Modified carbon-based calcium-iron layered double-metal hydroxide catalyst as well as preparation and application thereof

By loading a modified catalyst of calcium-iron layered double metal hydroxide on activated carbon fibers and using a non-radical oxidation pathway to activate PMS, the problem of efficient removal of sulfamethoxazole in antibiotic wastewater is solved, achieving high efficiency, economy and environmental protection. Degradation effect and avoid contamination caused by dissolution of metal ions.

CN118743994AActive Publication Date: 2024-10-08NANJING TECH UNIV

Patent Information

Application Number
CN202410772737.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-08
Estimated Expiration
2044-06-17

AI Technical Summary

Technical Problem

Existing technologies are difficult to efficiently and economically remove sulfamethoxazole in antibiotic wastewater, and traditional advanced oxidation methods have secondary pollution problems caused by dissolution of metal ions. The application of non-radical reaction technology in complex wastewater is limited.

Method used

Develop a modified carbon-based calcium iron layered double metal hydroxide catalyst (CaFe-LDH/ACF), which is prepared by loading calcium iron layered double metal hydroxide on activated carbon fibers using hydrothermal and ion exchange methods. , a non-radical oxidative pathway combining singlet oxygen and electron transfer to activate persulfate (PMS) for the degradation of sulfamethoxazole.

Benefits of technology

It achieves efficient and selective oxidative degradation of sulfamethoxazole under a wide range of pH conditions. The catalyst is green and environmentally friendly, has high economic benefits, and avoids secondary pollution caused by dissolution of metal ions. The catalyst can be recycled and reused.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a modified carbon-based calcium-iron layered double-metal hydroxide catalyst and preparation and application thereof, and is characterized in that the catalyst is composed of a carrier and layered double-metal hydroxide, the carrier is activated carbon fiber ACF, and the layered double-metal hydroxide is calcium-iron layered double-metal hydroxide; wherein the loading mass percentage of the Ca element is 2.26-5.16%, and the molar ratio of Ca < 2 + > to Fe < 3 + > is (2-5): 1; the total specific surface area of the catalyst is 1000-1600m < 2 >. G <-1 >; the pore volume is 0.60 to 0.90 cm < 3 >. G <-1 >; and the average pore size is 1-3nm. The catalyst can efficiently activate SMX in PMS selective oxidation wastewater under the wide pH condition, and is high in degradation rate, convenient to recycle and high in repeated utilization rate and economic benefit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a modified carbon-based calcium iron layered double metal hydroxide catalyst and preparation and application thereof, belonging to the field of antibiotic wastewater treatment technology and novel catalytic materials and preparation thereof, and is specifically applied to activated PMS and selectively oxidizing SMX in antibiotic wastewater. Background Art

[0002] Sulfamethoxazole (SMX) is the most commonly used broad-spectrum antibacterial drug among sulfonamide antibiotics. It has the advantages of strong hydrophilicity, low cost and a wide antibacterial spectrum. Due to its certain antibacterial effect on a variety of pathogens, the demand for sulfamethoxazole in daily life has gradually increased. As one of the most commonly used antibiotics, sulfamethoxazole residues in the water environment pose a great threat to the health of humans and other animals and plants. Long-term accumulation in the human body may cause renal damage, drug resistance, carcinogenicity and mutagenicity, which is extremely harmful. Therefore, the development of efficient treatment technology for removing residual sulfamethoxazole in water has gradually become the focus of attention.

[0003] Sulfadimethoxazole is a difficult-to-degrade substance. At present, the main treatment technologies for sulfadimethoxazole include biological method, physicochemical method, advanced oxidation technology and the combination of the above methods. The research results show that the adsorption process of sulfadimethoxazole by activated sludge in secondary biological treatment is the main way to remove sulfadimethoxazole in the whole treatment process. Therefore, if the traditional sewage treatment process and the sludge are not treated with the corresponding deep treatment process after discharge, the residual sulfadimethoxazole will be discharged into the water body and soil environment with the effluent and residual sludge of the sewage treatment plant, resulting in serious antibiotic pollution of surface water, groundwater and farmland soil environment. After biological treatment, the biochemical indicators of many antibiotic wastewaters can basically meet the standards, but there are still a certain amount of difficult-to-degrade antibiotics and their products remaining in them, which poses a potential threat to the safety of water ecology; while the physicochemical method, especially the advanced oxidation treatment method, can effectively reduce the low-concentration sulfadimethoxine antibiotics remaining in the water body. The efficiency and time of the physicochemical method are greatly improved compared with the biological method, but the biggest disadvantage of the physicochemical method is that the treatment cost is relatively high. In recent years, advanced oxidation methods based on sulfate free radicals are also commonly used for the degradation of sulfamethoxazole. Sulfate free radicals can be obtained by catalyzing peroxymonosulfate (PMS) through thermal activation, alkali activation, ultrasound activation, transition metal ion activation, etc. In a homogeneous system, sulfate free radicals can be obtained by catalyzing peroxymonosulfate (PMS) through transition metal ions (Co 2+ , Mn 2+ , Fe 2+etc.) to activate persulfate; in heterogeneous systems, there are various heterogeneous catalysts such as zero-valent iron, single metal oxides, composite metal oxides, supported metal materials and metal-free carbon materials; external energy fields (light, sound, electricity, heat) can also directly activate persulfate or assist in improving reaction efficiency. The use of transition metal activation is simple to operate and has high economic benefits, but it will dissolve a large amount of metal ions and cause secondary pollution, which limits the widespread application of PMS in water treatment. Therefore, the development of new, efficient and economical physicochemical or combined treatment technologies is an effective way to achieve effective degradation of sulfamethoxazole wastewater and reduce environmental safety risks.

[0004] Compared with traditional advanced oxidation technologies, oxidation technologies based on non-radical reactions have mild oxidation ability, high selectivity, and are not easily affected by environmental matrices. They have great potential in water treatment. The non-radical reactions with relatively mild oxidation ability found in persulfate activation systems are conducive to the rapid mineralization of organic pollutants in natural water bodies and actual wastewater matrices. The non-radical reaction mechanisms in the persulfate activation and oxidation of organic pollutants mainly include: (1) the formation of surface-activated complexes (or surface-confined free radicals); (2) the promotion of electron transfer; (3) the generation of singlet oxygen ( 1 O2). This type of non-radical reaction pathway is mainly found in the persulfate activation system of carbon-based materials. Carbon materials with high specific surface area, good conductivity and stable chemical properties are usually used as catalyst carrier materials, but studies have found that carbon materials themselves or carbon materials that have been surface-modified and doped with heteroatoms have excellent ability to activate persulfate. By simply regulating the doping and defect levels of the carbon catalyst, the oxidation level of the reaction can be regulated: from mild and selective oxidation non-radical pathways to deep and non-selective oxidation free radical pathways. Generally, the composition of wastewater is complex, with many types of coexisting substrates, high concentrations, and great interference with the removal of target pollutants. Excessive PMS addition or energy input is often required to achieve effective removal of trace target pollutants. This not only significantly increases the treatment cost, but is also easily accompanied by toxic by-products, increasing environmental risks. Therefore, the development of selective activated PMS oxidation technology is of great significance for the innovation of deep water treatment technology. Based on the above research status, the idea of ​​the present invention is that loading metal or its oxide particles with special catalytic activity on carbon materials with high electrical conductivity and strength will help enhance the stability and dispersibility of the metal materials, solve the problem of easy agglomeration during the catalytic process, improve the catalytic activity and service life of the catalyst, and avoid the release of free metal ions during the treatment process.

[0005] In the field of activated PMS oxidation degradation of sulfamethoxazole, Ji et al. studied the effectiveness of thermally activated persulfate technology based on sulfate free radicals in degrading sulfonamide antibiotics. The results showed that sulfonamide antibiotics were rapidly and efficiently degraded, among which sulfate free radicals were the dominant oxidizing species, and they could selectively oxidize the aniline groups on sulfonamide antibiotics. Wu et al. studied the effectiveness of three different systems of UV-activated persulfate, bromate and hydrogen peroxide in degrading four sulfonamide antibiotics. The results showed that different systems had different degradation efficiencies for different antibiotics, but UV-activated persulfate had the highest mineralization rate for the four selected sulfonamide antibiotics, proving that the system can generate strong oxidizing free radicals and then deeply mineralize sulfonamide antibiotics. Nfodzo P et al. used metal ions Fe 2+ Activated PMS degrades SMX. In [SMX]:[PMS]:[Fe 2+ ]=1:80:80, SMX concentration was 9mg / L, pH=7, and the removal rate reached 95% after 180min treatment. 2+ Instead of Fe 2+ , in [SMX]:[PMS]:[Co 2+ ]=1:10:10, SMX concentration was 9 mg / L, and pH=7, and the removal rate was close to 100% after 180 minutes of treatment. Summary of the invention

[0006] The object of the present invention is to provide a novel modified carbon-based calcium iron layered double hydroxide catalyst (CaFe-LDH / ACF, referred to as CFLA). Another object of the present invention is to provide a method for preparing the above catalyst and to provide the use of the above catalyst in activating PMS to degrade SMX in antibiotic wastewater.

[0007] The technical scheme of the present invention is as follows: a modified carbon-based calcium iron layered double metal hydroxide catalyst, characterized in that the catalyst is composed of a carrier and a layered double metal hydroxide, the carrier is activated carbon fiber ACF, the layered double metal hydroxide is a calcium iron layered double metal hydroxide; wherein the loading mass percentage of the Ca element is 2.26-5.16%, and the Ca 2+ and Fe 3+ The molar ratio is (2-5):1; the total specific surface area of ​​the catalyst is 1000-1600m 2 ·g -1 ; pore volume is 0.60-0.90cm 3 ·g -1 ; The average pore diameter is 1~3nm.

[0008] The present invention also provides a method for preparing the above-mentioned modified carbon-based calcium iron layered double metal hydroxide catalyst, and the specific steps are as follows:

[0009] (1) Pretreatment of activated carbon fiber: The original activated carbon fiber was pretreated with an acid solution, and then the suspension was stirred evenly and fully contacted before further treatment. After filtration, the activated carbon fiber sample was washed with deionized water until the pH value of the filtrate was neutral, and then the sample was vacuum dried; the obtained sample was named ACF;

[0010] (2) Loading CaFe-LDH on ACF by hydrothermal method: Dissolve calcium salt and iron salt in deionized water, stir to fully dissolve and mix; then add urea, use urea as the growth liquid of layered double metal hydroxide, and obtain a metal mixed liquid. Add the ACF pretreated in step (1) to the above metal mixed liquid, mix well, and then transfer the above mixed liquid to a hydrothermal reactor for hydrothermal treatment; after the reaction is completed, cool naturally, filter and wash with deionized water until neutral (6.5-7.5), to obtain CaFeCO3-LDH / ACF;

[0011] (3) Ion exchange method to change the interlayer anions: The washed CaFe-CO3-LDH / ACF was transferred to a round-bottom flask, and a mixed solution containing hydrochloric acid and NaCl was added. The mixture was refluxed in an oil bath at a certain temperature and mechanically stirred to ensure sufficient reaction. After the reaction was completed, the mixture was naturally cooled, the product was taken out, and washed with deionized water until it was neutral (6.5-7.5). The mixture was vacuum dried to obtain CaFeCl-LDH / ACF, referred to as CFLA.

[0012] Preferably, the acid solution in step (1) is hydrochloric acid, sulfuric acid or nitric acid; the mass concentration of the acid solution is 5-10%; the volume ratio of the mass of the activated carbon fiber to the acid solution is 10-40 g·L -1 .

[0013] Preferably, the stirring speed in step (1) is 200-400 rpm, and the stirring time is 2-4 hours; the pH value of the filtrate is washed to 6.5-7.5; the vacuum drying temperature is 60-100° C., and the vacuum drying time is 8-14 hours.

[0014] Preferably, the calcium salt in step (2) is CaCl2·2H2O, the iron salt is FeCl3·6H2O, and the molar ratio of the calcium salt, the iron salt and the urea is (2-5):1:(5-20), Ca 2+ The concentration is 0.2-0.5 mol / L; the volume ratio of the added mass of pretreated activated carbon fiber ACF to pure water is 5-20 g·L -1 ; Stirring time is 0.5~1h.

[0015] Preferably, the mechanical stirring speed of calcium salt and iron salt dissolved in deionized water is 280-350 rpm, and the stirring time is 20-40 min; the mechanical stirring time of urea added to the above mixed solution is 20-40 min; the hydrothermal reaction time is 10-14 h, and the hydrothermal reaction temperature is 150-180° C.

[0016] Preferably, the molar ratio of hydrochloric acid, NaCl and iron salt in step (3) is (1-3):(17-43):1; the oil bath time is 8-16 hours, and the temperature is 90-120° C.; the mechanical stirring speed is 100-180 rpm; the drying temperature is 60-100° C., and the vacuum drying time is 10-14 hours.

[0017] The present invention also provides the use of the modified carbon-based calcium iron layered double metal hydroxide catalyst in the degradation of sulfamethoxazole SMX in wastewater. The specific steps are: adding CFLA catalyst to simulated SMX wastewater, wherein the pH of the simulated wastewater is adjusted to 2.00-12.00 and the SMX concentration is 10-40 mg·L -1 The concentration of PMS added to the wastewater is 1.00-2.00 mM, and the volume ratio of CFLA catalyst added mass to wastewater is 0.5-2 g·L -1 Place in a constant temperature shaking bed, set the rotation speed to 150-250 rpm, and shake at 20-55°C for 1-3 hours.

[0018] Beneficial effects:

[0019] (1) The catalyst of the present invention is green and environmentally friendly, can be synthesized on a large scale, can be recycled and reused, and has high economic benefits.

[0020] (2) The catalyst of the present invention is based on activated carbon fiber (ACF) and loaded with CaFe-LDH, which has a good activation effect on PMS under a wide range of pH conditions. 1 O2) and electron transfer, which accelerates the reaction process and has a good selective oxidation degradation effect on SMX. DETAILED DESCRIPTION

[0021] In order to better understand the present invention, the present invention is further described below by way of examples, which are only used for explanation and do not constitute any limitation to the present invention.

[0022] Embodiment 1:

[0023] (1) Prepare simulated wastewater containing SMX, with an SMX concentration of 10 mg·L -1 , the pH was adjusted to 2 using 0.1 M NaOH and HCl.

[0024] (2) Prepare the adsorbent, the steps are as follows:

[0025] (a) Pretreatment of ACF: 5.00 g of untreated activated carbon fiber was cut into small cubes of 1*1 cm, and the activated carbon fiber was pretreated with 500 ml of 5% HCl solution, and then the suspension was stirred at 200 rpm for 4 hours at 298 K before further treatment. After filtration, the ACF sample was washed with distilled water until the pH value of the filtrate was 6.5. The sample was then vacuum dried at 60 °C for 14 h, and the resulting sample was named ACF.

[0026] (b) Loading CaFe-LDH on ACF by hydrothermal method: Weigh 2.2196g (0.02mol) CaCl2·6H2O and 2.703g (0.01mol) FeCl3·6H2O (molar ratio 2:1) respectively and dissolve them in 100ml pure water, stir them by electric gravity for 40min at a speed of 280rpm to make them completely dissolved and mixed evenly, then weigh 3.003g (0.05mol) urea and add it to the above metal solution, continue stirring for 20min until it is completely dissolved. Then take 0.5g of ACF dried in step (a) and add it to the above solution, stir at 280rpm for 0.5h to make it completely mixed. Finally, transfer all the mixed solution to the inner tank of a 250ml hydrothermal reactor and perform hydrothermal treatment at 180℃ for 12 hours. After the reaction is completed, wait for it to cool naturally, filter it and wash it with deionized water until the pH is 7.0. Transfer the product to a round-bottom flask, add 100ml HCl (0.1M) and 10g NaCl (0.17mol), react in a 120℃ oil bath for 8h, and stir mechanically at a stirring speed of 180rpm. After the reaction is completed, cool it naturally, take out the product, and wash it with deionized water until the pH is 7.0. Finally, dry the washed product in vacuum at 60℃ for 14h to obtain CFLA. The total specific surface area of ​​the composite adsorbent before and after modification is 1329.26m 2 ·g -1 , the average pore diameter is 1.658 nm, and the average pore volume is 0.607 cm 3 ·g -1 The calcium loading in the composite adsorbent is 2.21%.

[0027] Weigh 0.05 g of the composite adsorbent CFLA prepared in this example, measure 100 ml of the SMX-containing simulated wastewater prepared in step (1), add CFLA to the simulated wastewater, add 1.0 mM PMS, and react at a constant temperature of 25°C for 180 min at a shaking speed of 150 rpm. Use high performance liquid chromatography to detect the SMX concentration. When the pH is 2, the SMX removal rate is 93.58%. The catalyst is recovered and reused. It was reused 5 times under the same conditions, and the removal rate was 91.21%.

[0028] Example 2

[0029] (1) Prepare simulated wastewater containing SMX, with an SMX concentration of 20 mg·L -1 , the pH was adjusted to 6 using 0.1 M NaOH and HCl.

[0030] (2) Prepare the adsorbent, the steps are as follows:

[0031] (a) Pretreatment of ACF: 10.00 g of untreated activated carbon fiber was cut into small cubes of 1*1 cm, and the activated carbon fiber was pretreated with 500 ml of 10% H2SO4 solution, and then the suspension was stirred at 298 K for 3 hours at 300 rpm before further treatment. After filtration, the ACF sample was washed with distilled water until the pH value of the filtrate was 7. The sample was then vacuum dried at 70 °C for 12 h, and the resulting sample was named ACF.

[0032] (b) Loading CaFe-LDH on ACF by hydrothermal method: Weigh 3.3294g (0.03mol) CaCl2·6H2O and 2.703g (0.01mol) FeCl3·6H2O (molar ratio 3:1) respectively and dissolve them in 100ml pure water, stir them by electric gravity for 30min at a speed of 300rpm to make them completely dissolved and mixed evenly, then weigh 6.006g (0.1mol) urea and add it to the above metal solution, continue stirring for 20min until it is completely dissolved. Then take 1.0g of ACF dried in step (a) and add it to the above solution, stir at 300rpm for 1h to make it completely mixed. Finally, transfer all the mixed solution to the inner tank of a 250ml hydrothermal reactor and perform hydrothermal treatment at 170℃ for 11 hours. After the reaction is completed, wait for it to cool naturally, filter it and wash it with deionized water until the pH is 7.0. Transfer the product to a round-bottom flask, add 100ml HCl (0.2M) and 15.0g (0.26mol) of NaCl, react in an oil bath at 110°C for 10h, and stir mechanically at a stirring speed of 160rpm. After the reaction is completed, cool it naturally, take out the product, and wash it with deionized water until the pH is 7.0. Finally, dry the washed product in vacuum at 70°C for 12h to obtain CFLA. The total specific surface area of ​​the composite adsorbent before and after modification is 1417.89m 2 ·g -1 , the average pore diameter is 1.732nm, and the average pore volume is 0.681cm 3 ·g -1 The calcium loading in the composite adsorbent is 3.81%.

[0033] Weigh 0.1 g of the composite adsorbent CFLA prepared in this example, measure 100 ml of the simulated wastewater containing SMX prepared in step (1), add CFLA to the simulated wastewater, add 1.5 mM PMS, and react at 35°C for 120 min at a constant temperature of 150 rpm. Use high performance liquid chromatography to detect the SMX concentration. When the pH is 6, the SMX removal rate is 98.91%. The catalyst is recovered and reused. It was reused 5 times under the same conditions, and the removal rate was 91.16%.

[0034] Example 3

[0035] (1) Prepare simulated wastewater containing SMX, with an SMX concentration of 30 mg·L -1 , the pH was adjusted to 9 using 0.1 M NaOH and HCl.

[0036] (2) Prepare the adsorbent, the steps are as follows:

[0037] (a) Pretreatment of ACF: 15.00 g of untreated activated carbon fiber was cut into small cubes of 1*1 cm, and the activated carbon fiber was pretreated with 500 ml of 5% HNO3 solution, and then the suspension was stirred at 400 rpm at 298 K for 4 hours before further treatment. After filtration, the ACF sample was washed with distilled water until the pH value of the filtrate was 7.5. The sample was then vacuum dried at 80 °C for 10 h, and the resulting sample was named ACF.

[0038] (b) Loading CaFe-LDH on ACF by hydrothermal method: Weigh 4.7392g (0.04mol) CaCl2·6H2O and 2.703g (0.01mol) FeCl3·6H2O (molar ratio 4:1) respectively and dissolve them in 100ml pure water, stir them by electric gravity for 20min at a speed of 310rpm to make them completely dissolved and mixed evenly, then weigh 9.009g (0.15mol) urea and add it to the above metal solution, continue stirring for 30min until it is completely dissolved. Then take 1.5g of ACF dried in step (a) and add it to the above solution, stir at 310rpm for 1.5h to make it completely mixed. Finally, transfer all the mixed solution to the inner tank of a 250ml hydrothermal reactor and perform hydrothermal treatment at 160℃ for 12 hours. After the reaction is completed, wait for it to cool naturally, filter it and wash it with deionized water until the pH is 7.5. Transfer the product to a round-bottom flask, add 100ml HCl (0.3M) and NaCl 20.0g (0.34mol), react in a 100℃ oil bath for 12h, and stir mechanically at a stirring speed of 140rpm. After the reaction is completed, cool it naturally, take out the product, and wash it with deionized water until the pH is 7.5. Finally, dry the washed product in vacuum at 80℃ for 11h to obtain CFLA. The total specific surface area of ​​the composite adsorbent before and after modification is 1386.64m 2 ·g -1 The average pore size is 1.706 nm and the average pore volume is 0.678 cm 3 ·g -1 The calcium loading in the composite adsorbent is 4.69%.

[0039] Weigh 0.15g of the composite adsorbent CFLA prepared in this embodiment, measure 100ml of the SMX-containing simulated wastewater prepared in step (1), put CFLA into the simulated wastewater, add 1.5mM PMS, and react at a constant temperature of 45°C for 120min at a shaking speed of 150rpm. High performance liquid chromatography was used to detect the SMX concentration. When the pH was 9, the SMX removal rate was 98.36%. The catalyst was recovered and reused. It was reused 5 times under the same conditions, and the removal rate was 90.66%.

[0040] Example 4

[0041] (1) Prepare simulated wastewater containing SMX, with an SMX concentration of 40 mg·L -1 , the pH was adjusted to 12 using 0.1 M NaOH and HCl.

[0042] (2) Prepare the adsorbent, the steps are as follows:

[0043] (a) Pretreatment of ACF: 20.00 g of untreated activated carbon fiber was cut into small cubes of 1*1 cm, and the activated carbon fiber was pretreated with 500 ml of 10% HCl solution, and then the suspension was stirred at 298 K at 300 rpm for 2 hours before further treatment. After filtration, the ACF sample was washed with distilled water until the pH value of the filtrate was 6.5. The sample was then vacuum dried at 100 °C for 8 h, and the obtained sample was named ACF.

[0044] (b) Loading CaFe-LDH on ACF by hydrothermal method: Weigh 5.549g (0.05mol) CaCl2·6H2O and 2.703g (0.01mol) FeCl3·6H2O (molar ratio 5:1) respectively and dissolve them in 100ml pure water, stir them by electric gravity for 20min at a speed of 350rpm to make them completely dissolved and mixed evenly, then weigh 12.012g (0.2mol) urea and add it to the above metal solution, continue stirring for 40min until it is completely dissolved. Then take 2.0g of ACF dried in step (a) into the above solution and stir at 350rpm for 2h to make it completely mixed. Finally, transfer all the mixed solution to the inner tank of a 250ml hydrothermal reactor and perform hydrothermal treatment at 150℃ for 14 hours. After the reaction is completed, wait for it to cool naturally, filter it and wash it with deionized water until the pH is 7.0. Transfer the product to a round-bottom flask, add 100ml HCl (0.3M) and 25.0g (0.43mol) of NaCl, react for 16h in a 90℃ oil bath, and stir mechanically at a speed of 100rpm. After the reaction is completed, cool it naturally, take out the product, and wash it with deionized water until the pH is 7.0. Finally, dry the washed product in vacuum at 90℃ for 10h to obtain CFLA. The total specific surface area of ​​the composite adsorbent before and after modification is 1389.26m 2 ·g -1 The average pore size is 1.719 nm and the average pore volume is 0.669 cm 3 ·g -1 The calcium loading in the composite adsorbent is 5.16%.

[0045] Weigh 0.2 g of the composite adsorbent CFLA prepared in this embodiment, measure 100 ml of the SMX-containing simulated wastewater prepared in step (1), put CFLA into the simulated wastewater, add 2.0 mM PMS, and react at 55°C for 60 min at a constant temperature of 150 rpm. High performance liquid chromatography was used to detect the SMX concentration. When the pH was 12, the SMX removal rate was 99.28%. The catalyst was recovered and reused. Under the same conditions, it was reused 5 times, and the removal rate was 91.35%.

Claims

1. A modified carbon-based calcium iron layered double metal hydroxide catalyst, characterized in that The catalyst is composed of a carrier and a layered double metal hydroxide, wherein the carrier is activated carbon fiber ACF, and the layered double metal hydroxide is a calcium iron layered double metal hydroxide; wherein the loading mass percentage of the Ca element is 2.26-5.16%, and the Ca 2+ and Fe 3+ The molar ratio is (2-5):1; the total specific surface area of ​​the catalyst is 1000-1600m 2 ·g -1 ; The pore volume is 0.60-0.90cm 3 ·g -1 ; The average pore diameter is 1~3nm.

2. A method for preparing the modified carbon-based calcium iron layered double metal hydroxide catalyst as claimed in claim 1, wherein the specific steps are as follows: (1) Pretreatment of activated carbon fiber: The raw activated carbon fiber was pretreated with an acid solution, and then the suspension was stirred evenly before further treatment; after filtration, the activated carbon fiber sample was washed with deionized water until the pH value of the filtrate was neutral, and then the sample was vacuum dried; the obtained sample was named ACF; (2) Loading CaFe-LDH on ACF by hydrothermal method: Dissolve calcium salt and iron salt in deionized water, stir to fully dissolve and mix; then add urea to obtain a metal mixture, add the ACF pretreated in step (1) to the above metal mixture, mix well, and then transfer the above mixture to a hydrothermal reactor for hydrothermal treatment; after the reaction is completed, cool naturally, filter and wash with deionized water until neutral, to obtain CaFeCO3-LDH / ACF; (3) Ion exchange method to change the interlayer anions: The washed CaFe-CO3-LDH / ACF was transferred to a round-bottom flask, and a mixed solution containing hydrochloric acid and NaCl was added. The mixture was refluxed in an oil bath at a certain temperature and mechanically stirred to ensure sufficient reaction. After the reaction was completed, the mixture was cooled naturally, the product was taken out, and washed with deionized water until neutral. After vacuum drying, CaFeCl-LDH / ACF, referred to as CFLA, was obtained.

3. The method according to claim 2, characterized in that The acid solution in step (1) is hydrochloric acid, sulfuric acid or nitric acid; the mass concentration of the acid solution is 5-10%; the volume ratio of the mass of the activated carbon fiber to the acid solution is 10-40 g·L -1 .

4. The method according to claim 2, characterized in that The stirring speed in step (1) is 200-400 rpm, and the stirring time is 2-4 hours; the pH value of the filtrate is washed to 6.5-7.5; the vacuum drying temperature is 60-100° C., and the vacuum drying time is 8-14 hours.

5. The method according to claim 2, characterized in that The calcium salt described in step (2) is CaCl2·2H2O, the iron salt is FeCl3·6H2O, and the molar ratio of the calcium salt, the iron salt and urea is (2-5):1:(5-20), Ca 2+ The concentration is 0.2-0.5 mol / L; the volume ratio of the added mass of pretreated activated carbon fiber ACF to pure water is 5-20 g·L -1 ; Stirring time is 0.5~1h.

6. The method according to claim 2, characterized in that The mechanical stirring speed of calcium salt and iron salt dissolved in deionized water is 280-350 rpm, and the stirring time is 20-40 min; the mechanical stirring time of urea added to the above mixed solution is 20-40 min; the hydrothermal reaction time is 10-14 h, and the hydrothermal reaction temperature is 150-180° C.

7. The method according to claim 2, characterized in that The molar ratio of hydrochloric acid, NaCl and iron salt described in step (3) is (1-3):(17-43):1; the oil bath time is 8-16 hours, and the temperature is 90-120° C.; the mechanical stirring speed is 100-180 rpm; the drying temperature is 60-100° C., and the vacuum drying time is 10-14 hours.

8. Use of the modified carbon-based calcium iron layered double metal hydroxide catalyst as claimed in claim 1 in degrading sulfamethoxazole SMX in wastewater.

9. The use according to claim 8, wherein the specific steps are: adding CFLA catalyst to simulated SMX wastewater, wherein the pH of the simulated wastewater is adjusted to 2.00-12.00 and the SMX concentration is 10-40 mg·L -1 The concentration of PMS added to the wastewater is 1.00-2.00 mM, and the volume ratio of CFLA catalyst added mass to wastewater is 0.5-2 g·L -1 Place in a constant temperature shaking bed, set the rotation speed to 150-250 rpm, and shake at 20-55°C for 1-3 hours.

Citation Information

Patent Citations

  • Preparation method and application of ferromanganese layered bimetal hydroxide catalyst

    CN111215091A

  • Catalyst for selectively oxidizing sulfamethoxazole by activating peroxymonosulfate as well as preparation and application of catalyst

    CN115430448A

  • Preparation method of regenerated cellulose supported cobalt ferrite catalyst and application of regenerated cellulose supported cobalt ferrite catalyst in pollutant degradation

    CN115957813A

  • Modified magnesium-iron layered double-metal hydroxide adsorbent as well as preparation and application thereof

    CN116920803A

  • Carbon-based magnesium-iron layered double-metal hydroxide adsorbent as well as preparation method and application thereof

    CN117046446A

Cited By

  • Magnetic calcium-iron layered double-metal hydroxide catalyst as well as preparation and application thereof

    CN119588359A