Metal organic framework magnetic catalyst as well as preparation method and application thereof

By preparing a metal-organic framework magnetic catalyst and using its core-shell structure to activate peracetic acid to degrade organophosphorus pesticides in water and adsorb inorganic phosphorus, the problems of organophosphorus pesticide degradation and inorganic phosphorus pollution in water are solved, and efficient degradation and catalyst resiliency are achieved. Recyclability.

CN118744015APending Publication Date: 2024-10-08CHINA CONSTR EIGHTH BUREAU SOUTH CHINA CONSTR CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410779483.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-08

Smart Images

  • Figure BDA0004896682400000061
    Figure BDA0004896682400000061
  • Figure HDA0004896682410000011
    Figure HDA0004896682410000011
  • Figure HDA0004896682410000012
    Figure HDA0004896682410000012
Patent Text Reader

Abstract

The invention provides a metal organic framework magnetic catalyst and a preparation method and application thereof.The preparation method comprises the steps that firstly, Fe3O4 nanoparticles doped with single metal are synthesized, then the magnetic nanoparticles serve as a core, a layer of metal organic framework UiO-66 constructed with Zr6O4 (OH) 4 clusters serving as nodes is synthesized outside the magnetic nanoparticles, and the metal organic framework UiO-66 is prepared. Finally, the metal organic framework magnetic catalyst with the core-shell structure is obtained. The metal organic framework magnetic catalyst provided by the invention is stable and recoverable, not only can effectively activate peracetic acid so as to degrade fenitrothion in water, but also can adsorb generated inorganic phosphorus in situ, so that the problem of secondary pollution is effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a catalyst, in particular to a metal organic framework magnetic catalyst and a preparation method and application thereof. Background Art

[0002] Organophosphorus pesticides are widely used to control plant diseases, insect pests and weeds. They are widely used in agricultural production due to their low toxicity and low residue levels. This type of pesticide is usually composed of derivatives of phosphoric acid, phosphonic acid, phosphosulfate or phosphosulfate, such as esters, amides or thiol derivatives. They contain pentavalent phosphorus atoms and are connected to oxygen (P=O) or sulfur (P=S) through double bonds. However, organophosphorus pesticides can easily enter the water environment in a variety of ways and may pose a threat to the health of humans and other animals through water. Although their concentrations in water are usually very low (ng / L-μg / L), most organophosphorus pesticides are highly toxic, and extremely low concentrations of contact may also pose risks to non-target organisms and humans, and may cause problems such as mutagenesis, neurosis, encephalopathy and visual impairment. Therefore, the effective removal of organophosphorus pesticides in water is crucial for environmental protection and human health.

[0003] Peracetic acid (PAA) is an organic peroxyacid that has been widely used in a variety of fields, including disinfectants, bactericides, bleaches, sterilants, oxidants, and polymerization catalysts. Compared with traditional disinfectants, the advantages of PAA in water disinfection and microbial inactivation include high sterilization ability, low dependence on pH, simple technical implementation, and reduced formation of toxic byproducts in post-treatment effluents. Therefore, PAA has become a powerful alternative to chlorinated disinfectants in water treatment. In addition to its use as a disinfectant, PAA can also effectively degrade organic micropollutants in water, such as endocrine disruptors, disinfection byproducts, and drugs, due to its high oxidation potential. Recent studies have focused more on the use of PAA in advanced oxidation processes (AOPs), which produce active species by activating PAA using external energy or catalysts. Transition metal activation has received widespread attention due to its simple operation, low cost and easy availability. However, there are problems in heterogeneous transition metal catalytic reaction systems that need to be solved, such as the difficulty in recovering catalysts and the easy agglomeration of nanoparticles.

[0004] In addition, studies have shown that organic phosphorus compounds in the advanced oxidation process will be converted into inorganic phosphorus, which is one of the main factors leading to eutrophication of water bodies. Therefore, after the degradation process of organic phosphorus compounds, chemical agents are usually added to remove inorganic phosphorus, but this method is complicated to operate and may cause secondary pollution such as excess sludge. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a metal organic framework magnetic catalyst. The metal organic framework magnetic catalyst prepared by the preparation method is stable and recyclable, can not only effectively activate peracetic acid to degrade fenitrothion in water, but also can in situ adsorb the inorganic phosphorus produced thereby, effectively avoiding the problem of secondary pollution.

[0006] In order to solve the above technical problems, the technical solution of the present invention is:

[0007] A method for preparing a metal organic framework magnetic catalyst comprises the following steps:

[0008] S1. Add FeCl3·6H2O and MnCl2·4H2O to ethylene glycol, stir for 30 min to obtain a precursor solution, add anhydrous sodium acetate and polyethylene glycol to the precursor solution, stir for 30 min to obtain a mixed solution, seal the mixed solution in an autoclave, and then place the autoclave in an oven, react at 150-200°C for 8-12h, and naturally cool to room temperature to obtain reactant 1;

[0009] S2. The reaction product obtained in step S1 was magnetically separated and washed with anhydrous ethanol and deionized water for 5 times, and then placed in a vacuum drying oven to obtain Mn-doped Fe3O4 nanoparticles;

[0010] S3. The Mn-doped Fe3O4 nanoparticles, ZrCl4, terephthalic acid and dimethylformamide obtained in step S2 were added to glacial acetic acid, ultrasonically stirred for 30 min, and then transferred to a reactor, reacted at 100-150 ° C for 24 h, and naturally cooled to room temperature to obtain reactant II;

[0011] S4. After magnetic separation, the reactant obtained in step S3 is washed with dimethylformamide and methanol for 5 times respectively, and then placed in a vacuum drying oven for vacuum drying to obtain a metal organic framework magnetic catalyst.

[0012] Furthermore, in step S1 of the present invention, the ratio of FeCl3·6H2O, MnCl2·4H2O, ethylene glycol, anhydrous sodium acetate and polyethylene glycol is (2-4) mmol: (2-4) mmol: 50 mL: (40-100) mmol: (5-8) g.

[0013] Furthermore, in step S1 of the present invention, the autoclave is a stainless steel autoclave lined with Teflon.

[0014] Furthermore, in step S2 of the present invention, the vacuum drying temperature is 40-60° C. and the time is 7-9 h.

[0015] Furthermore, in step S3 of the present invention, the ratio of Mn-doped Fe3O4 nanoparticles, ZrCl4, terephthalic acid, dimethylformamide and glacial acetic acid obtained in step S2 is (0.2-1) g: (0.4-1.6) g: (0.3-1.2) g: 100 mL: (4-16) mL.

[0016] Furthermore, in step S4 of the present invention, the vacuum drying temperature is 40-60° C. and the time is 7-9 h.

[0017] Another technical problem to be solved by the present invention is to provide a metal organic framework magnetic catalyst prepared by the above preparation method.

[0018] The present invention also provides the use of the metal organic framework magnetic catalyst in degrading fenitrothion in water.

[0019] Furthermore, the application comprises the following steps:

[0020] The metal organic framework magnetic catalyst was added into the wastewater containing fenitrothion, and the pH value was adjusted to 7, and then peracetic acid was added dropwise, and the mixture was placed in a constant temperature oscillator and shaken for 30 minutes.

[0021] Furthermore, the ratio of the metal organic framework magnetic catalyst, fenitrothion, sewage and peracetic acid is (80-240) mg:20 mg:1 L:(100-200) mg; the temperature of the constant temperature oscillator is 20-30° C., and the rotation speed is 150-200 r / min.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1) The present invention first synthesizes Fe3O4 nanoparticles doped with single metal Mn, and then uses the magnetic nanoparticles as the core, and synthesizes a layer of metal organic framework UiO-66 constructed with Zr6O4(OH)4 clusters as nodes on the outside, and finally obtains a metal organic framework magnetic catalyst with a core-shell structure. The catalyst can effectively activate peracetic acid PAA and degrade the organophosphorus pesticide fenitrothion in water. At the same time, since UiO-66 belongs to a Zr-based metal organic framework, it can in-situ adsorb inorganic phosphorus generated by the reaction, thereby effectively preventing secondary pollution. In addition, the catalyst has magnetism and is easy to separate solid and liquid for recycling, and the catalytic performance can be effectively improved through the synergistic effect between Fe and doped metal Mn.

[0024] 2) The preparation method of the present invention is simple to operate, the raw materials are readily available, and the production cost is low. In addition, the core-shell structure plays an important role in adjusting the physical and chemical properties of the material to achieve complementary advantages, preventing nanoparticles from agglomerating, and controlling particle interface reactions. Compared with other catalysts that activate the oxidant peracetic acid, the catalyst prepared by the present invention has the following advantages:

[0025] Fe3O4 nanoparticles are doped with Mn, and the synergistic effect between Fe and Mn greatly improves the catalytic activity; encapsulating Mn-doped Fe3O4 nanoparticles in a metal-organic framework gives the catalyst a certain magnetic property, making it easy to separate from water and showing excellent recyclability; the UiO-66 shell is rich in Zr-OH groups with high affinity for phosphate groups, which can efficiently adsorb inorganic phosphorus produced by the degradation reaction to avoid secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:

[0027] Figure 1 This is a transmission electron microscope TEM image of the metal organic framework magnetic catalyst prepared in Example 1 of the present invention;

[0028] Figure 2 This is the hysteresis curve of the metal organic framework magnetic catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0029] The present invention will be described in detail below in conjunction with specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0030] Example 1

[0031] The metal organic framework magnetic catalyst was prepared by the following steps:

[0032] S1. Add FeCl3·6H2O and MnCl2·4H2O to ethylene glycol, stir for 30 min to obtain a precursor solution, add anhydrous sodium acetate and polyethylene glycol to the precursor solution, stir for 30 min to obtain a mixed solution, seal the mixed solution in an autoclave, and then place a stainless steel autoclave lined with Teflon in an oven, react at 180°C for 10 h, and naturally cool to room temperature to obtain reactant 1; the ratio of FeCl3·6H2O, MnCl2·4H2O, ethylene glycol, anhydrous sodium acetate, and polyethylene glycol is 4mmol:4mmol:50mL:80mmol:6g;

[0033] S2. The reaction product obtained in step S1 was magnetically separated and washed with anhydrous ethanol and deionized water for 5 times, and then placed in a vacuum drying oven at 50°C for 8h to obtain Mn-doped Fe3O4 nanoparticles;

[0034] S3. The Mn-doped Fe3O4 nanoparticles, ZrCl4, terephthalic acid and dimethylformamide obtained in step S2 were added to glacial acetic acid in a ratio of 1g:1g:0.8g:100mL:4mL, and ultrasonically stirred for 30min before being transferred to a reactor, reacted at 120°C for 24h, and naturally cooled to room temperature to obtain reactant II;

[0035] S4. After magnetic separation, the reactant obtained in step S3 was washed with dimethylformamide and methanol for 5 times respectively, and then placed in a vacuum drying oven at 50° C. for 8 h to obtain a metal organic framework magnetic catalyst.

[0036] Figure 1 TEM image of the metal organic framework magnetic catalyst prepared in Example 1. Figure 1 It can be seen that the catalyst prepared in this example has an obvious core-shell structure, forming a composite material with Mn-doped Fe3O4 nanoparticles as the core and UiO-66 as the shell.

[0037] Figure 2 is the hysteresis curve of the metal organic framework magnetic catalyst prepared in Example 1, and its saturation magnetization (Ms) is 60.89emu / g. Figure 2 It can be seen that the metal organic framework magnetic catalyst prepared in Example 1 has good superparamagnetic properties, which is conducive to recycling from the solution in practical applications.

[0038] The use of the metal organic framework magnetic catalyst prepared in Example 1 in the degradation of fenitrothion in water comprises the following steps:

[0039] Add the metal organic framework magnetic catalyst to the sewage containing fenitrothion, adjust the pH value to 7, and then add peracetic acid dropwise. The ratio of metal organic framework magnetic catalyst, fenitrothion, sewage, and peracetic acid is 100 mg:20 mg:1 L:120 mg. Place it in a constant temperature oscillator and oscillate for 30 minutes. The temperature of the constant temperature oscillator is 25°C and the rotation speed is 180 r / min.

[0040] The water sample after the reaction was filtered through a water filter membrane with a pore size of 0.45 μm, and the concentrations of fenitrothion and total phosphorus in the liquid were determined; wherein fenitrothion was determined by liquid chromatography, and total phosphorus was determined by ammonium molybdate spectrophotometry (GB11893-89). The results showed that the removal rate of fenitrothion in Example 1 could reach 97.3%, and the removal rate of total phosphorus could reach 94.1%.

[0041] Example 2

[0042] The metal organic framework magnetic catalyst was prepared by the following steps:

[0043] S1. Add FeCl3·6H2O and MnCl2·4H2O to ethylene glycol, stir for 30 min to obtain a precursor solution, add anhydrous sodium acetate and polyethylene glycol to the precursor solution, stir for 30 min to obtain a mixed solution, seal the mixed solution in an autoclave, and then place a stainless steel autoclave lined with Teflon in an oven, react at 100°C for 12 h, and naturally cool to room temperature to obtain reactant 1; the ratio of FeCl3·6H2O, MnCl2·4H2O, ethylene glycol, anhydrous sodium acetate, and polyethylene glycol is 2mmol:3mmol:50mL:40mmol:5g;

[0044] S2. The reaction product obtained in step S1 was magnetically separated and washed with anhydrous ethanol and deionized water for 5 times, and then placed in a vacuum drying oven at 40°C for 9h to obtain Mn-doped Fe3O4 nanoparticles;

[0045] S3. The Mn-doped Fe3O4 nanoparticles, ZrCl4, terephthalic acid and dimethylformamide obtained in step S2 were added to glacial acetic acid in a ratio of 0.2 g: 0.4 g: 0.3 g: 100 mL: 5 mL, and ultrasonically stirred for 30 min before being transferred to a reactor, reacted at 100 ° C for 24 h, and naturally cooled to room temperature to obtain reactant II;

[0046] S4. After magnetic separation, the reactant obtained in step S3 was washed with dimethylformamide and methanol for 5 times respectively, and then placed in a vacuum drying oven at 40° C. for 9 hours to obtain a metal organic framework magnetic catalyst.

[0047] The use of the metal organic framework magnetic catalyst prepared in Example 2 in the degradation of fenitrothion in water comprises the following steps:

[0048] Add the metal organic framework magnetic catalyst to the sewage containing fenitrothion, adjust the pH value to 7, and then add peracetic acid dropwise. The ratio of metal organic framework magnetic catalyst, fenitrothion, sewage, and peracetic acid is 80 mg:20 mg:1 L:100 mg. Place it in a constant temperature oscillator and oscillate for 30 minutes. The temperature of the constant temperature oscillator is 20°C and the rotation speed is 200 r / min.

[0049] The water sample after the reaction was filtered through a water filter membrane with a pore size of 0.45 μm, and the concentrations of fenitrothion and total phosphorus in the liquid were determined; wherein fenitrothion was determined by liquid chromatography, and total phosphorus was determined by ammonium molybdate spectrophotometry (GB11893-89). The results showed that the removal rate of fenitrothion in Example 2 could reach 93.4%, and the removal rate of total phosphorus could reach 88.6%.

[0050] Example 3

[0051] The metal organic framework magnetic catalyst was prepared by the following steps:

[0052] S1. Add FeCl3·6H2O and MnCl2·4H2O to ethylene glycol, stir for 30 min to obtain a precursor solution, add anhydrous sodium acetate and polyethylene glycol to the precursor solution, stir for 30 min to obtain a mixed solution, seal the mixed solution in an autoclave, and then place a stainless steel autoclave lined with Teflon in an oven, react at 200°C for 8h, and naturally cool to room temperature to obtain reactant 1; the ratio of FeCl3·6H2O, MnCl2·4H2O, ethylene glycol, anhydrous sodium acetate, and polyethylene glycol is 3mmol:2mmol:50mL:100mmol:8g;

[0053] S2. The reaction product obtained in step S1 was magnetically separated and washed with anhydrous ethanol and deionized water for 5 times, and then placed in a vacuum drying oven at 60°C for 7h to obtain Mn-doped Fe3O4 nanoparticles;

[0054] S3. The Mn-doped Fe3O4 nanoparticles, ZrCl4, terephthalic acid and dimethylformamide obtained in step S2 were added to glacial acetic acid in a ratio of 0.8 g: 1.6 g: 1.2 g: 100 mL: 16 mL, and ultrasonically stirred for 30 min before being transferred to a reactor, reacted at 150 ° C for 24 h, and naturally cooled to room temperature to obtain reactant II;

[0055] S4. After magnetic separation, the reactant obtained in step S3 is washed with dimethylformamide and methanol for 5 times respectively, and then placed in a vacuum drying oven at 60° C. for 7 h to obtain a metal organic framework magnetic catalyst.

[0056] The use of the metal organic framework magnetic catalyst prepared in Example 3 in the degradation of fenitrothion in water comprises the following steps:

[0057] Add the metal organic framework magnetic catalyst to the sewage containing fenitrothion, the ratio of the metal organic framework magnetic catalyst, fenitrothion, sewage and peracetic acid is 240mg:20mg:1L:200mg, adjust the pH value to 7 and then add peracetic acid dropwise, place in a constant temperature oscillator and oscillate for 30 minutes, the temperature of the constant temperature oscillator is 30°C and the rotation speed is 150r / min.

[0058] The water sample after the reaction was filtered through a water filter membrane with a pore size of 0.45 μm, and the concentrations of fenitrothion and total phosphorus in the liquid were determined; wherein fenitrothion was determined by liquid chromatography, and total phosphorus was determined by ammonium molybdate spectrophotometry (GB11893-89). The results showed that the removal rate of fenitrothion in Example 3 could reach 90.6%, and the removal rate of total phosphorus could reach 82.5%.

[0059] Comparative Example 1:

[0060] The difference from Example 1 is that steps S3 and S4 are not included, and the other steps are the same. Mn-doped Fe3O4 nanoparticles are prepared, and then peracetic acid is activated according to the steps of Example 1 to remove fenitrothion in sewage.

[0061] Comparative Example 2:

[0062] The difference from Example 2 is that MnCl2·4H2O is not added in step S1, and the other steps are the same. A metal organic framework magnetic catalyst not doped with Mn is prepared, and then peracetic acid is activated according to the steps of Example 1 to remove fenitrothion in sewage.

[0063] The removal rates of fenitrothion and total phosphorus by the metal organic framework magnetic catalysts prepared in Examples 1-3 and the products obtained in Comparative Examples 1 and 2 are summarized as follows, as shown in Table 1:

[0064] Table 1.

[0065]

[0066] It can be seen from the removal rates of Example 1 and Comparative Example 1 in Table 1 that, on the basis of Comparative Example 1, Example 1 further comprises a Zr-based metal organic framework material, which can effectively improve the removal effect of the catalyst on the inorganic phosphorus produced after the oxidative degradation reaction.

[0067] It can be seen from the removal rates of Example 1 and Comparative Example 2 in Table 1 that, on the basis of Comparative Example 2, Example 1 further added MnCl2·4H2O to successfully prepare Mn-doped Fe3O4 magnetic nanoparticles, which can significantly improve the catalytic activity of the catalyst and enhance the degradation efficiency of fenitrothion.

[0068] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a metal organic framework magnetic catalyst, characterized in that: The following steps are involved: S1. Add FeCl3·6H2O and MnCl2·4H2O to ethylene glycol, stir for 30 min to obtain a precursor solution, add anhydrous sodium acetate and polyethylene glycol to the precursor solution, stir for 30 min to obtain a mixed solution, seal the mixed solution in an autoclave, and then place the autoclave in an oven, react at 150-200°C for 8-12h, and naturally cool to room temperature to obtain reactant 1; S2. The reaction product obtained in step S1 was magnetically separated and washed with anhydrous ethanol and deionized water for 5 times, and then placed in a vacuum drying oven to obtain Mn-doped Fe3O4 nanoparticles; S3. The Mn-doped Fe3O4 nanoparticles, ZrCl4, terephthalic acid and dimethylformamide obtained in step S2 were added to glacial acetic acid, ultrasonically stirred for 30 min, and then transferred to a reactor, reacted at 100-150 ° C for 24 h, and naturally cooled to room temperature to obtain reactant II; S4. After magnetic separation, the reactant obtained in step S3 is washed with dimethylformamide and methanol for 5 times respectively, and then placed in a vacuum drying oven for vacuum drying to obtain a metal organic framework magnetic catalyst.

2. The method for preparing a metal organic framework magnetic catalyst according to claim 1, characterized in that: In the step S1, the ratio of FeCl3·6H2O, MnCl2·4H2O, ethylene glycol, anhydrous sodium acetate and polyethylene glycol is (2-4) mmol: (2-4) mmol: 50 mL: (40-100) mmol: (5-8) g.

3. The method for preparing a metal organic framework magnetic catalyst according to claim 1, characterized in that: In the step S1, the autoclave is a stainless steel autoclave lined with Teflon.

4. The method for preparing a metal organic framework magnetic catalyst according to claim 1, characterized in that: In step S2, the vacuum drying temperature is 40-60° C. and the time is 7-9 hours.

5. The method for preparing a metal organic framework magnetic catalyst according to claim 1, characterized in that: In the step S3, the ratio of the Mn-doped Fe3O4 nanoparticles, ZrCl4, terephthalic acid, dimethylformamide and glacial acetic acid obtained in the step S2 is (0.2-1) g: (0.4-1.6) g: (0.3-1.2) g: 100 mL: (4-16) mL.

6. The method for preparing a metal organic framework magnetic catalyst according to claim 1, characterized in that: In step S4, the vacuum drying temperature is 40-60° C. and the time is 7-9 hours.

7. The metal organic framework magnetic catalyst prepared according to the preparation method of claims 1 to 6.

8. Use of the metal organic framework magnetic catalyst according to claim 7 in the degradation of fenitrothion in water.

9. The use according to claim 8, characterized in that: The following steps are involved: The metal organic framework magnetic catalyst was added into the wastewater containing fenitrothion, and the pH value was adjusted to 7, and then peracetic acid was added dropwise, and the mixture was placed in a constant temperature oscillator and shaken for 30 minutes.

10. The use according to claim 9, characterized in that: The ratio of the metal organic framework magnetic catalyst, fenitrothion, sewage and peracetic acid is (80-240) mg:20 mg:1 L:(100-200) mg; The temperature of the constant temperature oscillator is 20-30°C and the speed is 150-200r / min.

Citation Information

Patent Citations

  • Synthesis method of magnetic metal organic framework composite material

    CN103657596A

  • Magnetic metal-organic framework material with core-shell structure and preparation method therefor

    CN105233799A

  • Core / shell-type iron-based metal organic framework photo-Fenton catalyst, preparation and application thereof

    CN105833915A

  • Composite magnetic photocatalyst preparation method

    CN108620134A

  • Manganese oxide nanowire loaded ferroferric oxide magnetic Fenton catalyst as well as one-step synthesis method and application thereof

    CN111054377A