Catalyst
By using a combined structure catalyst of Ir and Pt layers in PEMFC and depositing it on microstructured whiskers, the problem of catalyst cost and durability after iridium doping is solved, the mass activity and surface area of the catalyst are improved, and the fuel cell life is extended. service life.
Patent Information
- Application Number
- CN202410697687.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-04-13
- Filing Date
- 2019-04-11
- Publication Date
- 2024-10-01
AI Technical Summary
The high cost and durability problems of platinum catalysts in existing polymer electrolyte membrane fuel cells (PEMFC), especially the increase in catalyst mass activity and cost after iridium doping.
Adopting a combined structure of Ir layer and Pt layer, the average thickness of the Ir layer is between 0.04 nanometers and 30 nanometers, the average thickness of the Pt layer is between 0.04 nanometers and 50 nanometers, and the atomic ratio is in the range of 0.01:1 to 10:1. Through deposition technology Catalysts are prepared by methods such as sputtering and atomic layer deposition, and are deposited on microstructured whiskers to increase the surface area and durability of the catalyst.
Significantly improve the mass activity, specific surface area and fuel cell performance of the oxygen reduction reaction (ORR) electrocatalyst, extend the durability of the catalyst and reduce the cost.
Smart Images

Figure CN118738423A_ABST
Abstract
Description
[0001] This patent application is a divisional application of the patent application with application number 201980025540.6, application date April 11, 2019, and invention name “Catalyst”.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims the benefit of U.S. Provisional Patent Application No. 62 / 657,184, filed April 13, 2018, the disclosure of which is incorporated herein by reference in its entirety.
[0004] This invention was made with Government support awarded by DOE under Contract No. DE-EE0007270. The Government has certain rights in this invention. Background Art
[0005] Fuel cells generate electricity through electrochemical oxidation of a fuel and reduction of an oxidant. Fuel cells are generally classified according to the type of electrolyte and the type of fuel and oxidant reactants. One type of fuel cell is a polymer electrolyte membrane fuel cell (PEMFC), in which the electrolyte is a polymer ion conductor and the reactants are hydrogen fuel and oxygen as an oxidant. Oxygen is generally provided by ambient air.
[0006] PEMFC generally requires the use of electrocatalysts to increase the reaction rates of hydrogen oxidation reaction (HOR) and oxygen reduction reaction (ORR), which improves PEMFC performance. PEMFC electrocatalysts generally contain platinum, a relatively expensive precious metal. It is generally desirable to minimize the platinum content in PEMFC, thereby increasing the catalyst activity (specific activity) per unit catalyst surface area and increasing the catalyst surface area (specific surface area or specific area) per catalyst mass. HOR and ORR occur on the catalyst surface, so increasing the specific surface area and / or specific activity can reduce the device to minimize cost. However, sufficient platinum content is required to provide sufficient catalytic activity and PEMFC device performance. Therefore, it is necessary to improve the catalyst activity (mass activity) per unit catalyst mass. There are two general methods for improving mass activity, that is, the amount of catalyst required to achieve the desired absolute performance, thereby reducing costs.
[0007] To maximize specific area, PEMFC electrocatalysts are typically present in the form of nanoscale thin films or particles on a support material. An exemplary support material for nanoparticle PEMFC electrocatalysts is carbon black, and an exemplary support material for thin film electrocatalysts is whiskers.
[0008] To increase specific activity, PEMFC Pt ORR electrocatalysts generally also contain certain transition metals such as cobalt or nickel. Without being bound by theory, it is believed that the incorporation of certain transition metals into the Pt lattice causes the contraction of Pt atoms on the catalyst surface, which increases the kinetic reaction rate by changing the molecular oxygen binding and dissociation energies and the binding energies of reaction intermediates and / or observed species.
[0009] PEMFC electrocatalysts can be doped with other precious metals. For example, HOR PEMFC Pt electrocatalysts can be alloyed with ruthenium to improve tolerance to carbon monoxide (a known Pt catalyst poison). HOR and ORR PEMFC electrocatalysts can also be doped with iridium to promote the activity of oxygen evolution reaction (OER). In the absence of fuel and during the startup and shutdown of the PEMFC system, the improved OER activity can improve the durability of PEMFC under unintentional operation. However, the incorporation of iridium into PEMFCCORR electrocatalysts can lead to reduced mass activity and increased catalyst costs. Iridium has a lower specific activity than platinum for ORR, which may lead to reduced catalyst mass activity. Iridium is also a precious metal, so its incorporation can increase costs. PEMFC Pt electrocatalysts can also be doped with gold, which is also a precious metal and can increase costs. It is known that gold is relatively inactive for HOR and ORR in acidic electrolytes. Since gold tends to be preferentially separated to the surface of the electrocatalyst, the incorporation of gold can lead to significant deactivation of HOR and ORR, thereby preventing active catalytic sites.
[0010] PEMFC electrocatalysts may have different structures and compositional forms. The structures and compositional forms are usually adjusted by specific processing methods during electrocatalyst manufacture, such as changes in electrocatalyst deposition methods and annealing methods. PEMFC electrocatalysts may be uniform in composition, layered in composition, or may contain a composition gradient throughout the electrocatalyst. Adjusting the composition distribution within the electrocatalyst may improve the activity and durability of the electrocatalyst. PEMFC electrocatalyst particles or nanoscale films may have a substantially smooth surface or may have atomic or nanoscale roughness. PEMFC electrocatalysts may be uniform in structure or may be nanoporous, consisting of nanoscale pores and solid catalyst ligaments.
[0011] In a PEMFC device, electrocatalysts may lose performance over time due to various degradation mechanisms, which induce structural changes and composition changes. Such performance losses may shorten the practical life of such systems. For example, electrocatalyst degradation may occur due to loss of electrocatalyst activity per unit surface area and loss of electrocatalyst surface area. For example, electrocatalyst specific activity may be lost due to dissolution of electrocatalyst alloying elements. Nanoparticles and nanoscale thin film electrocatalysts may lose surface area, for example due to loss of Pt dissolution, particle sintering, agglomeration, and surface roughness.
[0012] There is a need for additional electrocatalysts and systems containing such catalysts, including those that address one or more of the problems discussed above. Summary of the invention
[0013] In one aspect, the present disclosure provides a catalyst comprising an Ir layer having an outer layer having a layer comprising Pt directly thereon, wherein the Ir layer has an average thickness in a range of 0.04 nm to 30 nm (in some embodiments, 0.04 nm to 20 nm, 0.05 nm to 20 nm, 0.05 nm to 10 nm, 0.05 nm to 8 nm, 0.05 nm to 6 nm, 0.05 nm to 5 nm, 0.05 nm to 10 nm, 0.05 nm to 20 nm, 0.05 nm to 30 nm, 0.05 nm to 10 nm, 0.05 nm to 20 nm, 0.05 nm to 20 nm, 0.05 nm to 3 ... In some embodiments, the Pt-containing layer has an average thickness in the range of 0.04 nm to 50 nm (in some embodiments, in the range of 0.04 nm to 40 nm, 0.05 nm to 3 nm, 0.05 nm to 2 nm, 0.05 nm to 1.64 nm, 0.05 nm to 1 nm, 0.05 nm to 0.98 nm, 0.05 nm to 0.39 nm, 0.05 nm to 0.36 nm, or even 0.8 nm to 0.85 nm). 0.04 nm to 30 nm, 0.04 nm to 20 nm, 0.04 nm to 10 nm, 0.04 nm to 5 nm, 0.04 nm to 4 nm, 0.04 nm to 3 nm, 0.04 nm to 2.99 nm, 0.04 nm to 2.5 nm, 0.04 nm to 2 nm, 0.04 nm to 1.57 nm, 0.04 nm to 1 nm, 0.04 nm to 0.71 nm, 0.04 nm to 0.34 nm, or even within the range of ... 04 nm to 0.31 nm), wherein Pt and Ir are present in an atomic ratio in the range of 0.01:1 to 10:1 (in some embodiments, in the range of 0.04:1 to 2.85:1, 0.35:1 to 1.79:1, 0.72:1 to 1.18:1, 0.19:1 to 5.90:1, 0.31:1 to 5.90:1, 0.76:1 to 1.88:1, or even in the range of 0.85:1 to 3.87:1). In some embodiments, the catalyst surface area is at least 5% greater (in some embodiments, at least 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, or even at least 49%) than the catalyst surface area that would be present in the absence of the Ir layer.
[0014] In another aspect, the present disclosure provides a method for preparing the catalyst described herein, the method comprising depositing any of the layers via a deposition technique independently selected from sputtering (including reactive sputtering), atomic layer deposition, metal organic chemical vapor deposition, molecular beam epitaxy, ion soft landing, thermal physical vapor deposition, electrospray ionization vacuum deposition, and pulsed laser deposition. In some embodiments, the method further comprises annealing at least one of the layers.
[0015] In another aspect, the present disclosure provides an article comprising a nanostructured element comprising a microstructured whisker having an outer surface having a catalyst as described herein thereon. In some embodiments of the article, the first layer is directly on the microstructured whisker.
[0016] In another aspect, the present disclosure provides a method of preparing an article as described herein, the method comprising depositing any of the layers on a microstructured whisker via a deposition technique independently selected from sputtering (including reactive sputtering), atomic layer deposition, metal organic chemical vapor deposition, molecular beam epitaxy, ion soft landing, thermal physical vapor deposition, electrospray ionization vacuum deposition, and pulsed laser deposition. In some embodiments, the method further comprises annealing at least one of the layers.
[0017] In another aspect, the present disclosure provides a method for preparing a catalyst described herein, the method comprising electrochemically cycling the catalyst.
[0018] Surprisingly, the incorporation of an Ir layer underneath the ORR electrocatalyst layer can lead to increased mass activity, specific surface area, durability, and fuel cell performance of the ORR electrocatalyst.
[0019] The catalysts described herein may be used, for example, in fuel cell membrane electrode assemblies. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a side view of an exemplary catalyst described herein.
[0021] Figure 2 is a diagram of an exemplary fuel cell.
[0022] Figure 3 is a graph of electrocatalyst mass activity as a function of catalyst loading for the catalysts of Examples 1 to 12 and Comparative Examples A to E, normalized to platinum content.
[0023] Figure 4 is a graph of electrocatalyst mass activity as a function of catalyst loading normalized to the sum of platinum and iridium content for the catalysts of Examples 1 to 12, Comparative Examples A to E and J.
[0024] Figure 5 is a graph of electrocatalyst specific surface area normalized to the sum of platinum and iridium content as a function of catalyst loading for the catalysts of Examples 1 to 12, Comparative Examples A to E and J.
[0025] Figure 6 is a graph of the electrocatalyst specific surface area normalized to the sum of platinum and iridium content for the catalysts of Examples 1 to 12, Comparative Examples A to E and J as a function of the thickness of the catalyst on the support whiskers.
[0026] Figure 7 is 0.02 A / cm2 as a function of catalyst loading for Examples 1 to 12 and Comparative Examples A to E 2 Plot of cell voltage versus current density.
[0027] Figure 8 is a graph of the change in electrocatalyst mass activity after accelerated durability testing as a function of catalyst loading for Examples 3 to 6 and 10 and Comparative Examples A and B.
[0028] Fig. 9 is 0.02 A / cm after accelerated durability testing as a function of catalyst loading for Examples 3 to 6 and 10 and Comparative Examples A and B 2 The battery voltage change curve is shown below.
[0029] Fig.10 is a high angle annular dark field transmission electron micrograph of the catalyst of Example 10 at 1,000,000x magnification after deposition of the catalyst onto optional support whiskers.
[0030] Fig.11 is a high angle annular dark field transmission electron micrograph of the catalyst of Example 10 at 1,000,000x magnification after annealing the catalyst.
[0031] Fig.12 is a high angle annular dark field transmission electron micrograph of the catalyst of Example 10 at 1,000,000x magnification after testing the catalyst in a fuel cell.
[0032] Fig.13 is a high angle annular dark field transmission electron micrograph of the catalyst of Example 10 at 1,000,000x magnification after accelerated durability testing of the catalyst in a fuel cell.
[0033] Fig.14 is a high angle annular dark field transmission electron micrograph and energy dispersive X-ray spectroscopy elemental map of the catalyst of Example 10 at 3,000,000x magnification after deposition of the catalyst onto optional support whiskers.
[0034] Fig.15 is a high angle annular dark field transmission electron micrograph and energy dispersive X-ray spectroscopy elemental map of the catalyst of Example 10 at 3,000,000x magnification after annealing the catalyst.
[0035] Fig.16 is a high angle annular dark field transmission electron micrograph and energy dispersive X-ray spectroscopy elemental map of the catalyst of Example 10 at 3,000,000x magnification after testing the catalyst in a fuel cell.
[0036] Fig.17 is a high angle annular dark field transmission electron micrograph and energy dispersive X-ray spectroscopy elemental map of the catalyst of Example 10 at 3,000,000x magnification after accelerated durability testing of the catalyst in a fuel cell.
[0037] Fig.18 is a high angle annular dark field transmission electron micrograph of the catalyst of Example 3 at 3,000,000x magnification after accelerated durability testing of the catalyst in a fuel cell.
[0038] Fig.19 is a high angle annular dark field transmission electron micrograph and energy dispersive X-ray spectroscopy elemental distribution map of the catalyst of Example 3 at 3,000,000x magnification after accelerated durability testing of the catalyst in a fuel cell.
[0039] Fig. 20 is a high angle annular dark field transmission electron micrograph of the catalyst of Example 2 at 3,000,000x magnification after testing the catalyst in a fuel cell.
[0040] Fig.21 is a graph of electrocatalyst mass activity normalized to platinum content as a function of catalyst loading for the catalysts of Examples 3 and 8 to 12 and Comparative Examples F to I. DETAILED DESCRIPTION
[0041] In some embodiments, the average thickness of the Ir layer is in the range of 0.04 nm to 30 nm (in some embodiments, in the range of 0.04 nm to 20 nm, 0.05 nm to 20 nm, 0.05 nm to 10 nm, 0.05 nm to 8 nm, 0.05 nm to 6 nm, 0.05 nm to 5 nm, 0.05 nm to 4 nm, 0.05 nm to 3 nm, 0.05 nm to 2 nm, 0.05 nm to 1.64 nm, 0.05 nm to 1 nm, 0.05 nm to 0.98 nm, 0.05 nm to 0.39 nm, 0.05 nm to 0.36 nm, or even 0.8 nm to 0.85 nm). In some embodiments, the average thickness of the layer comprising Pt is in the range of 0.04 nm to 50 nm (in some embodiments, in the range of 0.04 nm to 40 nm, 0.04 nm to 30 nm, 0.04 nm to 20 nm, 0.04 nm to 10 nm, 0.04 nm to 5 nm, 0.04 nm to 4 nm, 0.04 nm to 3 nm, 0.04 nm to 2.99 nm, 0.04 nm to 2.5 nm, 0.04 nm to 2 nm, 0.04 nm to 1.57 nm, 0.04 nm to 1 nm, 0.04 nm to 0.71 nm, 0.04 nm to 0.34 nm, or even in the range of 0.04 nm to 0.31 nm).
[0042] In some embodiments, Pt and Ir are present in an atomic ratio ranging from 0.01:1 to 10:1 (in some embodiments, ranging from 0.04:1 to 2.85:1, 0.35:1 to 1.79:1, 0.72:1 to 1.18:1, 0.19:1 to 5.90:1, 0.31:1 to 5.90:1, 0.76:1 to 1.88:1, or even in the range of 0.85:1 to 3.87:1).
[0043] In some embodiments, the catalyst surface area is at least 5% greater (in some embodiments, at least 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 20, 25, 30, 35, 40, 45, or even at least 49%) than the catalyst surface area would be in the absence of the Ir layer.
[0044] In some embodiments, the catalyst material further comprises at least one pair of alternating layers, wherein the first alternating layers comprise Ir, and wherein the second alternating layers comprise Pt.
[0045] In some embodiments, the catalyst further comprises nanoscale metal grains extending from the surface of the catalyst. In some embodiments, the surface metal grains comprise at least 10 atomic % (in some embodiments, at least 15 atomic %, 20 atomic %, 25 atomic %, 30 atomic %, 40 atomic %, 50 atomic %, 60 atomic %, 70 atomic %, 75 atomic %, 80 atomic %, 90 atomic %, 95 atomic %, 98 atomic %, 99 atomic %, or even at least 99.9 atomic %) of Ir. In some embodiments, the length of the surface metal grains is in the range of 0.25 nm to 10 nm (in some embodiments, in the range of 0.25 nm to 8 nm, 0.25 nm to 6 nm, 0.25 nm to 4 nm, 0.25 nm to 3 nm, 0.25 nm to 2 nm, 0.25 nm to 1 nm, 1 nm to 10 nm, 1 nm to 8 nm, 1 nm to 6 nm, 1 nm to 4 nm, 1 nm to 3 nm, or even in the range of 1 nm to 2 nm). In some embodiments, the length of the surface metal grains is less than 8 nanometers (in some embodiments, less than 7 nanometers, 6 nanometers, 5 nanometers, 4 nanometers, 3 nanometers, 2 nanometers, or even less than 1 nanometer). In some embodiments, the diameter of the surface metal grains is in the range of 0.25 nanometers to 5 nanometers (in some embodiments, in the range of 0.25 nanometers to 4 nanometers, 0.25 nanometers to 3 nanometers, 0.25 nanometers to 2 nanometers, 0.25 nanometers to 1 nanometer, 1 nanometer to 5 nanometers, 1 nanometer to 4 nanometers, 1 nanometer to 3 nanometers, or even 1 nanometer to 2 nanometers). In some embodiments, the diameter of the surface metal grains is less than 5 nanometers (in some embodiments, less than 4 nanometers, 3 nanometers, 2 nanometers, or even less than 1 nanometer).
[0046] In some embodiments, the layer comprising Pt further comprises Ni. In some embodiments, the atomic ratio of Pt to Ni is in the range of 0.5:1 to 5:1 (in some embodiments, in the range of 0.5:1 to 2:1, 0.5:1 to 1:1, 0.57:1 to 0.69:1, or even 0.58:1 to 0.62:1).
[0047] In some embodiments, the catalyst material comprises a nanostructured element comprising a microstructured whisker having an outer surface, the outer surface having an Ir layer thereon, the Ir layer having an outer layer, the outer layer having a layer comprising Pt directly thereon. In some embodiments, the Ir layer is directly on the microstructured whisker. In some embodiments, the catalyst material further comprises at least one pair of alternating layers disposed between the outer surface of the microstructured whisker and the layer comprising Ir, wherein the first alternating layer comprises Ir and is directly on the microstructured whisker, and wherein the second alternating layer comprises Pt.
[0048] See also Figure 1 , the exemplary catalyst 99 described herein includes an Ir layer 110 having an outer layer 115, the outer layer having a Pt-containing layer 120 directly thereon (i.e., directly on the outer layer 115). The average thickness of the Ir layer 110 on the microstructured whiskers is in the range of 0.04 nm to 30 nm. The average thickness of the Pt-containing layer 120 on the microstructured whiskers 101 is in the range of 0.04 nm to 50 nm. Pt and Ir are present in an atomic ratio in the range of 0.01:1 to 10:1. As shown, the optional nanostructured element 100 includes a microstructured whisker 101 having an outer surface 105 having an Ir layer 110 located thereon (i.e., located on the outer surface 105).
[0049] In some embodiments, the microstructured whiskers are attached to a backing (eg, a film). In some embodiments, the backing has microstructures on at least one of its surfaces.
[0050] Suitable whiskers can be provided by techniques known in the art, including those described in U.S. Pat. Nos. 4,812,352 (Debe), 5,039,561 (Debe), 5,338,430 (Parsonage et al.), 6,136,412 (Spiewak et al.), and 7,419,741 (Vernstrom et al.), the disclosures of which are incorporated herein by reference. Generally, microstructured whiskers can be provided by, for example, vacuum depositing (e.g., by sublimation) a layer of organic or inorganic material on a substrate (e.g., a microstructured catalyst transfer polymer sheet), and then, in the case of perylene red deposition, converting the perylene red pigment into microstructured whiskers by thermal annealing. Typically, the vacuum deposition step is performed at or below about 10 -3The exemplary microstructures were prepared by thermal sublimation and vacuum annealing of an organic pigment, CI Pigment Red 149 (ie, N,N'-di(3,5-dimethylphenyl)perylene-3,4:9,10-bis(dicarboximide)). Methods for preparing organic microstructured layers are reported, for example, in Materials Science and Engineering, Vol. A158, (1992), pp. 1-6; J. Vac. Sci. Technol. A, 5(4), July / August 1987, pp. 1914-1916; J. Vac. Sci. Technol. A, 6, (3), May / August 1988, pp. 1907-1911; "Thin Solid Films", Vol. 186, 1990, pp. 327-47; J. Mat. Science Magazine, 25, 1990, pp. 5257-68; "Rapidly Quenched Metals", Proc. of the Fifth International Conference on Rapidly Quenched Metals, Würzburg, Germany Int. Conf. on Rapidly Quenched Metals, Wurzburg, Germany) (September 3-7, 1984), edited by S. Steeb et al., Elsevier Science Publishers BV, New York (1985), pp. 1117-1124; Photo. "Sci. and Eng. (Materials Science and Engineering)", 24, (4), July / August 1980, pp. 211-216; and U.S. Patent Application Nos. 4,340,276 (Maffitt et al.) and 4,568,598 (Bilkadi et al.), the disclosures of which are incorporated herein by reference. The properties of catalyst layers using carbon nanotube arrays are reported in the paper "High Dispersion and Electrocatalytic Properties of Platinum on Well-Aligned Carbon Nanotube Arrays," Carbon, 2004, Vol. 42, pp. 191-197. The properties of catalyst layers using fusilli or wooly silica are reported, for example, in U.S. Patent Application Publication No. 2004 / 0048466A1 (Gore et al.).
[0051] Vacuum deposition can be performed in any suitable apparatus (see, e.g., U.S. Patent Applications 5,338,430 (Parsonage et al.), 5,879,827 (Debe et al.), 5,879,828 (Debe et al.), 6,040,077 (Debe et al.), and 6,319,293 (Debe et al.), and U.S. Patent Application Publication 2002 / 0004453A1 (Haugen et al.), the disclosures of which are incorporated herein by reference). An exemplary apparatus is schematically shown in U.S. Patent 5,338,430 (Parsonage et al.). Figure 4 A, and discussed in the accompanying text, wherein a substrate is mounted on a drum which is then rotated over a sublimation or evaporation source for deposition of an organic precursor (eg, perylene red pigment) which is then annealed to form whiskers.
[0052] Typically, the nominal thickness of the deposited perylene red pigment is in the range of about 50 nm to 500 nm. Typically, the average cross-sectional size of the whiskers is in the range of 20 nm to 60 nm, the average length is in the range of 0.3 microns to 3 microns, and the areal number density is in the range of 30 whiskers / square micron to 70 whiskers / square micron.
[0053] In some embodiments, the whiskers are attached to a backing. Exemplary backings include polyimide, nylon, metal foil, or other materials capable of withstanding thermal annealing temperatures up to 300° C. In some embodiments, the average thickness of the backing is in the range of 25 microns to 125 microns.
[0054] In some embodiments, the backing has a microstructure on at least one upper surface of its surface. In some embodiments, the microstructure is composed of feature structures of substantially uniform shape and size, which are at least three times (in some embodiments, at least four times, five times, ten times or more) the average size of the whiskers. The shape of the microstructure can be, for example, V-shaped grooves and peaks (see, for example, U.S. Pat. No. 6,136,412 (Spiewak et al.), the disclosure of which is incorporated herein by reference) or cones (see, for example, U.S. Pat. No. 7,901,829 (Debe et al.), the disclosure of which is incorporated herein by reference). In some embodiments, some portions of the microstructure features extend over the average or majority microstructured peaks in a periodic manner, such as every 31st V-groove peak is 25% or 50% or even 100% higher than the V-groove peaks on either side thereof. In some embodiments, the portion of the feature structure extending over the majority of microstructured peaks may be at most 10% (in some embodiments, at most 3%, 2% or even at most 1%). In a roll-to-roll coating operation, when the coated substrate moves on the surface of the roller, the use of occasionally higher microstructural features can be beneficial to protect the uniformly smaller microstructural peaks. Occasionally, the higher feature portion contacts the surface of the roller without contacting the peak of the smaller microstructure, so as the substrate moves during the coating process, very little microstructural material or whisker material may be scratched or otherwise damaged. In some embodiments, the microstructural features are substantially less than half the thickness of the membrane, wherein when the membrane electrode assembly is prepared, the catalyst will be transferred to the membrane. This makes it impossible for the higher microstructural features to penetrate through the membrane during the catalyst transfer process, wherein the higher microstructural features can be stacked on the opposite side of the membrane. In some embodiments, the highest microstructural features are less than 1 / 3 or 1 / 4 of the membrane thickness. For the thinnest ion exchange membrane (e.g., a thickness of about 10 microns to 15 microns), it may be advantageous to have a substrate with a microstructural feature with a height not greater than about 3 microns to 4.5 microns. In some embodiments, it may be desirable for the steepness of the sides of the V-shaped or other microstructured features or the angles included between adjacent features to be approximately 90° to facilitate catalyst transfer during the lamination transfer process and to increase the surface area of the electrode relative to the planar geometric surface of the base backing, which comes from the square root of two (1.414) times the surface area of the microstructured layer.
[0055] Generally speaking, catalyst can be deposited by technology known in the art. Exemplary deposition techniques include those independently selected from the following: sputtering (including reactive sputtering), atomic layer deposition, metal organic chemical vapor deposition, molecular beam epitaxy, thermal physical vapor deposition, electrospray ionization vacuum deposition and pulsed laser deposition. Other general details can be found in, for example, U.S. Patents 5,879,827 (Debe et al.), 6,040,077 (Debe et al.) and 7,419,741 (Vernstrom et al.), the disclosures of which are incorporated herein by reference. Thermal physical vapor deposition methods use suitable high temperatures (for example, by resistance heating, electron beam guns or lasers) to melt or sublimate the target (source material) into a gaseous state, which then passes through a vacuum space and then condenses the gasified form onto the substrate surface. Thermal physical vapor deposition equipment is known in the art, including, for example, metal evaporators or organic molecular evaporators available from CreaPhys GmbH, Dresden, Germany, under the trade names "METAL Evaporator (ME Series)" or "ORGANIC MOLECULAR EVAPORATOR (DE Series)", respectively; another example of an organic material evaporator is available from Mantis Deposition LTD, Oxfordshire, UK, under the trade name "ORGANIC MATERIAL SEVAPORATIOR (ORMA Series)". The catalyst material comprising multiple alternating layers can be sputtered, for example, from multiple targets (e.g., Pt from a first target, Ni from a second target, Ir from a third target, and from (one or more) targets comprising more than one element (e.g., Pt and Ni)). If the catalyst coating is done using a single target, it is desirable that the coating be applied to the gas distribution layer, gas dispersion layer, catalyst transfer layer or membrane in a single step so that the heat of condensation of the catalyst coating sufficiently heats the catalyst or support Pt, Ni or Ir atoms (if applicable) and the substrate surface below, thereby providing sufficient surface mobility so that the atoms mix well and form thermodynamically stable alloy domains. Alternatively, for example, a high temperature or heated substrate may be provided to promote the atomic mobility. In some embodiments, sputtering is performed at least in part in an atmosphere comprising argon. Catalysts in the form of organometallics may be deposited, for example, by soft landing or reactive landing techniques of mass-selected ions. Soft landing of mass-selected ions is used to transfer catalytically active metal complexes together with organic ligands from the gas phase to an inert surface. This method can be used to prepare materials with defined active sites, thereby achieving highly controlled molecular design for surfaces under ambient or conventional vacuum conditions.Additional details can be found, for example, in Johnson et al., Chem., 2010, 82, pp. 5718-5727, and Johnson et al., Chemistry: A European Journal, 2010, vol. 16, pp. 14433-14438, the disclosures of which are incorporated herein by reference.
[0056] The planar equivalent thickness of a single deposited catalyst layer is the thickness if deposited on a substantially flat planar substrate. The planar equivalent thickness may depend on, for example, the area catalyst loading and catalyst density of the layer. For example, the deposited Pt / cm 2 The surface area is 10 μg and the density is 21.45 g / cm 3 The plane equivalent thickness of the single-layer Pt is calculated to be 4.7 nm, and the Ni layer with the same area loading (8.90 g / cm 3 ) has a thickness of 11.2 nm and has an Ir layer with the same area loading (22.56 g / cm 3 One or more layers may be deposited to obtain a catalyst material having a total planar equivalent thickness equal to the sum of the planar equivalent thicknesses of each constituent layer.
[0057] In some embodiments, the thickness of the catalyst material is the planar equivalent thickness of the catalyst material divided by the combined surface area of the whiskers and the backing. For example, the combined surface area is 10 cm 2 Surface area / cm 2 A planar equivalent thickness of 20 nm of catalyst material deposited onto a planar backing surface including microstructured whiskers will result in a catalyst thickness of 2 nm on the whiskers. The surface area of the whiskers depends on the whisker cross-sectional dimensions, whisker length, and whisker areal density (number of whiskers per unit area of backing). In some embodiments, the surface area of the whiskers is between 1 and 100 cm 2 / cm 2 The surface area of the backing is within the range (in some embodiments, within 2 cm 2 / cm 2 Up to 50cm 2 / cm 2 , 5cm 2 / cm 2 Up to 25cm 2 / cm 2 or even 5cm 2 / cm 2 Up to 15cm 2 / cm 2 In some embodiments, the surface area of the backing may be within the range of 1 cm 2 / cm2 Up to 10cm 2 / cm 2 The planar backing area is within the range (in some embodiments, within 1 cm 2 / cm 2 Up to 5cm 2 / cm 2 within the range of 1cm 2 / cm 2 Up to 2cm 2 / cm 2 The combined surface area of the whiskers and the backing is the product of the whisker surface area and the backing surface area. For example, a surface area of 1.5 cm 2 Surface area / cm 2 The surface area of the backing is 10 cm 2 / cm 2 The whiskers of the backing area will produce 15cm 2 Combined surface area / cm 2 The combined surface area of the planar backing area.
[0058] In some embodiments, the method for preparing the catalyst material of this article includes annealing the catalyst. Generally speaking, annealing can be completed by techniques known in the art, including heating the catalyst material by, for example, in an oven or a heating furnace, with a laser and with infrared technology. Annealing can be carried out in, for example, an inert or reactive gas environment. Although not wanting to be limited by theory, it is believed that annealing can cause structural changes on the atomic scale, which can affect the activity and durability of the catalyst. In addition, it is believed that annealing can induce mobility in the atomic composition of nano-scale particles and films, which can lead to the growth of particles or film grains. In the case of multi-element mixtures, alloys or layered particles and films, it is believed that annealing can induce, for example, separation of components in particles or films to the surface, forming random, disordered alloys, and forming ordered intermetallic compounds, depending on the component element properties and annealing environment. For additional details on annealing, see, for example, van der Vliet et al., Nature Materials, 2012, 11, pp. 1051-1058; Wang et al., Nature Materials, 2013, 12, pp. 81-87, and U.S. Pat. No. 8,748,330 B2 (Debe et al.), the disclosures of which are incorporated herein by reference.
[0059] In some embodiments, the catalyst is substantially non-porous (i.e., the catalyst includes spherical and / or non-spherical void volumes, wherein at least 75% of the void volume is contained within the catalyst film (in some embodiments, 85%, 90%, 95%, 99% or even 100% is contained within the catalyst film), and wherein the average diameter of the void volume is less than 1 nm (in some embodiments, less than 0.8 nm, 0.6 nm, 0.4 nm, 0.2 nm or even 0.01 nm)).
[0060] In some embodiments, the method for preparing the catalyst described herein comprises depositing any of the layers via a deposition technique independently selected from sputtering (including reactive sputtering), atomic layer deposition, metal organic chemical vapor deposition, molecular beam epitaxy, ion soft landing, thermal physical vapor deposition, electrospray ionization vacuum deposition, and pulsed laser deposition. In some embodiments, the method for preparing the catalyst described herein comprises annealing at least one of the layers.
[0061] In some embodiments, the method for preparing the catalyst described herein comprises electrochemically cycling the catalyst. In some embodiments, the method for preparing the catalyst described herein comprises cycling the catalyst in an acidic electrolyte. In some embodiments, the method for preparing the catalyst described herein comprises cycling the catalyst between 0.60V and 1.00V relative to the potential of a standard hydrogen electrode.
[0062] In some embodiments, the microstructured whiskers are attached to a backing (eg, a film). In some embodiments, the backing has microstructures on at least one of its surfaces.
[0063] The catalysts described herein can be used, for example, in a fuel cell membrane electrode assembly (MEA). "Membrane electrode assembly" refers to a layered interlayer of fuel cell materials including a membrane, an anode electrode layer, and a cathode electrode layer, and a gas diffusion layer. Typically, the cathode catalyst layer comprises a catalyst described herein, but in some embodiments, the anode catalyst layer independently comprises a catalyst described herein.
[0064] In some embodiments, the article comprises a catalyst described herein. In some embodiments, the article does not comprise a conductive carbon-based material.
[0065] The MEA includes, in order:
[0066] a first gas distribution layer having first and second opposing major surfaces;
[0067] an anode catalyst layer having a first major surface and a second major surface opposite to each other, the anode catalyst comprising a first catalyst;
[0068] Electrolyte membrane;
[0069] a cathode catalyst layer having a first major surface and a second major surface that are opposite to each other, the cathode catalyst layer comprising a second catalyst; and
[0070] A second gas distribution layer has first and second opposite major surfaces.
[0071] The electrolyte membrane conducts the reaction intermediate ions between the anode catalyst layer and the cathode catalyst layer. The electrolyte membrane preferably has high durability in an electrochemical environment, including chemical and electrochemical oxidation stability. The electrolyte membrane preferably has low ionic resistance for the transmission of reaction intermediate ions, but is a relatively impermeable barrier to other ions, electrons and reaction substances. In some embodiments, the electrolyte membrane is a proton exchange membrane (PEM), which conducts cations. In a PEM fuel cell, the electrolyte membrane preferably conducts protons. PEM is generally a partially fluorinated or perfluorinated polymer consisting of a structural backbone and a cation exchange side group, and PEM is purchased from EIduPont de Nemours and Company, Wilmington, Delaware under the trade name "NAFION"; purchased from Solvay in Brussels, Belgium under the trade name "AQUIVION"; purchased from 3M Company in St. Paul, Minnesota under the trade name "3M PFSA MEMBRANE"; and purchased from Asahi Glass Co. in Tokyo, Japan under the trade name "FLEMION".
[0072] The gas distribution layer generally delivers gas uniformly to the electrode, and in some embodiments the gas distribution layer is conductive. With respect to a fuel cell, it also has the effect of removing water in the form of steam or liquid. The gas distribution layer is usually porous to allow reactants and products to be transmitted between the electrode and the flow field. The source of the gas distribution layer includes carbon fibers randomly oriented to form a porous layer, in the form of a nonwoven paper or woven fabric. Nonwoven carbon paper can be purchased from Mitsubishi Rayon Co., Ltd., Tokyo, Japan, for example under the trade name "GRAFIL U-105". It was purchased from Toray Corp. in Tokyo, Japan under the trade designation “TORAY”; from AvCarb Material Solutions in Lowell, Massachusetts under the trade designation “AVCARB”; from SGL Group, the Carbon Company in Wiesbaden, Germany under the trade designation “SIGRACET”; from Freudenberg FCCT SE & Co. KG, Fuel Cell Component Technologies in Weinheim, Germany under the trade designation “Freudenberg”; and from Engineered Fibers Technology (EFT) in Shelton, Connecticut under the trade designation “SPECTRACARB GDL.” Woven carbon fabrics or cloths are available, for example, from ElectroChem Inc., Woburn, MA, under the trade designations "EC-CC1-060" and "EC-AC-CLOTH"; from NuVant Systems Inc., Crown Point, Indiana, under the trade designations "ELAT-LT" and "ELAT"; from BASF Fuel Cell GmbH, North America, under the trade designation "E-TEK ELAT LT"; and from Zoltek Corp., St. Louis, Missouri, under the trade designation "ZOLTEK CARBON CLOTH." The nonwoven paper or woven fabric may be treated to alter its hydrophobicity (e.g., by treatment with a polytetrafluoroethylene (PTFE) suspension followed by drying and annealing). The gas dispersion layer typically includes a porous layer of submicron electronically conductive particles (e.g., carbon) and a binder (e.g., PTFE). While not wanting to be limited by theory, it is believed that the gas dispersion layer facilitates reactant and product water transport between the electrode and the gas distribution layer.
[0073] At least one of the anode or cathode catalyst is a catalyst as described herein. In some embodiments, the catalyst surface area is at least 5% greater than the catalyst surface area that would be present in the absence of the Ir layer (in some embodiments, at least 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, or even at least 49%). The "other catalyst layer" can be a conventional catalyst known in the art and is provided by techniques known in the art (e.g., U.S. Pat. Nos. 5,759,944 (Buchanan et al.), 5,068,161 (Keck et al.), and 4,447,506 (Luczak et al.), the disclosures of which are incorporated herein by reference.
[0074] A fuel cell is an electrochemical device that combines hydrogen fuel and oxygen from the air to generate electricity, heat, and water. A fuel cell does not utilize combustion, and therefore, generates little, if any, hazardous effluent. A fuel cell converts hydrogen fuel and oxygen directly into electrical energy, and operates at much higher efficiencies than, for example, an internal combustion generator.
[0075] Reference Figure 2 , the exemplary fuel cell 200 includes a first gas distribution layer 201 adjacent to an anode 203. Adjacent to the anode 203 is an electrolyte membrane 204. A cathode 205 is located adjacent to the electrolyte membrane 204, and a second gas distribution layer 207 is located adjacent to the cathode 205. In operation, hydrogen fuel is introduced into the anode portion of the fuel cell 200, passing through the first gas distribution layer 201 and being located on the anode 203. At the anode 203, the hydrogen fuel is separated into hydrogen ions (H + ) and electron (e - ).
[0076] The electrolyte membrane 204 allows only hydrogen ions or protons to pass through the electrolyte membrane 204 to the cathode portion of the fuel cell 200. Electrons cannot pass through the electrolyte membrane 204, but flow through an external circuit in the form of an electric current. This current can provide power to an electrical load 217 (such as an electric motor) or be directed to an energy storage device (such as a rechargeable battery).
[0077] Oxygen flows into the cathode side of the fuel cell 200 through the second distribution layer 207. As the oxygen passes through the cathode 205, the oxygen, protons, and electrons combine to generate water and heat.
[0078] Exemplary embodiments
[0079] 1A. A catalyst comprising an Ir layer having an outer layer having a layer comprising Pt directly thereon, wherein the Ir layer has an average thickness in a range of 0.04 nm to 30 nm (in some embodiments, 0.04 nm to 20 nm, 0.05 nm to 20 nm, 0.05 nm to 10 nm, 0.05 nm to 8 nm, 0.05 nm to 6 nm, 0.05 nm to 5 nm, 0.05 nm to 4 nm, In some embodiments, the Pt-containing layer has an average thickness in the range of 0.04 nm to 50 nm (in some embodiments, in the range of 0.04 nm to 40 nm, 0.04 nm to 57 nm, 0.05 nm to 10 nm, 0.05 nm to 20 nm, 0.05 nm to 15 nm, 0.05 nm to 20 nm, 0.05 nm to 10 nm, 0.05 nm to 15 nm, 0.05 nm to 20 nm, 0.05 nm to 15 nm, 0.05 nm to 10 nm, 0.05 nm to 0.98 nm, 0.05 nm to 0.39 nm, 0.05 nm to 0.36 nm, or even 0.8 nm to 0.85 nm). 0.04 nm to 1 nm, 0.04 nm to 0.71 nm, 0.04 nm to 0.34 nm, or even in the range of 0.04 nm to 30 nm, 0.04 nm to 20 nm, 0.04 nm to 10 nm, 0.04 nm to 5 nm, 0.04 nm to 4 nm, 0.04 nm to 3 nm, 0.04 nm to 2.99 nm, 0.04 nm to 2.5 nm, 0.04 nm to 2 nm, 0.04 nm to 1.57 nm, 0.04 nm to 1 nm, 0.04 nm to 0.71 nm, 0.04 nm to 0.34 nm, or even in the range of 0.04 nm to 0.31 nm), and wherein the Pt and the Ir are present in an atomic ratio in the range of 0.01:1 to 10:1 (in some embodiments, in the range of 0.04:1 to 2.85:1, 0.35:1 to 1.79:1, 0.72:1 to 1.18:1, 0.19:1 to 5.90:1, 0.31:1 to 5.90:1, 0.76:1 to 1.88:1, or even in the range of 0.85:1 to 3.87:1).
[0080] 2A. The catalyst of exemplary embodiment 1A, wherein the catalyst surface area is at least 5% (in some embodiments, at least 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 20, 25, 30, 35, 40, 45, or even at least 49%) greater than the catalyst surface area that would exist in the absence of the Ir layer.
[0081] 3A. The catalyst of example embodiment 1A or 2A, further comprising at least one pair of alternating layers, wherein the first alternating layers comprise Ir, and wherein the second alternating layers comprise Pt.
[0082] 4A. The catalyst of any preceding A exemplary embodiment, wherein the catalyst further comprises nanoscale metal grains extending from a surface of the catalyst.
[0083] 5A. A catalyst according to exemplary embodiment 4A, wherein the surface metal grains comprise at least 10 atomic % (in some embodiments, at least 15 atomic %, 20 atomic %, 25 atomic %, 30 atomic %, 40 atomic %, 50 atomic %, 60 atomic %, 70 atomic %, 75 atomic %, 80 atomic %, 90 atomic %, 95 atomic %, 98 atomic %, 99 atomic %, or even at least 99.9 atomic %) Ir.
[0084] 6A. A catalyst according to exemplary embodiments 4A or 5A, wherein the length of the surface metal grains is in the range of 0.25 nm to 10 nm (in some embodiments, in the range of 0.25 nm to 8 nm, 0.25 nm to 6 nm, 0.25 nm to 4 nm, 0.25 nm to 3 nm, 0.25 nm to 2 nm, 0.25 nm to 1 nm, 1 nm to 10 nm, 1 nm to 8 nm, 1 nm to 6 nm, 1 nm to 4 nm, 1 nm to 3 nm, or even in the range of 1 nm to 2 nm).
[0085] 7A. The catalyst of either exemplary embodiment 4A or 5A, wherein the surface metal grains have a length of less than 8 nm (in some embodiments, less than 7 nm, 6 nm, 5 nm, 4 nm, 3 nm, 2 nm, or even less than 1 nm).
[0086] 8A. The catalyst of either exemplary embodiment 4A or 5A, wherein the surface metal grains have a diameter in the range of 0.25 nm to 5 nm (in some embodiments, in the range of 0.25 nm to 4 nm, 0.25 nm to 3 nm, 0.25 nm to 2 nm, 0.25 nm to 1 nm, 1 nm to 5 nm, 1 nm to 4 nm, 1 nm to 3 nm, or even 1 nm to 2 nm).
[0087] 9A. The catalyst of example embodiments 4A or 5A, wherein the surface metal grains have a diameter less than 5 nanometers (in some embodiments, less than 4 nanometers, 3 nanometers, 2 nanometers, or even less than 1 nanometer).
[0088] 10A. The catalyst according to any of the preceding A exemplary embodiments, wherein the layer comprising Pt further comprises Ni.
[0089] 11A. The catalyst of exemplary embodiment 10A, wherein the atomic ratio of Pt to Ni is in the range of 0.5:1 to 5:1 (in some embodiments, in the range of 0.5:1 to 2:1, 0.5:1 to 1:1, 0.57:1 to 0.69:1, or even 0.58:1 to 0.62:1).
[0090] 1B. An article comprising nanostructured elements comprising microstructured whiskers having an outer surface having a catalyst according to any of the preceding A exemplary embodiments thereon.
[0091] 2B. The article of example embodiment 1B, wherein the Ir layer is directly on the microstructured whiskers.
[0092] 3B. The catalyst of either exemplary embodiment 1B or 2B, wherein the article further comprises at least one pair of alternating layers disposed between the outer surface of the microstructured whiskers and the layer comprising Ir, wherein a first alternating layer comprises Ir and is directly on the microstructured whiskers, and wherein a second alternating layer comprises Pt.
[0093] 4B. The catalyst according to any preceding B exemplary embodiment, wherein the microstructured whiskers are attached to a backing (eg, a film).
[0094] 5B. The catalyst of exemplary embodiment 4B, wherein the backing has a microstructure on at least one of its surfaces.
[0095] 6B. The article of any preceding B exemplary embodiment, which does not comprise an electrically conductive carbon-based material.
[0096] 1C. A method for preparing an article according to any of the aforementioned A exemplary embodiments, the method comprising depositing any of the layers via a deposition technique independently selected from sputtering (including reactive sputtering), atomic layer deposition, metal organic chemical vapor deposition, molecular beam epitaxy, ion soft landing, thermal physical vapor deposition, electrospray ionization vacuum deposition and pulsed laser deposition.
[0097] 2C. A method for preparing an article according to any of the aforementioned B exemplary embodiments, the method comprising depositing any of the layers on a microstructured whisker via a deposition technique, the deposition technique being independently selected from sputtering (including reactive sputtering), atomic layer deposition, metal organic chemical vapor deposition, molecular beam epitaxy, ion soft landing, thermal physical vapor deposition, electrospray ionization vacuum deposition, and pulsed laser deposition.
[0098] 3C. The method according to any of the preceding C exemplary embodiments, further comprising annealing at least one of the layers.
[0099] 1D. A method for preparing a catalyst according to any of the preceding A exemplary embodiments, the method comprising electrochemically cycling the catalyst.
[0100] 2D. The method of example embodiment ID, further comprising circulating the catalyst in an acidic electrolyte.
[0101] 3D. The method of example embodiments 1D or 2D further comprising cycling the catalyst within a range of 0.60 V to 1.00 V relative to the potential of a standard hydrogen electrode.
[0102] The following examples further illustrate the advantages and embodiments of the present invention, but the specific materials and amounts thereof mentioned in these examples, as well as other conditions and details, should not be construed as unduly limiting the present invention. Unless otherwise indicated, all parts and percentages are by weight.
[0103] Example
[0104] Preparation Example A
[0105] Microstructured whiskers for use as catalyst supports were prepared according to the methods described in U.S. Pat. Nos. 5,338,430 (Parsonage et al.), 4,812,352 (Debe), and 5,039,561 (Debe), also incorporated herein by reference, using a microstructured catalyst transfer substrate (or MCTS) described in U.S. Pat. No. 6,136,412 (Spiewak et al.), incorporated herein by reference. Perylene red pigment (i.e., N,N'-di(3,5-dimethylphenyl)perylene-3,4:9,10-bis(dicarboximide)) Pigment Red 149, also referred to as "PR149", available from Clariant, Charlotte, NC) was sublimation vacuum deposited onto a nominally 200 nm thick MCTS and then annealed. After deposition and annealing, a highly oriented crystalline structure is formed: its aspect ratio is large, with a controllable length of about 0.5 microns to 2 microns, a width of about 0.03 microns to 0.05 microns, an area density of about 30 whiskers per square micron, and the orientation of the structure is basically perpendicular to the substrate below it.
[0106] Comparative Example A
[0107] A nanostructured thin film (NSTF) catalyst layer was prepared by sequentially sputtering a catalyst film onto a microstructured whisker layer using a DC-magnetron sputtering process, Preparation Example A. A vacuum sputtering deposition system was used with a typical Ar sputtering gas pressure of about 3.3 mTorr (0.44 Pa) and a 5 in x 15 in (12.7 cm x 38.1 cm) rectangular Pt sputtering target. The system base pressure was typically 2.5 x 10 -5 Torr (0.0033 Pa), the background gas usually measured is water vapor. The coating is deposited by using ultra-high purity Ar as the sputtering gas.
[0108] A single Pt layer with an in-plane equivalent thickness of about 0.25 nm was first deposited from a pure Pt target onto the whiskers on MCTS. The Pt deposition process was repeated 50 times. The resulting deposit consisted of a single continuous Pt film with an overall continuous Pt in-plane equivalent thickness of about 12.6 nm, summarized in Table 1 below.
[0109] Table 1
[0110]
[0111] Since the metal is deposited onto an MCTS substrate coated with an inherently rough NSTF support, the metal film thickness on the support is thinner than the equivalent thickness on the plane by the overall support factor and the substrate roughness factor. It is estimated that the NSTF support can provide 10 cm 2 Surface area / cm 2 planar area, and MCTS provides an additional 1.4cm 2 surface area, so the total surface area is 14cm 2 . Distributed in 14cm 2 / cm 2 The equivalent thickness of the 12.6 nm plane on the surface is about 0.9 nm.
[0112] The bulk composition of representative areas of the electrocatalyst was analyzed using X-ray fluorescence spectrometry (XRF). Representative catalyst samples were evaluated using a wavelength dispersive X-ray fluorescence spectrometer (purchased from Rigaku Corporation, Tokyo, Japan under the trade name "PRIMUS II") on MCTS, and the fluorescence spectrometer was equipped with a rhodium (Rh) X-ray source, a vacuum atmosphere environment, and a 20-mm diameter measurement area. Each sample was analyzed three times to obtain the mean and standard deviation of the measured Pt, Ni, and Ir signal intensities, and the mean and standard deviation were proportional to the loading. The Pt, Ni, and Ir loadings of the electrocatalyst were determined by comparing their measured XRF intensities with the XRF intensities obtained with standard NSTF electrocatalysts containing Pt, Ni, and Ir with known area loadings. The composition of the catalyst was calculated based on the Pt, Ni, and Ir loadings determined by XRF. The loading and composition information of Comparative Example A is provided in Table 2 below. Comparative Example A contains 27 micrograms / cm 2 of Pt and contains no measurable Ni or Ir.
[0113] Table 2
[0114]
[0115] Next, the electrochemical performance of the catalysts was evaluated by assembling into a membrane electrode assembly (MEA) and using the catalysts as fuel cell cathodes, as described below. Typically, at least 2 MEAs were fabricated for each catalyst type, evaluated, and the average values reported.
[0116] The Comparative Example A catalyst and NSTF PtCoMn coated anode catalyst whiskers (0.05 mg) on MCTS were then laminated using a laminator (available from ChemInstruments, Inc., West Chester Township, OH, under the trade designation “HL-101”). Pt / cm 2 , Pt 69 Co 28 Mn 3) was transferred to either side of a 24 micron thick proton exchange membrane (obtained from 3M Company, St. Paul, Minnesota, USA under the trade designation "3M PFSA 825EW" (neat)) to form a catalyst coated membrane (CCM). The three-layer stack was manually fed into a laminator using hot rollers at 270°F (132°C), 150 psi (1.03 MPa) roll gap, and rotated at a speed equivalent to 0.5 fpm (0.25 cm / s). The MCTS layer was peeled off immediately after lamination, leaving the catalyst coated whiskers embedded on either side of the PEM. The CCM was installed with identical gas diffusion layers (obtained from 3M Company under the trade designation "3M 2979 GASDIFFUSION LAYERS") on the anode and cathode, at 50 cm 2 Active area test cell (trade name "50CM 2 The "CELL HARDWARE" was obtained from Fuel Cell Technologies, Inc., Albuquerque, NM) with a quad serpentine flow field, and the gasket was selected to compress the gas diffusion layer by 10%. The comparative example A catalyst was evaluated as a fuel cell cathode.
[0117] After assembly, the test cell was connected to a test station (available from Fuel Cell Technologies, Inc. under the trade name "SINGLE FUEL CELL TEST STATION"). The MEA was then operated under a conditioning regime for approximately 40 hours to achieve apparent steady-state performance. The regime consisted of repeated cycles of operating and shut-down phases, each lasting approximately 40 minutes and 45 minutes, respectively. During the operating phase, the MEA was operated at 75°C cell temperature, 70°C dew point, 101 / 101 kPaA H 2 / air operated MEA, where H 2 The constant flow rates of H and air were 800 standard cubic centimeters per minute (sccm) and 1800 standard cubic centimeters per minute, respectively. During the 40-minute operating phase, the cell voltage alternated between 5-minute long polarization cycles between 0.85 V and 0.25 V, and a 5-minute long potential was maintained at 0.40 V. During the 45-minute off phase, the cell potential was set to the open circuit voltage, allowing H 2 and air flow until the battery stopped, and the battery temperature was cooled to room temperature, while liquid water was injected into the anode and cathode battery inlets at 0.26 g / min and 0.40 g / min, respectively.
[0118] After conditioning the MEA, the electrocatalysts were characterized for relevant Beginning of Life (BOL) characteristics, including relevant H 2The catalyst activity, surface area and operating performance under Mg / air test conditions are described below.
[0119] Saturated with 150 kPaA H 2 / O 2 , 80℃ battery temperature at 900mV relative to 100% H 2 The reference electrode / counter electrode measures the absolute activity of the cathode oxygen reduction reaction (ORR) for 1200 seconds. ORR absolute activity (A / cm 2 or mA / cm 2 ) is obtained by adding the current density measured after a holding time of 1050 s to the electron short circuit and hydrogen crossover current densities, which are estimated from the 2 mV / s cyclic voltammogram, using N 2 Add working electrode instead of O 2 The ORR absolute activity (A / cm 2 平面 ) divided by the cathode Pt area loading (mg / cm 2 ) to obtain Pt mass activity (A / mg Pt ), or by dividing the corrected ORR absolute activity by the cathode total platinum group metal (PGM) area loading to obtain the PGM mass activity (A / mg PGM ), thereby calculating the electrocatalyst mass activity, which is a measure of the catalyst activity per unit of precious metal content. The mass activity of Pt and PGM in Comparative Example A is 0.16 A / mg Pt and 0.16A / mg PGM , reported in Table 3 below.
[0120] Table 3
[0121]
[0122] At saturated H2O at 101 kPa absolute pressure (kPaA) 2 / N 2 The surface enhancement factor (SEF, m) of the cathode catalyst was measured by cyclic voltammetry (100 mV / s, 0.65 V-0.85 V, average of 100 scans) at a cell temperature of 70 °C. 2 PGM / m 2 平面 or similar cm 2 PGM / cm 2 平面 By taking the integral of the oxidation wave and the reduction wave, hydrogen underpotential deposition (H UPD ) Charge (microC / cm 2 平面) and divide it by 220 microC / cm 2 Pt To estimate SEF, we can use -SEF(m 2 PGM / m 2 平面 ) divided by the area PGM load (g PGM / m 2 平面 ), calculate the specific surface area of the electrocatalyst (m 2 PGM / g PGM ), which is a measure of the dispersion of the catalyst. The specific area of Comparative Example A is 11.4 m 2 PGM / g PGM , reported in Table 3 above.
[0123] The corrected ORR absolute activity (A / cm 2 平面 ) divided by SEF (cm 2 PGM / cm 2 平面 ) to obtain (A / cm 2 PGM- ) or when converting the unit to mA / cm 2 PGM (A / cm 2 ) was multiplied by 1000 mA / A) to calculate the oxygen reduction specific activity of the cathode catalyst. The specific activity of Comparative Example A was 1.37 mA / cm 2 PGM , summarized in Table 3 above.
[0124] After the activity and surface area characterization was completed, the H of the MEA was measured. 2 / Air performance. The MEA was operated at 80°C cell temperature with the cathode exposed to air (68°C dew point, 150 kPaA, constant stoichiometry 2.5) and the anode exposed to H 2 (68°C dew point, 150 kPaA, constant stoichiometric ratio 2.0). The MEA current density (J) was increased from 0.02 A / cm 2 Increase gradually until the battery voltage reaches 0.40V or J reaches 2A / cm 2 , the scan is now in the reverse direction. The J step interval is 10 / decade and 0.1A / cm 2 Polarization data were collected at approximately 1 Hz at each J with a dwell time of 120 seconds. The reported polarization data are the average of all data points at each J setting in the high to low current portion of the polarization curve. The polarization curves were linearly interpolated to provide the2 and 0.32A / cm 2 The battery voltage at a battery current density of 0.1 V and the current density at a battery voltage of 0.50 V are summarized in Table 4 below.
[0125] Table 4
[0126] Example <![CDATA[0.02A / cm 2 V in volts]]> <![CDATA[0.32A / cm 2 V in volts]]> <![CDATA[J at 0.50 V, A / cm 2 > Comparative Example A 0.799 0.603 0.500 Comparative Example B 0.837 0.728 1.657 Comparative Example C 0.707 <<0.4 0.116 Comparative Example D 0.768 0.573 0.442 Comparative Example E 0.843 0.761 1.805 Comparative Example F 0.803 0.639 0.651 Comparative Example G 0.812 0.654 0.897 Comparative Example H 0.818 0.659 0.897 Comparative Example I 0.820 0.668 1.112 Comparative Example J 0.547 <<0.4 0.043 Example 1 0.735 0.406 0.186 Example 2 0.810 0.614 0.655 Example 3 0.846 0.708 1.261 Example 4 0.859 0.741 1.397 Example 5 0.856 0.739 1.479 Example 6 0.865 0.752 1.466 Example 7 0.858 0.743 1.157 Example 8 0.771 0.436 0.264 Example 9 0.811 0.620 0.531 Example 10 0.839 0.697 1.152 Embodiment 11 0.843 0.702 1.234 Example 12 0.836 0.683 1.173 Example 13 0.822 0.660 0.996 Comparative Example K 0.832 0.670 1.065 Comparative Example L 0.814 0.670 1.048 Comparative Example M 0.025 <<0.4 <0.05 Embodiment 14 0.838 0.697 1.173 Embodiment 15 0.851 0.729 1.225 Comparative Example N 0.751 0.380 0.217 Comparative Example O 0.822 0.636 0.490
[0127] Next, the catalyst durability was evaluated using an accelerated stress test (AST). During AST, the MEA was operated at 80°C cell temperature with the cathode exposed to nitrogen (80°C dew point, 100 kPaA, constant current 1800 sccm) and the anode exposed to H 2 (80℃ dew point, 100kPaA, constant flow 800sccm). 2 The anode electrode reference potential was set using a potentiostat (obtained from Biologic Science Instruments, Seyssinet-Pariset, France under the trade designation "MPG-205") and the cathode electrode potential was cycled 30,000 times between 0.60 V and 1.00 V using a triangle wave at 50 mV / s. After the 30,000 cycles were completed, the MEA was reconditioned and the cathode activity, surface area, and H were measured again. 2 / Air performance. Mass activity, specific area, specific activity, 0.02A / cm2 of Comparative Example A after AST 2 The battery voltage at 0.32A / cm 2 The changes in the cell voltage at 0.50 V and the current density at 0.50 V are listed in Table 5 below.
[0128] Table 5
[0129]
[0130] Comparative Example B
[0131] Comparative Example B was prepared and characterized as described for Comparative Example A, except that the Pt deposition process was modified to achieve a Pt areal loading of 54 μg / cm 2 The results are provided in Tables 3 to 5 above.
[0132] Comparative Example CE
[0133] Comparative Examples CE were prepared and characterized as described for Comparative Example A, except that the Pt deposition process was modified to result in Pt areal loadings of 13, 24, and 98 μg / cm 2AST was not used to evaluate the durability of the Comparative Example CE catalysts. The results are provided in Tables 3 and 4 above.
[0134] Comparative Example F
[0135] Comparative Example F was prepared and characterized as described for Comparative Example A, except that the deposition process was modified to produce different Pt area loadings and an Ir layer was also deposited on the surface of the Pt. A nanostructured thin film (NSTF) catalyst layer was prepared by sequentially sputtering a catalyst film onto a microstructured whisker layer using a DC-magnetron sputtering process, Preparation Example A. A vacuum sputtering deposition system was used with a typical Ar sputtering gas pressure of about 3.3 mTorr (0.44 Pa) and 5 inch x 15 inch (12.7 cm x 38.1 cm) rectangular Pt and Ir sputtering targets. The system base pressure was typically 2.5x10 -5 Torr (0.0033 Pa), the background gas usually measured is water vapor. The coating is deposited by using ultra-high purity Ar as the sputtering gas.
[0136] First, a single Pt layer with a planar equivalent thickness of about 1.4 nm was deposited from a pure Pt target onto the whiskers on MCTS. The Pt deposition process was performed 10 times to obtain a Pt layer with a thickness of about 30 μg / cm 2 Next, a single Ir layer with a planar equivalent thickness of 0.58 nm was deposited. The Ir deposition process was performed once to obtain approximately 1.3 μg / cm 2 The durability of the catalyst of Comparative Example F was evaluated using AST. The results are provided in Tables 3 to 5 above.
[0137] Comparative Example GI
[0138] Comparative Example GI was prepared and characterized as described for Comparative Example F, except that the Ir deposition process was modified to result in Ir areal loadings of approximately 3.3, 9.9, and 12.7 μg / cm, respectively. 2 The durability of the Comparative Example G and H catalysts was evaluated using AST, while the Comparative Example I catalyst was not evaluated. The results are provided in Tables 3 to 5 above.
[0139] Comparative Example J
[0140] Comparative Example J was prepared and characterized as described for Comparative Example F, except that the deposition process was modified so that only Ir was deposited.
[0141] Nanostructured thin film (NSTF) catalyst layers were prepared by sequentially sputtering a catalyst film onto a microstructured whisker layer using a DC-magnetron sputtering process, Preparation Example A. A vacuum sputtering deposition system was used with a typical Ar sputtering gas pressure of about 3.3 mTorr (0.44 Pa) and a 5 in x 15 in (12.7 cm x 38.1 cm) rectangular Ir sputtering target. The system base pressure was typically 2.5 x 10 -5 Torr (0.0033Pa), the background gas usually measured is water vapor. The coating is deposited by using ultra-high purity Ar as the sputtering gas. First, a single Ir layer with a planar equivalent thickness of about 1.1nm is deposited from a pure Ir target onto the whiskers on MCTS. The Ir deposition process is performed 10 times to obtain about 26 μg / cm 2 area load.
[0142] After deposition, the electrocatalyst on MCTS was placed in a quartz tube furnace (purchased under the trade designation “LINDBERG BLUE M” from Thermo Electron Corporation, Waltham, MA, USA) and heated under flowing H 2 After about 20 minutes of temperature ramp, the catalyst was annealed at the above temperature for about 0.5 hours and then cooled to room temperature over a period of about 3 hours. After cooling to room temperature, the tube furnace was purged with nitrogen for about 15 minutes to remove any residual H 2 , after which the catalyst on the substrate was removed from the furnace. The durability of Comparative Example J was evaluated using AST. The results are provided in Tables 3 to 5 above.
[0143] Example 1
[0144] The Example 1 catalyst was prepared and characterized as described for Comparative Example J, except that the Pt layer was then deposited after the Ir was deposited onto the whiskers on MCTS. The catalyst was then sequentially annealed using the same protocol as described in Comparative Example J. The durability of the Example 1 catalyst was not evaluated under AST.
[0145] Nanostructured thin film (NSTF) catalyst layers were prepared by sequentially sputtering a catalyst film onto a microstructured whisker layer using a DC-magnetron sputtering process, Preparation Example A. A vacuum sputtering deposition system was used with a typical Ar sputtering gas pressure of about 3.3 mTorr (0.44 Pa) and 5 in x 15 in (12.7 cm x 38.1 cm) rectangular Pt and Ir sputtering targets. The system base pressure was typically 2.5 x 10 -5 Torr (0.0033 Pa), the background gas usually measured is water vapor. The coating is deposited by using ultra-high purity Ar as the sputtering gas.
[0146] First, a single Ir layer with a planar equivalent thickness of about 1.1 nm was deposited from a pure Ir target onto the whiskers on MCTS. The Ir deposition process was performed 10 times to obtain about 26 μg / cm 2 Next, a single Pt layer with a planar equivalent thickness of 0.47 nm was deposited. The Pt deposition process was performed twice to obtain approximately 1.1 μg / cm 2 The results are provided in Tables 3 and 4 above.
[0147] Embodiment 2-7
[0148] Examples 2 to 7 were prepared and characterized as described for Example 1, except that the Pt deposition process was modified to result in Pt areal loadings of approximately 4.2, 9.3, 19, 31, 47, and 75 μg / cm, respectively. 2 Examples 3 to 6 were evaluated for durability under AST, but Example 2 was not evaluated. The results are provided in Tables 3 to 5 above.
[0149] After the fuel cell test, the nanoscale structure of the catalyst of Example 2 was additionally analyzed by transmission electron microscopy (TEM). After the durability test, the nanoscale structure and composition of the catalyst of Example 3 were additionally analyzed by TEM and energy dispersive X-ray spectroscopy (EDS).
[0150] Example 8
[0151] The catalyst of Example 8 was prepared and characterized as described for Example 1, except that the Pt and Ir contents were different, as shown in Table 2 above.
[0152] Nanostructured thin film (NSTF) catalyst layers were prepared by sequentially sputtering a catalyst film onto a microstructured whisker layer using a DC-magnetron sputtering process, Preparation Example A. A vacuum sputtering deposition system was used with a typical Ar sputtering gas pressure of about 3.3 mTorr (0.44 Pa) and 5 in x 15 in (12.7 cm x 38.1 cm) rectangular Pt and Ir sputtering targets. The system base pressure was typically 2.5 x 10 -5 Torr (0.0033 Pa), the background gas usually measured is water vapor. The coating is deposited by using ultra-high purity Ar as the sputtering gas.
[0153] First, a single Ir layer with a planar equivalent thickness of about 0.38 nm was deposited from a pure Ir target onto the whiskers on MCTS. The Ir deposition process was performed twice to obtain about 1.7 μg / cm 2 Next, a single Pt layer with a planar equivalent thickness of 0.40 nm was deposited. The Pt deposition process was performed 12 times to obtain approximately 10.2 μg / cm 2The durability of the catalyst of Example 8 was not evaluated using AST. The results are provided in Tables 3 and 4 above.
[0154] Examples 9-12
[0155] Examples 9 to 12 were prepared and characterized as described for Example 8, except that the Ir deposition process was modified to result in Ir areal loadings of approximately 5.4, 12, 31, and 52 μg / cm, respectively. 2 The durability of Example 10 was evaluated under AST, but Examples 9, 11 and 12 were not evaluated. The results are provided in Tables 3 to 5 above.
[0156] In addition, the nanostructure and composition of the catalyst of Example 10 were analyzed by TEM and EDS after catalyst deposition, after annealing, after fuel cell testing, and after durability testing with AST. The results are shown in Figures 10 to 17 middle.
[0157] Example 13
[0158] Example 13 was prepared and characterized as described for Example 3, except that the catalyst was not annealed and its durability was not evaluated under AST. The results are provided in Tables 3 and 4 above.
[0159] Comparative Example K
[0160] Comparative Example K was prepared and characterized as described for Example 10, except that the deposition order of Pt and Ir was reversed. Approximately 10 μg / cm 2 Pt was then deposited at about 14 μg / cm 2 The durability of Comparative Example K was not evaluated under AST. The results are provided in Tables 3 and 4 above.
[0161] Comparative Example L
[0162] Comparative Example L was prepared and characterized as described for Example 10, except that the deposition conditions were changed to produce multiple alternating thinner layers of Pt and Ir to promote the formation of the PtIr alloy catalyst. A single Ir layer with a planar equivalent thickness of about 0.52 nm was first deposited from a pure Ir target onto the whiskers on MCTS. Next, a single Pt layer with a planar equivalent thickness of 0.33 nm was deposited. The Ir and Pt deposition process was performed alternately 12 times to obtain about 10.3 μg / cm 2 The Pt area loading is about 14 μg / cm 2 The durability of Comparative Example L was not evaluated under AST. The results are provided in Tables 3 and 4 above.
[0163] Comparative Example M
[0164] Comparative Example M was prepared and characterized as described for Example 10, except that 10 μg / cm 2 Au was used instead of Ir, and AST was not used to evaluate the durability of Comparative Example M. The results are provided in Tables 3 and 4 above.
[0165] Embodiment 14
[0166] The Example 14 catalyst was prepared and characterized as described for Example 1, except that the Pt and Ir contents were different and the Pt layer also contained Ni. The durability of the Example 14 catalyst was not evaluated using AST.
[0167] Nanostructured thin film (NSTF) catalyst layers were prepared by sequentially sputtering a catalyst film onto a microstructured whisker layer using a DC-magnetron sputtering process, Preparation Example A. A vacuum sputtering deposition system was used with a typical Ar sputtering gas pressure of about 3.3 mTorr (0.44 Pa) and 5 inch x 15 inch (12.7 cm x 38.1 cm) rectangular Pt, Ir, and Ni sputtering targets. The system base pressure was typically 2.5×10 -5 Torr (0.0033 Pa), the background gas usually measured is water vapor. The coating is deposited by using ultra-high purity Ar as the sputtering gas.
[0168] First, a single Ir layer with a planar equivalent thickness of about 0.89 nm was deposited from a pure Ir target onto the whiskers on MCTS. The Ir deposition process was repeated 5 times to obtain about 11 μg Ir / cm 2 Next, a single Pt layer with a planar equivalent thickness of 2.3 nm was deposited, and a single Ni layer with a planar equivalent thickness of 2.8 nm was deposited. The Pt deposition process and the Ni deposition process were performed twice in sequence, resulting in a total of about 9.3 μg / cm 2 The Pt area loading is about 4.9 μg / cm 2 The results are provided in Tables 3 and 4 above.
[0169] Embodiment 15
[0170] Example 15 was prepared and characterized as described for Example 14, except that the Pt and Ni deposition processes were modified so that the Pt area loading was about 21 μg / cm 2 , and the Ni area loading is about 10 μg / cm 2 The Ir area content is similar to that of Example 14, which is about 11 μg / cm 2 The durability of Example 15 was evaluated using AST. The results are provided in Tables 3 to 5 above.
[0171] Comparative Example N
[0172] Comparative Example N was prepared and evaluated as described for Example 14, except that Ir was not deposited. The durability of Comparative Example N was evaluated using AST. The results are provided in Tables 3-5 above.
[0173] Comparative Example O
[0174] Comparative Example 0 was prepared and characterized as described for Example 14, except that Ir was deposited onto the surface of the multiple alternating Pt and Ni layers and the Ir deposition process was modified to deposit approximately 5 μg / cm 2 The durability of Comparative Example O was evaluated using AST. The results are provided in Tables 3 to 5 above.
[0175] Figure 3 Table 3 above summarizes the Pt mass activity of Comparative Examples A to E and Examples 1 to 12 as a function of total PGM (Pt+Ir) area loading. Comparative Examples A to E do not include an Ir underlayer. Examples 1 to 12 do include an Ir underlayer directly on the microstructured whiskers.
[0176] The Pt mass activities of Comparative Examples A to E range from 0.14 A / mg to 0.16 A / mg and are comparable to those of Comparative Examples A to E. 2 and 98 μg / cm 2 The Pt area loading between them is relatively independent.
[0177] In the similar PGM area loading range, the Pt mass activity of Examples 1 to 7 and 8 to 12 is higher than that of the Comparative Example. For Examples 1 to 7 (different amounts of Pt on fixed Ir mat loading), as the Pt area loading increases from about 75 μg / cm 2 Reduced to 1.1 μg / cm 2 , Pt mass activity from 0.20A / mg Pt Increased to 1.45A / mg Pt The maximum Pt mass activity obtained by Example 1 is about 10 times that of Pt.
[0178] As the Ir area loading increases from 1.7 μg / cm 2 Increased to 35 μg / cm 2 The Pt mass activity of Examples 8 to 12 (fixed amount of Pt on variable Ir mat loading) is between 0.28 A / mg Pt Up to 0.84A / mg Pt and as the Ir content further increases to 52 μg / cm 2, the Pt mass activity did not change significantly. The maximum Pt mass activity obtained from Examples 10 to 12 was about 5 times that of pure Pt.
[0179] Since iridium is a noble metal, it is also conventional to compare mass activities based on the total PGM content. Figure 4 Table 3 above summarizes the PGM mass activity of Comparative Examples A to E, Comparative Example J, Examples 1 to 7, and Examples 8 to 12 as a function of total PGM (Pt+Ir) area loading. Comparative Examples A to E do not include an Ir pad. Examples 1 to 12 include an Ir pad. Comparative Example J does not include Pt. As the Pt area loading increases from 1.1 μg / cm 2 Increased to 31 μg / cm 2 The mass activity of PGM in Examples 1 to 7 is 0.06A / mg PGM Up to 0.27A / mg PGM Then as the Pt area loading further increases to 75 μg / cm 2 , PGM mass activity decreased to 0.15A / mg PGM The PGM mass activities of Examples 2 and 7 are comparable to pure Pt, and enhanced mass activities are obtained through an intermediate Pt area loading range, indicating an optimal Pt:Ir ratio or an optimal Pt thickness relative to Ir thickness combination. Comparative Example J (i.e., pure Ir) produces a PGM mass activity of -0.05 A / mg, indicating that at 0.90 V, parasitic losses such as electron shorting are greater than the oxygen reduction current density.
[0180] Figure 5 The specific areas of Comparative Examples A to E, Comparative Example J, and Examples 1 to 12 as a function of total PGM (Pt+Ir) area loading are compared to Table 3 above.
[0181] As the Pt loading increases from 98 μg / cm 2 Reduced to 24 μg / cm 2 , the specific area of pure Pt is from 8.0m 2 / g increased to 13.2m 2 / g, which is consistent with the expected trend as the thickness of the Pt film on the support decreases. However, as the Pt area loading is further reduced to 13 μg / cm 2 , the area is reduced to 10.4m 2 / g, which may be due to film instability leading to dewetting of the catalyst from the support. This suggests that for film stability, the Pt catalyst can exist between 13 μg / cm 2 and 24 μg / cm 2 Critical minimum area load between (thickness).
[0182] In contrast, the specific area of the Pt / Ir samples is generally significantly higher than that of the pure Pt catalyst. For Examples 1-7, as the Pt content increases from 75 μg / cm 2 Reduced to 1.1 μg / cm 2 , the specific area is from 9.9m 2 / g increases monotonically to 22.4m 2 / g. The specific area of pure Ir (Comparative Example J) is 22.6m 2 / g, similar to the specific area in Example 1.
[0183] For Examples 8-12, when the Ir content is increased from 1.1 μg / cm 2 Changed to 52 μg / cm 2 When the specific area is between 17.0 and 15.4 m 2 / g, which is higher than pure Pt in a similar total PGM loading range. Surprisingly, only 1.7 μg / cm 2 The Ir (about 0.05 nm thick on the support, much less than a monolayer (about 0.2 nm)) produced a larger area increase than pure Pt. Without being bound by theory, this result suggests that the Ir acts as a stabilizing anchor between the PR149 support and the overlying Pt, thereby reducing the extent of dewetting.
[0184] Essentially, the specific surface area of a catalyst on a support depends on the thickness of the catalyst on the support, the surface area of the support on which the catalyst is wetted, and the inherent roughness of the catalyst. Therefore, the specific surface area should also be evaluated as a function of the thickness of the catalyst on the support. The thickness on the support is a fundamental characteristic of the catalyst that is partly necessary for the specific surface area to be determined.
[0185] Figure 6 The specific surface areas of Comparative Examples A to E, Examples 1 to 7, and Examples 8 to 12 are summarized as a function of thickness on the support, as calculated in Table 1 above. The trend of specific area with thickness is similar to Figure 5 Shown is the trend of specific area with PGM area loading. Figure 5 and Figure 6 The modest difference between the two is because the thickness on the support is related to the PGM area loading via the density component, with the PGM area loading of Pt and Ir (21.45 g / cm 3 and 22.56g / cm 3 ) is slightly different, and while not wanting to be limited by theory, it is believed that this is due to the absolute area loading of the constituent elements.
[0186] Table 6 below summarizes the percent increase in specific area for Examples 1 to 12 relative to Comparative Examples A to E at the same catalyst thickness on a whisker support.
[0187] Table 6
[0188]
[0189] The comparative example data were not available at the exact thickness on the support as in the examples. Using the data of Comparative Examples A to E, the specific surface areas at the specific thicknesses of Examples 1 to 12 were estimated using linear interpolation and extrapolation. For example, the Pt+Ir thickness on the support of Example 1 was 0.86 nm, and the measured specific surface area was 22.4 m 2 The Pt thickness of Comparative Examples D and A (not including Ir) is 0.80 and 0.90, respectively, and the related specific area is 13.2 m 2 / g and 11.4m 2 Using linear interpolation, the estimated specific area of the comparative example at a thickness of 0.86 nm was estimated to be 12.2 m 2 / g. The specific area of Example 1 is 84.5% higher than the estimated value of Pt alone at the same thickness on the support ((22.4-12.2) / 12.2*100%). A similar analysis was performed on the data of Comparative Examples A to E and Examples 1 to 12. Based on thickness, the specific areas of Examples 1 to 12 range from 24.3% to 84.5% higher than those of Comparative Examples A to E.
[0190] Figure 7 Table 4 above summarizes the results of Comparative Examples A to E and Examples 1 to 12 at 0.02 A / cm 2 The cell voltages measured at current densities of 1.5 Å and 1.5 Å. At similar PGM area loadings, Examples 2 to 11 produced higher cell voltages than the Comparative Examples. Examples 1 to 12 also produced higher cell voltages than Comparative Example J (pure Ir), which produced a cell voltage of only about 0.55 V ( Figure 7 not shown).
[0191] Table 5 and Figure 8 The changes in mass activity after electrochemical accelerated durability testing of Examples 3 to 6 and 10 and Comparative Examples A and B are summarized. Under this test, the catalyst was cycled 30,000 times between 0.60V-1.00V (an approximate representation of a fuel cell drive cycle). The changes in mass activity for Examples 3 to 6 and Example 10 ranged from -4% to -19%, which is less than the -43% to -59% changes observed with Comparative Examples A and B.
[0192] Table 5 above also summarizes the changes in specific area and specific activity after AST. The changes in specific area of Examples 3 to 6 and 10 are in the range of +3% to -12%, which is less than the changes of -30% to -39% of Comparative Examples A and B. The changes in specific activity of Examples 3 to 6 and 10 are in the range of +6% to -8%, which is less than the changes of -18% to -33% of Comparative Examples A and B.
[0193] Table 5 and Fig. 9 The 0.02 A / cm after the durability test of Examples 3 to 6 and 10 and Comparative Examples A and B is summarized. 2 The cell voltage change at the current density was smaller in Examples 3 to 6 and Example 10 (-6 mV to -13 mV) than in Comparative Examples A and B (-53 mV to -63 mV).
[0194] Table 5 above also summarizes 0.32A / cm 2 The cell voltage change at 0.50V and the current density change percentage at 0.50V cell voltage. Compared with the 189mV to 160mV loss of Comparative Examples A and B, Examples 3 to 6 and Example 10 have a current density loss of 0.32A / cm 2 The losses at 0.50V cell voltage ranged from 4mV to 36mV. At 0.50V cell voltage, the current density changes for Examples 3 to 6 and 10 ranged from -4% to +9% compared to a 67% loss for both Comparative Examples A and B.
[0195] As shown in Table 5 (above) and Figure 8 and Fig. 9 As shown, the Ir underlayer produces durability improvement over the comparative example. Figures 10 to 17 It is shown that the Pt on Ir structure formed by depositing a layer containing Pt onto a layer containing Ir is retained after electrochemical cycling, such as in a fuel cell. Without being bound by theory, it is believed that the Ir mat layer is more strongly attached to the whisker support than the Pt is attached to the whisker support, and the attachment of Pt to Ir is stronger than the attachment of Pt to the whisker support. It is believed that these differences in the attachment energies of Pt-whiskers, Ir-whiskers, and Pt-Ir can contribute to the enhanced structural stability.
[0196] The catalyst of Example 10 was subjected to transmission electron microscopy (TEM) analysis to determine the distribution of the catalyst structure on the whisker support. Fig.10 ), after annealing ( Fig.11 ), after fuel cell testing ( Fig.12 ) and after accelerated durability testing ( Fig.13 ), analyzed in four different states. Figures 10 to 13 Each shows the structure of a portion of a whisker coated with one or both catalysts. The lighter areas have a higher catalyst density than the darker areas. Fig.10), the catalyst morphology consists of a discontinuous 2nm-4nm thick coating of partially molten metal catalyst grains on a whisker support. After annealing ( Fig.11 ), many of the grains have melted, forming a mostly but not completely continuous 2nm-4nm thick catalyst metal coating on the whisker support. Fig.12 ) and durability tests ( Fig.13 ) after which further grain agglomeration occurs.
[0197] The catalyst of Example 10 was subjected to transmission electron microscopy (TEM) and energy dispersive X-ray spectroscopy (EDS) analysis to determine the distribution of Pt and Ir on the whisker support. Fig.14 ), after annealing ( Fig.15 ), after fuel cell testing ( Fig.16 ) and after accelerated durability testing ( Fig.17 ), analyzed in four different states. The left image of each figure is a dark field TEM image, and the right image of each figure is an EDS-determined composition map over the same spatial area as the left image. The image shows a portion of the catalyst on a single whisker support. EDS analysis shows that in all states, the surface is essentially composed of pure Pt or a Pt-rich surface layer, about 1nm-2nm thick, located on top of a 1nm-2nm thick Ir layer or Ir-rich layer below. After durability testing, some Fe-rich areas were observed at the surface on top of the Pt layer.
[0198] TEM and EDS analysis were also performed on Example 3, which had a thicker layer than Example 10 containing 26 μg / cm 2 Ir underlayer, the latter has 12 μg / cm 2 Ir. Fig.18 TEM images after durability testing are shown. Fig.19 Dark field TEM images and matching EDS composition maps are shown. After durability testing, Fig.18 The presence of elongated grains extending from the surface is shown. The diameter of the grains is in the range of 3nm-8nm. Some of the grains are spherical while others are elongated. Fig.19 These surface grains are shown to be Ir or Ir-rich.
[0199] Fig. 20 TEM images of Example 2 catalyst on whisker support after fuel cell testing are summarized. Example 2 catalyst has a continuous catalyst film of about 5nm-10nm thickness and grains extending from the surface of the catalyst film. The size of the surface grains ranges from about 3nm to 8nm.
[0200] based on Figures 10 to 20TEM and EDS analysis shown, Ir-rich surface grains are formed after electrochemical potential cycling. The surface grains on the thin film catalyst provide a higher catalyst surface area than the thin film catalyst alone. Without being bound by theory, Ir-rich surface grains can form during potential cycling due to the difference in resistance to electrochemical dissolution between Pt and Ir.
[0201] As shown in Table 3 above, pure Ir (Comparative Example J) has no measurable oxygen reduction activity at 0.900 V. Surprisingly, the catalyst of the Examples (which may have an Ir-rich surface grain region covering the Pt catalyst) has an enhanced Pt mass activity compared to the pure Pt catalyst. Without being bound by theory, it is believed that the Ir-rich surface grains may also contain a thin sub-nm thick Pt layer. Such a thin Pt layer cannot be reliably detected by EDS. Without being bound by theory, it is believed that the sub-nm Pt layer on the Ir-rich surface grains will have a higher Pt mass activity than a similar Pt layer on the planar Ir layer due to the higher specific surface area.
[0202] Table 3 and Fig.21 The Pt mass activities of Comparative Examples F to I and Examples 3 and 8 to 12, which contain Pt and Ir in different structures, are summarized. Comparative Examples F to I contain Ir with varying area loading on top of a Pt layer with a fixed area loading, and Examples 3 and 8 to 12 contain Ir with varying area loading below a Pt layer with a fixed area loading. The Pt mass activities of Comparative Examples F to I are in the range of 0.14 A / mg to 0.10 A / mg. The Pt mass activities of Examples 3 and Examples 8 to 12 are higher than those of Comparative Examples F to I, and are in the range of 0.28 A / mg to 0.84 A / mg. The higher mass activities of the catalysts of Examples 3 and Examples 8 to 12 than those of Comparative Examples F to I are partly due to the higher specific surface area, as shown in Table 3 above.
[0203] Table 3 above summarizes the mass activity, specific area and specific activity of Example 10 and Comparative Examples K and L. Example 10 has a mass activity, specific area and specific activity of 12 μg Ir / cm 2 The Ir pad contains 9 μg Pt / cm 2 Comparative Example K has 14 μg Pt / cm 2 The Pt pad contains 14 μg Ir / cm 2 Comparative Example L contains the same amount of Pt and Ir as Comparative Example K, but Pt and Ir are deposited as multiple alternating thin layers to enable the formation of a PtIr alloy. The Pt mass activity and specific surface area of Example 10, Comparative Example K, and Comparative Example L are 0.63 A / mg, 0.52 A / mg, and 0.59 A / mg, respectively, and 18.7 m 2 / g, 16.8m 2 / g and 16.9m 2The higher Pt mass activity of Example 10 than that of Comparative Examples K and L is attributed to the higher specific surface area.
[0204] Table 3 above summarizes the mass activity, specific area, and specific activity of Example 10 and Comparative Example M. Example 10 includes an Ir pad and a surface Pt catalyst, and Comparative Example M includes an Au pad and a surface Pt catalyst. Both Ir and Au are corrosion-resistant precious metals. The mass activity, specific area, and specific activity of Pt in Example 10 are 0.63 A / mg, 18.7 m / mg, and 1.3 m / mg, respectively. 2 / g and 1.47mA / cm 2 , which is higher than 0.004A / mg and 0.2m / mg obtained by Comparative Example M. 2 / g and 0.33mA / cm 2 Without being bound by theory, it is believed that Pt, Ir, and Au may have surface segregation energies, which are a measure of thermodynamically stable configurations in a multi-metal system. These energies depend on the electrochemical environment, including electrode potentials, electrolytes, and bystander species, as well as reactants such as oxygen. For the Pt and Au system in Comparative Example M, the thermodynamic stability of the catalyst configuration with Au on the Pt surface may be energetically superior to the configuration of Pt on the Au surface. Au does not have measurable ORR activity at 0.900 V in an acidic electrolyte, or an electrochemically measurable specific surface area by hydrogen adsorption and desorption.
[0205] Table 3 above summarizes the mass activities of Examples 3 and 13 (Pt with Ir underlayer) and Comparative Examples A to E (pure Pt). Example 13 has the same composition and manufacturing method as Example 3, except that Example 13 is not annealed. Comparative Examples A to E are not annealed. The Pt mass activities of Example 3 and Example 13 are 0.84A / mg and 0.60A / mg, respectively, and the Pt mass activities of Comparative Examples A to E are in the range of 0.14A / mg-0.16A / mg. Both the annealed examples and the unannealed examples produced higher mass activities than Comparative Examples A to E, which is attributed to the higher specific surface area. The mass activity of the annealed Example 3 catalyst is higher than that of the unannealed Example 13, which is attributed to the higher specific activity (1.11mA / cm 2 Compare 0.81mA / cm 2 ).like Fig.11 and Fig.12 As shown, annealing can promote improved wetting of Pt on Ir. Without being bound by theory, it is believed that annealing can promote improvement in specific activity due to a reduction in the Pt-Pt bond distance of surface Pt atoms, and the oxygen reduction specific activity depends on the Pt-Pt bond distance.
[0206] Table 3 above summarizes the Pt mass activities of Example 14 and Comparative Examples N and O. Example 14 includes a surface layer comprising a PtNi alloy on an Ir underlayer. The areal Pt loading of Example 14 is 9 / cm 2 . Comparative Example N comprises a PtNi alloy similar to Example 14, but without an Ir underlayer. Comparative Example O comprises a similar PtNi alloy with a surface Ir layer. The Pt mass activities of Example 14, Comparative Example N, and Comparative Example O are 0.89 A / mg, 0.24 A / mg, and 0.44 A / mg, respectively. The higher Pt mass activity of Example 14 is due in part to the higher surface area. The specific surface area of Example 14 is 23 m 2 / g, which is 26.7% higher than that of Comparative Example N, and 27.7% higher than that of Comparative Example O. The Ir underlayer effectively improves the activity of the surface Pt alloy by increasing the specific surface area.
[0207] Table 5 above compares the mass activity, specific area, specific activity, 0.02 and 0.32 A / cm of Example 15 and Comparative Examples N and O after accelerated durability testing. 2 The cell voltage at 0.50 V and the cell current density at 0.50 V are shown. Example 14 lost 24% after the durability test, while Comparative Examples N and O lost 58% and 36%. The presence of Ir in the mat layer with the PtNi alloy surface catalyst produced less mass activity loss than the PtNi alloy catalyst alone or the PtNi catalyst with the surface Ir layer.
[0208] Foreseeable variations and modifications of the present disclosure will be apparent to those skilled in the art without departing from the scope and spirit of the present invention.The present invention should not be limited to the embodiments shown in this application for illustrative purposes.
Claims
1. A catalyst comprising an Ir layer, the Ir layer having an outer layer, the outer layer having a Pt-containing layer directly thereon, wherein the average thickness of the Ir layer is in the range of 0.04 nm to 30 nm, wherein the average thickness of the Pt-containing layer is in the range of 0.04 nm to 50 nm, wherein the average thickness of the catalyst is the sum of the average thickness of the Ir layer and the average thickness of the Pt-containing layer, and wherein the Pt and the Ir are present in an atomic ratio in the range of 0.01:1 to 10:
1.
2. The catalyst of claim 1, wherein the catalyst further comprises nanoscale metal grains extending from a surface of the catalyst.
3. The catalyst of claim 2, wherein the surface metal grains comprise at least 10 atomic % Ir. The catalyst according to claim 2 , wherein the length of the surface metal grains is in the range of 0.25 nm to 10 nm. The catalyst according to claim 2 , wherein the diameter of the surface metal grains is in the range of 0.25 nm to 5 nm. The catalyst according to claim 1 , wherein the layer comprising Pt further comprises Ni.
7. The catalyst according to claim 6, wherein the atomic ratio of Pt to Ni is in the range of 0.5:1 to 5:
1.
8. The catalyst of claim 1, wherein the catalyst has a surface area at least 20% greater than the surface area that would exist in the absence of the Ir layer.
9. An article comprising nanostructured elements comprising microstructured whiskers having an outer surface having the catalyst of claim 1 thereon.
10. The article of claim 9, wherein the microstructured whiskers are attached to a backing.
11. The article of claim 10, which does not contain conductive carbon-based materials.
12. A method for preparing a catalyst according to claim 1, the method comprising depositing any of the layers via a deposition technique independently selected from sputtering, atomic layer deposition, metal organic chemical vapor deposition, molecular beam epitaxy, ion soft landing, thermal physical vapor deposition, electrospray ionization vacuum deposition and pulsed laser deposition.
13. The method of claim 12, further comprising annealing at least one of the layers.
14. The method of claim 12, further comprising cycling the catalyst between 0.60 V to 1.00 V relative to the potential of a standard hydrogen electrode.
Citation Information
Patent Citations
Suboxide fuel cell catalyst for enhanced reformate tolerance
US20020004453A1
Method and apparatus for forming high surface area material films and membranes
US20040048466A1
Catalyst material
US5759944A
Microtextured catalyst transfer substrate
US6136412A