Battery piece, passivation method thereof and photovoltaic module

By using passivation liquid to form a passivation layer on the cutting surface of photovoltaic cells, the problems of poor film formation selectivity and high equipment cost in ALD technology are solved, achieving efficient and low-cost passivation effect, and improving photoelectric conversion efficiency. and product yield.

CN118738149APending Publication Date: 2024-10-01LONGI GREEN ENERGY TECH CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410831432.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Among the existing cutting surface passivation methods for photovoltaic cells, ALD technology has problems such as poor film formation selectivity, high equipment cost, high process energy consumption, long process time, and low cell efficiency.

Method used

Passivation liquid is used to replace gaseous raw materials, and a passivation layer is formed on the cutting surface through the passivation liquid. The particle size of the passivation material is less than or equal to 150 nanometers. The process is carried out at normal temperature and pressure, reducing equipment complexity and energy consumption, and improving the process. efficiency and product yield.

Benefits of technology

It achieves high efficiency, density and smoothness of the passivation layer on the cutting surface, improves photoelectric conversion efficiency, reduces process equipment costs and battery damage, expands the processing window, and improves product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738149A_ABST
    Figure CN118738149A_ABST
Patent Text Reader

Abstract

The invention provides a battery piece, a passivation method of the battery piece and a photovoltaic module, and relates to the technical field of photovoltaics. The battery piece comprises a cutting surface; the cutting surface is formed in the process of slicing the solar cell to form a cell piece; the cutting surface passivation layer is located on the cutting surface; the cutting surface passivation layer is formed in a passivation solution mode; the particle size of the passivation material in the cutting surface passivation layer is smaller than or equal to 150 nanometers. According to the invention, winding plating is almost avoided, the photoelectric conversion efficiency of the cell is improved, the process equipment is greatly simplified, the process energy consumption and the product cost are further reduced, the process efficiency of forming the cutting surface passivation layer is high, the thickness range of the cutting surface passivation layer is wider, in addition, the processing window of the cell is wider, the product yield is higher, and the production cost is reduced. And moreover, the passivation effect on the cutting surface is good, and the photoelectric conversion efficiency of the battery piece is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photovoltaic technology, and in particular to a solar cell and a passivation method thereof, and a photovoltaic module. Background Art

[0002] The solar cell is sliced ​​to form a cell. The cell has cutting damage on the cutting surface formed by slicing. It is necessary to form a cutting surface passivation layer on the cutting surface to achieve defect passivation and improve the photoelectric conversion efficiency.

[0003] At present, an ALD (Atomic Layer Deposition) method is mainly used to form a cutting surface passivation layer on the cutting surface.

[0004] However, since ALD introduces gaseous raw materials, the gaseous raw materials are usually evenly distributed in the entire space, resulting in poor selectivity in the film-forming area. A cut surface passivation layer will grow around the surface of the cell, reducing the photoelectric conversion efficiency of the cell. Secondly, the gaseous raw materials used in ALD are usually very easy to self-ignite, and high requirements are placed on equipment safety protection. It is usually necessary to adopt multiple safety controls and alarm structures such as high vacuum chambers, multiple interlock valves, and vacuum sleeves to prevent leakage. Therefore, the equipment is expensive and the process energy consumption is high. In addition, ALD has a low film-forming rate and a long process time. Since the passivation of the cut surface requires a thicker film layer, the ALD process is difficult to implement. At the same time, the ALD process takes a long time to form a cut surface passivation layer, and the process conditions are harsh, which poses a risk of reducing battery efficiency and yield. Summary of the invention

[0005] The invention provides a solar cell and a passivation method thereof and a photovoltaic module, aiming to solve the problems of severe passivation plating on the cut surface of the existing solar cell, high cost and difficulty in implementation.

[0006] A first aspect of the present invention provides a battery cell, comprising:

[0007] Cutting surface; the cutting surface is formed in the process of slicing the solar cell to form the cell;

[0008] A cut surface passivation layer is located on the cut surface; the cut surface passivation layer is formed by a passivation liquid; and the particle size of the passivation material in the cut surface passivation layer is less than or equal to 150 nanometers.

[0009] In the present invention, the passivation layer of the cut surface is formed by a passivation liquid. Compared with the related art, the passivation liquid replaces the gaseous raw material. The passivation liquid does not have the spatial diffusion phenomenon. The passivation layer of the cut surface is formed only in the contact area of ​​the passivation liquid. Therefore, the selectivity of the film-forming area is strong, and there is almost no plating, which improves the photoelectric conversion efficiency of the battery cell. Secondly, the passivation liquid is relatively stable and non-toxic in the air, avoiding the flammable and explosive risks brought by hazardous chemicals. Therefore, the process can be carried out at room temperature and pressure. The passivation liquid is used to form the passivation layer of the cut surface without a vacuum environment, which reduces the functional modules of the equipment such as safety protection, alarm, and vacuum, greatly simplifies the process equipment, and thus reduces the process energy consumption and product cost. Thirdly, the process time of forming the passivation layer of the cut surface by the passivation liquid is short, the process efficiency of forming the passivation layer of the cut surface is high, the thickness range of the passivation layer of the cut surface formed by the passivation liquid is relatively wide, and the formation of the passivation layer of the cut surface with the required thickness is easy to achieve, and according to the principle of chemical reaction kinetics, the shorter the contact time, the smaller the damage, and the shorter the process time further reduces the damage to the battery cell. In addition, a passivation liquid is used to form a passivation layer on the cut surface, and the thickness and coverage of the passivation layer on the cut surface are easy to control, so that the method has a wider processing window and a higher product yield. At the same time, a passivation liquid is used to form a passivation layer on the cut surface, and the particle size of the passivation material is less than or equal to 150 nanometers. The passivation layer thus formed is denser and smoother, and has better passivation performance. In summary, the battery cell provided by the present invention has almost no winding plating, and the process equipment is greatly simplified, thereby reducing process energy consumption and product costs, and the process efficiency is high, with less damage to the battery cell, a wide processing window, a high product yield, and a good passivation effect on the cut surface.

[0010] Optionally, the passivation material of the cut surface passivation layer is selected from at least one of aluminum oxide, silicon oxide, and titanium oxide, which has a good passivation effect on the cut surface, further improving the photoelectric conversion efficiency of the cell.

[0011] Optionally, the cut surface passivation layer covers a surface area of ​​the cut surface, and the proportion of the surface area of ​​the cut surface to be greater than or equal to 90% is.

[0012] Optionally, the cutting surface includes: a laser affected area and a non-laser affected area, and in the laser affected area, the cutting surface passivation layer covers the laser affected area;

[0013] Alternatively, the cut surface passivation layer covers most of the laser affected area.

[0014] Optionally, the cutting surface includes: a laser affected area and a non-laser affected area, and in the non-laser affected area, the absolute value of the difference between the maximum thickness and the minimum thickness of the passivation layer of the cutting surface is less than or equal to 50% of the maximum thickness.

[0015] Optionally, the cutting surface includes: a laser affected area and a non-laser affected area, and on the non-laser affected area and near the geometric center area of ​​the cutting surface, the surface flatness of the cutting surface passivation layer is less than or equal to 50% of the maximum thickness of the cutting surface passivation layer.

[0016] Optionally, when the maximum thickness of the cut surface passivation layer is less than or equal to 2 um, the surface flatness of the cut surface passivation layer is less than or equal to 1 um; preferably, the surface flatness of the cut surface passivation layer is less than or equal to 600 nm.

[0017] Optionally, when the maximum thickness of the cut surface passivation layer is less than or equal to 5 um, the surface flatness of the cut surface passivation layer is less than or equal to 2.5 um; preferably, the surface flatness of the cut surface passivation layer is less than or equal to 2 um.

[0018] Optionally, the thickness of the cutting surface passivation layer in an edge region close to the cutting surface is smaller than the thickness of the cutting surface passivation layer in an area close to a geometric center of the cutting surface.

[0019] Optionally, the thickness of the cutting surface passivation layer in an edge region close to the cutting surface is greater than the thickness of the cutting surface passivation layer in an area close to a geometric center of the cutting surface.

[0020] Optionally, the thickness of the cut surface passivation layer is 30 nm to 10000 nm; preferably, the thickness of the cut surface passivation layer is 50 nm to 8000 nm.

[0021] Optionally, the battery cell further includes: a first surface and a second surface both intersecting the cutting surface; the first surface and the second surface are opposite to each other; the first surface and the second surface both include cutting edges adjacent to the cutting surface;

[0022] The first surface does not have the cutting surface passivation layer, or the first surface is only plated with the cutting surface passivation layer on one side close to the cutting edge; and / or,

[0023] The second surface does not have the cutting surface passivation layer, or the second surface is plated with the cutting surface passivation layer only on one side close to the cutting edge.

[0024] Optionally, the cut surface passivation layer is plated around only one side of the first surface close to the cut edge, and the cut surface passivation layer is plated around but does not cover the metal area on the first surface;

[0025] and / or,

[0026] The cut surface passivation layer is plated around only one side of the second surface close to the cut edge; the cut surface passivation layer is plated around but does not cover the metal area on the second surface.

[0027] Optionally, the cutting surface passivation layer is plated on only one side of the first surface close to the cutting edge, and the width of the cutting surface passivation layer plated on the first surface is less than or equal to 0.5 mm; and / or,

[0028] The cutting surface passivation layer is plated on only one side of the second surface close to the cutting edge, and the width of the cutting surface passivation layer plated on the second surface is less than or equal to 0.5 mm.

[0029] Optionally, it further includes: a surface passivation layer located on the first surface and the second surface;

[0030] The cut surface passivation layer is plated around the surface passivation layer on only one side of the first surface close to the cut edge; and / or,

[0031] The cut surface passivation layer is plated around the surface passivation layer on only one side of the second surface close to the cut edge;

[0032] Wherein, the surface passivation layer is used to protect the battery cell and reduce reflection.

[0033] Optionally, the thickness of the cut surface passivation layer plated around the cut surface is less than or equal to the thickness of the cut surface passivation layer.

[0034] A second aspect of the present invention provides a photovoltaic module, comprising:

[0035] A plurality of battery strings electrically connected to each other, wherein the battery string is formed by connecting a plurality of battery cells as described in any of the above items in series in sequence;

[0036] Two adjacent battery cells in the battery string are connected by a conductive member;

[0037] The conductive member passes through the plane where the passivation layer of the cut surface of the battery cell is located.

[0038] A third aspect of the present invention provides a method for passivating a battery cell, comprising:

[0039] Slicing the solar cell to obtain a cell sheet; the cell sheet includes a cutting surface formed by slicing;

[0040] A passivation liquid is coated on the cut surface of the battery cell to form a cut surface passivation layer; the particle size of the passivation material in the passivation layer is less than or equal to 150 nanometers.

[0041] Optionally, the cell passivation method further includes:

[0042] The passivation liquid is formed by configuring a solute and a solvent; the passivation liquid is at least one of a solution, a suspension, a colloid, and a precursor liquid.

[0043] Optionally, slicing the solar cell to obtain a cell sheet includes:

[0044] After the passivation layers on two opposite surface cut surfaces of the solar cell are prepared, slicing is performed to obtain a cell; the passivation layers on the surface cut surfaces are used to protect the cell and reduce reflection.

[0045] Optionally, the coating includes at least one of dipping, scraping, slit coating, spraying, printing, and rolling.

[0046] Optionally, when the coating is performed by immersion, the height of the battery cell in contact with the passivation solution is less than or equal to 4 mm;

[0047] When the coating is performed by a method other than the immersion method, the height of the battery cell in contact with the passivation solution is less than or equal to 2 mm.

[0048] Optionally, the step of coating a passivation liquid on the cut surface of the cell to form a cut surface passivation layer includes:

[0049] A passivation liquid is coated on the cut surface of the battery cell to form a passivation liquid film, and then activated to obtain a cut surface passivation layer.

[0050] Optionally, the temperature during the activation process is less than or equal to 600°C.

[0051] The above-mentioned cell passivation method, cell, and photovoltaic module have the same or similar beneficial effects, and will not be described again here to avoid repetition. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0053] Figure 1 A local SEM schematic diagram of a passivation layer on a cut surface in a non-laser affected area in an embodiment of the present invention is shown;

[0054] Figure 2 A local SEM schematic diagram of a passivation layer on a cut surface in another non-laser-affected area in an embodiment of the present invention is shown;

[0055] Figure 3A flow chart showing the steps of a method for passivating a battery cell according to an embodiment of the present invention is shown;

[0056] Figure 4 The following is a flowchart showing an operation of a method for passivating a battery cell according to an embodiment of the present invention.

[0057] Description of the accompanying drawings:

[0058] 1-solar cell, 11-slicing position, 2-cell, 21-cutting surface passivation layer, 3-passivation liquid, 4-heating device. DETAILED DESCRIPTION

[0059] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0060] The present invention provides a cell, the cell includes a cutting surface, the cutting surface is formed in the process of slicing a solar cell to form a cell, and the position of the solar cell slice is the cutting surface formed by the cell slice. There is no specific limitation on the specific morphology of the cutting surface, and there is no specific limitation on the number of cutting surfaces on a cell 2. For example, for a 2-slice, the number of cutting surfaces on a cell may be 1, and for a 3-slice, the number of cutting surfaces on some cells is 1, and the number of cutting surfaces on some cells is 2. There is no specific limitation on the type of silicon substrate of the cell, and it may be a monocrystalline silicon substrate, a polycrystalline silicon substrate, etc. The cell may be a double-sided cell, a back-contact cell, etc., and there is no specific limitation on the type of the cell.

[0061] The number of cells obtained by slicing the solar cell is not specifically limited. For example, the cell may be cut along the midline of the light-facing surface and the backlight surface of the solar cell to obtain two half cells.

[0062] The cell may also include: a cut surface passivation layer, which is located on the cut surface. The passivation material in the cut surface passivation layer refers to the material that plays the main passivation role in the cut surface passivation layer. The cut surface passivation layer is formed by a passivation liquid. Compared with the related technology, the passivation liquid replaces the gaseous raw material. The passivation liquid does not have the spatial diffusion phenomenon. The cut surface passivation layer is formed only in the passivation liquid contact area. Therefore, the selectivity of the film forming area is strong, and there is almost no plating, which improves the photoelectric conversion efficiency of the cell. Secondly, the passivation liquid is relatively stable and non-toxic in the air, avoiding the flammable and explosive risks brought by hazardous chemicals. Therefore, the process can be carried out at room temperature and pressure. The cut surface passivation layer is formed by the passivation liquid without a vacuum environment, which reduces the safety protection, alarm, vacuum and other functional modules of the equipment, greatly simplifies the process equipment, and thus reduces the process energy consumption and product cost. Thirdly, the process time of forming the passivation layer of the cut surface by using the passivation liquid is short, the process efficiency of forming the passivation layer of the cut surface is high, the thickness range of the passivation layer of the cut surface by using the passivation liquid is relatively wide, and it is easy to form the passivation layer of the cut surface of the required thickness. Moreover, according to the principle of chemical reaction kinetics, the shorter the contact time, the smaller the damage. The shorter process time further reduces the damage to the battery cell. In addition, the passivation liquid is used to form the passivation layer of the cut surface, and the thickness and coverage of the passivation layer of the cut surface are easy to control, so that the processing window of the method is wide and the product yield is high. At the same time, the passivation liquid is used to form the passivation layer of the cut surface, and the particle size of the passivation material is less than or equal to 150 nanometers (nm). The passivation layer formed thereby is relatively dense and relatively flat, and the passivation performance is better. Optionally, the passivation material of the passivation layer of the cut surface in the present invention is selected from at least one of aluminum oxide, silicon oxide, and titanium oxide, which has a good passivation effect on the cut surface, further improving the photoelectric conversion efficiency of the battery cell. In summary, the battery cell provided by the present invention has almost no winding plating, and the process equipment is greatly simplified, thereby reducing the process energy consumption and product cost, and the process efficiency is high, with less damage to the battery cell, a wide processing window, a high product yield, and a good passivation effect on the cut surface.

[0063] For example, the particle size of the passivation material can be 150nm, 140nm, 120nm, 110nm, 100nm, 97nm, 90nm, 80nm, 70nm, 60nm, 50nm, 43nm, 30nm.

[0064] Optionally, the surface area of ​​the cut surface covered by the passivation layer of the cut surface accounts for a proportion greater than or equal to 90% of the surface area of ​​the cut surface. Since the cut surface passivation layer has a higher coverage of the cut surface, the passivation effect on the cut surface of the battery cell is better. The surface area of ​​the cut surface of the battery cell covered by the passivation layer of the cut surface refers to: the surface area of ​​the portion of the cut surface of the battery cell covered by the passivation layer of the cut surface.

[0065] For example, the surface area of ​​the cut surface of the battery cell covered by the passivation layer is 90%, 92%, 94%, 95%, 95.3%, 96%, 97%, 98%, 98.2%, 98.9%, 99%, 99.5%, 99.9%, 100% of the surface area of ​​the cut surface of the battery cell.

[0066] Optionally, the cutting surface of the cell may include: a laser-affected zone and a non-laser-affected zone. For example, when the silicon substrate of the solar cell is a single crystal, the laser-affected zone presents a polycrystalline state after melting, and the non-laser-affected zone presents a cracked state of a single crystal lattice. The position corresponding to the laser grooving in the cutting surface is roughly the laser-affected zone, and the position corresponding to the stress slicing or physical slicing in the cutting surface is roughly the non-laser-affected zone. Under normal circumstances, the area of ​​the laser-affected zone in the cutting surface is extremely small, and it is mainly the non-laser-affected zone. The surface flatness of the passivation layer of the cutting surface located on the non-laser-affected zone of the cutting surface and close to the geometric center area of ​​the cutting surface is less than or equal to 50% of the maximum thickness of the passivation layer of the cutting surface, the surface flatness of the passivation layer of the cutting surface is small, the surface of the passivation layer of the cutting surface is relatively flat, the thickness is relatively uniform, and the passivation quality of the passivation layer of the cutting surface is good. The possible reason is that the non-laser affected area has a lower flatness due to the lack of laser influence. Moreover, in the present invention, after the passivation layers of the two opposite surface cut surfaces of the solar cell are prepared, slicing is performed. The cut surfaces will not be affected by the wet method and the coating process. The formed cut surface passivation layer has a better film quality. Moreover, the cut surface passivation layer will not be affected by the wet method and the coating process. The cut surface passivation layer has a better film quality and a lower flatness.

[0067] Optionally, the surface flatness of the passivation layer of the cutting surface located on the non-laser affected area of ​​the cutting surface and close to the geometric center area of ​​the cutting surface is less than or equal to 50% of the maximum thickness of the passivation layer of the cutting surface, indicating that the passivation layer of the cutting surface formed on the non-laser affected area of ​​the present application has good thickness uniformity and better passivation performance. Moreover, since the area of ​​the laser affected area in the cutting surface accounts for a very small proportion, it is mainly the non-laser affected area, and the surface flatness of the passivation layer of the cutting surface on the non-laser affected area of ​​the cutting surface is relatively small, that is to say, the surface flatness of the passivation layer of the entire cutting surface is basically small. The passivation layer of the entire cutting surface formed by the present application has good thickness uniformity and better passivation performance.

[0068] The calculation of the surface flatness of the passivation layer of the cutting surface is as follows: a reference line and 10 peaks and 10 troughs are selected in the passivation layer of the cutting surface in the non-laser affected area of ​​the cutting surface, and the 10 peaks and 10 troughs are located on both sides of the reference line. Surface flatness = (sum of the absolute values ​​of the heights of the 10 peaks + sum of the absolute values ​​of the depths of the 10 troughs) / 10. The absolute value of the peak height refers to the distance between the peak and the reference line, which is a positive value, and the absolute value of the trough height refers to the distance between the trough and the reference line, which is also a positive value.

[0069] Optionally, the surface flatness of the cutting surface passivation layer located on the non-laser affected area of ​​the cutting surface and near the geometric center area of ​​the cutting surface can be 50%, 43.7%, 40%, 36.7%, 35%, 32.1%, 30%, 27.9%, 26.8%, 25%, 24.6%, 25%, 23.1%, 22%, 20%, 14.3%, 10%, 6.7%, 5%, 1.2%, 0.4%, or 0.1% of the maximum thickness of the cutting surface passivation layer.

[0070] Optionally, in the laser affected area, the cut surface passivation layer covers the laser affected area; or, the cut surface passivation layer covers most of the laser affected area. That is to say, in the laser affected area, the cut surface passivation layer completely covers the laser affected area, that is, in the laser affected area, the surface area covered by the cut surface passivation layer accounts for 100% of the surface area of ​​the laser affected area, or, the cut surface passivation layer has a higher coverage ratio of the laser affected area, because the damage to the laser affected area is relatively large, and the cut surface passivation layer completely covers the laser affected area or most of the laser affected area, which can play a better passivation effect on the entire cell, reducing the risk of the laser affected area being exposed to the outside without being covered by the passivation layer. Alternatively, the laser affected area may have some convex parts, and the cut surface passivation layer only fails to cover the above-mentioned convex parts, but the pits outside the convex parts and the surroundings of the convex parts will be filled and covered by the cut surface passivation layer, so the passivation effect on the entire cell is also good.

[0071] It should be noted that the "vast majority" here may mean that: in the laser affected zone, the surface area covered by the passivation layer of the cut surface accounts for a proportion greater than or equal to 80% of the surface area of ​​the laser affected zone. For example, in the laser affected zone, the surface area covered by the passivation layer of the cut surface accounts for a proportion of 80%, 81%, 85%, 87.2%, 90%, 92.6%, 93%, 94.5%, 95%, 96.9%, 97%, 98%, 99.2%, 99.9% of the surface area of ​​the laser affected zone.

[0072] Optionally, in the non-laser affected area, the absolute value of the difference between the maximum thickness and the minimum thickness of the passivation layer on the cut surface is less than or equal to 50% of the maximum thickness. That is, in the non-laser affected area, the thickness of the passivation layer on the cut surface is relatively uniform, the surface of the passivation layer on the cut surface is relatively flat, and the passivation quality of the passivation layer on the cut surface is good.

[0073] For example, in the non-laser affected area, the absolute value of the difference between the maximum thickness and the minimum thickness of the passivation layer on the cutting surface can be 50%, 47.2%, 45%, 40%, 37.6%, 35%, 32.3%, 34%, 31%, 30%, 25%, 24.6%, 27%, 20%, 18.6%, or 15% of the maximum thickness.

[0074] Figure 1 This is a partial schematic diagram of the passivation layer on the cut surface in the non-laser affected area. Figure 1 As shown, the absolute value of the difference between the maximum thickness of the cut surface passivation layer and the minimum thickness of the cut surface passivation layer is: 4.987 μm-3.493 μm=1.494 μm, 4.987 μm×0.5=2.4935 μm, and 1.494 μm is less than 2.4935 μm.

[0075] Optionally, in the non-laser affected area, the absolute value of the difference between the maximum thickness and the minimum thickness of the passivation layer on the cutting surface is less than or equal to 50%, 43.7%, 40%, 36.7%, 35%, 32.1%, 30%, 27.9%, 26.8%, 25%, 24.6%, 25%, 23.1%, 22%, 20%, 14.3%, 10%, 6.7%, 5%, 1.2%, 0.4%, or 0.1% of the maximum thickness.

[0076] More specifically, when the maximum thickness of the passivation layer of the cutting surface is less than or equal to 2um, the surface flatness of the passivation layer of the cutting surface is less than or equal to 1um in the non-laser affected area and near the geometric center area of ​​the cutting surface; preferably, when the maximum thickness of the passivation layer of the cutting surface is less than or equal to 2um, the surface flatness of the passivation layer of the cutting surface is less than or equal to 600nm in the non-laser affected area and near the geometric center area of ​​the cutting surface, and the surface flatness of the passivation layer of the cutting surface on the non-laser affected area of ​​the cutting surface is smaller, that is, the surface flatness of the passivation layer of the entire cutting surface is basically smaller, and the thickness uniformity of the passivation layer of the entire cutting surface formed in the present application is better, and the passivation performance is better.

[0077] For example, when the maximum thickness of the passivation layer of the cutting surface is less than or equal to 2 um, the surface flatness of the passivation layer of the cutting surface in the non-laser affected area and near the geometric center area of ​​the cutting surface can be 600 nanometers, 540 nanometers, 570 nanometers, 500 nanometers, 465 nanometers, 400 nanometers, 390 nanometers, 360 nanometers, 350 nanometers, 320 nanometers, 300 nanometers, 290 nanometers, 277 nanometers, 260 nanometers, 250 nanometers, 100 nanometers, and 10 nanometers.

[0078] More specifically, when the maximum thickness of the passivation layer of the cutting surface is less than or equal to 5um, the surface flatness of the passivation layer of the cutting surface is less than or equal to 2.5um in the non-laser affected area and near the geometric center area of ​​the cutting surface; preferably, when the maximum thickness of the passivation layer of the cutting surface is less than or equal to 5um, the surface flatness of the passivation layer of the cutting surface is less than or equal to 2um in the non-laser affected area and near the geometric center area of ​​the cutting surface, and the surface flatness of the passivation layer of the cutting surface in the non-laser affected area of ​​the cutting surface is smaller, that is, the surface flatness of the passivation layer of the entire cutting surface is basically smaller, and the thickness uniformity of the passivation layer of the entire cutting surface formed in the present application is better, and the passivation performance is better.

[0079] For example, when the maximum thickness of the passivation layer of the cutting surface is less than or equal to 5um, the surface flatness of the passivation layer of the cutting surface in the non-laser affected area and near the geometric center area of ​​the cutting surface can be 2um, 1.73um, 1.5um, 1.2um, 1um, 990nm, 800nm, 600nm, 540nm, 570nm, 500nm, 465nm, 400nm, 390nm, 360nm, 350nm, 320nm, 300nm, 290nm, 277nm, 260nm, 250nm, 100nm, 10nm.

[0080] It should be noted that the edge area of ​​the cutting surface refers to: the area within 5um from the boundary line of the cutting surface, and the non-laser affected area mentioned in this application and close to the geometric center area of ​​the cutting surface may refer to: the area on the cutting surface except the edge area.

[0081] Optionally, the thickness of the passivation layer of the cutting surface near the edge area of ​​the cutting surface is less than the thickness of the passivation layer of the cutting surface near the geometric center area of ​​the cutting surface. The edge area of ​​the cutting surface refers to: the area within 5um from the boundary line of the cutting surface, and the area near the geometric center of the cutting surface refers to the area on the cutting surface except the edge area. That is, the passivation layer of the cutting surface is thicker near the geometric center of the cutting surface, and thinner near the boundary line of the cutting surface. The main reason may be that the passivation liquid is affected by gravity and surface tension, and then Figure 2As shown, the surface of the passivation layer on the cut surface is arc-shaped, which can increase the scattering and refraction of light, increase the optical path of light in the battery cell, increase the light absorption effect of the battery cell, and improve the performance of the battery cell. Figure 2 is a scanning electron microscope image (SEM) of the passivation layer of the cut surface of the present application, Figure 2 In the figure, the silicon substrate with lines on the left is the silicon substrate, and the passivation layer is on the right. The boundary between the two is relatively clear and smooth. For example, the thickness of the passivation layer on the cutting surface starts to decrease from the cutting surface geometry to the position near the boundary line of the cutting surface, and the thickness of the passivation layer on the cutting surface decreases to about 100nm.

[0082] Optionally, the thickness of the passivation layer of the cutting surface near the edge area of ​​the cutting surface is greater than the thickness of the passivation layer of the cutting surface near the geometric center area of ​​the cutting surface. The edge area of ​​the cutting surface refers to: the area within 5um from the boundary line of the cutting surface, and the area near the geometric center of the cutting surface refers to the area on the cutting surface except the edge area. That is, the passivation layer of the cutting surface is thinner near the geometric center of the cutting surface, and thicker near the boundary line of the cutting surface. The main reason may be the result of the action of the automated equipment, and then the surface of the passivation layer of the cutting surface is curved, which can increase the scattering and refraction of light, increase the optical path of light in the battery cell, increase the light absorption effect of the battery cell, and improve the performance of the battery cell.

[0083] Optionally, the thickness of the passivation layer on the cut surface is 30 nm to 10000 nm, which indicates that the process window of the present application is relatively wide and the controllable range is relatively large, and a suitable thickness can be selected according to the required passivation performance. For example, the thickness of the formed cutting surface passivation layer can be 30nm to 3000nm, or 200nm to 800nm. For another example, the thickness of the cutting surface passivation layer can be 30nm, 32.3nm, 35nm, 40nm, 43.5nm, 50nm, 53.1nm, 57.8nm, 60nm, 100nm, 150nm, 200nm, 300nm, 360nm, 400nm, 600nm, 700nm, 800nm, 1000nm, 1100nm, 1200nm, 1300nm, 1600nm, 2000nm, 2200nm, 2600nm, 3000nm, 5000nm, 8000nm, 9000nm, or 10000nm.

[0084] Optionally, the thickness of the cut surface passivation layer is 50nm to 8000nm. When the thickness of the cut surface passivation layer is within this range, the cut surface passivation layer has better passivation performance. For example, the thickness of the cut surface passivation layer can be 50nm, 56.1nm, 59nm, 60nm, 92nm, 140nm, 200nm, 280nm, 330nm, 423nm, 500nm, 647nm, 800nm, 1000nm, 1010nm, 1324nm, 1500nm, 1722nm, 1800nm, 2230nm, 2500nm, 3500nm, 5000nm, 6000nm, 7000nm, 8000nm.

[0085] For example, when the thickness of the passivation layer on the cut surface is 50 nm or more, the passivation effect is good, and the passivation effect will not decrease as the thickness of the passivation layer on the cut surface becomes thicker. In particular, when the thickness of the passivation layer on the cut surface is 1000 nm or more, the passivation effect is still effective and good. Moreover, the thickness of the passivation layer on the cut surface is relatively appropriate and can also cover the cutting burrs on the cutting edge, so that the position of the first surface close to the cutting edge and the position of the second surface close to the cutting edge are relatively flat, which can avoid damaging the conductive parts located here in the subsequently formed photovoltaic module.

[0086] Optionally, the cell further includes: a first surface and a second surface that intersect with the cutting surface, the first surface and the second surface are opposite, and one of the first surface and the second surface is the light-facing surface of the cell, and the other is the backlight surface of the cell. The first surface and the second surface both include a cutting edge adjacent to the cutting surface, and the cutting edge here is an intersection line that intersects with the first surface or the second surface in the cutting surface. There is no passivation layer of the cutting surface on the first surface, or the first surface is only coated with the passivation layer of the cutting surface on one side close to the cutting edge, and the passivation layer of the cutting surface introduced in the cell is less, or there is almost no plating, which improves the photoelectric conversion efficiency of the cell. And / or, there is no passivation layer of the cutting surface on the second surface, or the passivation layer of the cutting surface is only coated with the passivation layer of the cutting surface on one side close to the cutting edge, and the passivation layer of the cutting surface introduced in the cell is less, or there is almost no plating, which improves the photoelectric conversion efficiency of the cell.

[0087] Optionally, the first surface is coated with a passivation layer on only one side close to the cutting edge, and the metal area on the first surface is not covered by the passivation layer on the cutting surface; and / or the second surface is coated with a passivation layer on only one side close to the cutting edge; the metal area on the second surface is not covered by the passivation layer on the cutting surface. After the passivation layer on the cutting surface is coated on the first surface and / or the second surface of the battery cell, it does not cover the metal area of ​​the battery cell, which is equivalent to the passivation layer on the cutting surface not covering the effective working area of ​​the battery, or the coating position is the invalid working area of ​​the battery cell, so the coating of the present application does not affect the operation and photoelectric conversion efficiency of the battery. Wherein, there is a carrier transport layer of the battery cell below the metal area, and the metal area includes but is not limited to the collector electrode area, the bus electrode area, etc.

[0088] In addition, the passivation layer of the cut surface is often in the non-working area on the first surface or the second surface of the edge of the cell, that is, the non-effective area. It can be understood that although there is a carrier transport layer on the edge of the cell, there is no metal contact on this area and the current cannot be conducted outward, so the passivation layer of the cut surface does not affect the operation of the battery and the photoelectric conversion efficiency. Here, the edge of the cell refers to the position close to the cut edge on the first surface or the second surface.

[0089] Optionally, the cut surface passivation layer is plated on only one side of the first surface close to the aforementioned cutting edge, and the width of the cut surface passivation layer plated on the first surface is less than or equal to 0.5 mm. The cut surface passivation layer in the cell introduces less plating, or there is almost no plating. In addition, since the width of the cut surface passivation layer plated on the first surface is small, it is not plated to the metal area on the first surface, or the location of the plating is the invalid working area of ​​the cell, so the plating of the present application does not affect the operation and photoelectric conversion efficiency of the battery, and improves the photoelectric conversion efficiency of the cell. The width of the cut surface passivation layer plated here refers to: the maximum size of the cut surface passivation layer plated on the first surface in a direction perpendicular to the cutting edge on the first surface. If the cutting edge is a curve, it is perpendicular to its tangent here.

[0090] For example, the cutting surface passivation layer is plated on only one side of the first surface close to the aforementioned cutting edge, and the width of the cutting surface passivation layer plated on the first surface is 0.5mm, 0.4mm, 0.3mm, 0.25mm, 0.2mm, 0.18mm, 0.15mm, 0.1mm, 0.09mm, 0.07mm, 0.05mm, 0.01mm, 9000nm, 8000nm, 5000nm, 1000nm, 900nm, 700nm, 100nm, 90nm, 50nm, 10nm, 5nm.

[0091] Optionally, the cut surface passivation layer is plated on only one side of the second surface close to the cutting edge, and the width of the cut surface passivation layer plated on the second surface is less than or equal to 0.5 mm. The cut surface passivation layer in the cell introduces less plating, or almost no plating. In addition, since the width of the cut surface passivation layer plated on the second surface is small, it is not plated to the metal area on the second surface, or the location of the plating is the invalid working area of ​​the cell. Therefore, the plating of the present application does not affect the operation and photoelectric conversion efficiency of the battery, and improves the photoelectric conversion efficiency of the cell. The width of the cut surface passivation layer plated here refers to: the maximum size of the cut surface passivation layer plated on the second surface in the direction perpendicular to the cutting edge on the second surface. If the cutting edge is a curve, it is perpendicular to its tangent here.

[0092] For example, the cutting surface passivation layer is plated on only one side of the second surface close to the aforementioned cutting edge, and the width of the cutting surface passivation layer plated on the second surface is 0.5mm, 0.42mm, 0.3mm, 0.25mm, 0.2mm, 0.18mm, 0.15mm, 0.1mm, 0.08mm, 0.07mm, 0.05mm, 0.02mm, 9000nm, 6000nm, 5000nm, 2000nm, 900nm, 700nm, 500nm, 90nm, 50nm, 10nm, and 4nm.

[0093] Optionally, the thickness of the cut surface passivation layer of the wrap-around plated is less than or equal to the thickness of the cut surface passivation layer. For example, the thickness of the cut surface passivation layer of the wrap-around plated is 600nm, the thickness of the cut surface passivation layer is 1000nm, the thickness of the cut surface passivation layer of the wrap-around plated to the first surface, and / or, the thickness of the cut surface passivation layer on the second surface is smaller, and the wrap-around plated effect is smaller.

[0094] For example, the thickness of the cut surface passivation layer plated around the first surface, and / or on the second surface may be 60%, 50%, 40%, 30%, 26%, 25%, 20%, 17%, 15%, 11%, 10%, or 6% of the thickness of the cut surface passivation layer on the cut surface.

[0095] Optionally, the cell further includes: a surface passivation layer located on the first surface and the second surface, the surface passivation layer being used to protect the cell and reduce reflection. The surface passivation layer on the first surface is plated with the cut surface passivation layer only on one side close to the cutting edge, and / or the surface passivation layer on the second surface is plated with the cut surface passivation layer only on one side close to the cutting edge, and the width of the cut surface passivation layer plated on the surface passivation layer is less than or equal to 0.5 mm, that is, the surface passivation layer is formed first and then the cut surface passivation layer is formed, and the thickness of the cut surface passivation layer is 30 nanometers to 10000 nanometers, the thickness of the cut surface passivation layer is relatively thick, and can cover the cutting burrs of the cutting edge, etc., so that the position of the first surface close to the cutting edge and the position of the second surface close to the cutting edge are relatively flat, and in the subsequent process of forming the electrode by screen printing, the cutting burrs can be prevented from damaging the screen of the screen printing, and the life of the screen can be improved.

[0096] The present invention also provides a photovoltaic module, which includes a plurality of battery strings electrically connected to each other, and the battery strings can be connected in series or in parallel, which is not specifically limited. The battery string is formed by a plurality of battery cells as described above connected in series in sequence, and two adjacent battery cells in the battery string are connected by a conductive member to form an electrical connection. The photovoltaic module also has the same or similar beneficial effects as the aforementioned passivation method and battery cell, and will not be described here to avoid repetition.

[0097] Optionally, the conductive member passes through the plane where the passivation layer of the cut surface of the cell is located, that is, the conductive member on a cell passes through the plane where the passivation layer of the cut surface of the cell is located, and is connected to the next adjacent cell. The passivation effect of the passivation layer of the cut surface is good, which can prevent the risk of hidden cracks at the edge of the cell due to stress release through the series connection of the conductive member. In addition, the conductive member contacts or overlaps the edge of the passivation layer of the cut surface of the cell, which can reduce the risk of leakage and reduce the probability of burrs or protrusions on the edge of the cell damaging the conductive member.

[0098] The photovoltaic module may further include: packaging films located on opposite sides of the solar cell, etc., and other structures included in the photovoltaic module are not specifically limited.

[0099] The present invention provides a method for passivating a battery cell, referring to Figure 3 The passivation method of the battery cell may include the following steps.

[0100] Step 101, slicing the solar cell to obtain a cell sheet; the cell sheet includes a cutting surface formed by slicing.

[0101] The solar cell 1 can be sliced ​​by non-destructive cutting, such as laser grooving, followed by stress slicing or physical slicing. The method of slicing the solar cell 1 is not specifically limited in this application. The position 11 of the slice of the solar cell 1 is the cutting surface formed by the cell slice. There is no specific limitation on the specific morphology of the cutting surface, and the cutting surface can be a plane or a curved surface, which is not specifically limited. The cutting surface of the cell 2 is the area to be passivated. The number of cutting surfaces on a cell 2 is not specifically limited. For example, for 2-slicing, the number of cutting surfaces on a cell can be 1. For 3-slicing, the number of cutting surfaces on some cells is 1, and the number of cutting surfaces on some cells is 2. There is no specific limitation on the type of silicon substrate of the cell, which can be a monocrystalline silicon substrate, a polycrystalline silicon substrate, etc. The cell can be a double-sided cell, a back-contact cell, etc., and there is no specific limitation on the type of cell.

[0102] The number of cells 2 obtained by slicing the solar cell 1 is not specifically limited. Figure 2 In the process, the solar cell 1 can be cut along the midline of the light-facing surface and the backlight surface to obtain two half-sheets.

[0103] Optionally, the aforementioned step 101 may include: after the preparation of the passivation layers of the two opposite surface cut surfaces of the solar cell is completed, slicing is performed to obtain a cell, the passivation layers of the surface cut surfaces are used to protect the cell and reduce reflection, the solar cell includes a light-facing side and a backlight side in the thickness direction of the solar cell, the side that mainly receives light during normal operation of the solar cell is its light-facing side, the backlight side is opposite to the light-facing side, the two opposite surface cut surface passivation layers of the solar cell refer to: a front cut surface passivation layer located on the light-facing side of the solar cell and a back cut surface passivation layer located on the backlight side of the solar cell, the front cut surface passivation layer and the back cut surface passivation layer are opposite in the thickness direction of the solar cell, the front cut surface passivation layer and the back cut surface passivation layer both play a role in protecting the cell and reducing reflection. In the present invention, after forming the front cut surface passivation layer and the back cut surface passivation layer, slicing is performed, the cut surface will not be affected by the wet process and the coating process, the formed cut surface passivation layer film quality is good, and the cut surface passivation layer will not be affected by the wet process and the coating process, and the passivation effect of the cut surface passivation layer is good.

[0104] It should be noted that before setting the surface cut surface passivation layer for the solar cell, a functional layer is usually set on the solar cell, and the above-mentioned functional layer mainly plays the role of carrier transport. In the present invention, after the preparation of the two opposite surface cut surface passivation layers, slicing can be performed before the metal electrode is made, or slicing can be performed after the metal electrode is made, without specific limitation. When slicing is performed after the metal electrode is made, the cut surface will not be affected by the metal electrode process, and the formed cut surface passivation layer film has better quality. Moreover, the cut surface passivation layer will not be affected by the metal electrode process, and the passivation effect of the cut surface passivation layer is better.

[0105] Step 102, coating a passivation liquid on the cut surface of the cell to form a cut surface passivation layer; the particle size of the passivation material in the cut surface passivation layer is less than or equal to 150 nanometers.

[0106] There is no limitation on the specific composition of the passivation liquid. Optionally, the passivation material of the cut surface passivation layer formed can be selected from at least one of aluminum oxide, silicon oxide, and titanium oxide. The passivation liquid can be in the form of a solution, a suspension, a precursor liquid, a colloid, etc., and there is no specific limitation on the form of the passivation liquid. In the cut surface passivation layer formed, the passivation material is at least one of aluminum oxide, silicon oxide, and titanium oxide. At the same time, the passivation liquid is used to form the cut surface passivation layer, and the particle size of the passivation material is less than or equal to 150 nanometers. The passivation layer thus formed is denser and smoother, and has better passivation performance. Optionally, the passivation material of the cut surface passivation layer in the present invention is selected from at least one of aluminum oxide, silicon oxide, and titanium oxide, which has a good passivation effect on the cut surface, further improving the photoelectric conversion efficiency of the battery cell. In summary, the battery cell provided by the present invention has almost no winding plating, and the process equipment is greatly simplified, thereby reducing the process energy consumption and product cost, and the process efficiency is high, with less damage to the battery cell, a wide processing window, a high product yield, and a good passivation effect on the cut surface.

[0107] The method of coating the passivation liquid 3 on the cut surface of the battery cell 2 may include: at least one of immersion, scraping, slit coating, spraying, printing, and roll coating. The coating method is flexible and diverse and suitable for a variety of scenarios. In addition, the above coating method can also improve the distribution uniformity of the formed liquid film, so that the formed cut surface passivation layer is more uniform. It should be noted that the printing here may include: at least one of screen printing, transfer printing, roll-to-roll printing, and 3D printing.

[0108] Reference Figure 4, when the coating method is the immersion method, the depth of the battery cell contacting the passivation solution is less than or equal to 4 millimeters (mm), specifically, the height of the battery cell immersed in the passivation solution is less than or equal to 4 millimeters, and the formed cut surface passivation layer can not only meet the passivation requirements, but also basically has no plating around. The battery cell is immersed in the passivation solution, which means that the battery cell is immersed in the passivation solution in the direction in which the cut surface of the battery cell is closest to the passivation solution, or in other words, the battery cell is immersed in the passivation solution in the direction in which the cut surface of the battery cell and the liquid surface of the passivation solution are relative. The height of the battery cell immersed in the passivation solution refers to: the maximum size of the part of the battery cell that penetrates into the passivation solution in the direction in which the cut surface of the battery cell is closest to the passivation solution. In other words, the height of the battery cell immersed in the passivation solution refers to: the maximum size of the part of the battery cell that penetrates into the passivation solution in the direction perpendicular to the liquid surface of the passivation solution. For example, the passivation liquid is contained in a container, and the height of the battery cell immersed in the passivation liquid can be 4mm, 3.7mm, 3.5mm, 3.4mm, 3mm, 2.9mm, 2.1mm, 2mm, 1.9mm, 1.5mm, 1.4mm, 1.3mm, 1.89mm, 1.1mm, 1.8mm, 1mm, 0.97mm, 0.9mm, 0.74mm, and 0.5mm.

[0109] Optionally, when the coating method is any one of scraping, slit coating, spraying, printing, and roller coating other than immersion, the height of the battery cell in contact with the passivation solution is less than or equal to 2 mm, and the formed cut surface passivation layer can not only meet the passivation requirements, but also basically has no plating around. The battery cell contacts the passivation solution means that the battery cell is contacted with the passivation solution in the direction in which the cut surface of the battery cell is closest to the passivation solution, or in other words, the battery cell is contacted with the passivation solution in the direction in which the cut surface of the battery cell and the liquid surface of the passivation solution are relative. The height of the battery cell in contact with the passivation solution refers to: the maximum size of the part of the battery cell in contact with the passivation solution in the direction in which the cut surface of the battery cell is closest to the passivation solution. In other words, the height of the battery cell in contact with the passivation solution refers to: the maximum size of the part of the battery cell in contact with the passivation solution in the direction perpendicular to the liquid surface of the passivation solution. For example, the height at which the battery cell contacts the passivation solution may be 2 mm, 1.9 mm, 1.73 mm, 1.5 mm, 1.33 mm, 1.89 mm, 1.21 mm, 1.8 mm, 1 mm, 0.97 mm, 0.9 mm, 0.74 mm, or 0.5 mm.

[0110] It should be noted that the wrap plating mentioned in the full text refers to the formation of a cut surface passivation layer on the remaining surfaces of the cell except the cut surface. In the related art, ALD is used to form a cut surface passivation layer, and usually wrap plating is performed on each surface of the cell. If the process of forming the cut surface passivation layer is completed after the electrode is formed, the wrap-plated cut surface passivation layer will affect the conductive interconnection points on the front and back of the cell, such as welding points, etc., resulting in poor contact, and will cause local EL (electroluminescence or field luminescence) dark spots, affecting the performance and quality of the cell. In the related art, ALD is used to form a cut surface passivation layer. If the process of forming the cut surface passivation layer is completed before the electrode is formed, the wrap-plated cut surface passivation layer is not conductive, resulting in the electrode formed on it being unable to conduct the current in the area, which also leads to a decrease in the performance of the cell. Through the improvement of the present application, since there is basically no wrap plating in the cell, the performance and quality of the cell are good.

[0111] A passivation liquid is coated on the cut surface of the battery cell 2 to form a passivation liquid film, and activated to obtain a passivation layer on the cut surface. The activation here refers to a process in which the passivation layer on the cut surface has a good passivation effect after heating. The passivation liquid film here can be dried in an environment of normal temperature and pressure, and then heated and activated by a heating device 4, or the passivation liquid film here can be dried in a heating device 4, and activated simultaneously during the heating and drying process, which is not specifically limited.

[0112] Optionally, the temperature during the activation process is less than or equal to 600°C, and the activation temperature is more suitable. On the one hand, the passivation effect of the cut surface passivation layer 21 activated at this activation temperature is better. On the other hand, this activation temperature will basically have no adverse effects on other structures of the battery cell, and is suitable for various types of battery cells.

[0113] For example, the temperature during the activation process can be 200°C to 600°C. For another example, the temperature during the activation process can be 80°C, 100°C, 200°C, 220°C, 273°C, 280°C, 299°C, 300°C, 330°C, 370°C, 400°C, 500°C, or 600°C.

[0114] There is no specific limitation on the duration of activation. For example, the duration of activation may be 3 to 10 minutes.

[0115] In the present invention, firstly, the gaseous raw material is replaced by the passivation liquid, and the passivation liquid does not have the spatial diffusion phenomenon, and the cut surface passivation layer is formed only in the passivation liquid contact area, so the selectivity of the film-forming area is strong, and there is almost no plating, which improves the photoelectric conversion efficiency of the battery cell. Secondly, the passivation liquid is relatively stable and non-toxic in the air, avoiding the flammable and explosive risks brought by hazardous chemicals, so the process can be carried out at room temperature and pressure, and the passivation liquid is used to form the cut surface passivation layer without a vacuum environment, reducing the safety protection, alarm, vacuum and other functional modules of the equipment, greatly simplifying the process equipment, and thus reducing the process energy consumption and product cost. Thirdly, the process time of forming the cut surface passivation layer by the passivation liquid is short, the process efficiency of forming the cut surface passivation layer is high, the thickness range of the cut surface passivation layer formed by the passivation liquid is relatively wide, and the formation of the cut surface passivation layer of the required thickness is easy to achieve, and according to the principle of chemical reaction kinetics, the shorter the contact time, the smaller the damage, and the shorter the process time further reduces the damage to the battery cell. In addition, a passivation liquid is used to form a passivation layer for the cut surface, and the thickness and coverage of the passivation layer for the cut surface are easy to control, so that the method has a wide processing window and a high product yield. The material of the passivation layer for the cut surface formed in the present invention is selected from at least one of aluminum oxide, silicon oxide, and titanium oxide, and has a good passivation effect on the cut surface, further improving the photoelectric conversion efficiency of the battery cell. In summary, the passivation method for the battery cell provided by the present invention has almost no plating, greatly simplifies the process equipment, thereby reducing process energy consumption and product cost, and has high process efficiency, less damage to the battery cell, a wide processing window, a high product yield, and a good passivation effect on the cut surface.

[0116] More specifically, within the same time period, the cut surface of the battery cell is passivated using the ALD method of the related art, and the cut surface of the battery cell is passivated using the passivation method of the present application. The comparison results of the two are shown in Table 1 below.

[0117] Table 1: Comparison of passivation results

[0118]

[0119] It can be concluded from Table 1 that within the same length of time, the thickness of the cut surface passivation layer formed on the cut surface of the cell by the present application has reached 30nm to 10000nm, but the thickness of the cut surface passivation layer formed on the cut surface of the cell by the ALD method has only reached 10nm to 50nm. It can be seen that the speed of forming the cut surface passivation layer in the passivation method of the present application is significantly faster than that in the ALD method. The first surface and the second surface in Table 1 both intersect with the cut surface of the cell, and the first surface and the second surface are opposite to each other. Of the first surface and the second surface here, one is the light-facing surface of the cell, and the other is the backlight surface of the cell. During the normal operation of the cell, the surface that mainly absorbs light is the light-facing surface, and the backlight surface is opposite to the light-facing surface. It can be concluded from Table 1 above that in the process of forming the cut surface passivation layer by the present application, the winding plating is also significantly less than the winding plating by the ALD method. Moreover, as the preparation time is greatly extended, the thickness of the cut surface passivation layer formed by the ALD method will basically not exceed 50nm. The thickness of the cut surface passivation layer formed by the ALD method is relatively small, and it is difficult to form a thicker cut surface passivation layer, and the passivation effect is poor. In addition, the passivation method of the battery cell of the present application usually takes less than or equal to 5 minutes to form a cut surface passivation layer of appropriate thickness on the cut surface of the battery cell, while the time required by the ALD method is much longer than 5 minutes, and the passivation method of the present application is more efficient.

[0120] Optionally, before the aforementioned step 101, the method may further include: configuring the aforementioned passivation solution with a solute and a solvent, the passivation solution being at least one of a solution, a suspension, a colloid, and a precursor liquid, and the specific passivation solution being a suspension, a solution, a colloid, or a precursor liquid is not specifically limited. In the case where the passivation solution is a suspension, the particle size of the solute of the suspension is less than or equal to 150 nm, and the particle size of the solute is small, which is conducive to forming a dense and uniform cut surface passivation layer. The surface tension of the passivation solution relative to the silicon substrate of the battery cell can be adjusted to reduce the diffusion range of the passivation solution, which can ensure that the battery cell has almost no plating. The particle size of the solute refers to the diameter or equivalent diameter of the solute.

[0121] For example, when the passivation solution is a suspension, the particle size of the solute of the suspension can be 150nm, 140nm, 120nm, 110nm, 100nm, 97nm, 90nm, 80nm, 70nm, 60nm, 50nm, 43nm, or 30nm.

[0122] Optionally, the passivation liquid can be a suspension, which is relatively mild and has little damage to the battery cell. In the related art, TMA (trimethylaluminum) is used in the process of forming the passivation layer of the cut surface by ALD. TMA is a metal organic reagent and a strong alkaline liquid. Experiments show that organic reagents, strong acids, and strong alkalis all have a relatively serious corrosive effect on battery cells. Therefore, compared with the related art, the passivation liquid in this application is a suspension, which can reduce the damage to the battery cell.

[0123] The cut surface passivation layer formed in the present application is dense and uniform, the thickness uniformity of the cut surface passivation layer is good, and the passivation performance is good. The cut surface passivation layer formed in the present application has a high coverage of the cut surface, or in other words, the surface area of ​​the cut surface of the battery cell covered by the cut surface passivation layer accounts for a proportion greater than or equal to 90% of the surface area of ​​the cut surface of the battery cell. Since the cut surface passivation layer has a high coverage of the cut surface, the passivation effect on the cut surface of the battery cell is better. The surface area of ​​the cut surface of the battery cell covered by the cut surface passivation layer refers to: the surface area of ​​the cut surface of the battery cell covered by the cut surface passivation layer.

[0124] By adopting the passivation method of the present application, the photoelectric conversion efficiency of the cell can be increased by at least 0.1%. For example, taking the back contact cell as an example, the cell performance of the cell before and after the passivation cutting surface is tested under the same test conditions, and the test results are shown in Table 2 below.

[0125] Table 2: Comparison of cell performance before and after passivation

[0126] state <![CDATA[Jsc(mA / cm 2 )]]> Voc(V) FF(%) Eff(%) Before passivation 41.0 0.740 81.3 24.66 After passivation 41.1 0.741 81.6 24.87

[0127] In Table 2, Jsc is the short-circuit current density of the cell, Voc is the open-circuit voltage, FF is the fill factor, and Eff is the conversion efficiency. It can be concluded from Table 2 that after the passivation of the present application, the conversion efficiency of this type of back-contact cell is increased by more than 0.1%.

[0128] It should be noted that, for the method embodiments, for the sake of simplicity of description, they are all expressed as a series of action combinations, but those skilled in the art should be aware that the embodiments of the present application are not limited by the described order of actions, because according to the embodiments of the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions involved are not necessarily required by the embodiments of the present application.

[0129] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0130] Through the description of the above implementation methods, those skilled in the art can clearly understand that the above-mentioned embodiment methods can be implemented by means of software plus a necessary general hardware platform, and of course by hardware, but in many cases the former is a better implementation method. Based on such an understanding, the technical solution of the present invention, or the part that contributes to the prior art, can be embodied in the form of a software product, which is stored in a storage medium (such as ROM / RAM, a magnetic disk, or an optical disk), and includes a number of instructions for enabling a terminal (which can be a mobile phone, a computer, a server, an air conditioner, or a network device, etc.) to execute the methods described in each embodiment of the present invention.

[0131] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A battery cell, characterized in that: include: Cutting surface; The cutting surface is formed in the process of slicing the solar cell to form the cell; A cutting surface passivation layer, located on the cutting surface; The cut surface passivation layer is formed by means of a passivation liquid; The particle size of the passivation material in the cut surface passivation layer is less than or equal to 150 nanometers.

2. The battery cell according to claim 1, characterized in that: The cut surface passivation layer covers the surface area of ​​the cut surface, and the proportion of the surface area of ​​the cut surface to be covered by the passivation layer is greater than or equal to 90%.

3. The battery cell according to claim 1, characterized in that: The cutting surface comprises: a laser-affected area and a non-laser-affected area, wherein the cutting surface passivation layer covers the laser-affected area; Alternatively, the cut surface passivation layer covers most of the laser affected area.

4. The battery cell according to claim 1, characterized in that: The cutting surface comprises: a laser-affected area and a non-laser-affected area. In the non-laser-affected area, the absolute value of the difference between the maximum thickness and the minimum thickness of the passivation layer of the cutting surface is less than or equal to 50% of the maximum thickness.

5. The battery cell according to claim 1, characterized in that: The cutting surface includes: a laser-affected area and a non-laser-affected area. On the non-laser-affected area and near the geometric center of the cutting surface, the surface flatness of the cutting surface passivation layer is less than or equal to 50% of the maximum thickness of the cutting surface passivation layer.

6. The battery cell according to claim 1, characterized in that: The thickness of the cutting surface passivation layer in the edge region close to the cutting surface is smaller than the thickness of the cutting surface passivation layer in the geometric center region close to the cutting surface.

7. The battery cell according to claim 1, characterized in that: The thickness of the cutting surface passivation layer in the edge region close to the cutting surface is greater than the thickness of the cutting surface passivation layer in the geometric center region close to the cutting surface.

8. The battery cell according to claim 1, characterized in that: The thickness of the cut surface passivation layer is 30 nm to 10000 nm; preferably, the thickness of the cut surface passivation layer is 50 nm to 8000 nm.

9. The battery cell according to any one of claims 1 to 8, characterized in that: The battery cell further includes: a first surface and a second surface both intersecting the cutting surface; the first surface and the second surface are opposite to each other; the first surface and the second surface both include cutting edges adjacent to the cutting surface; The first surface does not have the cutting surface passivation layer, or the first surface is only plated with the cutting surface passivation layer on one side close to the cutting edge; and / or, The second surface does not have the cutting surface passivation layer, or the second surface is plated with the cutting surface passivation layer only on one side close to the cutting edge.

10. The battery cell according to claim 9, characterized in that: The cut surface passivation layer is plated around only one side of the first surface close to the cut edge, and the cut surface passivation layer is plated around but does not cover the metal area on the first surface; and / or, The cut surface passivation layer is plated around only one side of the second surface close to the cut edge; the cut surface passivation layer is plated around but does not cover the metal area on the second surface.

11. The battery cell according to claim 9, characterized in that: Also includes: a surface passivation layer located on the first surface and the second surface; The cut surface passivation layer is plated around the surface passivation layer on only one side of the first surface close to the cut edge; and / or, The cut surface passivation layer is plated around the surface passivation layer on only one side of the second surface close to the cut edge; Wherein, the surface passivation layer is used to protect the battery cell and reduce reflection.

12. The battery cell according to claim 9, characterized in that: The thickness of the cut surface passivation layer plated around the substrate is less than or equal to the thickness of the cut surface passivation layer.

13. A photovoltaic module, characterized in that: include: A plurality of battery strings electrically connected to each other, wherein the battery string is formed by connecting a plurality of battery cells according to any one of claims 1 to 12 in series in sequence; Two adjacent battery cells in the battery string are connected by a conductive member; The conductive member passes through the plane where the passivation layer of the cut surface of the battery cell is located.

14. A method for passivating a battery cell, characterized in that: include: Slicing the solar cell to obtain a cell sheet; The battery cell includes a cutting surface formed by slicing; Coating a passivation solution on the cut surface of the battery cell to form a cut surface passivation layer; The particle size of the passivation material in the cut surface passivation layer is less than or equal to 150 nanometers.

15. The method for passivating a battery cell according to claim 14, characterized in that: Also includes: The passivation solution is formed by configuring a solute and a solvent; The passivation liquid is at least one of a solution, a suspension, a colloid, and a precursor liquid.

16. The method for passivating a battery cell according to claim 15, characterized in that: When the coating is performed by immersion, the height of the battery cell in contact with the passivation solution is less than or equal to 4 mm; When the coating is performed by a method other than the immersion method, the height of the battery cell in contact with the passivation solution is less than or equal to 2 mm.

Citation Information

Cited By

  • Preparation method of solar cell and solar cell

    CN120187147A

  • Solar cell and photovoltaic module

    CN121013509A

  • Solar cells and photovoltaic modules

    CN121013509B

  • Solar cell and photovoltaic module

    US12701820B2

  • Solar cell and photovoltaic module

    WO2025171776A1