Method for manufacturing gas diffusion layer for fuel cell, and gas diffusion layer for fuel cell

By using a copper methyl acetylene solution to form porous carbon in the graphene multilayer cavity wall in the gas diffusion layer for fuel cells, the problems of insufficient conductivity and gas diffusivity in the existing technology are solved, and efficient gas diffusion is achieved. Layer manufacturing and water retention adjustment simplify the process.

CN118738414APending Publication Date: 2024-10-01TOYOTA BOSHOKU KK +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410347738.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing gas diffusion layers for fuel cells have deficiencies in electrical conductivity, gas diffusivity and water retention capacity adjustment, and the manufacturing method is complex and difficult to simplify.

Method used

The copper methyl acetylene solution is stirred to form a linear structure, entangled and filled on the surface of the porous substrate sheet, and then calcined in the range of 1000°C to 1200°C to form porous carbon composed of graphene multilayer cavity walls. And the crushing step optimizes the structure to form a mesoporous hollow linear crystal structure.

Benefits of technology

It achieves high electrical conductivity, excellent gas diffusion and good water retention capacity adjustment ability, simplifies the manufacturing process of the gas diffusion layer, and reduces the calcination temperature and energy requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738414A_ABST
    Figure CN118738414A_ABST
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a gas diffusion layer for a fuel cell and a gas diffusion layer for a fuel cell. A method for manufacturing a gas diffusion layer for a fuel cell includes a stirring step for stirring a solution containing a precursor to form a linear structure of the precursor and entangling the linear structure in the solution, an adding step for adding the precursor to a surface layer portion of a porous base sheet or a base sheet precursor to fill pores in the surface layer portion, and a calcining step for calcining the base material sheet or the base material sheet precursor and the precursor in a range of 1000 DEG C to 1200 DEG C, thereby forming a porous carbon composed of multilayer cavity walls of graphene and having mesoporosity and a hollow linear crystal structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for manufacturing a gas diffusion layer for a fuel cell and a gas diffusion layer for a fuel cell. Background Art

[0002] A polymer electrolyte fuel cell includes a fuel cell stack formed by stacking a plurality of single cells. Each single cell includes: a membrane electrode assembly including a solid polymer electrolyte membrane (hereinafter referred to as "electrolyte membrane") and two catalyst layers sandwiching the electrolyte membrane, two gas diffusion layers sandwiching the membrane electrode assembly, an anode side diaphragm, and a cathode side diaphragm. The anode side diaphragm and the cathode side diaphragm sandwich the two gas diffusion layers.

[0003] As such a gas diffusion layer, Japanese Laid-Open Patent Publication No. 2022-42074 discloses a gas diffusion electrode. The gas diffusion electrode disclosed in the publication includes a sheet-like porous substrate and a microporous layer configured to contact one surface of the porous substrate. Examples of porous substrates include carbon paper, carbon cloth, and carbon nonwoven fabrics. The microporous layer is formed by coating one surface of the porous substrate with a paste coating liquid mixed and dispersed with conductive fine particles, a binder, a solvent, a thickener, etc. The conductive particles are carbon black such as acetylene black having an average particle size in the range of 20nm to 150nm. The binder is, for example, polytetrafluoroethylene (PTFE).

[0004] There is a need for such a gas diffusion layer for fuel cells which is producible by a simple process. In addition, there is a need for further improvement of the gas diffusion layer for fuel cells with regard to the regulation of electrical conductivity, gas diffusivity and water retention. Summary of the invention

[0005] This Summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.

[0006] In one general aspect, a method for manufacturing a gas diffusion layer for a fuel cell is provided. The method includes: a stirring step for stirring a solution containing copper methylacetylene as a precursor to form a linear structure of the precursor and to entangle the linear structures in the solution; an adding step for adding the precursor to the surface layer of a porous substrate sheet or a substrate sheet precursor to fill the pores in the surface layer; and a calcining step for calcining the substrate sheet or the substrate sheet precursor and the precursor in the range of 1000° C. to 1200° C. to grow a multilayer cavity wall of graphene and thermally remove copper, thereby forming a porous carbon composed of a multilayer cavity wall of graphene and having a mesoporosity and a hollow linear crystal structure.

[0007] In another general aspect, a method for manufacturing a gas diffusion layer for a fuel cell is provided. The method includes: a stirring step for stirring a solution containing copper methylacetylene as a precursor to form a linear structure of the precursor and to entangle the linear structures in the solution; a first calcining step for calcining the precursor in a range of 1000° C. to 1200° C. to grow a multilayer cavity wall of graphene and to thermally remove copper, thereby forming a porous carbon composed of a multilayer cavity wall of graphene and having a mesoporosity and a hollow linear crystal structure; a pulverizing step for pulverizing the porous carbon while maintaining the crystal structure; an adding step for adding the porous carbon to the surface layer of a porous substrate sheet by applying or spraying a solution containing the pulverized porous carbon to the surface layer of the porous substrate sheet, thereby filling the pores in the surface layer; and a second calcining step for calcining the substrate sheet and the porous carbon to integrate the porous carbon with the substrate sheet.

[0008] In a further general aspect, the gas diffusion layer for a fuel cell comprises a porous substrate sheet and porous carbon, wherein the porous carbon is formed integrally with the substrate sheet in a manner that fills the holes in the surface layer of the substrate sheet. The porous carbon is composed of a multilayer cavity wall of graphene and comprises a structure in which hollow linear crystals having mesoporosity are entangled with each other. The linear diameter of the crystal is in the range of 100nm to 500nm. The diameter of the hole formed by the entangled crystals is in the range of 10nm to 200nm.

[0009] Other features and aspects will be apparent from the following detailed description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 It is a cross-sectional view of a single cell of a fuel cell.

[0011] Figure 2 is a cross-sectional view schematically showing a gas diffusion layer according to a first embodiment.

[0012] Figure 3is a SEM image of the surface layer portion of the gas diffusion layer according to the first embodiment.

[0013] Figure 4 is a SEM image of the surface layer portion of the gas diffusion layer according to the first embodiment.

[0014] Figure 5 is a SEM image of porous carbon forming the gas diffusion layer according to the first embodiment.

[0015] Figure 6 is a SEM image of porous carbon forming the gas diffusion layer according to the first embodiment.

[0016] Figure 7 is a SEM image of porous carbon forming the gas diffusion layer according to the first embodiment.

[0017] Figure 8 is a SEM image of porous carbon forming the gas diffusion layer according to the first embodiment.

[0018] Fig. 9 is a TEM image of porous carbon forming the gas diffusion layer according to the first embodiment.

[0019] Fig.10 is a TEM image of the precursor during the drying step according to the first embodiment.

[0020] Fig.11 is a flowchart showing a manufacturing process of the gas diffusion layer according to the first embodiment.

[0021] Fig.12 is a schematic diagram showing a substrate sheet to which a solution containing a precursor has been applied.

[0022] Fig.13 is a flowchart showing a manufacturing process of a gas diffusion layer according to the second embodiment.

[0023] Fig.14 is a schematic diagram showing a sheet-like precursor covered on a substrate sheet.

[0024] Fig.15 is a flowchart showing a manufacturing process of a gas diffusion layer according to a third embodiment.

[0025] Fig.16 is a schematic diagram showing a substrate sheet to which a solution containing pulverized porous carbon has been applied.

[0026] Fig.17 This is a SEM image of the porous carbon of the comparative example.

[0027] Fig.18 This is a SEM image of the porous carbon of this comparative example.

[0028] Throughout the drawings and detailed description, like reference numerals refer to like elements. The drawings may not be drawn to scale, and the relative size, proportion, and depiction of elements in the drawings may be exaggerated for clarity, illustration, and convenience. DETAILED DESCRIPTION

[0029] This description provides a comprehensive understanding of the described methods, devices and / or systems. Variations and equivalents of the described methods, devices and / or systems will be apparent to those of ordinary skill in the art. The sequence of operations is exemplary and, except for operations that must occur in a particular order, may be readily apparent to those of ordinary skill in the art. Descriptions of functions and components that are well known to those of ordinary skill in the art may be omitted.

[0030] Exemplary embodiments may have different forms and are not limited to the described examples. However, the described examples are thorough and complete, and convey the full scope of the disclosure to those skilled in the art.

[0031] In the present specification, “at least one of A and B” should be understood to mean “only A, only B, or both A and B”.

[0032] First embodiment

[0033] Now refer to Figures 1 to 12 , 17 and 18 describe a gas diffusion layer for a fuel cell and a method for producing the gas diffusion layer for a fuel cell according to the first embodiment.

[0034] The polymer electrolyte fuel cell includes a fuel cell stack formed by stacking a plurality of unit cells 10 .

[0035] like Figure 1 As shown, each single cell 10 includes a membrane electrode assembly 13, two gas diffusion layers 20 sandwiching the membrane electrode assembly 13, an anode side diaphragm (not shown), and a cathode side diaphragm (not shown). The diaphragm sandwiches the two gas diffusion layers 20. The membrane electrode assembly 13 includes a solid polymer electrolyte membrane (hereinafter, referred to as electrolyte membrane 11) and two catalyst layers 12 sandwiching the electrolyte membrane 11.

[0036] like Figure 1 and 2 As shown, the gas diffusion layer 20 includes a porous substrate sheet 21 and porous carbon 22 formed integrally with the substrate sheet 21 so as to fill pores in a surface layer portion 21 a of the substrate sheet 21 .

[0037] The base sheet 21 of the present embodiment is a carbon cloth having a fiber diameter of about 7 μm and pores of about 1 to 2 μm.

[0038] like Figures 3 to 8 As shown, the porous carbon 22 is composed of multi-layer cavity walls of graphene and includes a structure in which hollow linear crystals having mesoporosity are entangled with each other.

[0039] like Figure 3 As shown, the pores formed between the carbon fibers (ie, macrofibers) of the base sheet 21 are filled with the porous carbon 22 .

[0040] like Fig. 9 As shown, the porous carbon 22 has a pore structure separated by multi-layer cavity walls of graphene.

[0041] The diameter of the crystals is in the range of 100nm to 500nm. The diameter of the holes formed by the intertwined crystals is in the range of 10nm to 200nm.

[0042] Next, we will refer to Fig.11 A process of manufacturing the gas diffusion layer 20 of the present embodiment will be described.

[0043] like Fig.11 As shown, the method for producing the gas diffusion layer 20 of the present embodiment includes a precursor synthesis step, a stirring step, an adding step, a drying step, and a calcining step.

[0044] The precursor synthesis step is a step for synthesizing methylacetylene copper as a precursor by a known method.

[0045] The stirring step is a step for stirring a solution containing copper methylacetylene as a precursor to form a linear structure and to entangle the linear structures with each other in the solution. Water is used as a solvent. Adding a small amount of ethanol to the solvent makes the stretching of the precursor easy.

[0046] In the stirring step, the linear structure of the precursor is formed by stirring the solution containing methylacetylene copper. At this time, in the subsequent heating step, due to the difference in specific gravity between copper and carbon, copper becomes spherical or elliptical, and carbon becomes linear covering copper. In addition, the linear structures of the precursor are entangled with each other in the solution.

[0047] like Fig.12 As shown, the adding step is a step for adding the precursor 22A to the surface layer portion 21 a of the porous base sheet 21 to fill the pores in the surface layer portion 21 a .

[0048] In the adding step, the precursor 22A is added to the surface layer portion 21a by applying or spraying the solution containing the precursor 22A to the surface layer portion 21a. In the present embodiment, the phenolic resin solution containing the precursor 22A is applied to the surface layer portion 21a of the substrate sheet 21 so that the solution penetrates into the pores in the surface layer portion 21a of the substrate sheet 21.

[0049] The drying step is a step for heating the precursor 22A added to the surface layer portion 21a of the base sheet 21 to a temperature in the range of 170°C to 300°C under vacuum to dry the precursor 22A. Therefore, although phase separation of copper and carbon occurs, the shape of the precursor 22A is easily maintained.

[0050] Fig.10 The separation of copper and methylacetylene polymer is shown during the heating of the precursor 22A to a temperature in the range of 60°C to 200°C in the drying step. Specifically, Fig.10 It shows how the copper becomes spherical and the methyl groups are released out of the system as methane and ethylene gases.

[0051] The calcination step is a step for calcining the base sheet 21 and the precursor 22A in the range of 1000° C. to 1200° C. to grow multilayer cavity walls of graphene and thermally remove copper to form the porous carbon 22 .

[0052] The calcining step is preferably carried out at a pressure below atmospheric pressure.

[0053] In the calcination step, the precursor 22A and the substrate sheet 21 are calcined together in the range of 1000° C. to 1200° C. to sublime and remove copper. The copper in contact with a portion of the carbon of the precursor 22A melts at a temperature higher than or equal to 1000° C. At this time, an ideal two-dimensional surface of carbon is generated due to the surface tension generated in the carbon, so that the carbon grows into a multi-layer cavity wall of graphene. This forms a porous carbon 22 composed of a multi-layer cavity wall of graphene and including a structure in which hollow linear crystals having mesoporosity are entangled with each other.

[0054] The melting point of copper is 1085° C. However, in the case of particles having a size of 50 nm or less, liquefaction of copper proceeds below 1000° C. due to a decrease in the melting point.

[0055] Fig.17 and 18 The SEM image of the porous carbon of the comparative example is shown. The porous carbon of the comparative example is formed by dropping the precursor of the present embodiment into a furnace and performing vacuum calcination.

[0056] This embodiment has the following advantages.

[0057] (1-1) The manufacturing method for the gas diffusion layer 20 includes a stirring step, an adding step, and a calcining step.

[0058] In the case of this method, since the calcination temperature is in the range of 1000° C. to 1200° C., the calcination temperature is lowered compared to, for example, the conventional manufacturing method of calcining methylacetylene silver at 2000° C. This allows a reduction in the size of a calcination furnace and the energy required for calcination.

[0059] Furthermore, copper is preferred over silver for growing thick multi-layered cavity walls of graphene to increase conductivity.

[0060] Therefore, the above method can obtain the gas diffusion layer 20 by simple steps, in which the pores of the surface layer portion 21a of the substrate sheet 21 are filled with the porous carbon 22. The porous carbon 22 functions as the microporous layer 23. Therefore, the gas diffusion layer 20 having the microporous layer 23 can be manufactured by a simple method.

[0061] (1-2) In the adding step, the precursor 22A is added to the surface layer portion 21 a by applying or spraying a solution containing the precursor 22A to the surface layer portion 21 a .

[0062] In the case of this method, the precursor 22A is added to the surface portion 21a by applying or spraying a solution containing the precursor 22A to the surface portion 21a in the adding step. Therefore, the precursor 22A is easily added to the surface portion 21a of the porous substrate sheet 21, thereby filling the pores in the surface portion 21a.

[0063] (1-3) The gas diffusion layer 20 includes a porous substrate sheet 21 and a porous carbon 22 formed integrally with the substrate sheet 21 in such a manner as to fill the pores in the surface layer portion 21a of the substrate sheet 21. The porous carbon 22 is composed of a multilayer cavity wall of graphene and includes a structure in which hollow linear crystals having mesoporosity are entangled with each other. The linear diameter of the crystal is in the range of 100 nm to 500 nm, and the diameter of the pores formed by the entangled crystals is in the range of 10 nm to 200 nm.

[0064] Because the porous carbon 22 is formed integrally with the substrate sheet 21, this composition increases the rigidity of the porous carbon 22, although the porous carbon 22 itself is brittle. And, because the porous carbon 22 is composed of a multilayer cavity wall of graphene, the porous carbon 22 has high conductivity. In addition, the wire diameter of the crystal is in the range of 100nm to 500nm, and the diameter of the pores formed by the mutually entangled crystals is in the range of 10nm to 200nm. The porous carbon 22 therefore has high gas diffusivity. Because water can be stored in a large number of mesopores in the crystal and can be discharged therefrom, the porous carbon 22 is excellent in regulating the water retention. The porous carbon 22 therefore functions as a microporous layer 23. In a fuel cell, when protons move from the anode to the cathode, water functions as a carrier for transporting protons. As described above, because the porous carbon 22 of the gas diffusion layer 20 is adjacent to the catalyst layer 12, the humidity of the catalyst layer 12 is adjusted by the porous carbon 22. As a result, the amount of water in the catalyst layer 12 can be increased, which contributes to an improvement in the fuel cell output.

[0065] Second embodiment

[0066] Now refer to Fig.13 and 14 The second embodiment will be described. The differences from the first embodiment will be mainly discussed.

[0067] like Fig.13 As shown, the method for producing the gas diffusion layer 20 according to the present embodiment is different from that of the first embodiment in that a sheet forming step and a drying step are provided between the stirring step and the adding step.

[0068] The sheet forming step is a step for forming the precursor 22A into a sheet-shaped precursor.

[0069] In the sheet forming step, the linear structure of the precursor 22A entangled with each other is formed into a sheet-like precursor. Examples of the method for forming the linear structure of the precursor 22A into a sheet-like precursor include a method of filtering a solution containing the precursor 22A with filter paper to form a sheet on the filter paper, a method of applying the solution to a planar jig, and a method of spraying the solution onto a planar jig.

[0070] The drying step is a step for heating the sheet-shaped precursor to a temperature in the range of 170° C. to 300° C. under vacuum to dry the precursor. Therefore, although phase separation of copper and carbon occurs, the shape of the precursor is easily maintained.

[0071] like Fig.14 As shown, in the adding step, the sheet-like precursor 22A is pressed toward the surface layer portion 21a in a state where the sheet-like precursor 22A covers the surface layer portion 21a. In this embodiment, the sheet-like precursor 22A is pressed toward the surface layer portion 21a with a roller (not shown).

[0072] After the adding step is performed, the calcining step is performed in the same manner as in the first embodiment.

[0073] This embodiment has the following advantages.

[0074] (2-1) The manufacturing method for the gas diffusion layer 20 includes a sheet forming step for forming the precursor 22A into a sheet-like precursor. In the adding step, the sheet-like precursor 22A is pressed toward the surface layer portion 21a in a state where the sheet-like precursor 22A covers the surface layer portion 21a.

[0075] In the case of this method, it is easy to add the precursor 22A having a uniform thickness to the surface layer portion 21 a of the porous base sheet 21 to fill the pores in the surface layer portion 21 a .

[0076] (2-2) Since the porous carbon 22 has a structure in which hollow linear crystals are entangled with each other, the microporous layer 23 can be easily formed into a thin film. Forming the microporous layer 23 into a thin film reduces the resistance overvoltage of the microporous layer 23.

[0077] Third embodiment

[0078] Now refer to Fig.15 and 16 A third embodiment is described.

[0079] like Fig.15 As shown, the manufacturing method for the gas diffusion layer 20 of the present embodiment includes a precursor synthesis step, a stirring step, a first calcination step, a pulverization step, an adding step, and a second calcination step.

[0080] The precursor synthesis step and the stirring step are the same as those in the first and second embodiments.

[0081] The first calcination step is a step for calcining the precursor in the range of 1000° C. to 1200° C. to grow multi-layer cavity walls of graphene and thermally remove copper to form porous carbon 22 .

[0082] The first calcination step is preferably carried out at a pressure below atmospheric pressure.

[0083] The first calcination step is the same as the calcination step according to the first embodiment, and copper is sublimated and removed by calcining the precursor 22A in the range of 1000° C. to 1200° C.

[0084] The pulverization step is a step for pulverizing the porous carbon 22 while maintaining the crystal structure.

[0085] like Fig.16 As shown, the adding step is a step for adding the porous carbon 22 to the surface portion 21a by applying or spraying a solution containing the crushed porous carbon 22 to the surface portion 21a of the porous substrate sheet 21, thereby filling the pores in the surface portion 21a. In this embodiment, a phenolic resin solution containing the crushed porous carbon 22 is applied to the surface portion 21a of the substrate sheet 21, so that the solution penetrates into the pores in the surface portion 21a of the substrate sheet 21.

[0086] The second calcination step is a step for calcining the substrate sheet 21 and the porous carbon 22 to integrate the porous carbon 22 and the substrate sheet 21 .

[0087] This embodiment has the following advantages.

[0088] (3-1) The manufacturing method for the gas diffusion layer 20 includes a stirring step, a first calcining step, a pulverizing step, an adding step, and a second calcining step.

[0089] In the case of the above method, since the calcination temperature of the first calcination step is in the range of 1000° C. to 1200° C., the calcination temperature is lowered compared to the conventional manufacturing method of calcining methylacetylene silver at, for example, 2000° C. This allows the size of the calcination furnace and the energy required for calcination to be reduced.

[0090] Furthermore, copper is preferred over silver for growing thick multi-layered cavity walls of graphene to increase conductivity.

[0091] Therefore, the above method can obtain the gas diffusion layer 20 by simple steps, in which the pores of the surface layer portion 21a of the substrate sheet 21 are filled with the porous carbon 22. The porous carbon 22 functions as the microporous layer 23. Therefore, the gas diffusion layer 20 having the microporous layer 23 can be manufactured by a simple method.

[0092] Deformation

[0093] The above-mentioned embodiment can be modified as follows: The above-mentioned embodiment and the following modifications can be combined as long as the combined modifications remain technically consistent with each other.

[0094] The fiber diameter of the carbon fibers forming the base sheet 21 and the size of the pores in the base sheet 21 may be changed.

[0095] The base sheet 21 is not limited to the carbon cloth, and may be carbon paper or carbon nonwoven fabric.

[0096] In the first and second embodiments, methylacetylene copper as a precursor is added to the surface layer 21a of the substrate sheet 21 in the adding step. Thereafter, in the calcining step, the substrate sheet 21 and the precursor are calcined in the range of 1000°C to 1200°C. Alternatively, methylacetylene copper as a precursor may be added to the surface layer of the substrate sheet precursor in the adding step. Thereafter, the substrate sheet precursor and the precursor may be calcined in the range of 1000°C to 1200°C in the calcining step. The substrate sheet precursor may be of any type as long as it becomes a substrate sheet by calcining, and is preferably, for example, a nonwoven fabric or paper made of polyacrylonitrile. Further, a nonwoven fabric or paper made of cellulose may be used. In this case, the substrate sheet precursor is calcined to form a substrate sheet. Therefore, when the precursor is calcined, the substrate sheet precursor is calcined at the same time to form a carbon paper or carbon nonwoven fabric as a substrate sheet.

[0097] Various changes in form and details may be made to the above examples without departing from the spirit and scope of the claims and their equivalents. These examples are for convenience of illustration only and not for the purpose of limitation. The description of the features in each example is considered to be applicable to similar features or aspects in other examples. If the sequence is performed in a different order, and / or if the components in the described system, architecture, device or circuit are combined in a different way, and / or replaced or supplemented by other components or their equivalents, suitable results can be obtained. The scope of the present disclosure is not limited by the specific embodiments, but by the claims and their equivalents. All changes within the scope of the claims and their equivalents are included in the present disclosure.

Claims

1. A method for manufacturing a gas diffusion layer for a fuel cell, the method comprising: a stirring step for stirring a solution containing copper methylacetylene as a precursor to form a linear structure of the precursor and to entangle the linear structures with each other in the solution; an adding step for adding the precursor to the surface layer portion of the porous substrate sheet or substrate sheet precursor to fill the pores in the surface layer portion; and A calcination step for calcining the substrate sheet or the substrate sheet precursor and the precursor at a temperature ranging from 1000° C. to 1200° C. to grow multi-layer cavity walls of graphene and thermally remove copper, thereby forming porous carbon composed of multi-layer cavity walls of graphene and having mesoporosity and a hollow linear crystal structure. 2 . The method for producing a gas diffusion layer for a fuel cell according to claim 1 , wherein the adding step includes adding the precursor to the surface layer portion by applying or spraying a solution containing the precursor to the surface layer portion.

3. The method for producing a gas diffusion layer for a fuel cell according to claim 1, further comprising a sheet forming step for forming the precursor into a sheet-shaped precursor, The adding step includes pressing the sheet-like precursor toward the surface layer portion in a state where the sheet-like precursor covers the surface layer portion.

4. A method for manufacturing a gas diffusion layer for a fuel cell, the method comprising: a stirring step for stirring a solution containing copper methylacetylene as a precursor to form a linear structure of the precursor and to entangle the linear structures with each other in the solution; A first calcination step for calcining the precursor in a range of 1000° C. to 1200° C. to grow multi-layer cavity walls of graphene and thermally remove copper, thereby forming porous carbon composed of multi-layer cavity walls of graphene and having a mesoporosity and a hollow linear crystal structure; a pulverizing step for pulverizing the porous carbon while maintaining the crystal structure; an adding step for adding the porous carbon to the surface layer portion of the porous substrate sheet by applying or spraying a solution containing the pulverized porous carbon to the surface layer portion, thereby filling the pores in the surface layer portion; and A second calcination step for calcining the substrate sheet and the porous carbon to integrate the porous carbon with the substrate sheet.

5. A gas diffusion layer for a fuel cell, comprising: a porous substrate sheet; and porous carbon, the porous carbon being formed integrally with the substrate sheet in such a manner as to fill the pores in the surface layer portion of the substrate sheet, wherein The porous carbon is composed of multi-layer cavity walls of graphene and includes a structure in which hollow linear crystals with mesoporosity are entangled with each other. The crystals have a linear diameter in the range of 100 nm to 500 nm, and The diameter of the pores formed by the mutually entangled crystals ranges from 10 nm to 200 nm.