Heterogeneous crystalline silicon battery and preparation method thereof

By performing double-sided texturing and polishing on the back of the silicon wafer of the heterogeneous crystalline silicon cell, a pyramid textured structure is formed, which solves the problems of amorphous silicon film uniformity and light absorption performance, and improves the conversion efficiency and reliability of the cell. And optimize the production process and reduce costs.

CN118738166APending Publication Date: 2024-10-01TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411105124.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

During the preparation process of heterogeneous crystalline silicon cells, the light absorption performance is reduced due to the poor uniformity of the amorphous silicon film and the thin silicon wafer, which affects the conversion efficiency.

Method used

A double-sided texturing process is used to form a mask layer on the back of the silicon wafer, and the non-busbar area mask is removed and polished to form a pyramid textured structure, which improves the uniformity of amorphous silicon film layer deposition and long-wave spectrum internal reflection, and enhances the battery's performance. Optical properties.

Benefits of technology

It improves the photoelectric conversion efficiency and reliability of heterogeneous crystalline silicon cells, reduces production costs, meets environmental protection requirements, and improves the overall performance and consistency of components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738166A_ABST
    Figure CN118738166A_ABST
Patent Text Reader

Abstract

The invention discloses a heterogeneous crystalline silicon battery and a preparation method thereof, the whole front surface and a back surface main grid region of the prepared heterojunction battery have textured structures, and meanwhile, a back surface non-main grid region is a polished surface structure; the whole front surface of the heterojunction cell keeps a textured structure with better light trapping property, and the back surface is polished by a non-main gate region, so that the deposition uniformity of an intrinsic amorphous silicon thin layer is improved, the electrical property of the heterojunction cell is improved, the internal reflection of a long-wave spectrum can be increased, the short-circuit current is increased, and the conversion efficiency of the cell is improved; meanwhile, the textured design of the back main gate region can enhance the pull-out force of the gate lines and improve the reliability of the module; the method is simple in process step, easy to operate and suitable for mass production application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of solar cells, and in particular to a heterogeneous crystalline silicon cell and a preparation method thereof. Background Art

[0002] Heterojunction with intrinsic thin layer (HJT) solar cells are attracting more and more attention in the industry. The structure of heterojunction cells is usually centered on an N-type silicon substrate. A layer of intrinsic amorphous silicon thin film is deposited between doped amorphous silicon (P-type and N-type) and the N-type silicon substrate. After taking this process measure, the performance of the PN junction is improved, and the conversion efficiency of heterojunction solar cells is improved. The heterojunction symmetrical cell structure and low-temperature manufacturing process make it suitable for thin-film production. The thinning of silicon wafers has a certain impact on the optical and electrical properties of the cell. Research on improving the optical and electrical properties of heterojunction cells is becoming a hot topic.

[0003] After texturing, a layer of intrinsic amorphous silicon film needs to be deposited on the heterojunction cell. Since the thickness of the amorphous silicon film is at the nanometer level, while the size of the textured pyramid is at the micrometer level, the texture will affect the uniformity of the intrinsic amorphous silicon deposition, thereby affecting the passivation performance of the amorphous silicon film. On the other hand, heterojunction cells usually use thinner silicon wafers due to their symmetrical structure and for cost reduction considerations. Thin silicon wafer heterojunction cells have a certain degree of reduction in light absorption performance. Therefore, in order to improve the cell conversion efficiency, it is necessary to compensate for the optical aspects of the heterojunction cell. Summary of the invention

[0004] The object of the present invention is to provide a heterogeneous crystalline silicon cell and a method for preparing the same, so as to improve the performance and reliability of the heterogeneous crystalline silicon cell.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides a method for preparing a heterogeneous crystalline silicon cell, comprising:

[0006] Providing a silicon wafer having a front side and a back side opposite to each other;

[0007] Performing double-sided texturing on the silicon wafer to obtain a first texturing structure and a second texturing structure respectively;

[0008] forming a mask layer on the back side of the silicon wafer and performing patterning to expose the back side non-main gate region; and

[0009] The back non-main grid area is polished to form a polished surface, and the tower base height of the polished surface is less than 0.5 μm.

[0010] Optionally, the first velvet structure and the second velvet structure have a pyramid velvet morphology, the base width of the pyramid velvet is 0.5 to 8 μm, and the front reflectivity is 8% to 15%.

[0011] Optionally, the tower base width of the polished surface is 8 to 20 μm, and the reflectivity is 30% to 38%.

[0012] Optionally, after the double-sided texturing, the method further includes: forming a mask on the front side of the silicon wafer.

[0013] Optionally, a silicon nitride or silicon oxide mask is deposited on the front and back sides of the silicon wafer, and the mask thickness is 20 to 80 nm.

[0014] Optionally, the process of patterning to expose the back non-bus grid area includes: printing a corrosive slurry on the back non-bus grid area to remove a mask layer of the back non-bus grid area.

[0015] Optionally, after removing the mask layer of the back non-main gate area, the method further includes the step of: cleaning with a photoresist remover, and the cleaning time does not exceed 30 seconds.

[0016] Optionally, the cleaning process uses a dilute hydrofluoric acid solution, hot sulfuric acid, oxygen plasma, an organic solvent or an alkaline solution for cleaning;

[0017] Wherein, the volume concentration of the dilute hydrofluoric acid solution is less than 1%.

[0018] Optionally, in the process of polishing the non-main gate area, the polishing liquid is a KOH solution or a NaOH solution.

[0019] Optionally, after polishing the back non-main gate area, the method further includes the steps of removing the remaining mask layer and cleaning the silicon wafer.

[0020] The present invention also provides a heterogeneous crystalline silicon cell, wherein the front side of the heterogeneous crystalline silicon cell has a first velvet structure on the entire surface, the rear main grid region has a second velvet structure, and the rear non-main grid region is a polished surface.

[0021] Optionally, the first velvet structure and the second velvet structure have a pyramid velvet morphology, the base width of the pyramid velvet is 0.5 to 8 μm, and the front reflectivity is 8% to 15%.

[0022] Optionally, the tower base height of the polished surface is less than 0.5 μm, the tower base width is 8 to 20 μm, and the reflectivity is 30% to 38%.

[0023] The present invention provides a heterogeneous crystalline silicon cell and a preparation method thereof. After double-sided texturing, a mask layer is formed on the back side of a silicon wafer, the mask of the non-main grid area on the back side is removed, and then the non-main grid area on the back side is polished. The heterogeneous crystalline silicon cell thus prepared has a pyramid texturing surface on the entire front side and the main grid area on the back side, thereby ensuring that the light trapping capability of the heterojunction on the front side is improved. The non-main grid area on the back side is a polishing surface, thereby enhancing the uniformity of deposition of the amorphous silicon film layer and improving the internal reflection of the long-wave spectrum, thereby increasing the utilization rate of the long-wave spectrum, while ensuring that the texturing structure of the main grid area on the back side can form better contact with the low-temperature metal slurry, thereby enhancing the pull-off force of the grid line and improving the reliability of the component. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a flow chart of a method for preparing a heterogeneous crystalline silicon cell according to an embodiment of the present invention;

[0025] Figure 2 It is a schematic diagram of the structure after double-sided velveting in an embodiment of the present invention;

[0026] Figure 3 It is a schematic diagram of the structure after a mask layer is formed on the back side of a silicon wafer in an embodiment of the present invention;

[0027] Figure 4 is a schematic diagram of a structure after patterning is performed on a mask layer in an embodiment of the present invention;

[0028] Figure 5 It is a schematic diagram of the structure after polishing in an embodiment of the present invention.

[0029] In the figure, 1, front side; 101, first velvet structure; 2, back side; 21, back side main grid area; 22, back side non-main grid area; 201, second velvet structure; 3, mask layer. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The serial numbers of the components herein, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" and "coupling" mentioned in this application, unless otherwise specified, include direct and indirect connections (couplings). In the description of the present invention, it should be understood that the orientation or positional relationship indicated by the terms "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc. are based on the orientation or positional relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation to the present invention.

[0032] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0033] The present invention is described in more detail in the following paragraphs by way of example with reference to the accompanying drawings. The advantages and features of the present invention will become more apparent from the following description and claims. It should be noted that the drawings are in very simplified form and in non-precise proportions, and are only used to facilitate and clearly assist in illustrating the purpose of the embodiments of the present invention.

[0034] Embodiment 1

[0035] Please refer to Figure 1 - Figure 5 This embodiment provides a method for preparing a heterogeneous crystalline silicon cell, comprising the steps of:

[0036] S1. providing a silicon wafer, wherein the silicon wafer has a front side 1 and a back side 2 opposite to each other;

[0037] S2, performing double-sided texturing on the silicon wafer to obtain a first textured structure 101 and a second textured structure 201 respectively;

[0038] S3, forming a mask layer 3 on the back side 2 of the silicon wafer, and performing patterning to expose the back side non-main gate region 22; and

[0039] S4, polishing the back non-main grid region 22 to form a polished surface, wherein the tower base height of the polished surface is less than 0.5 μm.

[0040] In step S1, preferably, the silicon wafer is an N-type silicon substrate.

[0041] Please continue to refer to Figure 2 In step S2, the first velvet structure 101 and the second velvet structure 201 both have a pyramid velvet morphology, the base width of the pyramid velvet is 0.5 to 8 μm, and the front reflectivity is 8% to 15%.

[0042] Specifically, in this embodiment, a 20-50wt% KOH solution or a 5-10wt% NaOH solution is used to react at a temperature of 75-82°C for 4-12 minutes, and an anisotropic corrosion reaction occurs on the surface of the silicon wafer to generate a surface positive pyramid morphology.

[0043] In step S2, the silicon wafer is subjected to double-sided texturing treatment to form the first textured structure 101 and the second textured structure 201, and a microstructure is created by using chemical or mechanical methods such as acid etching or grinding to improve the light absorption rate of the silicon wafer.

[0044] By texturing both sides of the silicon wafer, the light absorption area of ​​the silicon wafer surface is increased, thereby improving the photoelectric conversion efficiency of the battery. The textured structure helps to reduce reflection loss and increase light absorption.

[0045] Please continue to refer to Figure 3 In step S3, a mask layer 3 is formed on the back side 2 of the silicon wafer. The mask layer 3 may be made of photoresist, oxide or other materials to protect the silicon wafer from being damaged in subsequent processing steps.

[0046] Depositing the mask layer 3 helps to protect the surface of the silicon wafer and reduce surface damage during subsequent processing, thereby improving the electrical performance of the battery.

[0047] Furthermore, after step S2, the method further includes: forming a mask layer 3 (not shown) on the front side 1 of the silicon wafer.

[0048] In this embodiment, preferably, a silicon nitride or silicon oxide mask is deposited on the front side 1 and the back side 2 of the silicon wafer, respectively, and the mask thickness is 20-80 nm.

[0049] Preferably, the mask layer 3 is formed on both the front and back sides of the silicon wafer, which is beneficial to integrally protect the silicon wafer.

[0050] Please continue to refer to Figure 4 In step S3 , the process of patterning the mask layer 3 to expose the back non-bus grid area 22 includes: printing a corrosive acidic slurry on the back non-bus grid area 22 to remove the mask layer 3 of the back non-bus grid area.

[0051] The mask layer 3 of the non-main gate area 22 on the back side is removed so that only a specific area is exposed, which facilitates the subsequent polishing process in a targeted manner and improves the processing accuracy and efficiency.

[0052] After removing the mask of the back non-main gate region 22, the back non-main gate region 22 of the silicon wafer is polished. In a specific example, the polishing may use a chemical mechanical polishing (CMP) method or other suitable polishing technology to obtain a smooth surface.

[0053] The polishing treatment of the back non-main grid area 22 can reduce surface defects, improve the mechanical strength of the silicon wafer and the long-term stability of the battery, and reduce the performance degradation of the battery during long-term use.

[0054] In this embodiment, after step S3 exposes the back non-main gate region 22 , the step S3 further includes the step of: performing cleaning, and the cleaning time does not exceed 30 seconds.

[0055] The cleaning process is carried out using a dilute hydrofluoric acid solution, hot sulfuric acid, oxygen plasma, an organic solvent or an alkaline solution.

[0056] Preferably, a dilute hydrofluoric acid solution is used for cleaning, wherein the volume concentration of the dilute hydrofluoric acid solution is less than 1%, so as to ensure that the mask of the back non-main gate region 22 is completely removed.

[0057] Please continue to refer to Figure 5 In step S4, during the process of polishing the back non-main gate area 22, the polishing liquid is a KOH solution or a NaOH solution.

[0058] Furthermore, after polishing, the back non-main grid region 22 is a polished surface, the tower base width of the polished surface is 8 to 20 μm, and the reflectivity is 30% to 38%.

[0059] After step S4, after polishing the back non-main gate region 22, the process further includes the steps of removing the remaining mask layer 3 and cleaning the silicon wafer.

[0060] In step S4, the silicon wafer is cleaned by RCA cleaning, which may specifically include the following steps:

[0061] SC-1 cleaning (standard cleaning 1):

[0062] SC-1 cleaning fluid is usually composed of NH4OH (ammonia water), H2O2 (hydrogen peroxide) and H2O (water) with a concentration ratio of 1:1:5 to 1:2:7; SC-1 cleaning is used to remove organic matter, particles and some metal ions.

[0063] During the cleaning process, the silicon wafer is immersed in SC-1 cleaning solution for 3 to 5 minutes and then rinsed at room temperature.

[0064] SC-2 cleaning (standard cleaning 2):

[0065] SC-2 cleaning fluid is composed of HCl (hydrochloric acid), H2O2 (hydrogen peroxide) and H2O (water) with a concentration ratio of 1:1:6 to 1:2:7; SC-2 cleaning is used to remove inorganic particles and metal ions.

[0066] During the cleaning process, the silicon wafer is immersed in the solution for a period of time, usually at a temperature of about 80°C, to enhance the cleaning effect.

[0067] Rinse:

[0068] After the above two cleaning steps, the silicon wafer needs to be thoroughly rinsed with high-purity water to remove residual chemicals.

[0069] Drying:

[0070] After cleaning and rinsing, the silicon wafer needs to be dried. Drying methods include nitrogen blowing, centrifugal drying or hot plate drying.

[0071] In other examples, the way the silicon wafers are cleaned can be adjusted based on needs and existing conditions.

[0072] In summary, this embodiment provides a method for preparing a heterogeneous crystalline silicon cell, after the double-sided texturing of the silicon wafer, a mask layer is formed on the back of the silicon wafer, and an acid corrosive slurry is printed or sprayed on the non-main grid area on the back to remove the mask of the non-main grid area on the back, and then the non-main grid area on the back is polished; by improving the polishing method of the back of the silicon wafer in the process of preparing the heterogeneous crystalline silicon cell, this embodiment makes up for the optical aspect of the heterojunction cell to reduce the reflection on the cell surface, improve the light utilization rate and the overall performance of the cell, and enhance the anti-reflection ability of the cell; in addition, in this embodiment, by optimizing the process flow, reducing unnecessary material consumption and processing steps, the production cost is reduced and the market competitiveness of the product is improved; the use of chemicals and the generation of waste are reduced, which is more in line with environmental protection requirements and is conducive to achieving sustainable production; due to the standardization and precise control of the process steps, it can be ensured that the produced batteries have high consistency, which is convenient for large-scale production and management.

[0073] Embodiment 2

[0074] An embodiment of the present invention provides a heterogeneous crystalline silicon cell, which can be formed according to the method of embodiment 1, or obtained according to other methods.

[0075] Please refer to Figure 5 The heterogeneous crystalline silicon cell disclosed in this embodiment includes: a first velvet structure 101 having a whole surface on the front side, a second velvet structure 201 on the back main grid area 21 , and a polished surface on the back non-main grid area 22 .

[0076] The first velvet structure 101 and the second velvet structure 201 have a pyramid velvet morphology, the base width of the pyramid velvet is 0.5-8 μm, and the front reflectivity is 8%-15%.

[0077] Furthermore, the tower base height of the polished surface is less than 0.5 μm, the tower base width is 8 to 20 μm, and the reflectivity is 30% to 38%.

[0078] The pyramid-shaped velvet structure can effectively increase the surface area of ​​the battery, thereby improving the efficiency of absorbing sunlight. This structure can cause light to be reflected and refracted multiple times on the surface of the battery, extending the path of light in the battery and increasing the amount of light absorbed.

[0079] The low front reflectivity (8% to 15%) means that more light is absorbed by the battery instead of being reflected, which directly improves the photoelectric conversion efficiency of the battery.

[0080] Secondly, the second velvet structure 201 of the back main grid area 21 helps to improve the collection efficiency of charge carriers. In the main grid area, the velvet structure helps to improve the transmission of charge carriers, thereby improving the overall performance of the battery; the polished surface of the back non-main grid area 22 helps to reduce surface losses, such as light reflection and scattering losses, further improving battery efficiency.

[0081] Therefore, the structural design provided in this embodiment improves the performance optimization of the battery and also takes into account the process compatibility in the actual production process, making the battery preparation process more efficient and economical, and helping to maintain the stable performance of the battery during long-term use.

[0082] The battery structure disclosed in this embodiment maintains a velvet structure with good light trapping properties on the entire front surface, while the back surface is polished in the non-main grid area, which not only improves the uniformity of the deposition of the intrinsic amorphous silicon thin layer and improves the electrical performance of the heterojunction battery, but also increases the internal reflection of the long-wave spectrum and increases the short-circuit current, thereby improving the battery conversion efficiency; at the same time, the velvet structure design of the main grid area on the back side enhances the grid line pull-off force and improves the component reliability.

[0083] In summary, the present invention proposes a heterogeneous crystalline silicon cell and a preparation method thereof, wherein the entire front surface of the prepared heterojunction cell and the main grid area on the back have a velvet structure, while the non-main grid area on the back is a polished surface structure; the entire front surface of the heterojunction cell maintains a velvet structure with good light trapping properties, and by polishing the non-main grid area on the back, not only the uniformity of the deposition of the intrinsic amorphous silicon thin layer is improved to improve the electrical performance of the heterojunction cell, but also the internal reflection of the long-wave spectrum is increased, the short-circuit current is increased, and thus the cell conversion efficiency is improved; in addition, the velvet structure design of the main grid area on the back enhances the pull-off force of the grid line and improves the reliability of the component; the preparation method of the heterogeneous crystalline silicon cell provided by the present invention not only improves the conversion efficiency and stability of the cell, but also optimizes the production process, reduces the cost, and has good application prospects and economic benefits.

[0084] Obviously, the above embodiments are only illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those with ordinary knowledge in the relevant technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.

Claims

1. A method for preparing a heterogeneous crystalline silicon cell, characterized in that: include: Providing a silicon wafer having a front side and a back side opposite to each other; Performing double-sided texturing on the silicon wafer to obtain a first texturing structure and a second texturing structure respectively; Forming a mask layer on the back side of the silicon wafer and performing patterning to expose the back side non-main gate area; as well as The back non-main grid area is polished to form a polished surface, and the tower base height of the polished surface is less than 0.5 μm.

2. The method for preparing a heterogeneous crystalline silicon cell according to claim 1, characterized in that: The first velvet structure and the second velvet structure have a pyramid velvet morphology, the base width of the pyramid velvet is 0.5 to 8 μm, and the front reflectivity is 8% to 15%.

3. The method for preparing a heterogeneous crystalline silicon cell according to claim 1, characterized in that: The tower base width of the polishing surface is 8-20 μm, and the reflectivity is 30%-38%.

4. The method for preparing a heterogeneous crystalline silicon cell according to claim 1, characterized in that: After the double-sided texturing, the method further includes: forming a mask on the front side of the silicon wafer.

5. The method for preparing a heterogeneous crystalline silicon cell according to claim 4, characterized in that: Silicon nitride or silicon oxide masks are deposited on the front and back sides of the silicon wafer, and the mask thickness is 20-80 nm.

6. The method for preparing a heterogeneous crystalline silicon cell according to claim 1, characterized in that: The process of patterning to expose the back non-main grid area includes: printing a corrosive slurry on the back non-main grid area to remove the mask layer of the back non-main grid area.

7. The method for preparing a heterogeneous crystalline silicon cell according to claim 6, characterized in that: After removing the mask layer of the non-main gate area on the back side, the method further includes the following steps: cleaning, and the cleaning time does not exceed 30 seconds.

8. The method for preparing a heterogeneous crystalline silicon cell according to claim 7, characterized in that: The cleaning process uses dilute hydrofluoric acid solution, hot sulfuric acid, oxygen plasma, organic solvent or alkaline solution for cleaning; Wherein, the volume concentration of the dilute hydrofluoric acid solution is less than 1%.

9. The method for preparing a heterogeneous crystalline silicon cell according to claim 1, characterized in that: In the process of polishing the back non-main grid area, the polishing liquid is a KOH solution or a NaOH solution.

10. The method for preparing a heterogeneous crystalline silicon cell according to claim 1, characterized in that: After polishing the back non-main gate area, the method further includes removing the remaining mask layer and cleaning the silicon wafer.

11. A heterogeneous crystalline silicon cell, characterized in that: The front side of the heterogeneous crystalline silicon cell has a first velvet structure on the entire surface, the main grid area on the back side has a second velvet structure, and the non-main grid area on the back side is a polished surface.

12. The heterogeneous crystalline silicon cell according to claim 11, characterized in that: The first velvet structure and the second velvet structure have a pyramid velvet morphology, the base width of the pyramid velvet is 0.5 to 8 μm, and the front reflectivity is 8% to 15%.

13. The heterogeneous crystalline silicon cell according to claim 11, characterized in that: The tower base height of the polishing surface is less than 0.5 μm, the tower base width is 8 to 20 μm, and the reflectivity is 30% to 38%.