Method for manufacturing semiconductor-on-insulator multilayer structure

By adding interstitial nitrogen and oxygen to the supporting substrate of the semiconductor-on-insulator multilayer structure to form controlled oxygen precipitates and nitrogen precipitates, combined with the design of the well-rich layer, the problems of slip line and high resistivity stability are solved problem, achieving resistance to slip lines and resistivity control, and is suitable for component manufacturing in the high-frequency field.

CN118743012APending Publication Date: 2024-10-01SOITEC SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380022662.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-11
Filing Date
2023-03-10
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When manufacturing semiconductor-on-insulator type multi-layer structures, it is difficult for the existing technology to resist the development of slip lines and maintain high resistivity at the same time. Especially under the trend of miniaturization, slip lines are becoming increasingly intolerable, and at the same time, high resistivity Stability and mechanical stress control are difficult to achieve.

Method used

Using a support substrate containing interstitial nitrogen and oxygen, oxygen precipitates and nitrogen precipitates are formed through nucleation and stabilization stages, and their size and concentration are controlled between 10nm and 50nm and between 107cm-3 and 1010cm-3, and are assembled during assembly Well-rich layers are added in stages to limit dislocation propagation and resistivity control.

Benefits of technology

It achieves effective resistance to slip lines, maintains high resistivity stability, avoids deformation and photolithography pattern alignment problems caused by mechanical stress, and is suitable for component manufacturing in high-frequency fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743012A_ABST
    Figure CN118743012A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a semiconductor-on-insulator structure (1), comprising the following steps:-a donor substrate connecting a support substrate (2) with a semiconductor layer (4), the support substrate (2) having a resistivity greater than or equal to 500 Omega. Cm and containing interstitial nitrogen (6) and interstitial oxygen (7), the initial concentration of interstitial oxygen (6) in the support substrate (2) is between 15 old ppma and 25 old ppma, the electrically insulating layer (3) being located at the interface between the support substrate (2) and the donor substrate; and-transferring the semiconductor layer (4) onto a support substrate, the method further comprising a nucleation step comprising a heat treatment to precipitate a portion of the oxygen (7) and nitrogen (6) to form a nucleus (9) of a precipitate (8), and a stabilization step comprising a heat treatment to grow the nucleus to a size between 10 nm and 50 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing a multilayer structure of semiconductor-on-insulator type. Background Art

[0002] The structure of the semiconductor-on-insulator type is a multilayer structure comprising a supporting substrate, an electrically insulating layer arranged on the supporting substrate, and a semiconductor layer arranged on the insulating layer, wherein the supporting substrate is usually made of a semiconductor material (e.g., silicon), the electrically insulating layer is usually an oxide layer (e.g., a silicon oxide layer), and the semiconductor layer is usually a silicon layer. This structure is called a "semiconductor-on-insulator" structure, and when the semiconductor material is silicon, it is particularly called a "silicon-on-insulator" (SOI) structure. The oxide layer is located between the substrate and the semiconductor layer. The oxide layer is then referred to as "buried" and is referred to as a "BOX" (buried oxide). In the following, the term "SOI" will be used to represent the general structure of the semiconductor-on-insulator type.

[0003] Such an SOI structure can be obtained by a process involving transferring a single-crystalline semiconductor layer produced from a donor substrate onto the front side of a supporting substrate, an electrically insulating layer being located at the interface between the transferred semiconductor layer and the supporting substrate.

[0004] For applications in the high frequency range, one problem is to manufacture a specific SOI structure whose performance qualities are not affected by electrical losses caused by the flow of electrons from the conductive channels formed in or on the semiconductor layer to the supporting substrate. To this end, the process can, for example, include using a supporting substrate with a high resistivity and optionally combining the supporting substrate with a well-rich layer.

[0005] Another problem is to produce SOI structures that can withstand severe thermal treatments without the generation of slip lines. Slip lines consist of fracture planes where the crystal structure is deflected. In the absence of obstacles, dislocations can propagate up to the surface of the plate, where they generate steps of atomic planes or slip lines. In subsequent lithography stages, such steps can lead in particular to problems of misalignment of the lithographic pattern (a problem known to those skilled in the art as "overlay"). In order to limit the appearance of these slip lines, the process can use a substrate as a support substrate into which oxygen has been previously introduced at relatively high concentrations into the interstitial positions. The interstitial oxygen blocks the propagation of dislocations and thus prevents the appearance of steps on the surface of the plate.

[0006] However, interstitial oxygen has the disadvantage of creating a heat donor, which can lead to a change in the resistivity of the supporting substrate. Interstitial oxygen tends to lead to a decrease in the value of the resistivity. In fact, especially for applications in the radio frequency range, the resistivity needs to be controlled at a relatively high value and kept stable.

[0007] To overcome this drawback, one solution consists in using a substrate that is less enriched in interstitial oxygen as a support substrate. According to the previously standardized measurement specification ASTM79, the interstitial oxygen concentration of such a substrate (commonly referred to as "low Oi") is typically between 6 ppma and 10 ppma, where the unit ppma stands for "parts per million of an atom". For large electronic components manufactured from these substrates, this interstitial oxygen concentration is a relatively satisfactory compromise, which is able to limit the number of slip lines while controlling the resistivity of the substrate.

[0008] However, with the trend towards miniaturization, the development of slip lines in small electronic components, even in very small amounts, is becoming increasingly difficult to tolerate. The use of weaker enriched substrates may result in interstitial oxygen contents that are too low to achieve the desired performance qualities. Solutions that simply consist of increasing the interstitial oxygen content of the substrate are unsatisfactory, since too high an Oi concentration no longer makes it possible to control the resistivity value.

[0009] On the other hand, one solution that can be envisaged consists in increasing the initial concentration of interstitial oxygen of the supporting substrate and causing it to precipitate in the form of oxygen precipitates or in the form of defects known by the abbreviation BMD (bulk-shaped micro defects) by applying a thermal treatment.

[0010] The initial concentration of interstitial oxygen in the substrate is typically greater than 27 ppma. Using a substrate highly enriched in interstitial oxygen (often referred to as "high Oi"), it is possible to obtain a concentration of about 10 10 Oxygen precipitates or defects / cm 3 The oxygen precipitates are then large enough and numerous enough to block the propagation of dislocations in the same way as interstitial oxygen.

[0011] However, this construction does not allow the resistivity of the supporting substrate to be controlled and maintained at a stable and sufficiently high value for applications in the radio frequency range. Furthermore, if the number of oxygen precipitates is too high and too large, they can generate mechanical stresses locally in the core of the material, which can lead to global deformation of the substrate. Deformation of the substrate can also be the cause of alignment problems for lithographic patterns. Summary of the invention

[0012] One object of the present invention is to design a semiconductor-on-insulator type structure such that the supporting substrate has good resistance to the subsequent development of slip lines while exhibiting a high and controlled resistivity without generating significant mechanical stresses in the supporting substrate that could cause its overall deformation.

[0013] In this context, the term "high resistivity" is understood to mean a resistivity greater than or equal to 500 Ω.cm.

[0014] Another object of the present invention is to design a semiconductor-on-insulator type structure which, in the subsequent functionalization stage, does not give rise to overlay problems known to those skilled in the art, even for the manufacture of components for use in the high-frequency field, wherein the gate length of the structure is less than 65 nm, for example less than or about 22 nm.

[0015] To this end, the invention provides a method for producing a multilayer structure of semiconductor-on-insulator type, said method comprising the following stages:

[0016] - assembling a support substrate with a donor substrate for the semiconductor layer to be transferred, said support substrate having a resistivity greater than or equal to 500 Ω.cm and containing interstitial nitrogen and interstitial oxygen, the initial concentration of interstitial oxygen in said support substrate being between 15 and 25 ppma (measured according to standard ASTM 79), an electrically insulating layer being located at the interface between the support substrate and the donor substrate,

[0017] - transferring the semiconductor layer to a supporting substrate,

[0018] The method further comprises a nucleation phase and a stabilization phase, wherein the nucleation phase is suitable for precipitating at least part of the interstitial oxygen and at least part of the interstitial nitrogen in a controlled manner, thereby forming seeds of oxygen precipitates and nitrogen precipitates, and the stabilization phase is suitable for growing the seeds of oxygen precipitates and nitrogen precipitates to a size between 10 nm and 50 nm.

[0019] The addition of interstitial nitrogen helps resist the propagation of dislocations without reducing the resistivity of the supporting substrate. In addition, due to its affinity for oxygen, it aids in the precipitation of interstitial oxygen.

[0020] Adding interstitial oxygen in combination with the addition of interstitial nitrogen at controlled concentrations between "low Oi" and "high Oi" substrate concentrations can further improve resistance to subsequent development of slip lines, including for substrates with very thin thicknesses, where overlay issues become critical.

[0021] Control of the size and concentration of oxygen and nitrogen precipitates during the nucleation and growth phases also enables control of the resistance to the subsequent development of slip lines by limiting the propagation of dislocations within the support substrate. Furthermore, by more or less fixing the interstitial nitrogen and interstitial oxygen, the phases enable control of the resistivity of the support substrate, including the resistivity of a high-resistance support substrate for applications in the high-frequency range.

[0022] According to other features of the present invention, which are used alone or in combination when technically feasible:

[0023] - before the assembly stage, the method further comprises forming a well-rich layer on the support substrate, the well-rich layer being arranged between the support substrate and the electrically insulating layer,

[0024] - the forming of the well-rich layer comprises depositing a polysilicon layer on a supporting substrate,

[0025] - the deposition of the polysilicon layer is carried out after a stabilization phase of oxygen and nitrogen precipitation,

[0026] -The initial concentration of interstitial nitrogen in the support substrate is 10 14 atoms / cm 3 Up to 10 15 atoms / cm 3 between,

[0027] - At the end of the stabilization phase, the support substrate contains oxygen precipitates and nitrogen precipitates at a concentration of 10 7 cm -3 Up to 10 10 cm -3 The concentration is preferably between 10 8 cm -3 Up to 10 9 cm -3 between,

[0028] the nucleation phase and the stabilization phase each comprise a heat treatment, the temperature applied in the nucleation heat treatment being lower than the temperature applied in the stabilization heat treatment and the duration of the nucleation heat treatment being shorter than the duration of the stabilization heat treatment,

[0029] - a nucleation phase comprises applying a temperature between 650° C. and 800° C., preferably between 700° C. and 750° C., for a period of more than one hour, preferably two hours,

[0030] a stabilization phase comprising applying a temperature greater than 900° C., preferably 950° C., for a period greater than two hours, preferably four hours,

[0031] -Before the assembly phase, the nucleation phase and the stabilization phase proceed directly one after another.

[0032] The present invention also relates to a substrate for microelectronics, optoelectronics and / or optics, said substrate comprising, from its back side to its front side, a supporting substrate, an electrically insulating layer and a semiconductor layer, characterized in that said supporting substrate is made of a semiconductor material and has a resistivity greater than or equal to 500 Ω.cm and contains a concentration of 10 7 cm -3 Up to 10 10 cm -3 The oxygen precipitates and nitrogen precipitates are between 10 nm and 50 nm in size.

[0033] According to other features of the present invention, which are used alone or in combination when technically feasible:

[0034] - the substrate further comprises a well-rich layer, the well-rich layer being between the supporting substrate and the electrically insulating layer,

[0035] The residual concentration of interstitial oxygen in the support substrate is less than 15 ppma, preferably less than 12 ppma (measured according to standard ASTM 79). BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Other features and advantages of the present invention will become apparent from the following detailed description with reference to the accompanying drawings, in which:

[0037] - Figure 1 shows a semiconductor-on-insulator type multilayer structure according to the present invention, the supporting substrate contains oxygen and nitrogen precipitates (white circles), residual interstitial nitrogen (black crosses) and residual interstitial oxygen (black spots),

[0038] - FIG. 2A to FIG. 2F An embodiment of the method according to the invention is shown, in which a support substrate ( Figure 2A ), followed by the nucleation phase ( Figure 2B ), the stage where the seed crystal grows to produce stable oxygen and nitrogen precipitates (white circles) ( Figure 2C ), an optional stage of forming a well-rich layer on a supporting substrate ( Figure 2D ), a stage of arranging a donor substrate for the semiconductor layer to be transferred on a supporting substrate ( Figure 2E ) and the stage of transferring the semiconductor layer ( Figure 2F ), thus obtaining Figure 1 A semiconductor-on-insulator type multilayer structure is shown in FIG.

[0039] For reasons of readability, the drawings are not necessarily drawn to scale. DETAILED DESCRIPTION

[0040] A first subject of the invention is a multilayer structure of the semiconductor-on-insulator type, which exhibits a specific resistance to the propagation of dislocations and, therefore, minimizes the formation of slip lines during a back-end heat treatment. In addition, the resistivity of the supporting substrate of the multilayer structure is stable during the heat treatment. As an example, the multilayer structure according to the invention can exhibit a gate length of less than 65 nm, for example about 22 nm, while no slip lines or very few slip lines are generated when a temperature of about 450° C. is applied for one hour. In addition, the supporting substrate of the multilayer structure can exhibit a target resistivity between 500 Ohm.cm and 5000 Ohm.cm while remaining stable. The multilayer structure of the semiconductor-on-insulator type, which is the subject of the invention, has applications, for example, in the radiofrequency field, where a high-resistance supporting substrate has particular advantages.

[0041] Figure 1 An embodiment of such a multilayer structure 1 according to the invention is shown. The multilayer structure 1 comprises, in order from the back side to the front side of the structure, a supporting substrate 2, an electrically insulating layer 3 and a semiconducting layer 4.

[0042] The support substrate 2 of the multilayer structure 1 is made of a high-resistance semiconductor material. The resistivity of the support substrate is greater than or equal to 500 ohm.cm. The high resistivity gives the support substrate the ability to limit electrical losses and improve the radio frequency performance quality of the structure.

[0043] The supporting substrate 2 of the multilayer structure 1 contains oxygen and nitrogen precipitates 8, also referred to by the abbreviation BMD (bulk microscopic defects). BMD exhibit the property of blocking the propagation of dislocations, which tend to develop when the multilayer structure 1 is subjected to a heat treatment. Thus, the BMD are able to prevent the dislocations from rising to the surface of the multilayer structure 1, which would shift its atomic plane. Such a shift is in particular the cause of alignment problems known to those skilled in the art by the term "overlay".

[0044] The size of the oxygen and nitrogen precipitates 8 in the support substrate 2 of the multilayer structure 1 is between 10 nm and 50 nm, preferably between 40 nm and 50 nm. The size range thus selected constitutes an advantageous compromise, which can significantly limit the number of slip lines generated at the surface without generating excessive mechanical stresses in the material. This is because too small oxygen and nitrogen precipitates will not effectively block the development of dislocations. On the other hand, too large precipitates will risk generating high mechanical stresses in the material, causing the material to deform. Therefore, through this compromise, the above-mentioned overlay phenomenon is minimized.

[0045] The concentration of oxygen precipitate and nitrogen precipitate 8 in the support substrate 2 is 10 7 Sediment / cm 3 Up to 1010 Sediment / cm 3 between 10 and 15 8 Sediment / cm 3 Up to 10 9 Sediment / cm 3 If the concentration of the precipitate is less than 10 7 Sediment / cm 3 , the amount of oxygen precipitates and nitrogen precipitates is insufficient to effectively block the propagation of dislocations. If the concentration of precipitates is greater than 10 10 Sediment / cm 3 , the risk of creating mechanical stresses in the material becomes significant.

[0046] The size and density of the oxygen and nitrogen precipitates 8 were measured by laser scattering tomography (referred to by the abbreviation LST).

[0047] The supporting substrate 2 may also contain residual interstitial nitrogen 6 and residual interstitial oxygen 7 (i.e. not forming precipitates 8). Like BMD, interstitial oxygen 7 and interstitial nitrogen 6 counteract the propagation of dislocations. However, interstitial oxygen 7 may contribute to the generation of heat donors, which presents a risk of uncontrolled reduction of resistivity. These heat donors are generated when the multilayer structure 1 is subjected to a back-end heat treatment, for example when a temperature between 375°C and 450°C is applied to the structure for a few minutes to one or two hours. This type of heat treatment is typically applied to the multilayer structure during a final anneal, which is intended to repair defects generated in the final stages of chip manufacturing (known to those skilled in the art as the term "back-end process"). During this "passivation" anneal, the hydrogen present in the furnace atmosphere diffuses as far as the interface, thereby repairing dangling bonds.

[0048] In order to limit the phenomenon of generating hot donors, the concentration of residual interstitial oxygen 7 of the support substrate 2 is less than 15 ppma, preferably less than 12 ppma. This is because, the lower the concentration of interstitial oxygen 7 in the support substrate 2, the better the control of the resistivity of the substrate 2 in various applications of the multilayer structure 1.

[0049] As mentioned above, the term old ppma means "parts per million of atoms" according to the previous standardized measurement specification ASTM 79.

[0050] The concentration of interstitial oxygen 7 is determined by a model for the generation of thermal donors: a thermal treatment of 450° C. for one hour is applied to the substrate, known to those skilled in the art as the abbreviation DGA (denoting the term donor generation annealing), and the resistivity of the substrate is measured before and after the DGA thermal treatment. The model makes it possible to relate the variation between two measurements of the resistivity, which is associated with the generation of thermal donors, to the concentration of residual interstitial oxygen. The resistivity is measured by SRP (Spreading Resistance Test).

[0051] Optionally, the structure 1 further comprises a well-rich layer 5, which is preferably made of polycrystalline silicon or porous silicon and is arranged between the support substrate 2 and the electrical insulating layer 3. The well-rich layer is capable of capturing charges accumulated under the first electrical insulating layer 3. For radio frequency applications of the multilayer structure 1, the well-rich layer 5 is particularly advantageous.

[0052] The electrically insulating layer 3 may be an oxide layer, for example a silicon oxide layer. Other materials may be envisaged, for example silicon nitride or silicon oxynitride. The semiconductor layer 4 is a layer made of a semiconductor material, for example a single-crystal silicon layer. In a non-limiting manner, the semiconductor layer 4 may be replaced by an active layer of any other material, in particular a piezoelectric layer, such as, for example, lithium tantalate or lithium niobate. Other materials may be used, for example gallium nitride, gallium arsenide or indium phosphide.

[0053] Manufacturing method

[0054] A second subject of the invention is a method for producing a multilayer structure as described above, said method forming oxygen and nitrogen precipitates in a supporting substrate of the multilayer structure by precipitating interstitial oxygen and interstitial nitrogen.

[0055] refer to Figure 2A , a substrate 2 is initially provided. The substrate 2 is made of a high-resistance semiconductor material, which initially contains interstitial nitrogen 6 and interstitial oxygen 7. The substrate 2 is, for example, a circular silicon plate with a diameter of 300 mm. The substrate 2 can be prepared by pulling an ingot of semiconductor material in an atmosphere of molecular oxygen and nitrogen. The content of interstitial oxygen and interstitial nitrogen is usually controlled by the manufacturer of the ingot and indicated in the technical specifications of the substrate.

[0056] The addition of interstitial nitrogen 6 in addition to interstitial oxygen 7 enables a substrate to be obtained that is more resistant to the propagation of dislocations. Due to its affinity for oxygen, interstitial nitrogen 6 facilitates the precipitation of oxygen precipitates and nitrogen precipitates. For the same initial concentration of interstitial oxygen 7 of substrate 2, the addition of interstitial nitrogen 6 enables a greater density of precipitates to be produced. Furthermore, the precipitates produced in the presence of interstitial nitrogen 6 are smaller. The interstitial nitrogen 6 content of substrate 2 is preferably between 10 and 20%. 14 atoms / cm 3 Up to 10 15 atoms / cm 3 between.

[0057] The concentration of interstitial oxygen 7 of substrate 2 is chosen to be greater than that of a substrate called "low Oi", so that said oxygen can precipitate. However, the concentration of interstitial oxygen 7 of substrate 2 is chosen to be less than that of a substrate called "high Oi", so that during precipitation a smaller density of precipitates is produced than starting from a "high Oi" substrate. Furthermore, the size of said precipitates is smaller than that of the precipitates produced in a "high Oi" substrate. Furthermore, at the end of precipitation, the concentration of residual interstitial oxygen is less than that of a "high Oi" substrate.

[0058] In this way, the substrate obtained is more resistant to the propagation of dislocations than a "low Oi" substrate. The density and size of the precipitates generate mechanical stresses less than those obtained starting from a "high Oi" substrate. The low concentration of residual interstitial oxygen makes it possible to limit the generation of thermal donors and therefore to better control the resistivity of the substrate.

[0059] In other words, the concentration of interstitial oxygen 7 of substrate 2 is between that of a "low Oi" substrate and that of a "high Oi" substrate. The concentration of interstitial oxygen 7 of substrate 2 is preferably between 15 ppma and 25 ppma.

[0060] Subsequently, preferred embodiments of the method are described. FIG. 2B to FIG. 2F , the method comprises at least the following consecutive stages:

[0061] a nucleation phase (c) to produce seeds 9 of oxygen and nitrogen precipitates within the support substrate 2,

[0062] - a stabilization phase (d) to allow the seed growth of oxygen and nitrogen precipitates 8 within the support substrate 2,

[0063] - an optional stage (e) of forming a well-rich layer 5 on the supporting substrate 2,

[0064] - a stage (a) of arranging a donor substrate for the semiconductor layer 4 to be transferred on the support substrate 2, the electrically insulating layer 3 being located at the interface between the support substrate 2 and the layer 4 to be transferred,

[0065] - Phase (b) of transferring the semiconductor layer 4 .

[0066] Nucleation phase (c) and stabilization phase (d)

[0067] In the nucleation stage (c), interstitial nitrogen 6 and interstitial oxygen 7 diffuse within the material of the substrate 2. In addition, bonds between some atoms of the semiconductor material are broken, and new bonds are formed between atoms of the semiconductor material and nitrogen, between atoms of the semiconductor material and oxygen, and between nitrogen and oxygen, thereby forming seeds 9 of oxygen precipitates and nitrogen precipitates, and obtaining a structure such as Figure 2B The structure shown.

[0068] In the stabilization phase (d), a portion of the seeds 9 of nitrogen and oxygen precipitates generated in the nucleation phase (c) will grow in the form of grains 8, while the other seeds (the smallest ones) will dissolve. The growth of the grains 8 will stabilize said grains 8, so that they will have less tendency to dissolve again under the action of subsequent treatments, in particular heat treatments. Figure 2C The structure obtained at the end of the stabilization phase (d) is shown in FIG.

[0069] The nucleation phase (c) and the stabilization phase (d) each comprise a thermal treatment, the parameters of which are fixed so as to obtain, at the end of phase (d), oxygen and nitrogen precipitates 8, whose size is between 10 nm and 50 nm, preferably greater than 40 nm, due to the presence of interstitial nitrogen 6 and interstitial oxygen 7 concentrations intermediate between "low Oi" and "high Oi". Thus, the precipitates produced by the method according to the invention are smaller than those obtained starting from a "high Oi" substrate. As mentioned above, this size range of precipitates represents a good compromise, obtaining a better resistance to dislocation propagation than a "low Oi" substrate, while observing less mechanical stress than a "high Oi" substrate.

[0070] Furthermore, the parameters of the nucleation phase (c) and the stabilization phase (d) are preferably fixed so as to produce a 7 Sediment / cm 3 Up to 10 10 Sediment / cm 3 between 10 and 15 8 Sediment / cm 3 Up to 10 9 Sediment / cm 3 The density of nitrogen precipitates and oxygen precipitates 8 is between 1 and 2, i.e. a defect density lower than that obtained starting from a "high Oi" substrate. Precipitates in this concentration range are obtained in particular by the presence of interstitial nitrogen 6 and the initial concentration of interstitial oxygen 7 of the substrate 2. As mentioned above, this concentration range of precipitates represents a good compromise, obtaining a good resistance to dislocation propagation while limiting stresses.

[0071] The nucleation phase (c) comprises, for example, applying to the support substrate 2 a heat treatment at a temperature between 650° C. and 800° C., preferably between 700° C. and 750° C., for a period of greater than one hour, preferably two hours.

[0072] The temperature of the heat treatment used in the nucleation stage (c) must be strictly less than 1000° C. This is because a temperature greater than or equal to 1000° C. will cause interstitial nitrogen 6 to diffuse excessively from substrate 2. A temperature less than 800° C. can further limit the diffusion of interstitial nitrogen 6 from substrate 2.

[0073] The stabilization phase (d) comprises, for example, a heat treatment during which a temperature greater than 900° C. and strictly less than 1000° C. is applied to the support substrate 2 for a period greater than two hours, preferably four hours.

[0074] The temperature of the heat treatment used in the stabilization stage (d) must be strictly less than 1000° C. This is because a temperature greater than or equal to 1000° C. will cause the seeds 9 of the oxygen precipitates and nitrogen precipitates generated in the nucleation stage (c) to dissolve again and the interstitial nitrogen 6 to diffuse out of the substrate 2, thereby failing to obtain the oxygen precipitates and nitrogen precipitates 8.

[0075] The temperature of the heat treatment used in the stabilization phase (d) is preferably greater than 900° C. Thus, the stabilization phase (d) enables a stable precipitate to be obtained during a heat treatment of more than one hour at a temperature of up to about 1200° C. The back-end processes to which the structure must subsequently be subjected generally exhibit a lower thermal budget, and therefore the precipitate is less likely to disappear during these subsequent processes.

[0076] Stage of forming a well-rich layer (e)

[0077] Optionally, refer to Figure 2D In stage (e), a well-rich layer 5 is formed on the support substrate 2 and is located between the support substrate 2 and the electrical insulating layer 3. As mentioned above, in radio frequency applications, the well-rich layer is particularly advantageous because it can capture charges accumulated under the electrical insulating layer 3. The well-rich layer can be made of polysilicon.

[0078] In the stage (e) of forming the well-rich layer, the support substrate 2 must not be at a temperature greater than 1200° C. for more than one or two hours. This is because, above 1200° C., the oxygen precipitates and the nitrogen precipitates 8 may redissolve and the interstitial nitrogen 6 diffuses out of the material of the support substrate 2.

[0079] The stage of forming the well-rich layer comprises, for example, chemical vapor deposition (CVD) or epitaxial deposition on a supporting substrate, with or without a seed, at a temperature that may be between 600° C. and 1100° C., depending on the technique used.

[0080] Optionally, a well-rich layer may be formed prior to the nucleation heat treatment.

[0081] This is because the above-mentioned nucleation phase (c) and stabilization phase (d) are carried out with a sufficiently low thermal budget to avoid or at least limit the recrystallization of the polysilicon of the well-rich layer 5 .

[0082] Preferably, the well-rich layer 5 is formed after the nucleation heat treatment (c), indeed even after the stabilization heat treatment (d), in order to prevent the structure of this layer from changing during these treatments.

[0083] Stage of assembling a donor substrate on a support substrate (a) and stage of transferring a semiconductor layer (b)

[0084] A stage (a) of assembling a donor substrate for the semiconductor layer 4 to be transferred is carried out on a support substrate 2, the electrically insulating layer 3 being located at the interface between the support substrate 2 and the semiconductor layer 4 to be transferred. A stage (b) of transferring the semiconductor layer 4 to be transferred is then carried out, so as to obtain a Figure 1 The multilayer structure 1 is shown.

[0085] The donor substrate for the first semiconductor layer 4 is provided in the form of a plate, for example a circular plate having the same size as the support substrate 2. The donor substrate comprises a semiconductor material, for example single-crystalline silicon.

[0086] Layer transfer can be done, for example, according to Smart Cut TM In this case, stage (a) comprises the following sub-stages:

[0087] -supply Figure 2E The donor substrate for the single-crystalline semiconductor layer 4 is shown,

[0088] - forming a weakened area in the first donor substrate to define the first semiconductor layer 4 to be transferred ( Figure 2E ),

[0089] - combining the donor substrate with the support substrate 2, with the electrically insulating layer 3 being located at the interface between the support substrate 2 and the donor substrate, thereby obtaining Figure 2F The structure shown.

[0090] Phase (b) comprises separating the donor substrate at the weakened area to transfer the semiconductor layer 4 and form Figure 1 The multilayer structure 1 is shown.

[0091] The weakened region may be produced by co-implanting helium atoms and hydrogen atoms in a donor substrate for the semiconductor layer. Alternatively, the weakened region may be produced by implanting hydrogen atoms or helium atoms alone.

[0092] Separation along the weakened area may be triggered by mechanical action, contribution of thermal energy (optionally in combination) or any other suitable method.

[0093] As Smart Cut TM In an alternative embodiment of the method, stage (a) may include bonding a donor substrate for the semiconductor layer 4 to be transferred to a supporting substrate 2, with the electrically insulating layer 3 being located at the interface, and stage (b) may include thinning the donor substrate from the side opposite to the side bonded to the supporting substrate 2 until the desired thickness of the semiconductor layer 4 is obtained.

[0094] The electrically insulating layer 3 is, for example, an oxide layer (eg, a silicon oxide layer). The electrically insulating oxide layer 3 may be formed on the support substrate 2 optionally covered with the well-rich layer 5, or on a donor substrate for the semiconductor layer 4 before combining the donor substrate with the support substrate.

[0095] In the stage (a) of assembling the donor substrate on the support substrate and the stage (b) of assembling the semiconductor layer 4 , the support substrate 2 must not be at a temperature greater than 1200° C. for more than one hour to avoid redissolution of the oxygen and nitrogen precipitates 8 .

[0096] If the multilayer structure comprises a well-rich layer 5 made of polycrystalline material, the temperature applied must not exceed 1100° C. for more than two hours in order not to cause recrystallization of said layer.

[0097] According to alternative embodiments of the method according to the invention, the nucleation phase (c) and the stabilization phase (d) can be carried out after the phase (a) of arranging the donor substrate on the support substrate 2, optionally covered with the well-rich layer 5, or after the phase (b) of transferring the semiconductor layer 4. According to each of these embodiments, each phase (a), (b), (c), (d) and (e) is also carried out as described above.

[0098] However, the phases before the nucleation phase (c) and the stabilization phase (d) must not include applying a temperature greater than or equal to 1000° C. for a period of more than about one hour to several hours. This is because a temperature greater than or equal to 1000° C. will cause the interstitial nitrogen 6 to diffuse out of the supporting substrate, so that the oxygen precipitate and the nitrogen precipitate 8 may not be formed.

[0099] According to other embodiments of the method according to the invention, the nucleation phase (c) and the stabilization phase (d) are not continuous, so that at least one of the phases (a), (b) and (e) can be placed between the nucleation phase (c) and the stabilization phase (d). According to each of these embodiments, each phase (a), (b), (c), (d) and (e) is also carried out as described above.

[0100] When stages (c) and (d) are discontinuous, the stage preceding the stabilization stage (d) must not include the application of a temperature greater than or equal to 1000° C. for a period of more than about one hour to several hours, so as not to cause diffusion of interstitial nitrogen 6 from the supporting substrate 2 and redissolution of the seeds 9 of oxygen and nitrogen precipitates produced in the nucleation stage (c).

[0101] Finally, whatever the embodiment chosen, the phase following the stabilization phase (d) must not involve the application of temperatures greater than 1200° C. for more than one hour, so as not to cause redissolution of the oxygen and nitrogen precipitates 8 .

Claims

1. A method for producing a multilayer structure (1) of the semiconductor-on-insulator type, said method The following phases are included: (a) assembling a support substrate (2) made of semiconductor material and a donor substrate for the semiconductor layer (4) to be transferred, the support substrate (2) having a resistivity greater than or equal to 500 Ω.cm and containing interstitial nitrogen (6) and interstitial oxygen (7), the initial concentration of interstitial oxygen (6) in the support substrate (2) being between 15 old ppma and 25 old ppma (measured according to standard ASTM 79), an electrically insulating layer (3) being located at the interface between the support substrate (2) and the donor substrate, (b) transferring the semiconductor layer (4) onto a supporting substrate, The method further comprises a nucleation phase (c) comprising a thermal treatment for precipitating at least part of the interstitial oxygen (7) and at least part of the interstitial nitrogen (6) in a controlled manner, thereby forming seeds (9) of oxygen and nitrogen precipitates (8), and a stabilization phase (d) comprising a thermal treatment for growing the seeds of oxygen and nitrogen precipitates to a size between 10 nm and 50 nm.

2. The method according to claim 1, before the assembly stage (a), the method further comprises forming a well-rich layer (5) on the support substrate (2), wherein the well-rich layer (5) is arranged between the support substrate (2) and the electrical insulation layer (3).

3. The method according to claim 2, in, The formation of the well-rich layer (3) comprises depositing a polysilicon layer on a supporting substrate.

4. The method according to claim 3, in, The deposition of the polysilicon layer is carried out after a stabilization phase (d) of the oxygen and nitrogen precipitates (8).

5. The method according to any one of claims 1 to 4, It is characterized in that The initial concentration of interstitial nitrogen (6) in the support substrate (2) is 10 14 atoms / cm 3 Up to 10 15 atoms / cm 3 between.

6. The method according to any one of claims 1 to 5, in, At the end of the stabilization phase (d), the support substrate (2) contains oxygen precipitates and nitrogen precipitates (8) at a concentration of 10 7 cm -3 Up to 10 10 cm -3 The concentration is preferably between 10 8 cm -3 Up to 10 9 cm -3 between.

7. The method according to any one of claims 1 to 6, It is characterized in that The nucleation phase (c) and the stabilization phase (d) each comprise a heat treatment, the temperature applied in the nucleation heat treatment (c) being lower than the temperature applied in the stabilization heat treatment (d), and the duration of the nucleation heat treatment (c) being shorter than the duration of the stabilization heat treatment (d).

8. The method according to any one of claims 1 to 7, in, The nucleation phase (c) comprises applying a temperature between 650°C and 800°C, preferably between 700°C and 750°C, for a period of greater than one hour, preferably two hours.

9. The method according to any one of claims 1 to 8, in, The stabilization phase (d) comprises applying a temperature greater than 900° C., preferably 950° C., for a period of greater than two hours, preferably four hours.

10. The method according to any one of claims 1 to 9, in, Prior to the assembly phase (a), the nucleation phase (c) and the stabilization phase (d) are carried out directly one after the other.

11. A multilayer structure of the semiconductor-on-insulator type, comprising, from its back side to its front side, a supporting substrate (2), an electrically insulating layer (3) and a semiconductor layer (4), It is characterized in that The support substrate (2) is made of a semiconductor material and has a resistivity greater than or equal to 500 Ω.cm and contains a concentration of 10 7 cm -3 Up to 10 10 cm -3 The oxygen precipitates and nitrogen precipitates (8) are between 10 nm and 50 nm in size.

12. The structure according to claim 11, further comprising a well-rich layer (5), the well-rich layer (5) being located between the supporting substrate (2) and the electrically insulating layer (3).

13. The structure according to any one of claims 11 and 12, It is characterized in that The residual concentration of interstitial oxygen (7) in the support substrate (2) is less than 15 ppma, preferably less than 12 ppma (measured according to standard ASTM 79).