line 212.

[0132] [Cross-sectional structure of display device 20]

[0133] Fig.17It is a schematic cross-sectional view showing the structure of a display device 20 according to an embodiment of the present invention. Fig.17 The display device 20 shown in FIG. Fig.15 The display device 20 shown is similar, but Fig.17 The structure above the insulating layer 39 in the display device 20 shown in FIG. Fig.15 The structure above the insulating layer 39 in the display device 20 shown is different. Fig.17 The display device 20 shown in FIG. Fig.15 The same configurations as those of the display device 20 shown will be omitted and the differences between the two will be described.

[0134] like Fig.17 As shown, the display device 20 has a pixel electrode 390, a light-emitting layer 392 and a common electrode 394 (light-emitting element DO) above the insulating layer 39. The pixel electrode 390 is arranged on the insulating layer 39 and inside the contact hole formed in the interlayer insulating layers 34, 38 and the insulating layer 39. An insulating layer 362 is arranged on the pixel electrode 390. An opening 363 is arranged in the insulating layer 362. The opening 363 corresponds to the light-emitting area. That is, the insulating layer 362 is used to divide the pixel. The light-emitting layer 392 and the common electrode 394 are arranged on the pixel electrode 390 exposed by the opening 363. The pixel electrode 390 and the light-emitting layer 392 are respectively arranged relative to each pixel. On the other hand, the common electrode 394 is commonly arranged relative to a plurality of pixels. Different materials are used for the light-emitting layer 392 according to the display color of the pixel.

[0135] In the second embodiment and the third embodiment, the semiconductor device described in the first embodiment is applied to the structure of the liquid crystal display device and the organic EL display device, but the semiconductor device can also be applied to display devices other than the above-mentioned display devices (for example, other self-luminous display devices or electronic paper display devices other than the organic EL display device). In addition, unless otherwise specified, the above-mentioned semiconductor device 10 can be applied to small and medium-sized display devices to large display devices. In addition, even when a large-area substrate is used for manufacturing, the deviation of the shape of the oxide semiconductor layer 26 in the semiconductor device 10 is small. Therefore, when the semiconductor device 10 is applied to the display device 20, the display unevenness can be reduced. In addition, the yield rate when manufacturing the display device 20 can be improved.

[0136] Example

[0137] (Example 1)

[0138] In this example, the results of verifying the etching resistance of an oxide semiconductor layer having a polycrystalline structure are described.

[0139] The samples used in this embodiment are described. A 30nm oxide semiconductor layer (Poly-OS) having a polycrystalline structure is formed on a silicon wafer. Next, a conductive film is formed on the oxide semiconductor layer. As the conductive film, four types of MoW structure, MoW / Al / MoW structure, Ti structure, and Ti / Al / Ti structure are used.

[0140] For the conductive film and oxide semiconductor layer of the MoW structure, samples obtained by wet etching with a mixed acid etching solution, samples obtained by wet etching with a H2O2 / NH3 solution, and samples obtained by dry etching with a fluorine-based gas were prepared. It should be noted that as a mixed acid etching solution, "Mixed Acid AT-2F (product name)" manufactured by RASA Industries, Ltd. was used. The proportion of phosphoric acid in the mixed acid etching solution is about 65%. In addition, the temperature of the mixed acid etching solution when etching each sample was set to 40°C, and the temperature of the 0.5% hydrofluoric acid solution was set to 22°C.

[0141] A sample was prepared in which a conductive film and an oxide semiconductor layer having a MoW / Al / MoW structure were wet-etched using a mixed acid etching solution.

[0142] For the Ti-structured conductive film and oxide semiconductor layer, samples obtained by wet etching using a H2O2 / NH3 solution, samples obtained by dry etching using a fluorine-based gas, and samples obtained by dry etching using a chlorine-based gas were prepared.

[0143] For the conductive film and oxide semiconductor layer of the Ti / Al / Ti structure, samples were prepared in which Ti was wet-etched with a H2O2 / NH3 solution, Al was wet-etched with a mixed acid etching solution, and Ti was wet-etched with a H2O2 / NH3 solution, as well as a sample obtained by dry-etching with a chlorine-based gas.

[0144] Next, the sample used in the comparative example is described. A 40nm IGZO oxide semiconductor layer is formed on a silicon wafer. Next, a conductive film is formed on the oxide semiconductor layer. A Ti structure is used as the conductive film. For the Ti structure conductive film and the oxide semiconductor layer, a sample obtained by dry etching with a chlorine-based gas is prepared.

[0145] Table 1 shows the etching rate [nm / sec] of the polycrystalline oxide semiconductor layer with respect to the overetching time estimated after processing various conductive films as this example.

[0146] [Table 1]

[0147]

[0148] As a comparative example, the etching rate of the oxide semiconductor layer (IGZO) was 1.00 nm / sec with respect to the overetching time estimated after processing the conductive film of the Ti structure.

[0149] As shown in Table 1, it is shown that the oxide semiconductor layer having a polycrystalline structure has higher etching resistance than the amorphous oxide semiconductor layer (IGZO). In addition, it is shown that the etching rate is 0.00nm / sec to 0.06nm / sec when etching with a mixed acid etching solution, when etching with a H2O2 / NH3 solution, and when etching with a fluorine-based gas. It is shown that even when etching with a chlorine-based gas, it has sufficiently high etching resistance compared to the oxide semiconductor layer (IGZO).

[0150] (Example 2)

[0151] Next, the first embodiment will be described. Figure 3 The electrical characteristics of the semiconductor device 10 manufactured according to the flowchart shown in the figure were verified.

[0152] In Example 2, samples A to H are described as the semiconductor device 10. Samples A to H are prepared by Figure 3 In the flowchart shown, the processes of step S1007 and step S1008 are omitted.

[0153] (Sample A)

[0154] A gate electrode 12GE is formed on the substrate, and gate insulating layers 14 and 16 are formed on the gate electrode 12GE. A 3 nm aluminum oxide layer is formed on the gate insulating layers 14 and 16 as a metal oxide film 18, and a 30 nm oxide semiconductor film 22 is formed on the metal oxide film 18. The oxide semiconductor film 22 is processed to form an oxide semiconductor layer 24, and an oxide semiconductor layer 26 (Poly-OS) with a polycrystalline structure is formed by performing OS annealing at 350° C. to 450° C. In addition, the metal oxide film 18 is removed by using the oxide semiconductor layer 26 as a mask, thereby forming a metal oxide layer 28.

[0155] A MoW / Al / MoW structure is formed as a conductive film on the oxide semiconductor layer 26, and the conductive film is wet-etched using a mixed acid etching solution to form a source electrode and a drain electrode. Next, after forming the interlayer insulating layer 34, a 10 nm aluminum oxide layer is formed as a metal oxide film 36, and after oxidation annealing, the metal oxide film 36 is removed. Finally, an interlayer insulating layer 38 is formed on the interlayer insulating layer 34. When the film thickness of the oxide semiconductor layer is measured after the formation of sample A, 1 nm is removed.

[0156] Samples B to H were formed by changing the structure of the conductive film for forming the source electrode and the drain electrode and the conditions of the etching method compared to Sample A.

[0157] (Sample B)

[0158] Sample B was formed under the same conditions as Sample A except that a MoW structure was used as the conductive film.

[0159] (Sample C)

[0160] Sample C was formed under the same conditions as sample A except that a MoW structure was formed as a conductive film and the conductive film was dry-etched using SF6 gas and O2 gas to form a source electrode and a drain electrode. When the film thickness of the oxide semiconductor layer was measured after sample C was formed, 2 nm was removed.

[0161] (Sample D)

[0162] Sample D was formed under the same conditions as sample A except that a Ti structure was formed as a conductive film and the conductive film was dry-etched using CF4 gas and O2 gas to form a source electrode and a drain electrode. When the film thickness of the oxide semiconductor layer was measured after sample D was formed, 2 nm was removed.

[0163] (Sample E)

[0164] Sample E was formed under the same conditions as sample A, except that a Ti / Al / Ti structure was formed as the conductive film and the conductive film was dry-etched using Cl 2 gas to form a source electrode and a drain electrode.

[0165] (Sample F)

[0166] Sample F was formed under the same conditions as Sample A, except that a Ti structure was formed as the conductive film and the conductive film was wet-etched using a H 2 O 2 / NH 3 solution to form a source electrode and a drain electrode.

[0167] (Sample G)

[0168] A Ti / Al / Ti structure was formed as a conductive film and the conductive film was wet-etched using an H2O2 / NH3 solution for Ti, a mixed acid etching solution for Al, and an H2O2 / NH3 solution for Ti to form a source electrode and a drain electrode. Sample G was formed under the same conditions as sample A.

[0169] (Sample H)

[0170] Sample H is a comparative example, and its formation method is different from that of samples A to G. A gate electrode is formed on a substrate, and a gate insulating layer is formed on the gate electrode. A 95 nm oxide semiconductor layer (IGZO (111)) is formed on the gate insulating layer. The oxide semiconductor layer is processed to form an oxide semiconductor layer, and OS annealing is performed at 350°C to 450°C.

[0171] A stacked structure of Ti / AlSi / Ti was formed on the oxide semiconductor layer as a conductive film, and the conductive film was dry-etched using Cl2 gas to form a source electrode and a drain electrode. Then, after forming an interlayer insulating layer, a 50nm aluminum oxide layer was formed as a metal oxide layer, and oxidation annealing was performed. It should be noted that the target film thickness of the oxide semiconductor layer by dry etching was set to 60nm.

[0172] Next, the electrical characteristics of samples A to H were measured. The measurement conditions of the electrical characteristics of samples A to H were as follows.

[0173] Channel area size: W / L = 6 μm / 6 μm

[0174] Source-drain voltage: 0.1V, 10V

[0175] ·Gate voltage: -40V~+40V(0.2V Step)

[0176] ·Measurement environment: room temperature, dark room

[0177] ·Measurement location: One point within the substrate surface

[0178] Fig.18 It is a graph showing the electrical characteristics (Id-Vg characteristics) of sample A, sample B, and sample C. Fig.19 It is a graph showing the electrical characteristics (Id-Vg characteristics) of sample D and sample F. Fig. 20 It is a graph showing the electrical characteristics (Id-Vg characteristics) of sample G, sample E, and sample H. The horizontal axis is the gate voltage Vg, and the vertical axis is the drain current (Id).

[0179] like Figure 18 to Figure 20 As shown, samples A to G having a polycrystalline oxide semiconductor layer (Poly-OS) have high mobility and can obtain good electrical characteristics. In contrast, sample H having an oxide semiconductor layer (IGZO) has lower mobility than the samples having an oxide semiconductor layer (Poly-OS).

[0180] (Example 3)

[0181] Next, the first embodiment will be described. Figure 3The electrical characteristics of the semiconductor device 10 manufactured according to the flowchart shown in the figure were verified. Here, the change in the electrical characteristics due to the difference in the film thickness of the metal oxide layer 28 was verified.

[0182] Samples I and J produced as the semiconductor device 10 in Example 3 are described below. Figure 3 The processes of step S1007 and step S1008 are omitted in the flowchart.

[0183] (Sample I)

[0184] A gate electrode 12GE is formed on the substrate, and gate insulating layers 14 and 16 are formed on the gate electrode 12GE. A 3 nm aluminum oxide layer is formed on the gate insulating layers 14 and 16 as a metal oxide film 18, and a 30 nm oxide semiconductor film 22 is formed on the metal oxide film 18. The oxide semiconductor film 22 is processed to form an oxide semiconductor layer 24, and an oxide semiconductor layer 26 having a polycrystalline structure is formed by performing OS annealing at 350° C. to 450° C. In addition, the metal oxide film 18 is removed by using the oxide semiconductor layer 26 as a mask, thereby forming a metal oxide layer 28.

[0185] A MoW / Al / MoW structure is formed as a conductive film on the oxide semiconductor layer 26, and the conductive film is wet-etched using a mixed acid etching solution to form a source electrode and a drain electrode. Next, after forming the interlayer insulating layer 34, a 10 nm aluminum oxide layer is formed as a metal oxide film 36, and after oxidation annealing is performed at 350°C, the metal oxide film 36 is removed. Finally, an interlayer insulating layer 38 is formed on the interlayer insulating layer 34.

[0186] (Sample J)

[0187] Sample J was formed under the same conditions as Sample I except that the film thickness of the metal oxide layer 28 was set to 10 nm.

[0188] Next, the electrical characteristics of the samples I and J were measured. The measurement conditions of the electrical characteristics of the samples I and J were as follows.

[0189] Channel area size: W / L = 6 μm / 6 μm

[0190] Source-drain voltage: 0.1V, 10V

[0191] ·Gate voltage: -40V~+40V(0.4V Step)

[0192] ·Measurement environment: room temperature, dark room

[0193] ·Measurement location: One point within the substrate surface

[0194] Fig.21 This is a graph showing the electrical characteristics (Id-Vg characteristics) of sample I. Fig. 22 It is a graph showing the electrical characteristics (Id-Vg characteristics) of sample J.

[0195] like Fig.21 and Fig. 22 As shown, it is shown that the threshold voltage shift of the semiconductor device is suppressed in both sample I and sample J. This is considered to be because the oxide semiconductor layer 26 is suppressed from being removed by etching, thereby reducing the formation of defects on the surface of the oxide semiconductor layer 26. Therefore, it is considered that the defects formed in the oxide semiconductor layer 26 are also sufficiently repaired by the subsequent oxidation annealing at 350°C or above, thereby contributing to suppressing the threshold voltage shift of the semiconductor device.

[0196] The various embodiments and variations described above as embodiments of the present invention can be implemented in appropriate combination as long as they do not contradict each other. In addition, solutions obtained by adding, deleting or changing the design of components or adding, omitting or changing the conditions of processes based on the semiconductor devices and display devices of the various embodiments and variations by those skilled in the art are also included in the scope of the present invention as long as they have the gist of the present invention.

[0197] Even if there are other effects different from the effects brought about by the schemes of the above-mentioned embodiments, if they are clearly known from the description of this specification or can be easily predicted by those skilled in the art, they are of course understood to be the effects brought about by the present invention.

Claims

1. A semiconductor device comprising: a gate electrode; a gate insulating layer on the gate electrode; a metal oxide layer on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; A source electrode and a drain electrode on the oxide semiconductor layer; and an interlayer insulating layer covering the source electrode and the drain electrode and in contact with the oxide semiconductor layer, The oxide semiconductor layer includes a first region overlapping with the source electrode or the drain electrode and a second region contacting with the interlayer insulating layer, A difference between the film thickness of the first region and the film thickness of the second region is 5 nm or less.

2. The semiconductor device according to claim 1, wherein The etching rate of the oxide semiconductor layer with respect to an etching solution used in forming the source electrode and the drain electrode is 0.1 nm / sec or less.

3. The semiconductor device according to claim 2, wherein: The etching solution is a solution containing at least two selected from the group consisting of phosphoric acid, acetic acid, nitric acid, hydrofluoric acid, hydrochloric acid, sulfuric acid and oxalic acid.

4. The semiconductor device according to claim 1, wherein The etching rate of the oxide semiconductor layer with respect to the etching gas used in forming the source electrode and the drain electrode is 0.5 nm / sec or less.

5. The semiconductor device according to claim 4, wherein: The etching gas is a gas containing fluorine, The etching rate is 0.1 nm / sec or less.

6. The semiconductor device according to claim 1, wherein The film thickness of the first region is not less than 10 nm and not more than 30 nm.

7. The semiconductor device according to claim 1, wherein The oxide semiconductor layer contains indium and at least one other metal element. The ratio of the indium to the indium and the at least one other metal element is 50% or more.

8. The semiconductor device according to claim 1, wherein The thickness of the metal oxide layer is not less than 1 nm and not more than 10 nm.

9. A method for manufacturing a semiconductor device, comprising: forming a gate electrode; forming a gate insulating layer on the gate electrode; forming a metal oxide film on the gate insulating layer; forming an oxide semiconductor layer having a polycrystalline structure over the metal oxide film; Using the oxide semiconductor layer as a mask, etching the metal oxide film to form a metal oxide layer; forming a conductive film on the oxide semiconductor layer; patterning the conductive film by etching to form a source electrode and a drain electrode; and forming an interlayer insulating layer covering the source electrode and the drain electrode and contacting the oxide semiconductor layer, The oxide semiconductor layer includes a first region overlapping with the source electrode or the drain electrode and a second region connected with the interlayer insulating layer. A difference between the film thickness of the first region and the film thickness of the second region is 5 nm or less.

10. The method for manufacturing a semiconductor device according to claim 9, wherein: In the etching, an etching liquid is used. The etching rate of the oxide semiconductor layer with respect to the etching solution is 0.1 nm / sec or less.

11. The method for manufacturing a semiconductor device according to claim 10, wherein: The etching solution is a solution containing at least two selected from the group consisting of phosphoric acid, acetic acid, nitric acid, hydrofluoric acid, hydrochloric acid, sulfuric acid and oxalic acid.

12. The method for manufacturing a semiconductor device according to claim 9, wherein: In the etching, an etching gas is used. An etching rate of the oxide semiconductor layer with respect to the etching gas is 0.5 nm / sec or less.

13. The method for manufacturing a semiconductor device according to claim 12, wherein: The etching gas is a gas containing fluorine, The etching rate is 0.1 nm / sec or less.

14. The method for manufacturing a semiconductor device according to claim 9, wherein: The film thickness of the first region is not less than 10 nm and not more than 30 nm.

15. The method for manufacturing a semiconductor device according to claim 9, wherein: The oxide semiconductor layer contains indium and at least one other metal element. The ratio of the indium to the indium and the at least one other metal element is 50% or more.

16. The method for manufacturing a semiconductor device according to claim 15, wherein: The oxide semiconductor layer is formed by heat treating an oxide semiconductor layer having an amorphous structure.

17. The method for manufacturing a semiconductor device according to claim 9, wherein: The thickness of the metal oxide layer is not less than 1 nm and not more than 10 nm.

Citation Information

Patent Citations

  • Semiconductor device

    JP2016184771A

  • Semiconductor device and display device having semiconductor device

    JP2018006730A

  • Semiconductor device manufacturing method

    JP2021108405A

  • Manufacturing method for semiconductor device

    JP2021141338A

  • Semiconductor device

    JP2021153196A