Secondary battery and electronic device

By using nickel-cobalt-manganese ternary materials with magnesium, aluminum elements, inorganic additives and dinitrile compounds in ternary lithium-ion batteries, the problems of battery cycle life and gas production are solved, and higher capacity retention and longer life are achieved. The low residual gas volume improves the overall performance of the battery.

CN118738518APending Publication Date: 2024-10-01NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410706979.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The cycle life and capacity retention rate of ternary lithium-ion batteries do not perform well in high-frequency use scenarios, and they produce large amounts of gas, which affects equipment performance and reliability.

Method used

The ternary material of nickel, cobalt and manganese is used with magnesium and aluminum elements, combined with inorganic additives and dinitrile compounds in the electrolyte, to form a synergistic effect to improve the toughness of the positive electrode interface film, improve the capacity retention rate of the secondary battery and reduce gas production.

Benefits of technology

The capacity retention rate of the secondary battery is significantly improved, the amount of residual gas is reduced, and the cycle performance and stability of the battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004872982740000131
    Figure BDA0004872982740000131
  • Figure BDA0004872982740000141
    Figure BDA0004872982740000141
Patent Text Reader

Abstract

The invention provides a secondary battery and an electronic device. The secondary battery includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode comprises a positive electrode current collector and a positive electrode material layer, the positive electrode material layer comprises a first material layer and a second material layer, and the second material layer is arranged between the positive electrode current collector and the first material layer; the first material layer comprises a nickel-cobalt-manganese ternary material, the nickel-cobalt-manganese ternary material comprises a first element, and the first element comprises a magnesium element and an aluminum element; the second material layer comprises an inorganic additive, the inorganic additive comprises a second element, and the second element comprises at least one of a titanium element, a chromium element, a yttrium element, a zirconium element, a lanthanum element, a niobium element, an indium element, a tin element, a zinc element or an antimony element; the electrolyte includes a dinitrile compound. The secondary battery provided by the invention has good capacity retention ratio and relatively low residual gas amount.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of secondary batteries, and specifically relates to a secondary battery and an electronic device. Background Art

[0002] Secondary batteries, also known as rechargeable batteries, are batteries that can be charged and discharged repeatedly. Among them, ternary lithium-ion batteries are widely used in portable electronic devices, electric vehicles and other fields due to their high charging efficiency. With the development of science and technology and the improvement of living standards, the frequency of use of ternary lithium-ion batteries has increased significantly, and their cycle life and other performance needs to be improved urgently. Summary of the invention

[0003] In view of this, the present application provides a secondary battery and an electronic device, which improves the cycle performance of the secondary battery and reduces gas production by combining the nickel-cobalt-manganese ternary material in the positive electrode, the first element and the second element with the dinitrile compound in the electrolyte.

[0004] In a first aspect, the present application provides a secondary battery, comprising a positive electrode, a negative electrode and an electrolyte. The positive electrode comprises a positive electrode current collector and a positive electrode material layer, the positive electrode material layer comprises a first material layer and a second material layer, the second material layer is arranged between the positive electrode current collector and the first material layer; the first material layer comprises a nickel-cobalt-manganese ternary material, the nickel-cobalt-manganese ternary material comprises a first element, the first element comprises magnesium and aluminum; the second material layer comprises an inorganic additive, the inorganic additive comprises a second element, the second element comprises at least one of titanium, chromium, yttrium, zirconium, lanthanum, niobium, indium, tin, zinc or antimony; the electrolyte comprises a dinitrile compound.

[0005] The positive electrode material layer in the secondary battery provided in the present application and the dinitrile compound in the electrolyte can play a synergistic role, improve the toughness of the positive electrode interface film, improve the capacity retention rate of the secondary battery and reduce gas production.

[0006] In some embodiments, the first material layer further comprises lithium manganese iron phosphate. The use of lithium manganese iron phosphate in combination with the above secondary battery system can further improve the capacity retention rate of the secondary battery and reduce the amount of residual gas.

[0007] In some embodiments, the second element includes indium, tin, and antimony, which can further improve the capacity retention rate and the amount of residual gas of the secondary battery.

[0008] In some embodiments, when the second element includes indium, tin and antimony, the mass ratio of indium, tin and antimony is 1:(0.6-1.4):(0.6-1.4). Indium, tin and antimony at this ratio can further improve the capacity retention rate and residual gas amount of the secondary battery.

[0009] In some embodiments, the nickel-cobalt-manganese ternary material includes a third element, the third element includes strontium and / or tungsten, and adding strontium and / or tungsten to the nickel-cobalt-manganese ternary material can further improve the capacity retention rate and residual gas amount of the secondary battery.

[0010] In some embodiments, the dinitrile compound includes succinonitrile, glutaronitrile, adiponitrile, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 1,8-dicyanooctane, 1,9-dicyanononane, 1,10-dicyanodecane, 1,12-dicyanododecane, tetramethylsuccinonitrile, 2-methylglutaronitrile, 2,4-dimethylglutaronitrile, 2,2,4,4-tetramethylglutaronitrile, 1,4-dicyanopentane, 2,6-dicyanoheptane, 2,7-dicyanooctane, 2,8-dicyanononane, 1,6-dicyanodecane, 1,2-dicyanobenzene, 1,3-dicyanobenzene, 1,4-dicyanobenzene, ethylene glycol bis(2-cyanoethyl) ether, diethylene glycol bis(2-cyanoethyl) ether, triethylene glycol bis(2-cyanoethyl) ether, ) ether, tetraethylene glycol di(2-cyanoethyl) ether, 3,6,9,12,15,18-hexaoxaeicosanoic acid dinitrile, 1,3-bis(2-cyanoethoxy)propane, 1,4-bis(2-cyanoethoxy)butane, 1,5-bis(2-cyanoethoxy)pentane, ethylene glycol di(4-cyanobutyl) ether, 1,4-dicyano-2-butene, 1,4-dicyano-2-methyl-2-butene, 1,4-dicyano-2-ethyl-2-butene, 1,4-dicyano-2,3-dimethyl-2-butene, 1,4-dicyano-2,3-diethyl-2-butene, 1,6-dicyano-3-hexene, 1,6-dicyano-2-methyl-3-hexene, 1,6-dicyano-2-methyl-5-methyl-3-hexene. The above-mentioned dinitrile compound can better cooperate with the positive electrode material layer of the present application to improve the capacity retention rate and residual gas amount of the secondary battery.

[0011] In some embodiments, the secondary battery satisfies the condition: based on the total mass of the positive electrode material layer, the mass content of the first element is n1, 1200ppm≤n1≤10000ppm. Exemplarily, based on the total mass of the positive electrode material layer, the mass content n1 of the first element is selected from 1200ppm, 1630ppm, 2110ppm, 2320ppm, 2820ppm, 3260ppm, 3600ppm, 4380ppm, 4720ppm, 5000ppm, 5390ppm, 6110ppm, 6390ppm, 7170ppm, 7370ppm, 7900ppm, 8380ppm, 8880ppm, 9520ppm, 9860ppm, 10000ppm or a value in the range composed of any two of these values. When the mass content of the first element in the positive electrode material satisfies the above range, the capacity retention rate and residual gas amount of the secondary battery can be further improved.

[0012] In order to further improve the capacity retention rate and residual gas amount of the secondary battery, the secondary battery in the present application satisfies: 2500ppm≤n1≤8000ppm. In particular, when 3000ppm≤n1≤6000ppm, after being combined with the second material layer and the electrolyte, the capacity retention rate and residual gas amount of the secondary battery can be more significantly improved.

[0013] In some embodiments, in the first element, the mass content ratio of magnesium and aluminum is 1: (0.8 to 1.2). For example, when the mass content of magnesium in the first element is 1 part, the mass content of aluminum is 0.8, 0.9, 1, 1.1, 1.2 or a value within the range of any two of these values. The magnesium and aluminum elements under this ratio can further improve the capacity retention rate and residual gas amount of the secondary battery. In particular, when the mass content ratio of magnesium and aluminum in the first element is 1: 1, the capacity retention rate and residual gas amount of the secondary battery are more significantly improved.

[0014] In some embodiments, based on the total mass of the positive electrode material layer, the mass content of the second element is n2, 1ppm≤n2≤5000ppm. Exemplarily, based on the total mass of the positive electrode material layer, the mass content of the second element n2 is selected from 1ppm, 50ppm, 530ppm, 540ppm, 1030ppm, 1120ppm, 1470ppm, 1590ppm, 1900ppm, 2290ppm, 2400ppm, 2710ppm, 2970ppm, 3200ppm, 3470ppm, 3730ppm, 4090ppm, 4240ppm, 4640ppm, 4980ppm, 5000ppm or a value in the range composed of any two of these values. In some preferred embodiments, 150ppm≤n2≤3500ppm. In some more preferred embodiments, 500ppm≤n2≤2000ppm. The second element satisfying the above mass content can cooperate closely with the electrolyte, exert a good reinforcing effect, improve the capacity retention rate of the secondary battery and reduce the amount of residual gas.

[0015] In some embodiments, based on the total mass of the positive electrode material layer, the mass content of the third element is n3, 1ppm≤n3≤5000ppm. Exemplarily, based on the total mass of the positive electrode material layer, the mass content n3 of the third element is selected from 1ppm, 30ppm, 330ppm, 570ppm, 1010ppm, 1200ppm, 1510ppm, 1610ppm, 2030ppm, 2370ppm, 2440ppm, 2680ppm, 3080ppm, 3380ppm, 3440ppm, 3880ppm, 4140ppm, 4260ppm, 4730ppm, 4880ppm, 5000ppm or a value in the range composed of any two of these values. In some more preferred embodiments, 1250ppm≤n3≤2500ppm. By controlling the mass content of strontium and / or tungsten, the capacity retention rate and residual gas amount of the secondary battery can be further improved.

[0016] In some embodiments, the negative electrode includes a negative electrode material layer, and the negative electrode material layer includes a silicon-based material. A secondary battery satisfying the above conditions can further improve the capacity retention rate and residual gas amount of the secondary battery.

[0017] In some embodiments, the electrolyte further includes vinylene carbonate (VC) and diethyl carbonate (DEC), and the sum of the mass percentages of vinylene carbonate and diethyl carbonate is 19% to 40% based on the mass of the electrolyte. Exemplarily, based on the mass of the electrolyte, the sum of the mass percentages of vinylene carbonate and diethyl carbonate is 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40% or a value in the range of any two of these values, preferably 19.3% to 29.7%. By further adding vinylene carbonate and diethyl carbonate to the electrolyte for coordination, controlling the mass percentages of the two in the electrolyte to meet the above range, it is beneficial to further improve the capacity retention rate and residual gas amount of the secondary battery.

[0018] In some embodiments, based on the mass of the electrolyte, the mass percentage of vinylene carbonate is 0.01% to 1%. For example, based on the mass of the electrolyte, the mass percentage of vinylene carbonate is 0.01%, 0.02%, 0.11%, 0.16%, 0.20%, 0.26%, 0.28%, 0.33%, 0.41%, 0.43%, 0.48%, 0.58%, 0.61%, 0.67%, 0.70%, 0.79%, 0.84%, 0.86%, 0.95%, 0.97%, 1% or a value in the range of any two of these values, preferably 0.3% to 0.7%. Regulating the mass percentage of vinylene carbonate in the electrolyte to the above range can further improve the capacity retention rate and residual gas amount of the secondary battery.

[0019] In some embodiments, based on the mass of the electrolyte, the mass percentage of diethyl carbonate is 19% to 39%. For example, based on the mass of the electrolyte, the mass percentage of diethyl carbonate is 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or a value in the range of any two of these values, preferably 21% to 29%. Regulating the mass percentage of diethyl carbonate in the electrolyte to the above range can further improve the capacity retention rate and residual gas amount of the secondary battery.

[0020] In some embodiments, the electrolyte further includes difluoroethyl acetate (DFA), and the mass percentage of difluoroethyl acetate is 0.01% to 3% based on the mass of the electrolyte. For example, based on the mass of the electrolyte, the mass percentage of difluoroethyl acetate is 0.01%, 0.02%, 0.26%, 0.35%, 0.62%, 0.75%, 0.82%, 0.97%, 1.12%, 1.32%, 1.47%, 1.65%, 1.82%, 1.99%, 2.07%, 2.28%, 2.40%, 2.62%, 2.82%, 2.94%, 3% or any two of these values ​​in the range of values, preferably 0.1% to 1.2%. By adding difluoroethyl acetate to the electrolyte and satisfying the above content range, after cooperating with the secondary battery system of the present application, the capacity retention rate and residual gas amount of the secondary battery can be further improved.

[0021] In some embodiments, based on the mass of the electrolyte, the mass percentage of the dinitrile compound is 0.1% to 5%. Exemplarily, based on the mass of the electrolyte, the mass percentage of the dinitrile compound is 0.1%, 0.2%, 0.5%, 0.7%, 0.9%, 1.2%, 1.5%, 1.8%, 2.1%, 2.2%, 2.6%, 2.8%, 3.0%, 3.5%, 3.5%, 3.8%, 4.2%, 4.4%, 4.6%, 4.8%, 5% or a value in the range of any two of these values, preferably 0.3% to 1.2%. The secondary battery that meets this condition has a better capacity retention rate and a lower amount of residual gas.

[0022] In a second aspect, the present application also provides an electronic device, which includes any one of the above-mentioned secondary batteries.

[0023] The secondary battery and electronic device provided in this application have the following beneficial effects:

[0024] The present application adds magnesium and aluminum elements to the nickel-cobalt-manganese ternary material to strengthen its structure, which can play a synergistic role when combined with inorganic additives and dinitrile compounds in the electrolyte. The dinitrile compounds can form a uniform protective film at the positive electrode interface in the present application, and cooperate with the first material layer and the second material layer in the positive electrode to stabilize the positive electrode and the electrolyte, so that the secondary battery has a better capacity retention rate and a lower amount of residual gas. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.

[0026] In order to solve the problems in the prior art, the present application provides a secondary battery, including a positive electrode, a negative electrode and an electrolyte. The positive electrode includes a positive electrode current collector and a positive electrode material layer, the positive electrode material layer includes a first material layer and a second material layer, the second material layer is arranged between the positive electrode current collector and the first material layer; the first material layer includes a nickel-cobalt-manganese ternary material, the nickel-cobalt-manganese ternary material includes a first element, the first element includes magnesium and aluminum; the second material layer includes an inorganic additive, the inorganic additive includes a second element, the second element includes at least one of titanium (Ti), chromium (Cr), yttrium (Y), zirconium (Zr), lanthanum (La), niobium (Nb), indium (In), tin (Sn), zinc (Zn) or antimony (Sb); the electrolyte includes a dinitrile compound.

[0027] In some embodiments, the nickel-cobalt-manganese ternary material is prepared by a method comprising the following steps: Co3O4, Li2CO3, an aluminum source, a magnesium source, a nickel source and a manganese source are mixed according to a ratio, and then calcined in a furnace at 700 to 1200°C for 7 to 20 hours to obtain a nickel-cobalt-manganese ternary material doped with a first element.

[0028] In some embodiments, Co3O4, Li2CO3, aluminum source, magnesium source, nickel source and manganese source can be mixed with raw materials providing strontium element and / or tungsten element according to a ratio to prepare a nickel-cobalt-manganese ternary material containing the first element and the third element.

[0029] In some embodiments, the second material layer includes an inorganic additive, and the inorganic additive includes a second element. In the present application, the inorganic additive is selected from inorganic metal oxides and / or inorganic metal hydroxides, such as titanium dioxide, chromium oxide, yttrium oxide, zirconium dioxide, lanthanum oxide, niobium monoxide, niobium dioxide, niobium trioxide, niobium pentoxide, indium trioxide, tin dioxide, zinc oxide, and antimony trioxide.

[0030] In some embodiments, the positive electrode material layer may be located on one or both sides of the positive electrode current collector. In some embodiments, the positive electrode current collector may be aluminum foil, and of course, other positive electrode current collectors commonly used in the art may also be used. In some embodiments, the thickness of the positive electrode current collector may be 1 μm to 200 μm. In some embodiments, the positive electrode material layer may be coated only on a partial area of ​​the positive electrode current collector. In some embodiments, the thickness of the positive electrode material layer may be 10 μm to 90 μm. It should be understood that these are exemplary only, and other suitable thicknesses may be used.

[0031] In some embodiments, as described above, the positive electrode material may include lithium iron manganese phosphate, and the lithium iron manganese phosphate may be doped and / or coated.

[0032] In some embodiments, the positive electrode material layer also includes a positive electrode binder and a positive electrode conductor. In some embodiments, the positive electrode binder may include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer, styrene-acrylate copolymer, styrene-butadiene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinyl acetate, polyvinylpyrrolidone, polyvinyl ether, polytetrafluoroethylene or polyhexafluoropropylene at least one. In some embodiments, the positive electrode conductor may include at least one of conductive carbon black, acetylene black, Ketjen black, graphene, carbon nanotubes or carbon fibers. In some embodiments, the mass ratio of the positive electrode material, positive electrode conductor and positive electrode binder in the positive electrode material layer may be (80-98): (0.5-10): (0.5-10). It should be understood that the above is only an example, and the positive electrode material layer may include any other suitable material, thickness and mass ratio.

[0033] In the present application, a dinitrile compound refers to an organic compound containing a hydrocarbon group and two cyano groups (-CN) connected by carbon atoms.

[0034] In some embodiments, the electrolyte further includes an ionizable lithium salt, and the ionizable lithium salt includes at least one of LiPF6, LiSbF6, LiAsF6, LiClO4, LiN(C2F5SO2)2, CF3SO3Li, LiC(CF3SO2)3 or LiC4BO8. In the present application, the concentration of the ionizable lithium salt in the electrolyte is not particularly limited, preferably 0.5 mol / L or more, more preferably 0.8 mol / L or more, and further preferably 1.0 mol / L or more. In addition, it is preferably 3 mol / L or less, more preferably 2 mol / L or less, further preferably 1.8 mol / L or less, and particularly preferably 1.6 mol / L or less. If the concentration of these ionizable lithium salts is too low, it may cause the conductivity of the electrolyte to be insufficient. On the other hand, if the concentration of these ionizable lithium salts is too high, it may cause the viscosity of the electrolyte to increase, thereby reducing the conductivity, which may cause the performance of the secondary battery to decrease.

[0035] In some embodiments, the electrolyte also includes at least one of lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), vinylene carbonate and diethyl carbonate (LiBOB), lithium tetrafluoroborate (LiBF4), lithium fluorosulfonate (LiSO3F), lithium bis(trifluoromethanesulfonyl imide) (LiTFSI), and lithium bis(fluorosulfonyl imide) (LiFSI).

[0036] In some embodiments, the electrolyte further includes at least one of a fluoroether compound and a fluorocarbonate compound, such as hydrofluoroether (HFE-458), fluoroethylene carbonate (FEC), and the like.

[0037] In some embodiments, the electrolyte may further include a non-aqueous solvent. The non-aqueous solvent may be selected from carbonate compounds, carboxylate compounds, ether compounds, phosphate compounds, other organic solvents, or combinations thereof.

[0038] Optionally, the carbonate compound may be a linear carbonate compound, a cyclic carbonate compound or a combination thereof. On the other hand, the carbonate compound may also be a fluorinated carbonate compound, a non-fluorinated carbonate compound or a combination thereof.

[0039] Specifically, examples of chain carbonate compounds are dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) or combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate or combinations thereof.

[0040] Specifically, examples of the carboxylate compound are methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone, methyl formate, or a combination thereof.

[0041] Specifically, examples of the ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.

[0042] Specifically, examples of the phosphate compound are trimethyl phosphate, triethyl phosphate, trioctyl phosphate, or a combination thereof.

[0043] Specifically, examples of other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, or a combination thereof.

[0044] In some embodiments, the negative electrode includes a negative electrode current collector and a negative electrode material layer disposed on the negative electrode current collector. The negative electrode material layer may be disposed on one side or both sides of the negative electrode current collector. In some embodiments, the negative electrode current collector may be at least one of a copper foil, a nickel foil, or a carbon-based current collector. In some embodiments, the thickness of the negative electrode current collector may be 1 μm to 200 μm. In some embodiments, the negative electrode material layer may be coated only on a partial area of ​​the negative electrode current collector. In some embodiments, the thickness of the negative electrode material layer may be 10 μm to 100 μm. It should be understood that these are exemplary only and other suitable thicknesses may be used.

[0045] In some embodiments, as described above, the negative electrode material layer includes a silicon-based material. In some embodiments, the silicon-based material includes at least one of silicon, a silicon-oxygen compound, a silicon-carbon compound, or a silicon alloy. In some embodiments, the negative electrode material includes a combination of a silicon-based material and a carbon material in a weight ratio of 1:(5-12).

[0046] In some embodiments, the negative electrode material layer may further include a negative electrode conductor and / or a negative electrode binder. The negative electrode conductor may include at least one of carbon black, acetylene black, Ketjen black, graphene, carbon nanotubes or carbon fibers. In some embodiments, the negative electrode binder may include at least one of carboxymethyl cellulose (CMC), polyacrylic acid, polyacrylate, polyacrylate, polyvinyl pyrrolidone, polyimide, polysiloxane or styrene-butadiene rubber. It should be understood that the materials disclosed above are exemplary only, and the negative electrode material layer may be made of any other suitable material.

[0047] In some embodiments, the negative electrode is prepared by a method comprising the following steps: mixing a negative electrode material, a negative electrode binder and deionized water to obtain a negative electrode slurry, coating the negative electrode slurry on the surface of the negative electrode current collector, and then drying, cold pressing, cutting and welding the tabs to obtain the negative electrode.

[0048] In some embodiments, the mass ratio of the negative electrode material, the negative electrode conductor and the negative electrode binder in the negative electrode material layer can be (80-99):(0.5-10):(0.5-10). It should be understood that this is only exemplary and not intended to limit the present application.

[0049] In some embodiments, the isolation film includes at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide or aramid. For example, the polyethylene includes at least one selected from high-density polyethylene, low-density polyethylene or ultra-high molecular weight polyethylene. In particular, polyethylene and polypropylene have a good effect on preventing short circuits and can improve the safety of the battery through the shutdown effect.

[0050] In some embodiments, the surface of the isolation membrane may further include a porous layer, the porous layer is disposed on at least one surface of the isolation membrane, the porous layer includes at least one of inorganic particles or binders, the inorganic particles are selected from aluminum oxide (Al2O3), silicon oxide (SiO2), magnesium oxide (MgO), titanium oxide (TiO2), hafnium dioxide (HfO2), tin dioxide (SnO2), cerium dioxide (CeO2), nickel oxide (NiO), zinc oxide (ZnO), calcium oxide (CaO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), silicon carbide (SiC), boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. In some embodiments, the pores of the isolation membrane have a diameter in the range of about 0.01 μm to 1 μm. The binder of the porous layer is selected from at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polytetrafluoroethylene or polyhexafluoropropylene. The porous layer on the surface of the isolation membrane can improve the heat resistance, oxidation resistance and electrolyte wetting performance of the isolation membrane, and enhance the adhesion between the isolation membrane and the electrode.

[0051] In some embodiments, the secondary battery is a lithium-ion battery, but the present application is not limited thereto.

[0052] In some embodiments of the present application, taking lithium-ion batteries as an example, the positive electrode, the separator, and the negative electrode are wound or stacked in sequence to form an electrode assembly, and then placed in a shell such as an aluminum-plastic film for packaging, and the electrolyte is injected, formed, and packaged to make a lithium-ion battery.

[0053] The embodiment of the present application also provides an electronic device including the above-mentioned secondary battery. The electronic device of the embodiment of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device can include, but is not limited to, a notebook computer, a pen input computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium ion capacitor, etc.

[0054] Some specific examples and comparative examples are listed below to better illustrate the present application, wherein a lithium-ion battery is used as an example. Unless otherwise specified, the raw materials used in the following examples are all from common commercial products, and the devices or equipment used are all purchased from conventional market sales channels.

[0055] Example 1

[0056] The secondary battery of this embodiment includes a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode includes a positive electrode material layer, the positive electrode material layer includes a first material layer and a second material layer, and the second material layer is arranged between the positive electrode current collector and the first material layer; the first material layer includes a nickel-cobalt-manganese ternary material, the nickel-cobalt-manganese ternary material includes a first element, and the first element includes a magnesium element and an aluminum element; the second material layer includes an inorganic additive, and the inorganic additive is tin dioxide; wherein, based on the total mass of the positive electrode material layer, the mass content of the magnesium element and the aluminum element in the first element is 1250ppm and 1250ppm respectively (the mass content ratio is 1:1), and the total mass content of the first element is n1=2500ppm; the mass content of the second element (tin element) is 150ppm. The electrolyte includes a dinitrile compound, and the dinitrile compound is adiponitrile, and the mass percentage of adiponitrile based on the mass of the electrolyte is 0.1%.

[0057] The secondary battery of this embodiment is prepared by a method comprising the following steps:

[0058] Preparation of positive electrode:

[0059] Tin dioxide was used as an inorganic additive. 65% by mass of tin dioxide, 15% by mass of acetylene black, and 15% by mass of PVDF were mixed, deionized water was added thereto and mixed evenly, and after forming a slurry, it was coated on both sides of a positive electrode current collector aluminum foil with a thickness of 10 μm, and dried to form a second material layer.

[0060] Nickel-cobalt-manganese ternary material (commercially available) was used as the positive electrode material, the positive electrode material, conductive carbon black, and binder polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 96.6:1.5:1.9, N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly under the action of a vacuum mixer to obtain a positive electrode slurry, wherein the solid content of the positive electrode slurry was 75wt%. The positive electrode slurry was evenly coated on the surface of the second material layer on one side of the positive electrode current collector aluminum foil, and dried at 120°C to obtain a positive electrode sheet coated with a first material layer with a thickness of 80μm on one side, and the above steps were repeated on the surface of the second material layer on the other side of the positive electrode current collector aluminum foil to obtain a positive electrode sheet coated with the first material layer on both sides, and then after cold pressing, cutting, and slitting, a positive electrode with a specification of 470mm×92mm was obtained.

[0061] Preparation of negative electrode: artificial graphite of negative electrode material, conductive carbon black of conductive agent, styrene-butadiene rubber (SBR) of binder and sodium carboxymethyl cellulose (CMC) of thickener are mixed in a weight ratio of 96.5:1.5:1:1, deionized water is added, and the mixture is stirred evenly under the action of a vacuum mixer to obtain negative electrode slurry, wherein the solid content of the negative electrode slurry is 75wt%. The negative electrode slurry is evenly coated on one side of the negative electrode current collector copper foil, and dried at 120°C to obtain a negative electrode sheet coated with a negative electrode material layer with a thickness of 90μm on one side, and the above steps are repeated on the other side of the negative electrode current collector copper foil to obtain a negative electrode sheet coated with a negative electrode material layer on both sides, and then after cold pressing, cutting and slitting, a negative electrode with a specification of 476mm×93.5mm is obtained.

[0062] Preparation of isolation membrane: A 10 μm thick polyethylene (PE) microporous membrane was selected as the isolation membrane.

[0063] Preparation of electrolyte: In an argon atmosphere glove box with a water content of less than 10ppm, ethylene carbonate (abbreviated as EC) and propylene carbonate (abbreviated as PC) are mixed in a mass ratio of 1:1 to obtain a base solvent, and then lithium salt LiPF6 and dinitrile compound are added to the base solvent, and the electrolyte is obtained after uniform mixing, wherein the mass content of LiPF6 is 12.5% ​​based on the mass of the electrolyte. In this embodiment, the dinitrile compound is adiponitrile, and the mass content of adiponitrile is 0.1% based on the total mass of the electrolyte.

[0064] Preparation of lithium-ion batteries: stack the positive electrode, separator, and negative electrode in order, so that the separator is between the positive and negative electrodes to play an isolating role, and wind them to obtain an electrode assembly. After welding the pole ears, place the electrode assembly in an outer packaging aluminum-plastic film, remove moisture at 80°C, inject the above-mentioned electrolyte, and obtain a lithium-ion battery after vacuum packaging, standing, formation, shaping, capacity testing and other processes.

[0065] The performance test method is as follows:

[0066] (1) Capacity retention after high and low temperature impact test

[0067] Take 4 lithium-ion batteries from each group, charge and discharge the 4 lithium-ion batteries respectively through the following steps, and calculate the discharge capacity retention rate of the batteries.

[0068] First, in an environment of 25°C, the first charge and discharge were performed. First, a constant current charge was performed at 0.5C, and constant voltage charge was performed after charging to 4.3V. Then, a constant current discharge was performed at a current of 1C, and the discharge was performed to 2.8V. The discharge capacity of the first cycle was recorded. Then, the lithium-ion battery was placed in an environment of -20°C for 100 charge and discharge cycles. After the low-temperature cycle was completed, the lithium-ion battery was transferred to an environment of 40°C within one hour for 200 charge and discharge cycles, and the discharge capacity of the 200th cycle under 40°C conditions was recorded.

[0069] Capacity retention rate=(discharge capacity at the 200th cycle / discharge capacity at the first cycle)×100%.

[0070] Evaluation was performed according to the following criteria: A higher capacity retention rate indicates that the performance of the secondary battery after the high and low temperature impact test is better.

[0071] A: Capacity retention rate is greater than 85%;

[0072] B: Capacity retention rate is greater than or equal to 82% and less than 85%;

[0073] C: Capacity retention rate is greater than or equal to 80% and less than 82%;

[0074] D: Capacity retention rate is greater than or equal to 75% and less than 80%;

[0075] E: The capacity retention rate is less than 75%.

[0076] (2) Test of residual gas volume:

[0077] After the electrolyte is injected into the lithium-ion secondary battery, it is left to stand at a temperature of 25°C for 5 hours. Next, the battery cell voltage is charged to 4.2V by a constant current method at a temperature of 25°C and 0.2C, and then an aging treatment is performed at a temperature of 60°C for 12 hours. Afterwards, the electrode part of the battery cell (the laminated part of the positive electrode, separator and negative electrode) is pressurized at 25kPa for 1 minute, and then the gas retention area on the electrode is measured using an ultrasonic inspection system (JAPANPROBE. "NAUT21"). The gas retention area ratio (%) is obtained by dividing the gas retention area by the electrode area. The smaller the gas retention area ratio, the less residual gas in the secondary battery.

[0078] A: The residual gas volume is less than or equal to 5%;

[0079] B: The residual gas volume is greater than or equal to 5% and less than 10%;

[0080] C: The residual gas volume is greater than or equal to 10% and less than 25%;

[0081] D: The amount of residual gas is greater than or equal to 25%.

[0082] The secondary batteries of the following embodiments and comparative examples are different from those of embodiment 1 only in that the positive electrode or the elements and mass contents in the positive electrode, and the components and mass contents in the electrolyte are adjusted according to Table 1. The specific adjustment contents and performance test results are shown in Table 1 below.

[0083] When adjusting the type of the second element, the corresponding metal oxide is used as the inorganic additive.

[0084] The secondary battery of Example 25 is different from that of Example 1 only in that the positive electrode material further includes lithium iron manganese phosphate, and the mass ratio of the nickel-cobalt-manganese ternary material to the lithium iron manganese phosphate is 3:7.

[0085] The secondary battery of Example 26 is different from that of Example 1 only in that the negative electrode includes a negative electrode material layer, and the negative electrode material layer includes artificial graphite and silicon dioxide. The preparation of the negative electrode of this embodiment includes the following steps: preparing a negative electrode material composed of artificial graphite and silicon oxide (SiO2) in a weight ratio of 9:1, and then mixing the negative electrode material, styrene-butadiene rubber and lithium carboxymethyl cellulose with deionized water in a mass ratio of 96.5:2.5:1, stirring evenly, and obtaining a negative electrode slurry. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 8 μm, and then dried at 110°C, and the above steps are repeated on the other surface of the negative electrode current collector, cold pressing, cutting, and welding the pole ears to obtain a negative electrode.

[0086] Table 1

[0087]

[0088]

[0089] In Table 1, " / " indicates that the substance is not added; N1: adiponitrile; N2: succinonitrile; N3: 1,6-dicyanohexane; N4: tetramethylsuccinonitrile; N5: 2,4-dimethylglutaronitrile; N6: ethylene glycol di(2-cyanoethyl) ether; N7: 1,4-bis(2-cyanoethoxy)butane; N8: 1,4-dicyano-2-butene; N9: 1,4-dicyano-2,3-dimethyl-2-butene; N10: 1,6-dicyano-2-methyl-5-methyl-3-hexene. () The internal ratio is the mass content ratio of the corresponding element in the nickel-cobalt-manganese ternary material.

[0090] It can be seen from Table 1 that the nickel-cobalt-manganese ternary material doped with magnesium and aluminum elements in the present application cooperates with the inorganic additives and the dinitrile compound in the electrolyte to produce a synergistic effect, which can greatly improve the capacity retention rate and residual gas amount of the secondary battery.

[0091] In particular, the present application further dopes tungsten element on the basis of doping the first element with a certain proportion of dinitrile compound in the nickel-cobalt-manganese ternary material, which can further improve the capacity retention rate and residual gas amount of the secondary battery.

[0092] In particular, the inorganic additive of the present application includes the second element, which can further improve the capacity retention rate and the amount of residual gas of the secondary battery.

[0093] In particular, the second element includes indium, tin, and antimony, which can further improve the capacity retention rate and the amount of residual gas of the secondary battery.

[0094] In particular, the use of a negative electrode material containing a silicon-based material in combination with a dinitrile compound added to the electrolyte can further improve the capacity retention rate of the secondary battery.

[0095] The secondary batteries of the following embodiments and comparative examples are different from those of embodiment 11 only in that the components and mass contents in the electrolyte are adjusted according to Table 2. The specific adjustment contents and performance test results are shown in Table 2 below.

[0096] Table 2

[0097] VC(%) DEC(%) VC+DEC(%) DFA(%) Capacity retention rate Residual gas volume Embodiment 11 / / / / B B Embodiment 27 0.1 18.9 19 / B B Embodiment 28 0.3 19 19.3 / B A Embodiment 29 0.7 19 19.7 / B A Embodiment 30 1 19 20 / B A Embodiment 31 0.3 21 21.3 / A A Embodiment 32 0.7 29 29.7 / A A Embodiment 33 1 39 40 / A B Embodiment 34 / / / 0.1 A B Embodiment 35 / / / 0.6 A A Embodiment 36 / / / 1.2 A A Embodiment 37 / / / 3 B A Embodiment 38 0.3 19 19.3 0.1 A A

[0098] In particular, the combination of nickel-cobalt-manganese ternary material with dinitrile compounds, vinylene carbonate and diethyl carbonate in the electrolyte can improve the capacity retention rate and residual gas amount of the secondary battery.

[0099] In particular, by adding difluoroethyl acetate to the nickel-cobalt-manganese ternary material and the dinitrile compound in the electrolyte, the capacity retention rate and the amount of residual gas in the secondary battery can be further improved.

[0100] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of disclosure involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features. For example, the above features are replaced with the technical features with similar functions disclosed in the present application.

Claims

1. A secondary battery comprising a positive electrode, a negative electrode and an electrolyte, characterized in that: The positive electrode comprises a positive electrode current collector and a positive electrode material layer, the positive electrode material layer comprises a first material layer and a second material layer, and the second material layer is arranged between the positive electrode current collector and the first material layer; The first material layer includes a nickel-cobalt-manganese ternary material, the nickel-cobalt-manganese ternary material includes a first element, and the first element includes a magnesium element and an aluminum element; The second material layer includes an inorganic additive, the inorganic additive includes a second element, and the second element includes at least one of titanium, chromium, yttrium, zirconium, lanthanum, niobium, indium, tin, zinc or antimony; The electrolyte includes a dinitrile compound.

2. The secondary battery according to claim 1, characterized in that: The first material layer further includes lithium manganese iron phosphate.

3. The secondary battery according to claim 1, characterized in that: The second element includes indium, tin and antimony.

4. The secondary battery according to claim 1, characterized in that: The nickel-cobalt-manganese ternary material also includes strontium and / or tungsten.

5. The secondary battery according to any one of claims 1 to 4, characterized in that: The dinitrile compounds include succinonitrile, glutaronitrile, adiponitrile, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 1,8-dicyanooctane, 1,9-dicyanononane, 1,10-dicyanodecane, 1,12-dicyanododecane, tetramethylsuccinonitrile, 2-methylglutaronitrile, 2,4-dimethylglutaronitrile, 2,2,4,4-tetramethylglutaronitrile, 1,4-dicyanopentane, 2,6-dicyanoheptane, 2,7-dicyanooctane, 2,8-dicyanononane, 1,6-dicyanodecane, 1,2-dicyanobenzene, 1,3-dicyanobenzene, 1,4-dicyanobenzene, ethylene glycol di(2-cyanoethyl) ether, diethylene glycol di(2-cyanoethyl) ether, triethylene glycol di(2-cyanoethyl) ether, At least one of tetraethylene glycol di(2-cyanoethyl) ether, 3,6,9,12,15,18-hexaoxaeicosanoic acid dinitrile, 1,3-bis(2-cyanoethoxy)propane, 1,4-bis(2-cyanoethoxy)butane, 1,5-bis(2-cyanoethoxy)pentane, ethylene glycol di(4-cyanobutyl) ether, 1,4-dicyano-2-butene, 1,4-dicyano-2-methyl-2-butene, 1,4-dicyano-2-ethyl-2-butene, 1,4-dicyano-2,3-dimethyl-2-butene, 1,4-dicyano-2,3-diethyl-2-butene, 1,6-dicyano-3-hexene, 1,6-dicyano-2-methyl-3-hexene, and 1,6-dicyano-2-methyl-5-methyl-3-hexene.

6. The secondary battery according to any one of claims 1 to 4, characterized in that: The secondary battery satisfies at least one of the following conditions: (1) Based on the total mass of the positive electrode material layer, the mass content of the first element is n1, 1200 ppm≤n1≤10000 ppm; (2) In the first element, the mass content ratio of magnesium element to aluminum element is 1:(0.8 to 1.2); (3) Based on the total mass of the positive electrode material layer, the mass content of the second element is n2, 1ppm≤n2≤5000ppm; (4) The nickel-cobalt-manganese ternary material also includes a third element, and the third element includes strontium and / or tungsten; based on the total mass of the positive electrode material layer, the mass content of the third element is n3, 1ppm≤n3≤5000ppm.

7. The secondary battery according to any one of claims 1 to 4, characterized in that: The negative electrode includes a negative electrode material layer, and the negative electrode material layer includes a silicon-based material.

8. The secondary battery according to any one of claims 1 to 4, characterized in that: The electrolyte further comprises vinylene carbonate and diethyl carbonate. Based on the mass of the electrolyte, the sum of the mass percentages of the vinylene carbonate and the diethyl carbonate is 19% to 40%.

9. The secondary battery according to claim 8, characterized in that: Based on the quality of the electrolyte, the electrolyte satisfies at least one of the following: (1) The mass percentage of the vinylene carbonate is 0.01% to 1%; (2) The mass percentage of diethyl carbonate is 19% to 39%.

10. The secondary battery according to any one of claims 1 to 4, characterized in that: The electrolyte further comprises difluoroethyl acetate, and based on the mass of the electrolyte, the mass percentage of the difluoroethyl acetate is 0.01% to 3%.

11. The secondary battery according to any one of claims 1 to 4, characterized in that: Based on the mass of the electrolyte, the mass percentage of the dinitrile compound is 0.1% to 5%. 12 . An electronic device comprising the secondary battery according to claim 1 .

Citation Information

Cited By

  • Secondary battery and electronic device

    WO2026143529A1

  • Secondary battery and electronic apparatus

    WO2026200026A1