Construction method of hollow sphere catalyst and application of hollow sphere catalyst in Fenton degradation of water pollutants

Through the construction method of hollow sphere catalyst, a hollow sphere catalyst with a large specific surface area is prepared by reacting styrene monomer and iron salt. Combined with the Fenton reaction, the problems of high antibiotic degradation cost and narrow application range in the existing technology are solved. Efficient, non-toxic antibiotic degradation effect is achieved.

CN118743993AInactive Publication Date: 2024-10-08HUNAN DEEYA ENVIRONMENTAL ENG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410778506.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the process of antibiotic degradation in wastewater, the existing technology has the problems of high catalyst cost, complex treatment process, and narrow application range, making it difficult to effectively degrade a variety of antibiotics.

Method used

Using the hollow sphere catalyst construction method, a hollow sphere catalyst with a large specific surface area and porous structure is prepared through the reaction of styrene monomer and iron salt, and reacts with hydrogen peroxide in the Fenton reaction to generate highly active OH, which is highly efficient. Oxidative degradation of antibiotics.

Benefits of technology

It achieves efficient degradation of a variety of antibiotics at room temperature, and the degradation products are non-toxic and harmless, reducing the leaching of catalyst metal ions, reducing treatment costs, and is suitable for wastewater treatment of tetracycline antibiotics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743993A_ABST
    Figure CN118743993A_ABST
Patent Text Reader

Abstract

The invention discloses a construction method of a hollow sphere catalyst, which comprises the following steps: 1) preparing a polystyrene colloidal dispersion liquid containing polystyrene microspheres by taking a styrene monomer as a raw material; and 2) adding an iron salt solution into the polystyrene colloidal dispersion liquid containing the polystyrene microspheres for reaction, then adding an alkaline solution for continuous reaction, performing solid-liquid separation after the reaction is completed, and calcining the obtained solid to obtain the hollow sphere catalyst. The prepared hollow sphere catalyst is large in specific surface area, the porous shell layer can serve as a substance transmission channel of the inner shell layer and the outer shell layer, the inner cavity of the hollow microsphere can serve as a reaction container, after the hollow sphere catalyst is applied to treatment of antibiotic-containing wastewater, the hydrogen peroxide decomposition rate can be increased, the antibiotic oxidative degradation rate is further increased, and the treatment effect is good. The production cost and the operation difficulty are reduced, and the catalyst can be repeatedly used and has a very good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sewage treatment, and in particular to a construction method of a hollow sphere catalyst and application thereof in Fenton degradation of water pollutants. Background Art

[0002] With the development of industrialization, environmental pollution caused by the discharge of toxic and harmful substances into water has become a major problem affecting the ecological environment. Various toxic and harmful pollutants are widely present in incompletely treated wastewater, such as industrial dyes, pharmaceuticals and agricultural chemicals. Among them, antibiotic residues may lead to the emergence of drug-resistant bacteria or cause endocrine disorders in humans. The treatment of antibiotics in wastewater has always been a difficult and key research topic.

[0003] A Chinese patent with publication number CN106698652B mentions a method for removing antibiotic resistance genes in sewage. The method adopts a combined process of biological treatment and membrane technology, organically couples biological treatment, membrane technology and the adsorption and interception of pollutants on the membrane surface, determines and optimizes the regulation and operation parameters of the membrane bioreactor biological process, and determines the optimal concentration of organic pollutants on the membrane surface for enhanced removal of antibiotic resistance genes in sewage, so that the removal of antibiotic resistance genes in sewage has achieved better results. However, its treatment process is complicated, and the equipment cost and production cost are high.

[0004] In addition, in the prior art, the Fenton reaction is also adopted to generate highly active OH by decomposing hydrogen peroxide through a catalyst to oxidize and degrade antibiotics in wastewater. In the traditional Fenton reaction process, FeSO4 is mostly used as a catalyst. This catalyst is a disposable agent. After the reaction, the wastewater is acidic, and hydrolysis generates a large amount of dangerous iron-containing sludge, which is wasteful and easy to cause secondary environmental problems. Subsequent treatment is cumbersome. The Chinese patent with application number CN201910401624.7 discloses a photo-Fenton oxidation catalyst and its preparation method and application. It uses urban sewage sludge as a carrier, and uses HCl, H2SO4, HNO3, H3PO4 and other acids for surface chemical modification, supplemented by ultrasonic or microwave physical modification, to prepare an efficient photo-Fenton oxidation catalyst, which has a good removal rate for ciprofloxacin under photo-Fenton conditions. However, it is found in actual use that its application range is narrow and it is difficult to meet the degradation needs of multiple antibiotics. Therefore, it is urgent to develop more types of sewage treatment catalysts that are conducive to antibiotic degradation. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a method for constructing a hollow sphere catalyst, so as to provide a catalyst that is beneficial to the degradation of multiple antibiotics in wastewater, further reduce the difficulty and cost of antibiotic degradation in wastewater, and improve the antibiotic degradation rate.

[0006] The second technical problem solved by the present invention is to provide the application of the hollow sphere catalyst in Fenton degradation of water pollutants.

[0007] The third technical problem solved by the present invention is to provide a method for treating antibiotic-containing wastewater.

[0008] The technical problem solved by the present invention is achieved by adopting the following technical solutions:

[0009] A method for constructing a hollow sphere catalyst comprises the following steps:

[0010] 1) using styrene monomer as a raw material, adding an initiator at 40 to 90° C. to prepare a polystyrene colloidal dispersion containing polystyrene microspheres;

[0011] 2) adding an iron salt solution to the dispersion to react, then adding an ammonia solution to continue the reaction, separating the solid and the liquid after the reaction is completed, and calcining the obtained solid to obtain a hollow sphere catalyst.

[0012] Furthermore, in step 1), the method for preparing the dispersion comprises:

[0013] Pretreatment: Add water to styrene monomer at room temperature to disperse it, introduce nitrogen for 0.5 to 1 hour, then keep stirring and heat to 40 to 90°C;

[0014] Polymerization reaction: adding an initiator solution to the pretreated solution to polymerize the styrene monomer, and obtaining the dispersion after the reaction is completed; during the polymerization reaction, the temperature is maintained at 40 to 90° C., and the reaction time is 5 to 24 hours.

[0015] Furthermore, the initiator is persulfate. The mass ratio of styrene monomer to initiator is 5-10:0.1-0.5.

[0016] Furthermore, the persulfate is preferably potassium persulfate.

[0017] Furthermore, step 2) specifically includes the following steps:

[0018] S1, dilute the dispersion and heat it to 50-90° C., then add an iron salt solution and react for 2-10 hours; the iron salt solution in this step is an iron salt soluble in water, such as iron nitrate, iron sulfate, iron chloride, etc.;

[0019] S2. Slowly add alkaline solution, keep warm at 50-90°C for 2-10 hours, cool and separate the solid and liquid to obtain a solid, wash the solid and calcine it.

[0020] Further, in step S1: the mass fraction of the polystyrene microspheres in the dispersion is 1-10%, the concentration of the iron salt solution is 0.02-0.1 mol / L; the volume ratio of the mass of the polystyrene microspheres in the polystyrene colloidal dispersion to the iron salt solution is 0.1-1 g: 10-50 mL;

[0021] Furthermore, in step S2, the alkaline solution is an ammonia solution, and the volume fraction of the ammonia solution is 0.1-5%. Less preferably, the alkaline solution is hexamethylenetetramine.

[0022] Furthermore, in step S2, calcination is carried out at 200-600°C, air is introduced during the calcination process, and the temperature is increased at a rate of 0.25-1°C / min. The calcination time is 1.5-2.5h, and a hollow sphere catalyst is obtained after the calcination is completed.

[0023] A hollow sphere catalyst is prepared by the method as described above, wherein the particle size of the hollow sphere catalyst is in the range of 70-600nm, the average pore size is 7-15nm, and the specific surface area is 50-150m 2 / g.

[0024] The hollow sphere catalyst is used in Fenton degradation of water pollutants.

[0025] A method for treating antibiotic-containing wastewater adopts the hollow ball catalyst as described above, and the treatment method comprises: mixing wastewater and the hollow ball catalyst, adding an appropriate amount of hydrogen peroxide, fully stirring at room temperature, and reacting for 3 to 5 hours; the mass fraction of the hydrogen peroxide is 25 to 35%, and the volume ratio of the hydrogen peroxide to the wastewater is 1 to 3:100; the ratio of the mass of the catalyst to the volume of the wastewater is 40 to 60 mg:100 mL.

[0026] Furthermore, the pH value range of the wastewater needs to be adjusted to 5.0-7.0 before treatment; the antibiotic content in the wastewater is ≤50 mg / L.

[0027] The technical solution of the present invention is particularly suitable for the treatment of wastewater containing tetracycline antibiotics, which include oxytetracycline, chlortetracycline, demeclocycline, doxycycline, minocycline, and methenomycin.

[0028] Beneficial effects: The method for constructing the hollow sphere catalyst described in the present invention adopts the method of first constructing polystyrene microspheres and then loading iron salts. The prepared hollow sphere catalyst has a large specific surface area, the porous shell layer can be used as a material transmission channel for the inner and outer shell layers, and the internal cavity of the hollow microsphere can be used as a reaction container. The large specific surface area can effectively increase the active surface area of ​​the catalysis, and has a good application prospect.

[0029] The sewage treatment method of the present invention can be carried out at room temperature and near-neutral pH environment, without complicated processes, and reduces the leaching of catalyst metal ions. The present invention uses a unique hollow ball catalyst to increase the rate of decomposing hydrogen peroxide, efficiently generate OH, and further oxidize and degrade antibiotics, and the degradation products are water and CO2, which are non-toxic and harmless. In addition, the hollow ball catalyst of the present invention is easy to separate from the liquid phase reaction system and can be recycled and reused, further reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the SEM image of the hollow sphere catalyst obtained in Example 1.

[0031] Figure 2 This is a SEM image of commercially available ordinary iron oxide nanoparticles.

[0032] Figure 3 a is the graph of tetracycline UV-visible response curve and standard curve; Figure 3 b is the standard curve of tetracycline at 355 nm.

[0033] Figure 4 Effect of different hollow sphere catalyst dosage on the degradation of tetracycline in sewage

[0034] Figure 5 The figure is a comparison of the wastewater degradation effects of the hollow sphere catalyst of the present invention and commercially available common iron oxide nanoparticles in different time periods.

[0035] Figure 6 The figure shows the effects of hollow sphere carriers with different particle sizes and commercially available nano iron oxide particles on tetracycline and COD. DETAILED DESCRIPTION

[0036] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.

[0037] Example 1

[0038] 1) Using styrene monomer as raw material, preparing a polystyrene colloidal dispersion containing polystyrene microspheres:

[0039] Pretreatment: Weigh 6.0408 g of styrene monomer, add enough water to disperse styrene; introduce nitrogen at room temperature, keep stirring for 0.5 h, and then raise the temperature to 70°C;

[0040] Polymerization reaction: Weigh 0.1073 g of potassium persulfate as an initiator and dissolve it in water; add the initiator solution to the pretreated styrene monomer and react at 70° C. for 5 hours until the reaction is complete. After the reaction is completed, a polystyrene colloidal dispersion containing polystyrene microspheres with a particle size of about 280 nm is obtained.

[0041] The polystyrene colloidal dispersion containing polystyrene microspheres is cooled to room temperature, and then, after centrifugation and washing, the obtained solid is ultrasonically dispersed in water again, and the mass fraction of the polystyrene microspheres in the polystyrene colloidal dispersion is adjusted to 4.82%; and the mixture is set aside.

[0042] 2) Preparation of hollow sphere catalyst:

[0043] S1, taking the polystyrene colloidal dispersion containing polystyrene microspheres; the polystyrene microsphere content in the polystyrene colloidal dispersion is 0.5027g; adding 25ml of deionized water, stirring and heating to 60°C; then adding 20mL of 0.05mol / L ferric nitrate solution, and keeping the reaction at 60°C for 2h;

[0044] S2. Disperse 200 μL of aqueous ammonia in 20 mL of water for standby use; slowly add aqueous ammonia solution to the system after the reaction in step 1), continue to keep warm at 60°C for 3 hours, cool naturally and obtain a solid by centrifugation, wash and dry the solid, and then calcine in air at 500°C at 1°C / min for 2 hours to obtain a Fe2O3 hollow sphere catalyst.

[0045] The results are as follows Figure 1 As shown, Figure 1 The electron microscope image of the hollow sphere catalyst obtained according to the above method shows that the particles are uniformly spherical. Figure 2 This is an electron microscope image of commercially available iron oxide nanoparticles, which have different particle sizes and uneven distribution.

[0046] Example 2

[0047] The hollow sphere catalyst described in this embodiment is prepared as follows:

[0048] 1) Using styrene monomer as raw material, preparing a polystyrene colloidal dispersion containing polystyrene microspheres:

[0049] Pretreatment: Weigh 7.0512 g of styrene monomer, add enough water to disperse styrene; introduce nitrogen at room temperature, keep stirring for 1 hour, and then heat to 90°C;

[0050] Polymerization reaction: Weigh 0.2010g of potassium persulfate as an initiator and dissolve it in water; add the initiator solution to the pretreated styrene monomer, react at 90°C for 24h until the reaction is complete, and after the reaction is completed, a polystyrene colloidal dispersion containing polystyrene microspheres with a particle size of about 380nm is obtained.

[0051] The polystyrene colloidal dispersion containing polystyrene microspheres is cooled to room temperature, and then after centrifugation and washing, the obtained solid is ultrasonically dispersed in water again, and the mass fraction of the polystyrene microspheres in the polystyrene colloidal dispersion is adjusted to 4.39%; and the mixture is set aside.

[0052] 2) Preparation of hollow sphere catalyst:

[0053] S1, taking the polystyrene colloidal dispersion containing polystyrene microspheres; the polystyrene microsphere content in the polystyrene colloidal dispersion is 0.9011 g; adding 100 mL of deionized water, stirring and heating to 50° C.; then adding 15 mL of 0.1 mol / L ferric chloride solution, and keeping the reaction at 90° C. for 5 hours;

[0054] S2. Disperse 500 μL of aqueous ammonia in 70 mL of water for standby use; slowly add aqueous ammonia solution to the system after the reaction in step 1), continue to keep warm at 90°C for 10 hours, cool naturally and obtain a solid by centrifugation, wash and dry the solid, and then calcine in air at 600°C at 0.5°C / min for 1.5 hours to obtain a Fe2O3 hollow sphere catalyst.

[0055] Example 3

[0056] The hollow sphere catalyst described in this embodiment is prepared as follows:

[0057] 1) Using styrene monomer as raw material, preparing a polystyrene colloidal dispersion containing polystyrene microspheres:

[0058] Pretreatment: Weigh 9.0186 g of styrene monomer, add enough water to disperse styrene; introduce nitrogen at room temperature, keep stirring for 1 hour, and then raise the temperature to 40°C;

[0059] Polymerization reaction: Weigh 0.4041 g of sodium persulfate as an initiator and dissolve it in water; add the initiator solution to the pretreated styrene monomer and react at 40° C. for 12 hours until the reaction is complete. After the reaction is completed, a polystyrene colloidal dispersion containing polystyrene microspheres with a particle size of about 442 nm is obtained.

[0060] The polystyrene colloidal dispersion containing polystyrene microspheres is cooled to room temperature, and then, after centrifugation and washing, the obtained solid is ultrasonically dispersed in water again, and the mass fraction of the polystyrene microspheres in the polystyrene colloidal dispersion is adjusted to 7.78%; and the mixture is set aside.

[0061] 2) Preparation of hollow sphere catalyst:

[0062] S1, taking the polystyrene colloidal dispersion containing polystyrene microspheres; the polystyrene microsphere content in the polystyrene colloidal dispersion is 0.7059 g; adding 50 mL of deionized water, stirring and heating to 90° C.; then adding 50 mL of 0.02 mol / L ferric sulfate solution, and keeping the reaction at 50° C. for 10 hours;

[0063] S2. Disperse 300 μL of aqueous ammonia in 50 mL of water for standby use; slowly add aqueous ammonia solution to the system after the reaction in step 1), continue to keep warm at 80°C for 5 hours, cool naturally and obtain a solid by centrifugation, wash and dry the solid, and then calcine at 350°C in air at 0.25°C / min for 2.5 hours to obtain a Fe2O3 hollow sphere catalyst.

[0064] Comparative Example 1

[0065] The hollow sphere catalyst described in this comparative example is prepared as follows:

[0066] Using styrene monomer as raw material, a polystyrene colloidal dispersion containing polystyrene microspheres is prepared:

[0067] Pretreatment: Weigh 7.8567 g of styrene monomer, add enough water to disperse the styrene; introduce nitrogen at room temperature and keep stirring for 0.5 h;

[0068] Polymerization reaction: Weigh 0.1103g potassium persulfate as an initiator and dissolve it in water; add the initiator solution to the pretreated styrene monomer and react at room temperature. It was found that the reaction could not occur at room temperature and the polystyrene colloidal dispersion containing polystyrene microspheres could not be obtained. This shows that the control of the reaction temperature is more critical.

[0069] Comparative Example 2

[0070] The hollow sphere catalyst described in this comparative example is prepared as follows:

[0071] Using styrene monomer as raw material, a polystyrene colloidal dispersion containing polystyrene microspheres is prepared:

[0072] Pretreatment: Weigh 15.0215 g of styrene monomer, add enough water to disperse the styrene; introduce nitrogen at room temperature, keep stirring for 0.5 h, and then raise the temperature to 70°C;

[0073] Polymerization reaction: Weigh 0.1073g potassium persulfate as an initiator and dissolve it in water; add the initiator solution to the pretreated styrene monomer and react at 70°C for 5 hours until the reaction is complete. After the reaction is completed, a polystyrene colloidal dispersion containing polystyrene microspheres is obtained. The particle size is about 800nm ​​as determined by electron microscopy. In this control example, due to improper control of the proportion of the styrene monomer raw material, the particle size is large and the effect is not ideal.

[0074] Comparative Example 3

[0075] The hollow sphere catalyst described in this comparative example is prepared as follows:

[0076] Using styrene monomer as raw material, a polystyrene colloidal dispersion containing polystyrene microspheres is prepared:

[0077] Pretreatment: Weigh 5.4739 g of styrene monomer, add enough water to disperse styrene; introduce nitrogen at room temperature, keep stirring for 0.5 h, and then raise the temperature to 70°C;

[0078] Polymerization reaction: Weigh 1.3206g potassium persulfate as an initiator and dissolve it in water; add the initiator to the pretreated styrene monomer and react at 70°C for 5h until the reaction is complete. After the reaction is completed, block polystyrene is obtained. In this control example, due to excessive addition of initiator, hollow spherical polystyrene particles cannot be formed, and subsequent experiments cannot be carried out.

[0079] Comparative Example 4

[0080] In this embodiment, the catalyst is iron oxide nanoparticles without any treatment.

[0081] (A) Verify the effect of different feed amounts of hollow sphere catalyst on the degradation rate of tetracycline.

[0082] A method for treating sewage containing antibiotics comprises the following steps:

[0083] 10 mg, 15 mg, 5 mg of the hollow sphere catalyst obtained in Example 1 and 20 mL of 50 mg / L tetracycline solution were added to a glass vial, mixed evenly, and then 0.4 mL of 30% H2O2 solution was added and reacted at room temperature for 3 hours.

[0084] For comparison, 10 mg of the hollow sphere catalyst obtained in Example 1 and 20 mL of a 50 mg / L tetracycline solution were added to a glass vial, mixed evenly, and then 0.8 mL of a 30% H2O2 solution was added and reacted at room temperature for 3 hours.

[0085] After the reaction is completed, the reaction solution and the catalyst are transferred to a centrifuge tube for centrifugation, and the supernatant is taken into a cuvette and measured at 355 nm using a UV-visible spectrophotometer. The concentration is calculated using the Lambert-Beer law, and the degradation rate is used to evaluate the effect.

[0086] The calculation method is as follows:

[0087] Lambert-Beer Law: A = Kbc (A is absorbance; K is the molar absorption coefficient, which is related to the properties of the absorbing substance and the wavelength of the incident light; b is the thickness of the absorption layer, which is related to the cuvette; c is the concentration of the absorbing substance)

[0088] (c0 is the initial concentration, c is the concentration at the end of the reaction)

[0089] The results are as follows Figure 3-4 shown.

[0090] in Figure 3 a is the graph of tetracycline UV-visible response curve and standard curve; Figure 3 b is the standard curve of tetracycline at 355 nm.

[0091] Figure 4 The effect of different feed amounts on the wastewater degradation effect. It can be seen that the ratio of hollow ball catalyst to hydrogen peroxide is more critical. When the hollow ball catalyst feed amount is insufficient, the degradation effect is not ideal. When the ratio of hollow ball catalyst to hydrogen peroxide reaches a certain range, the degradation rate is guaranteed. On this basis, continuing to increase the feed amount of hollow ball catalyst will reduce the degradation rate.

[0092] (ii) verifying the effects of the hollow sphere catalyst of the present invention and commercially available nano iron oxide particles on the degradation rate of tetracycline.

[0093] A method for treating sewage containing antibiotics comprises the following steps:

[0094] 10 mg of the hollow sphere catalyst obtained in Example 1 and 10 mg of the iron oxide nanoparticles described in Control Example 4 were added to a glass vial with 20 mL of a 50 mg / L tetracycline solution, mixed evenly, and then 0.4 mL of a 30% H2O2 solution was added and reacted at room temperature for 3 hours.

[0095] After the reaction is completed, the reaction solution and the catalyst are transferred to a centrifuge tube for centrifugation, and the supernatant is taken into a cuvette and measured at 355 nm using a UV-visible spectrophotometer. The concentration is calculated using the Lambert-Beer law, and the degradation rate is used to evaluate the effect.

[0096] The results are as follows Figure 5 As shown, it can be seen that compared with the commercially available nano iron oxide particles, the hollow sphere catalyst of the present invention has a better degradation effect on tetracycline in sewage over time.

[0097] Figure 5The comparison of wastewater degradation using 10 mg of the hollow sphere catalyst described in Example 1 and 10 mg of the commercially available common iron oxide nanoparticles described in Control Example 4 shows that the hollow sphere catalyst described in the present invention is better than the commercially available common iron oxide nanoparticles in degradation of antibiotics in wastewater.

[0098] (III) Verify the effect of hollow sphere carriers with different particle sizes and commercially available nano iron oxide particles on the degradation rate of tetracycline.

[0099] A method for treating sewage containing antibiotics comprises the following steps:

[0100] 10 mg of the hollow sphere catalyst obtained in Example 1 (particle size of about 280 nm), 10 mg of the hollow sphere catalyst obtained in Example 2 (particle size of about 380 nm), 10 mg of the hollow sphere catalyst obtained in Example 3 (particle size of about 442 nm), and 10 mg of the commercially available iron oxide nanoparticles described in Control Example 4 were added into glass vials respectively with 20 mL of 50 mg / L tetracycline solution, mixed evenly, then 0.4 mL of 30% H2O2 solution was added, and the mixture was reacted at room temperature for 3 hours.

[0101] After the reaction is completed, the reaction solution and the catalyst are transferred to a centrifuge tube for centrifugation, and the supernatant is taken into a cuvette and measured at 355 nm using a UV-visible spectrophotometer. The concentration is calculated using the Lambert-Beer law, and the degradation rate is used to evaluate the effect.

[0102] The results are as follows Figure 6 As shown in the shaded part, it can be seen that compared with the commercially available nano iron oxide particles, the hollow sphere catalyst of the present invention has a better degradation effect on tetracycline in sewage over time.

[0103] According to HJ 828-2017 "Determination of Chemical Oxygen Demand of Water Quality-Dichromate Method", the COD value of the solution after the reaction was tested.

[0104] The results are as follows Figure 6 As shown in the solid part in the middle, the hollow sphere catalyst within the particle size range of the present invention has a good degradation effect on COD and tetracycline in sewage, which is far superior to commercially available iron oxide nanoparticles.

[0105] It should be noted that the hollow sphere catalyst described in the present invention has a good degradation effect on tetracycline antibiotics such as oxytetracycline, chlortetracycline, demeclocycline, doxycycline, minocycline, and methacycline.

[0106] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for constructing a hollow sphere catalyst, It is characterized in that The steps include: 1) using styrene monomer as a raw material, adding an initiator at 40 to 90° C. to prepare a polystyrene colloidal dispersion containing polystyrene microspheres; 2) adding an iron salt solution to the dispersion to react, then adding an alkaline solution to continue the reaction, separating the solid and the liquid after the reaction is completed, and calcining the obtained solid to obtain a hollow sphere catalyst.

2. The method for constructing the hollow sphere catalyst according to claim 1, It is characterized in that In step 1), the preparation method of the dispersion comprises: Pretreatment: Add water to styrene monomer at room temperature to disperse it, introduce nitrogen for 0.5 to 1 hour, then keep stirring and heat to 40 to 90°C; Polymerization reaction: adding an initiator solution to the pretreated solution to polymerize the styrene monomer, and obtaining a polystyrene colloidal dispersion containing polystyrene microspheres after the reaction is completed; during the polymerization reaction, the temperature is maintained at 40 to 90° C., and the reaction time is 5 to 24 hours.

3. The method for constructing the hollow sphere catalyst according to claim 2, It is characterized in that The initiator is persulfate; the mass ratio of styrene monomer to initiator is 5-10:0.1-0.

5.

4. The method for constructing the hollow sphere catalyst according to claim 1, It is characterized in that Step 2) includes: S1, dilute the dispersion and heat it to 50-90° C., then add the iron salt solution and react for 2-10 hours; S2. Slowly add alkaline solution, keep warm at 50-90°C for 2-10 hours, cool and separate the solid and liquid to obtain a solid, wash the solid and calcine it.

5. The method for constructing the hollow sphere catalyst according to claim 4, It is characterized in that In step S1, the mass fraction of the polystyrene microspheres in the dispersion is 1-10%, and the concentration of the iron salt solution is 0.02-0.1 mol / L; the volume ratio of the mass of the polystyrene microspheres in the dispersion to the iron salt solution is 0.1-1 g:10-50 ml; in step S2, the alkaline solution is an ammonia solution, and the volume fraction of the ammonia solution is 0.1-5%.

6. The method for constructing the hollow sphere catalyst according to claim 4, It is characterized in that In step S2, calcination is carried out at 200-600°C, air is introduced during the calcination, and the temperature is increased at a rate of 0.25-1°C / min. The calcination time is 1.5-2.5h. After the calcination is completed, a hollow sphere catalyst is obtained.

7. A hollow sphere catalyst, It is characterized in that The hollow sphere catalyst is prepared by the method described in any one of claims 1 to 6, wherein the particle size range of the hollow sphere catalyst is 70-600 nm, the average pore size is 7-15 nm, and the specific surface area is 50-150 m 2 / g.

8. Use of the hollow sphere catalyst as claimed in claim 7 in Fenton degradation of water pollutants.

9. A method for treating sewage containing antibiotics, It is characterized in that The hollow ball catalyst as claimed in claim 7 is used, and the treatment method comprises: mixing wastewater and the hollow ball catalyst, adding an appropriate amount of hydrogen peroxide, stirring fully at room temperature, and reacting for 3 to 5 hours; the mass fraction of the hydrogen peroxide is 25 to 35%, and the volume ratio of the hydrogen peroxide to the wastewater is 1 to 3:100; the ratio of the mass of the catalyst to the volume of the wastewater is 40 to 60 mg:100 mL.

10. The method for treating antibiotic-containing wastewater according to claim 9, It is characterized in that The pH value must be adjusted to 5.0-7.0 before wastewater treatment; the antibiotic content in the wastewater should be ≤50mg / L.

Citation Information

Patent Citations

  • Method for producing size-controllable magnetic hollow spheres

    CN101444712A

  • Method for preparing monocrystal Fe2O3 nano particle self-assembled loosened spherical nano structure

    CN109112611A

  • Hollow cerium dioxide microsphere supported ferrihydrite heterogeneous Fenton-like catalyst and preparation method and application thereof

    CN110252316A

  • Nano iron oxide material and preparation method and application thereof

    CN110961107A