Fiber-connected metal organic framework (MOF) polymer solid electrolyte membrane and preparation method thereof, and lithium metal battery

The fiber-connected metal organic framework@polymer composite solid electrolyte membrane solves the problems of low ionic conductivity and insufficient mechanical strength of the solid electrolyte membrane at room temperature, achieves efficient lithium ion conduction and inhibits lithium dendrite growth, and improves lithium metal batteries. electrochemical performance and cycling stability.

CN118738540APending Publication Date: 2024-10-01DALIAN UNIV OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410733043.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing solid electrolyte membranes have low ionic conductivity and insufficient mechanical strength at room temperature, making it difficult to inhibit the growth of lithium dendrites, resulting in insufficient energy density and cycle stability of lithium metal batteries.

Method used

A fiber-connected metal-organic framework@polymer composite solid electrolyte membrane is used, which is prepared by electrospinning and in-situ coordination methods. The fiber-connected metal-organic framework in the base membrane interacts with the polymer electrolyte to improve mechanical strength and inhibit lithium dendrites. crystal growth.

Benefits of technology

Significantly improves lithium ion conductivity and mechanical strength, inhibits lithium dendrite growth, and improves the electrochemical performance, cycle stability, energy density and safety of lithium metal batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738540A_ABST
    Figure CN118738540A_ABST
Patent Text Reader

Abstract

The invention discloses a fiber-connected metal organic framework (MOF) polymer solid electrolyte membrane, a preparation method thereof and a lithium metal battery. The electrolyte membrane is formed by filling polymer electrolyte in a fiber-connected metal organic framework base membrane. The base membrane is obtained through an electrostatic spinning method and an in-situ coordination growth method, the fiber-connected metal organic framework base membrane and the polymer electrolyte are fused through an in-situ polymerization method to obtain the electrolyte membrane, and the ionic conductivity is gt; 1 mS cm <-1 >. And the lithium symmetric battery runs for more than 300 hours under the electroplating / stripping capacity and the current density of 0.1 mA h cm <-2 > and 0.1 mA cm <-2 >. The capacity retention ratio of LFP / PZPS / Li after 110 cycles under 0.2 C is greater than 94%, the specific discharge capacities under 0.1, 0.2, 0.5, 1 and 2C are respectively 157, 154, 142, 122 and 75 mAh g <-1 >, when the current density returns to 0.1 C, the specific discharge capacity is 155 mAh g <-1 >, and excellent long cycle stability and rate capability are achieved. The obtained solid-state electrolyte membrane is high in ionic conductivity and high in lithium metal negative electrode stability, and the electrochemical performance of a solid-state lithium metal battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of organic-inorganic composite solid electrolyte membrane lithium metal batteries, and relates to a fiber-connected metal organic skeleton@polymer solid electrolyte membrane and a preparation method thereof and a lithium metal battery. The solid lithium metal battery is assembled from a positive electrode, a negative electrode and the composite solid electrolyte membrane. Background Art

[0002] With the continuous development of the economy, people's demand for energy is increasing day by day, but the organic liquid electrolyte in traditional lithium-ion batteries is easy to leak and flammable, and there are serious safety problems such as fire and explosion. In addition, its energy density has basically reached its limit and cannot meet the needs of industries such as aerospace, new energy vehicles, high-speed rail, and large-scale energy storage grids for higher energy density of energy storage equipment. Solid electrolyte membranes have high thermal / electrochemical stability and mechanical strength. They can replace liquid electrolytes, match high-voltage positive electrodes and high-specific-capacity lithium metal negative electrodes, reduce battery safety risks and improve energy density and long-cycle stability. Therefore, the research and development of new solid electrolyte membranes is of great significance to promote the practical application of lithium metal batteries.

[0003] Solid electrolyte membranes separate the positive and negative electrodes and conduct lithium ions. They need to have high ionic conductivity, lithium ion migration number, mechanical strength, excellent electrode interface compatibility, and electrochemical stability. They mainly include inorganic, organic, and organic-inorganic composite solid electrolyte membranes. Polymer solid electrolyte membranes have the advantages of good flexibility, strong preparability, and low price. They can overcome the shortcomings of inorganic solid electrolytes such as oxides and sulfides, such as brittleness and poor compatibility with electrode interfaces. Polymer solid electrolyte membranes are considered to be one of the most promising solid electrolyte membranes, but the room temperature ionic conductivity is low (10 -7 ~10 -5 S cm -1 ) and low mechanical strength makes it difficult to inhibit the growth of lithium dendrites. In order to improve the ionic conductivity of the solid electrolyte membrane, increasing the movement of polymer segments or introducing plastic crystal materials such as succinonitrile, ionic liquids or liquid electrolytes are common strategies. However, this will reduce the mechanical strength of the membrane, resulting in a balance effect between the ionic conductivity and mechanical strength of the solid electrolyte membrane, causing the key problem of difficulty in inhibiting lithium dendrites when matching the lithium metal negative electrode. Therefore, it is necessary to develop a solid electrolyte membrane that efficiently conducts lithium ions, which is crucial to reducing the resistance to lithium ion transfer and inhibiting lithium dendrites, and promote the practical application of solid-state lithium metal batteries. Summary of the invention

[0004] Metal-organic frameworks are porous crystalline materials that form periodic network structures through self-assembly of metal ions / clusters and organic ligands. They have the characteristics of large specific surface area, easily adjustable pore structure and composition, and insulation. They are expected to improve the mechanical strength of polymer electrolyte membranes and inhibit side reactions between small molecules of plastic crystal materials and lithium metal through adsorption and other effects.

[0005] The object of the present invention is to provide a fiber-connected metal organic skeleton @ polymer solid electrolyte membrane, wherein the solid electrolyte membrane is obtained by filling a polymer electrolyte in a fiber-connected metal organic skeleton base membrane, wherein the polymer electrolyte contains a lithium salt and a plastic crystal material, and the fiber-connected metal organic skeleton evenly distributed in the base membrane can not only improve the mechanical strength of the membrane, but also reduce the lithium ion conduction resistance, promote lithium ion conduction, and improve ion conductivity. At the same time, it interacts with the plastic crystal material to inhibit the side reaction between the small molecules of the plastic crystal material and lithium metal, and guides the uniform distribution and deposition of lithium ions, thereby synergizing the high mechanical strength to inhibit the growth of lithium dendrites.

[0006] The second purpose of the present invention is to provide a method for preparing a fiber-connected metal organic framework @ polymer solid electrolyte membrane. Using polymers and organic ligands of metal organic frameworks as raw materials, a fiber-connected metal organic framework base membrane is obtained by electrospinning and in-situ coordination. This method is simple and easy to scale up and mass produce. The organic ligands in the base membrane can induce in-situ coordination of metal salts to achieve fiber-connected metal organic frameworks with uniform distribution. Then, a fiber-connected metal organic framework @ polymer composite solid electrolyte membrane is obtained by in-situ polymerization of polymer monomers (containing lithium salts and plastic crystal materials). This method further alleviates the solid / solid interface compatibility problem of the electrolyte membrane and the electrode in solid-state lithium metal batteries.

[0007] The third object of the present invention is to provide a lithium metal battery based on the above-mentioned fiber-connected metal organic framework@polymer composite solid electrolyte membrane to improve its electrochemical performance.

[0008] To achieve the above objectives, the present invention provides the following technical solutions:

[0009] A fiber-connected metal organic skeleton@polymer composite solid electrolyte membrane, wherein the electrolyte membrane is a fiber-connected metal organic skeleton base membrane filled with a polymer electrolyte, wherein the polymer electrolyte contains a lithium salt and a plastic crystal material; the base membrane is a fiber-connected, uniformly distributed metal organic skeleton with a mechanical strength of 2 to 60 MPa, and the porous structure and metal sites of the metal organic skeleton interact with the polymer electrolyte to enhance the stability to lithium, so that the lithium symmetric battery can operate stably for more than 300 hours.

[0010] Furthermore, in the fiber-connected metal organic framework-based membrane, the metal organic framework (MOF) includes ZIF-8, ZIF-67, UIO-66 or UIO-67, which is prepared by in-situ coordination of organic ligands and metal salts.

[0011] Furthermore, in the fiber-connected metal organic framework base membrane, the fiber is a polymer fiber for preparing the base membrane, including polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride, polyacrylonitrile, polyimide, polyetherimide or polybenzimidazole.

[0012] Furthermore, the polymer electrolyte is obtained by polymerizing a lithium ion-conducting polymer monomer in which a lithium salt and a plastic crystal material are dissolved.

[0013] The present invention also provides a method for preparing a fiber-connected metal organic framework@polymer composite solid electrolyte membrane, comprising the following steps:

[0014] (1) Preparation of fiber-connected metal-organic framework-based membranes

[0015] The polymer, organic ligand and solvent are mixed and stirred to form a uniform and viscous casting solution, and the casting solution is spun on an aluminum foil using an electrospinning machine; the polymer fiber membrane containing the organic ligand is immersed in a metal salt solution, and then the organic ligand solution is added to produce an in-situ coordination reaction, and the membrane is taken out, rinsed with a solvent and dried to obtain a fiber-connected metal organic skeleton-based membrane;

[0016] (2) Preparation of fiber-connected metal organic framework@polymer composite solid electrolyte membrane

[0017] The lithium salt is dissolved in the plastic crystal material, and then the polymer monomer is added and stirred evenly, and then the polymerization initiator is added and stirred evenly, and then dripped onto the fiber-connected metal organic skeleton base membrane prepared in step (1), and transferred into an oven for thermal polymerization to obtain a fiber-connected metal organic skeleton@polymer composite solid electrolyte membrane.

[0018] Furthermore, in step (1), the ligand is a ligand for preparing a metal organic framework, including 2-methylimidazole and its derivatives or terephthalic acid and its derivatives, and the metal salt is a metal salt for preparing a metal organic framework, including nitrate, acetate or sulfate; in step (2), the lithium salt includes lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate or lithium perchlorate; the plastic crystal material is succinonitrile, and the polymer monomer includes one or more of polyethylene glycol diacrylate, vinyl ethylene carbonate and 1,3-dioxolane.

[0019] Furthermore, in step (1), the solvent is a solvent that dissolves the polymer and the organic ligand, including N,N-dimethylformamide, N-methylpyrrolidone or acetonitrile.

[0020] Furthermore, in step (1), the mass ratio of the polymer, the organic ligand and the solvent in the membrane solution is 1:8:16 to 8:0.25:16.

[0021] Furthermore, in step (1), the mixing and stirring time of the polymer, organic ligand and solvent is 8 to 48 hours.

[0022] Furthermore, in step (1), the electrospinning speed is 0.001-2 mL min – 1 .

[0023] Furthermore, in step (1), the voltage of the electrospinning is 10 to 25 kV.

[0024] Furthermore, in step (1), the solvent of the metal salt solution and the organic ligand solution is a solvent for preparing a metal organic framework, which is methanol, ethanol or water.

[0025] Furthermore, in step (1), the concentration of the metal salt solution is 0.001 to 3 M, and the amount used is 1 to 500 mL.

[0026] Furthermore, in step (1), the polymer-based membrane containing organic ligands is immersed in the metal salt solution for a period of 5 minutes to 24 hours.

[0027] Furthermore, in step (1), the concentration of the organic ligand solution is 0.008 to 24 M, and the amount used is 1 to 500 mL.

[0028] Furthermore, in step (1), the in-situ coordination reaction time is 0.5 to 48 hours.

[0029] Furthermore, in step (1), the oven temperature is 60 to 100° C., and the drying time is 8 to 48 hours.

[0030] Furthermore, in step (2), the mass ratio of the plastic crystal material to the lithium salt is 1:15 to 20:3; the mass ratio of the sum of the mass of the plastic crystal material and the lithium salt to the mass of the polymer monomer is 20:63 to 100:3.

[0031] Furthermore, in step (2), the polymer monomer includes polyethylene glycol diacrylate.

[0032] Furthermore, in step (2), the mass of the polymerization initiator is 0.1 to 10% of the mass of the polymer monomer.

[0033] Furthermore, in step (2), the polymerization initiator is 2,2-azobisisobutyronitrile.

[0034] Furthermore, in step (2), the lithium salt is dissolved in the plastic crystal material, and then the polymer monomer is added and stirred evenly for 1 to 48 hours.

[0035] Furthermore, in step (2), the polymerization temperature is 60 to 100° C., and the polymerization time is 0.1 to 48 hours.

[0036] The present invention also provides a solid-state lithium metal battery, comprising a positive electrode, a negative electrode and a solid electrolyte membrane, wherein the solid electrolyte membrane is the fiber-connected metal organic skeleton@polymer composite solid electrolyte membrane.

[0037] Furthermore, the positive electrode is lithium iron phosphate or a ternary positive electrode material.

[0038] The beneficial effects of the present invention include:

[0039] The fiber-connected metal organic skeleton@polymer composite solid electrolyte membrane of the present invention has a base membrane of a metal organic skeleton connected by fibers and evenly distributed, which improves the mechanical strength and promotes the dissociation of anions in lithium salts through the porous structure and open metal sites, thereby improving the ionic conductivity (>1mS cm – 1 ) and lithium ion migration number (>0.6), and at the same time, through the porous structure and open metal sites interacting with the plastic crystal material, it is possible to inhibit its side reaction with the lithium metal negative electrode, induce the uniform distribution and deposition of lithium ions, and solve the problem of lithium dendrite growth.

[0040] The preparation method of a fiber-connected metal organic skeleton @ polymer composite solid electrolyte membrane of the present invention is to use polymer and organic ligand of metal organic skeleton as raw materials, obtain polymer fiber membrane containing organic ligand by electrostatic spinning method, the organic ligand in the membrane guides the in-situ coordination of metal salt of metal organic skeleton, obtain fiber-connected metal organic skeleton base membrane by in-situ coordination method, and realize fiber-connected metal organic skeleton with uniform distribution. The method is simple and easy to scale up and mass produce. Then, the fiber-connected metal organic skeleton @ polymer composite solid electrolyte membrane is obtained by in-situ polymerization of polymer monomer (containing lithium salt and plastic crystal material), and the method further alleviates the solid / solid interface compatibility problem between solid electrolyte membrane and electrode in solid lithium metal battery.

[0041] The solid-state lithium metal battery based on the fiber-connected metal organic framework@polymer composite solid electrolyte membrane of the present invention exhibits excellent electrochemical performance. – 2 and 0.1 mA cm – 2The lithium symmetric battery operated for more than 300 h at the plating / stripping capacity and current density. The capacity retention rate of LFP / PZPS / Li after 110 cycles at 0.2C was greater than 94%, and the discharge specific capacities at 0.1, 0.2, 0.5, 1, and 2C were 157, 154, 142, 122, and 75 mAh g, respectively. –1 When the current density returns to 0.1C, the battery discharge capacity is 155mAh g –1 , basically restored to its initial state, showing excellent long-cycle stability and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Electron micrographs of (a) the surface of PVDF-HFP (PVDF-HFP / DMIZ) fiber membrane containing organic ligands, (b) the surface of PVDF-HFP@ZIF-67 (PVDF-HFP / DMIZ@ZIF-67) base membrane, (c) the surface of PVDF-HFP fiber membrane@polymer electrolyte membrane (PPS) containing organic ligands (Comparative Example 1), and (d) the surface of fiber-connected metal organic framework@polymer composite solid electrolyte membrane (PZPS) prepared in Example 1.

[0043] Figure 2 The mechanical properties diagram of PVDF-HFP, PVDF-HFP / DMIZ, and PVDF-HFP / DMIZ@ZIF-67 base membranes.

[0044] Figure 3 (a) Impedance spectrum, (b) Linear sweep voltammetry curve, (c) polarization curve and impedance spectrum of the composite solid electrolyte membrane prepared in Example 1, wherein PPS is Comparative Example 1.

[0045] Figure 4 This is the constant current voltage curve of the lithium symmetric battery assembled in Example 1, where PPS is comparative example 1.

[0046] Figure 5 (a) Long cycle and (b) rate performance diagrams of the solid-state LiFePO4|Li battery assembled in Example 1, where PPS is comparative example 1. DETAILED DESCRIPTION

[0047] The specific experimental scheme of the present invention is described in detail below in conjunction with specific embodiments, but the present invention is not limited to the examples listed. Unless otherwise specified, the methods described are all conventional methods, and the raw materials and instruments used can be purchased on the market.

[0048] Example 1

[0049] (1) Preparation of polyvinylidene fluoride-hexafluoropropylene fiber-bonded ZIF-67 base membrane

[0050] Weigh 2g of 2-methylimidazole and 10g of N,N-dimethylformamide DMF and mix them, then add 2g of polyvinylidene fluoride-hexafluoropropylene PVDF-HFP and stir for 24h to form a uniform and viscous brown-black membrane liquid. The mass ratio of polyvinylidene fluoride-hexafluoropropylene, 2-methylimidazole and N,N-dimethylformamide is 2:2:10. Use an electrospinning machine to spin the membrane liquid on aluminum foil. The polyvinylidene fluoride-hexafluoropropylene fiber membrane (PVDF-HFP / DMIZ) containing 2-methylimidazole was immersed in 100 mL of 0.08 M cobalt nitrate methanol solution for 30 min, and then 100 mL of 0.32 M 2-methylimidazole methanol solution was added to allow an in-situ coordination reaction to occur for 24 h. The membrane was taken out, rinsed with a solvent, and dried in an oven at 80 °C for 24 h to obtain a polyvinylidene fluoride-hexafluoropropylene fiber connected to a ZIF-67 base membrane (PVDF-HFP / DMIZ@ZIF-67).

[0051] (2) Preparation of fiber-connected metal organic framework@polymer composite solid electrolyte membrane

[0052] 0.63 g of polyethylene glycol diacrylate, 1.2 g of succinonitrile and 0.8 g of lithium bis(trifluoromethanesulfonyl)imide were mixed and stirred for 6 h, with a mass ratio of 0.63:1.2:0.8, and then 0.0063 g of 2,2-azobisisobutyronitrile was added and stirred for 10 to 20 min until the mixture was uniformly mixed and dripped onto the PVDF-HFP fiber-connected ZIF-67 base membrane prepared in step (1), which was then transferred to a 70° C. oven for thermal polymerization for 12 h to obtain a fiber-connected metal organic framework@polymer composite solid electrolyte membrane, denoted as PZPS.

[0053] (3) Assembly of solid-state lithium metal batteries

[0054] Lithium iron phosphate powder, conductive carbon black Super P and binder PVDF powder with a mass ratio of 8:1:1 were ground in a mortar for 20 minutes to mix them evenly. N-methylpyrrolidone NMP was added, and after slurrying, it was coated on aluminum foil and placed in an oven at 60°C for drying for 24 hours. In a glove box with an argon atmosphere, a positive electrode sheet, the above-mentioned PVDF-HFP fiber connected to the ZIF-67 base film, a mixed solution of polyethylene glycol diacrylate and succinonitrile and lithium bistrifluoromethanesulfonyl imide and 2,2-azobisisobutyronitrile, metallic lithium, and nickel foam were added in the order of assembling a CR2025 button lithium metal battery, and a solid-state lithium metal battery, LFP / PZPS / Li, was obtained after thermal polymerization.

[0055] Comparative Example 1

[0056] The base membrane of this comparative example is a polyvinylidene fluoride-hexafluoropropylene fiber membrane (PVDF-HFP / DMIZ) containing 2-methylimidazole, and other conditions are the same as those in Example 1 to obtain PPS.

[0057] Comparative Example 2

[0058] This comparative example is an electrostatic spinning polyvinylidene fluoride-hexafluoropropylene fiber membrane (PVDF-HFP), 2-methylimidazole is not added to the spinning membrane solution, and other conditions are the same as those in Example 1, to obtain a PVDF-HFP fiber membrane.

[0059] Figure 1 Electron microscope images of (a) the surface of PVDF-HFP fiber membrane containing organic ligands, (b) the surface of PVDF-HFP / DMIZ@ZIF-67 base membrane, (c) the surface of PVDF-HFP fiber membrane@polymer electrolyte membrane (PPS) containing organic ligands (Comparative Example 1), and (d) the surface of fiber-connected metal organic framework@polymer composite solid electrolyte membrane (PZPS) prepared in Example 1. It can be seen that the ZIF-67 nanoparticle layer is evenly distributed on the PVDF-HFP fiber membrane and connected by the fiber containing ligands, which improves the mechanical strength of the membrane.

[0060] The size of ZIF-67 nanoparticles is about 1 μm. Fibers and particles are still visible on the surface of the composite solid electrolyte membrane, and the base membrane is filled with polymer electrolyte.

[0061] Figure 2 The figure shows the mechanical properties of PVDF-HFP, PVDF-HFP / DMIZ, and PVDF-HFP / DMIZ@ZIF-67 base membranes. It can be seen that the mechanical strength of pure PVDF-HFP fiber membrane is low, because it is difficult to form a pure PVDF-HFP membrane by electrospinning. Adding 2-methylimidazole (DMIZ) can improve the electrospinning film-forming property and the mechanical strength of the membrane. After further growing ZIF-67 on this membrane, the mechanical strength of the base membrane will be significantly improved to 2-60MPa.

[0062] Figure 3 The (a) impedance spectrum, (b) linear sweep voltammetry curve, (c) polarization curve and impedance spectrum of the composite solid electrolyte membrane prepared in Example 1 at 30°C, where PPS is comparative example 1. The ionic conductivity calculated from (a) is 0.9 mScm –1 Increased to 1.29mS cm –1 The electrochemical stability window obtained by (b) increased from 4.53 V to 4.86 V, and the lithium ion migration number calculated by (cd) increased from 0.39 to 0.63.

[0063] Figure 4This is a constant current voltage curve of the lithium symmetric battery assembled in Example 1, where PPS is comparative example 1. It can be seen that at 0.1 mA h cm – 2 and 0.1 mA cm – 2 At the plating / stripping capacity and current density, the lithium symmetric battery operated for more than 300 hours, while the comparative example 1 failed after 20 hours.

[0064] Figure 5 (a) Long cycle and (b) rate performance diagram of the solid-state LiFePO4|Li battery assembled in Example 1, where PPS is comparative example 1. The capacity retention rate of LFP / PZPS / Li after 110 cycles at 0.2C is greater than 94%, which is significantly better than the performance of LFP / PPS / Li battery. The discharge specific capacities of LFP / PZPS / Li battery at 0.1, 0.2, 0.5, 1, and 2C are 157, 154, 142, 122, and 75 mAh g, respectively. –1 When the current density returns to 0.1C, the battery discharge capacity is 155mAh g –1 , basically restored to the initial state, showing better rate performance than LFP / PPS / Li.

[0065] The fiber-connected metal organic framework@polymer composite solid electrolyte membrane provided by the present invention absorbs anions in lithium salts through porous and metal sites to promote their dissociation, thereby improving ionic conductivity (>1mS cm – 1 ) and lithium ion migration number (>0.6), while also inhibiting the side reactions between small molecules of plastic crystal materials and lithium metal, and guiding the uniform distribution and deposition of lithium ions, and coordinating the high mechanical strength of the fiber-connected and evenly distributed metal organic skeleton-based membrane to solve the problem of lithium dendrite growth, greatly improving the electrochemical performance of solid electrolyte membrane lithium metal batteries.

[0066] Finally, it should be noted that the above embodiment is only one of the implementation methods of the present invention and cannot be understood as limiting the scope of the present invention. Without departing from the scope of the present invention, any equivalent replacement or modification of the present invention shall not depart from the technical solution of the present invention and shall still fall within the protection scope of the present invention.

Claims

1. A fiber-connected metal organic framework@polymer composite solid electrolyte membrane, characterized in that: The electrolyte membrane is a polymer electrolyte filled in a fiber-connected metal-organic skeleton base membrane, wherein the polymer electrolyte contains lithium salt and plastic crystal material; the base membrane is a fiber-connected and evenly distributed metal-organic skeleton with a mechanical strength of 2 to 60 MPa, and the porous structure and metal sites of the metal-organic skeleton interact with the polymer electrolyte to enhance ionic conductivity and stability to lithium.

2. A fiber-connected metal organic framework@polymer composite solid electrolyte membrane as claimed in claim 1, characterized in that: The fiber includes polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride, polyacrylonitrile, polyimide, polyetherimide or polybenzimidazole; the metal organic framework includes ZIF-8, ZIF-67, UIO-66 or UIO-67.

3. The fiber-connected metal organic framework@polymer composite solid electrolyte membrane according to claim 1, characterized in that: The polymer electrolyte is obtained by polymerizing a lithium ion-conducting polymer monomer in which a lithium salt and a plastic crystal material are dissolved.

4. A method for preparing the fiber-connected metal organic framework@polymer composite solid electrolyte membrane according to claim 1, characterized in that: The steps include: (1) Preparation of fiber-connected metal-organic framework-based membranes The polymer, organic ligand and solvent are mixed and stirred to form a uniform and viscous membrane liquid, and the membrane liquid is spun on an aluminum foil using an electrospinning machine; the polymer fiber membrane containing the organic ligand is immersed in a metal salt solution, and then the organic ligand solution is added to produce an in-situ coordination reaction, and the membrane is taken out, rinsed with a solvent and dried to obtain a fiber-connected metal organic skeleton-based membrane; (2) Preparation of fiber-connected metal organic framework@polymer composite solid electrolyte membrane The lithium salt is dissolved in the plastic crystal material, and then the polymer monomer is added, and then the polymerization initiator is added and stirred evenly, and then dripped onto the fiber-connected metal organic skeleton base membrane prepared in step (1), and transferred into an oven for thermal polymerization to obtain a fiber-connected metal organic skeleton@polymer composite solid electrolyte membrane.

5. The method for preparing the fiber-connected metal organic framework@polymer composite solid electrolyte membrane according to claim 4, characterized in that: In step (1), the ligand includes 2-methylimidazole and its derivatives or terephthalic acid and its derivatives, and the metal salt includes nitrate, acetate or sulfate; in step (2), the lithium salt includes lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate or lithium perchlorate; the plastic crystal material includes one or more of succinonitrile, ionic liquid or liquid electrolyte; the polymer monomer includes one or more of polyethylene glycol diacrylate, vinyl ethylene carbonate or 1,3-dioxolane.

6. The method for preparing a fiber-connected metal organic framework@polymer composite solid electrolyte membrane according to claim 4, characterized in that: In step (1), the mass ratio of polymer, organic ligand and solvent in the membrane solution is 1:8:16 to 8:0.25:16; the speed of the electrospinning is 0.0001 to 2 mL min – 1 , the voltage is 5~30kV.

7. The method for preparing a fiber-connected metal organic framework@polymer composite solid electrolyte membrane according to claim 4, characterized in that: In step (1), the polymer fiber membrane containing organic ligands is immersed in the metal salt solution for 5 minutes to 24 hours; the concentration of the metal salt solution is 0.001 to 3M, and the amount is 1 to 500mL; the concentration of the organic ligand solution is 0.008 to 24M, and the amount is 1 to 500mL; the solvent of the metal salt and organic ligand solution is methanol, ethanol or water.

8. The method for preparing a fiber-connected metal organic framework@polymer composite solid electrolyte membrane according to claim 4, characterized in that: In step (1), the in-situ coordination reaction time is 0.5 to 48 hours.

9. The method for preparing a fiber-connected metal organic framework@polymer composite solid electrolyte membrane according to claim 4, characterized in that: The mass ratio of the plastic crystal material and the lithium salt in step (2) is 1:15 to 20:3; the mass ratio of the sum of the mass of the plastic crystal material and the lithium salt to the mass of the polymer monomer is 20:63 to 100:3; the mass of the polymerization initiator is 0.1 to 10% of the mass of the polymer monomer.

10. A solid-state lithium metal battery, comprising a positive electrode, a negative electrode and a solid electrolyte membrane, characterized in that: The solid electrolyte membrane is the fiber-connected metal organic framework@polymer composite solid electrolyte membrane as described in claim 1.

Citation Information

Cited By

  • Polymer solid electrolyte-negative electrode integrated structure, preparation method thereof and solid-state battery

    CN119381581A

  • Polymer solid electrolyte-negative electrode integrated structure and preparation method thereof, solid-state battery

    CN119381581B