Harmless treatment device for aluminum electrolysis waste refractory material and application of harmless treatment device in preparation of asphalt mixture
By designing a harmless treatment device for aluminum electrolysis waste refractory materials, using chemical treatment to prepare surface lipophilic materials, which are used in asphalt mixtures, solving the problems of traditional pavement material consumption and environmental pollution, and achieving resource recycling and performance promote.
Patent Information
- Application Number
- CN202410996644.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Aluminum electrolytic waste refractory materials contain harmful substances, which if not handled properly, will cause environmental pollution, and traditional pavement materials consume a large amount of natural resources. How to find environmentally friendly and sustainable material solutions while ensuring pavement performance is urgently needed. .
A device for the harmless treatment of waste refractory materials from aluminum electrolysis was designed. Surface lipophilic aluminum electrolysis products were prepared through chemical treatments such as sodium hydroxide, glacial acetic acid, epichlorohydrin and dodecyltriethoxysilane hydrolysis. Waste refractory materials (DS-CT-SPL) are used in asphalt mixtures to replace limestone powder and enhance the crack resistance and durability of the road surface.
It effectively reduces the consumption of high-quality limestone ore powder, reduces environmental pollution, improves the high-temperature stability and water stability of asphalt mixtures, realizes resource recycling, and significantly improves the performance of asphalt mixtures and social environmental benefits.
Smart Images

Figure CN118744149A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of highway pavement engineering, and in particular to a harmless treatment device for aluminum electrolysis waste refractory materials and an application thereof in preparing asphalt mixture. Background Art
[0002] With the rapid economic growth and accelerated urbanization in my country, the continuous expansion of the road traffic network, especially the development of expressways, coupled with the huge amount of maintenance and renovation of existing expressways, the demand for asphalt concrete has always remained high. The preparation and use of traditional pavement materials not only consumes a lot of natural resources, but also produces corresponding environmental impacts. Therefore, how to find more environmentally friendly and sustainable material solutions while ensuring pavement performance is an issue that the current highway construction industry urgently needs to pay attention to. At the same time, as an important basic raw material industry in my country, the aluminum electrolysis industry produces a huge amount of waste refractory materials (SPL) in its production process. How to properly handle these wastes containing toxic substances has become an urgent problem to be solved in the field of environmental protection and resource recycling.
[0003] Waste refractory materials from aluminum electrolysis contain harmful substances such as fluoride, cyanide and a small amount of heavy metals. If they are not properly treated and directly discharged or landfilled, they will cause serious pollution to the environment, affect the quality of groundwater and soil health, and threaten the ecological balance and human health. In addition, the output of waste refractory materials in the aluminum electrolysis industry is huge. With the continuous progress of industrial production, the accumulation of waste will continue to increase, and the pressure on the environment and resources will increase day by day.
[0004] In this context, the application of aluminum electrolysis waste refractory materials to asphalt pavement has become an innovative attempt. Through scientific and technical means, the harmful components in the waste can be effectively reduced and converted into new building materials with certain value. The treated materials can be used as fillers for asphalt mixtures to enhance the crack resistance and durability of the pavement. This method can not only reduce the environmental burden, but also reduce dependence on natural resources and realize the recycling of resources.
[0005] The present invention provides a device and a process method for harmlessly treating waste refractory materials from aluminum electrolysis, so that the waste refractory materials can be safely used in asphalt mixtures, thereby not only achieving harmless treatment of waste materials but also improving the pavement performance of the final product. Summary of the invention
[0006] The purpose of the present invention is to provide a device for harmlessly treating waste refractory materials from aluminum electrolysis, a method for using the device to harmlessly treat waste refractory materials from aluminum electrolysis and apply the method to prepare asphalt mixture.
[0007] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0008] The invention provides a harmless treatment device for waste refractory materials from aluminum electrolysis, comprising a sodium hydroxide solution bin, an acetic acid storage bin, an epichlorohydrin bin, a main reaction bin and a dodecyltriethoxysilane hydrolysis bin; a stirring blade and a stirring magnetic coupler are installed in the main reaction bin, the stirring magnetic coupler is installed on a base inside the main reaction bin, and the stirring magnetic coupler is connected to the stirring blade through a connecting rod; a main reaction bin control box is arranged at the bottom of the main reaction bin; a motor, a control operating system, a filter screen, a filter bucket, a centrifugal pump, a transmission shaft and a polytetrafluoroethylene drainage pipe are installed in the reaction bin control box; the motor is connected to the transmission shaft; the filter screen is connected to the upper part of the filter bucket, the centrifugal pump is connected to the lower part of the filter bucket, and the centrifugal pump is connected to the polytetrafluoroethylene drainage pipe; the sodium hydroxide solution bin, the acetic acid storage bin and the epichlorohydrin bin are respectively connected to an electric three-way reversing valve through a polytetrafluoroethylene pipe, and the polytetrafluoroethylene pipe is connected to the main reaction bin. The polytetrafluoroethylene pipe is connected to the electric three-way reversing valve and the metering pump in sequence and then connected to the reaction solution inlet; the dodecyltriethoxysilane hydrolysis chamber is connected to the metering pump through a polytetrafluoroethylene pipe, and the polytetrafluoroethylene pipe is connected to the metering pump and then connected to the reaction solution inlet; the top of the main reaction chamber is connected to the hot air heating furnace through a polytetrafluoroethylene hot air conveying pipe; a heating plate, a pH sensor and a temperature sensor are also installed in the main reaction chamber, and the control operating system is respectively connected to the heating plate, the hot air heating furnace, the pH sensor and the temperature sensor; the top of the main reaction chamber is covered by the main reaction chamber upper panel, and a solid material feeding port is provided on the top of the main reaction chamber, and the solid material feeding port is covered by the main reaction chamber upper panel, and the main reaction chamber upper panel is connected through a rotating shaft; a deionized water inlet is provided near the reaction solution inlet; a reaction chamber discharge port is provided at the lower end of the side wall of the main reaction chamber.
[0009] Furthermore, the filter has a pore size of 400 meshes and is replaceable.
[0010] Furthermore, the side walls of the main reaction chamber are wrapped with a heat-insulating outer layer.
[0011] Furthermore, the upper panel of the main reaction bin and the solid material feeding port are sealed by a polytetrafluoroethylene rubber ring; the main reaction bin and the reaction bin discharge port are sealed by a polytetrafluoroethylene rubber ring.
[0012] The present invention also provides a method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the method to prepare asphalt mixture, comprising using the harmlessly treating device for waste refractory materials from aluminum electrolysis, and the method comprises the following steps:
[0013] 1) Preparation of surface lipophilic aluminum electrolysis waste refractory materials:
[0014] ① Add aluminum electrolysis waste refractory powder, calcium hypochlorite solid and calcium chloride into the main reaction chamber through the solid material feeding port, add deionized water through the deionized water inlet, the volume of deionized water is 10 times the mass of calcium hypochlorite solid, start the motor, turn off the heating plate and pH sensor, stir the stirring blades with the stirring magnetic coupler, turn off the motor after reacting for more than 48 hours, start the centrifugal pump, filter out the waste liquid in the main reaction chamber, and discharge it through the polytetrafluoroethylene drainage pipe to obtain the wet sample SPL;
[0015] ② Wash the wet SPL obtained in step ① repeatedly, add deionized water through the deionized water inlet until the water level covers the solid sample, start the pH sensor and the motor, turn off the heating plate, stir for 15 minutes, start the centrifugal pump, filter out the waste liquid in the main reaction chamber, and discharge it through the polytetrafluoroethylene drainage pipe. Repeat the operation until the pH of the solution is 6-8, start the hot air heating furnace, the motor and the temperature sensor, and maintain the temperature in the main reaction chamber at 60°C until the solid sample is dry. The obtained dry SPL is ready for use;
[0016] ③ The chitosan acetic acid solution is introduced into the main reaction chamber from the glacial acetic acid storage chamber by controlling the electric three-way reversing valve, the volume of the chitosan acetic acid solution is determined by the metering pump, the chitosan acetic acid solution reacts with the dry SPL obtained in step ②, the motor, the heating plate and the temperature sensor are started, the temperature in the main reaction chamber is controlled to be 60°C, after stirring for 6 hours, the heating plate is turned off, the electric three-way reversing valve is controlled to allow the sodium hydroxide solution to enter the main reaction chamber from the sodium hydroxide solution chamber, the speed is controlled to be 50 rpm, after stirring for 5 minutes, the centrifugal pump is started, the waste liquid in the main reaction chamber is filtered out, and discharged through the polytetrafluoroethylene drainage pipe to obtain the wet sample CT-SPL;
[0017] ④ Wash the wet sample CT-SPL obtained in step ③ repeatedly, add deionized water through the deionized water inlet until the water level covers the solid sample, start the pH sensor and the motor, turn off the heating plate, stir for 15 minutes, start the centrifugal pump, filter out the waste liquid in the main reaction chamber, and discharge it through the polytetrafluoroethylene drainage pipe. Repeat the operation until the pH of the solution is 6 to 8, and the obtained CT-SPL is ready for use;
[0018] ⑤ By controlling the electric three-way reversing valve, epichlorohydrin is introduced from the epichlorohydrin bin into the main reaction bin, the volume of epichlorohydrin is determined by the metering pump, deionized water is added through the deionized water inlet, the epichlorohydrin aqueous solution reacts with the CT-SPL obtained in step ④, the motor, the heating plate and the temperature sensor are started, the temperature in the main reaction bin is controlled to be 50° C., after stirring for 6 hours, the heating plate is turned off, the centrifugal pump is started, the waste liquid in the main reaction bin is filtered out, and discharged through the polytetrafluoroethylene drainage pipe 32 to obtain the CT-SPL after cross-linking treatment;
[0019] ⑥ Repeatedly wash the cross-linked CT-SPL obtained in step ⑤, add deionized water through the deionized water inlet until the water level covers the solid sample, start the pH sensor and the motor, turn off the heating plate, stir for 15 minutes, start the centrifugal pump, filter out the waste liquid in the main reaction chamber, and discharge it through the polytetrafluoroethylene drainage pipe. Repeat the operation until the pH of the solution is 6 to 8, start the hot air heating furnace, the motor and the temperature sensor, and keep the temperature in the main reaction chamber at 60°C until the CT-SPL is dried for use;
[0020] ⑦ The dodecyltriethoxysilane ethanol aqueous solution is introduced into the main reaction chamber from the dodecyltriethoxysilane hydrolysis chamber by controlling the metering pump, and the dodecyltriethoxysilane ethanol aqueous solution reacts with the dry CT-SPL obtained in step ⑥, and the motor is started. After stirring for 24 hours, the centrifugal pump is started to filter out the waste liquid in the main reaction chamber and discharge it through the polytetrafluoroethylene drainage pipe to obtain a DS-CT-SPL wet sample;
[0021] ⑧ Dry the wet sample DS-CT-SPL obtained in step ⑦, start the hot air heating furnace, the motor and the temperature sensor, and maintain the temperature in the main reaction chamber at 60° C. until the solid sample is dry, and obtain the surface lipophilic aluminum electrolysis waste refractory material, which is recorded as DS-CT-SPL, and take out the dry DS-CT-SPL sample through the discharge port of the reaction chamber for use;
[0022] 2) Take asphalt, coarse and fine aggregates and DS-CT-SPL, place them in an oven at 180°C and heat them for 4 hours, then place the asphalt, DS-CT-SPL and coarse and fine aggregates in an asphalt mixture mixer for mixing, and after mixing for 2 minutes, an asphalt mixture of aluminum electrolysis waste refractory materials is obtained.
[0023] Furthermore, the mass ratio of the aluminum electrolysis waste refractory material, calcium hypochlorite and calcium chloride in step ① is 1:2:5; the aluminum electrolysis waste refractory material is obtained by grinding using a vibrating screen machine, and the aluminum electrolysis waste refractory material simultaneously satisfies the requirements that the proportion of less than 0.6 mm is 100%, the proportion of less than 0.15 mm is 90-100%, and the proportion of less than 0.075 mm is 90-100%.
[0024] Furthermore, the mass ratio of the dry SPL obtained in step ② to chitosan is 50:1.
[0025] Furthermore, the mass ratio of epichlorohydrin in step ⑤ to CT-SPL obtained in step ④ is 3:100 on an absolute dry mass basis.
[0026] Furthermore, the volume of dodecyltriethoxysilane in the dodecyltriethoxysilane ethanol aqueous solution is 1% of the total volume of the solution; the dodecyltriethoxysilane ethanol aqueous solution needs to be hydrolyzed for 48 hours before being added to the main reaction chamber; the dosage ratio of the dry CT-SPL obtained in step ⑥ to the dodecyltriethoxysilane ethanol aqueous solution is 1g:10mL.
[0027] Furthermore, the mass ratio of the asphalt, coarse and fine aggregates and DS-CT-SPL is 5:96:4; the asphalt is one of road petroleum asphalt No. 70 and SBS modified asphalt; and the coarse and fine aggregates are diabase.
[0028] Compared with the prior art, the present invention has the following technical effects:
[0029] (1) The present invention uses DS-CT-SPL to replace limestone powder, which can greatly reduce the consumption of high-quality limestone powder, alleviate the problem of mineral resource scarcity, and is beneficial to ecological environment protection. The surface of the treated DS-CT-SPL material is grafted with dodecyl carbon chain non-polar functional groups, showing lipophilicity, which solves the problem that the waste refractory materials from aluminum electrolysis have good compatibility with asphalt molecules, making the adhesion effect of waste refractory materials from aluminum electrolysis better and having strong water-resistant stripping ability; SPL is a hazardous solid waste. According to statistics, the annual discharge of waste refractory materials from aluminum electrolysis in my country is as high as 1.1 million tons. The present invention uses SPL to prepare DS-CT-SPL, which is widely used in asphalt concrete, which is beneficial to environmental governance, resource conservation, and turning waste into treasure.
[0030] (2) The present invention is to treat SPL with biomaterial chitosan after calcium salt precipitation, then use epichlorohydrin to cross-link CT-SPL, and finally perform lipophilic modification. This method gives SPL stability, excellent adhesion to asphalt, effectively controls the toxicity of SPL itself, enables it to be safely used in asphalt mixtures, and significantly improves the high temperature stability and water stability of asphalt mixtures, with significant social and environmental benefits.
[0031] (3) The device integrates heating, reaction and drying functions to achieve integrated harmless treatment of SPL. The integrated design simplifies the treatment process, avoids material transfer between multiple devices, and greatly improves the treatment efficiency; since all treatment steps are completed in the same device, there is no need to repeatedly heat or cool different devices, which greatly reduces energy consumption; compared with traditional treatment methods, the device is more energy-saving and environmentally friendly, which helps to reduce carbon emissions and energy waste. The device effectively reduces the pollution of SPL to the environment through efficient harmless treatment; the integrated device design makes the operation easier, and only one device needs to be maintained and managed, which reduces the workload and operation difficulty of the operator, and also reduces the equipment failure rate and maintenance cost, and improves the reliability of the system; since the device integrates multiple functions, it does not require multiple separate processing equipment, thereby greatly reducing the equipment footprint, which is particularly important for industrial sites with limited space, and can make more efficient use of limited space resources; by reducing material transfer losses and energy consumption, it reduces production costs, avoids fines and additional costs caused by environmental problems, and improves the overall economic benefits of the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a structural schematic diagram of a harmless treatment device for aluminum electrolysis waste refractory materials according to the present invention.
[0033] Markings in the figure: 1-sodium hydroxide solution warehouse, 2-epichlorohydrin warehouse, 3-glacial acetic acid storage warehouse, 4-polytetrafluoroethylene pipeline, 5-dodecyltriethoxysilane hydrolysis warehouse, 6-metering pump, 7-hot air heating furnace, 8-polytetrafluoroethylene hot air delivery pipe, 9-electric three-way reversing valve, 10-insulation outer layer, 11-reaction warehouse discharge port, 12-polytetrafluoroethylene rubber ring, 13-deionized water inlet, 14-reaction solution inlet, 15-pH sensor, 16-temperature sensor, 17-heating plate, 18-stirring blade Plate, 19-connecting rod, 20-stirring magnetic coupler, 21-transmission shaft, 22-control operating system, 23-motor, 24-rotating shaft, 25-upper panel of the main reaction bin, 26-solid material feeding port, 27-filter screen, 28-filter bucket, 29-centrifugal pump, 30-main reaction bin control box, 31-control system display, 32-polytetrafluoroethylene drainage pipe, 33-side of the main reaction bin control box, 34-main reaction bin control box base, 35-inner base of the main reaction bin, 36-main reaction bin. DETAILED DESCRIPTION
[0034] like Figure 1As shown, a harmless treatment device for aluminum electrolysis waste refractory materials of the present invention includes 5 chambers, namely a sodium hydroxide solution chamber 1, a glacial acetic acid storage chamber 3, an epichlorohydrin chamber 2, a main reaction chamber 36 and a dodecyltriethoxysilane hydrolysis chamber 5; a stirring blade 18 and a stirring magnetic coupler 20 are installed in the main reaction chamber 36, and the stirring magnetic coupler 20 is installed on a base 35 inside the main reaction chamber, and the stirring magnetic coupler 20 is connected to the stirring blade 18 through a connecting rod 19; a main reaction chamber control box 30 is arranged at the bottom of the main reaction chamber 36; a motor 23, a control operating system 22, a filter screen 27, a filter bucket 28, a centrifugal pump 29, a transmission shaft 21 and a polytetrafluoroethylene drainage pipe 3 are installed in the reaction chamber control box 30. 2; the motor 23 is connected to the transmission shaft 21; the motor 23 drives the transmission shaft 21 to rotate, the transmission shaft 21 then drives the stirring magnetic coupler 20 to rotate, the stirring magnetic coupler 20 then drives the stirring blades 18 and the connecting rod 19 to stir, the transmission shaft 21 and the stirring magnetic coupler 20 rotate without contact, and through the effect of the magnetic field, they play a role in water isolation; the filter screen 27 is connected to the upper part of the filter bucket 28, the centrifugal pump 29 is connected to the lower part of the filter bucket 28, the centrifugal pump 29 is connected to the polytetrafluoroethylene drainage pipe 32, and the filter screen 27, the filter bucket 28 and the centrifugal pump 29 discharge the reaction wastewater through the polytetrafluoroethylene drainage pipe 32; the sodium hydroxide solution warehouse 1, the glacial acetic acid storage warehouse 3 and the epichlorohydrin warehouse 2 are respectively connected to the motor through the polytetrafluoroethylene pipe 4 The three-way reversing valve 9 is connected, the polytetrafluoroethylene pipe 4 is connected to the electric three-way reversing valve 9 and the metering pump 6 in sequence, and then connected to the reaction solution inlet 14. The solution is introduced into the main reaction chamber 36 through the reaction solution inlet 14, which can effectively control the type and volume of the solution entering the main reaction chamber 36; the dodecyltriethoxysilane hydrolysis chamber 5 is connected to the metering pump 6 through the polytetrafluoroethylene pipe 4, and the polytetrafluoroethylene pipe 4 is connected to the metering pump 6 and then connected to the reaction solution inlet 14. The hydrolysis solution is introduced into the main reaction chamber 36 through the reaction solution inlet 14, which can effectively control the volume of the dodecyltriethoxysilane ethanol aqueous solution entering the main reaction chamber 36; the top of the main reaction chamber 36 is connected to the hot air heating furnace 7 through the polytetrafluoroethylene hot air conveying pipe 8 Then, the hot air heating furnace 7 delivers hot air into the main reaction chamber 36 through the polytetrafluoroethylene hot air conveying pipe 8; the main reaction chamber 36 is also equipped with a heating plate 17, a pH sensor 15 and a temperature sensor 16, and the control operation system 22 is respectively connected to the heating plate 17, the hot air heating furnace 7, the pH sensor 15 and the temperature sensor 16, and the values of the pH sensor 15 and the temperature sensor 16 are displayed by the control system display 31 on the control operation system 22; the top of the main reaction chamber 36 is covered by the main reaction chamber upper panel 25, and a solid material feeding port 26 is opened on the top of the main reaction chamber 36, and the solid material feeding port 26 is covered by the main reaction chamber upper panel 25, and the main reaction chamber upper panel 25 is connected through a rotating shaft 24;A deionized water inlet 13 is provided near the reaction solution inlet 14; a reaction chamber discharge port 14 is provided at the lower end of the side wall of the main reaction chamber 36.
[0035] Preferably, the filter screen 27 has a pore size of 400 meshes and is replaceable.
[0036] Preferably, the side walls of the main reaction chamber 36 are wrapped with a heat-insulating outer layer 10 .
[0037] Preferably, the main reaction chamber upper panel 25 and the solid material feeding port 26 are sealed by a polytetrafluoroethylene rubber ring 12 .
[0038] Preferably, the main reaction chamber 36 and the reaction chamber discharge port 11 are sealed by a polytetrafluoroethylene rubber ring 12 .
[0039] Example 1
[0040] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture, using the harmless treatment device for waste refractory materials from aluminum electrolysis, the method has the following steps:
[0041] 1) Preparation of surface lipophilic aluminum electrolysis waste refractory (DS-CT-SPL):
[0042] ① 1000g of aluminum electrolysis waste refractory powder (SPL), 2000g of calcium hypochlorite solid and 5000g of calcium chloride are added into the main reaction chamber 36 through the solid material feeding port 26, 20000mL of deionized water is added through the deionized water inlet 13, the motor 23 is started, the heating plate 17 and the pH sensor 15 are turned off, the stirring magnetic coupler 20 drives the stirring blade 18 to stir, and the motor 23 is stopped after the reaction for more than 48 hours, the centrifugal pump 29 is started, the waste liquid in the main reaction chamber 36 is filtered out, and discharged through the polytetrafluoroethylene drainage pipe 32; the SPL powder is obtained by grinding with a vibrating sieve machine, and the particle size of the SPL powder satisfies the following conditions at the same time: the proportion of less than 0.6mm is 100%, the proportion of less than 0.15mm is 90-100%, and the proportion of less than 0.075mm is 90-100%.
[0043] ② Wash the wet sample SPL obtained in step ① repeatedly, add deionized water through the deionized water inlet 13 until the water level covers the solid sample, start the pH sensor 15 and the motor 23, turn off the heating plate 17, stir for 15 minutes, start the centrifugal pump 29, filter out the waste liquid in the main reaction chamber 36, and discharge it through the polytetrafluoroethylene drainage pipe 32. Repeat the operation until the pH value of the solution is 6, start the hot air heating furnace 7, the motor 23 and the temperature sensor 16, maintain the temperature in the main reaction chamber 36 at 60°C, until the solid sample is dry, and the obtained dry SPL is ready for use.
[0044] ③ By controlling the electric three-way reversing valve 9 and the metering pump 6, 5000mL of chitosan acetic acid solution is introduced from the glacial acetic acid storage bin 3 into the main reaction bin 36, and the chitosan acetic acid solution reacts with the dry SPL obtained in step ②, the motor 23, the heating plate 17 and the temperature sensor 16 are started, and the temperature in the main reaction bin 36 is controlled to be 60°C. After stirring for 6 hours, the heating plate 17 is turned off, and the electric three-way reversing valve 9 is controlled to allow sodium hydroxide solution (2mol / L) to enter the main reaction bin 36 from the sodium hydroxide solution bin 1. The speed is controlled to be 50 rpm. After stirring for 5 minutes, the centrifugal pump 29 is started to filter out the waste liquid in the main reaction bin 36 and discharge it through the polytetrafluoroethylene drainage pipe 32 to obtain a wet sample CT-SPL; the volume concentration of the acetic acid solution used in preparing the chitosan acetic acid solution is 5%; the mass ratio of the dry SPL obtained in step ② to chitosan is 50:1.
[0045] ④ Repeatedly wash the wet sample CT-SPL obtained in step ③, add deionized water through the deionized water inlet 13 until the water level covers the solid sample, start the pH sensor 15 and the motor 23, turn off the heating plate 17, stir for 15 minutes, start the centrifugal pump 29, filter out the waste liquid in the main reaction chamber 36, and discharge it through the polytetrafluoroethylene drainage pipe 32. Repeat the operation until the pH of the solution is 6, and the obtained CT-SPL is ready for use.
[0046] ⑤ By controlling the electric three-way reversing valve 9 and the metering pump 6, 25.4 mL of epichlorohydrin is introduced into the main reaction chamber 36 from the epichlorohydrin chamber 2, and 3000 mL of deionized water is added through the deionized water inlet 13. The epichlorohydrin aqueous solution reacts with the CT-SPL obtained in step ④, and the motor 23, the heating plate 17 and the temperature sensor 16 are started to control the temperature in the main reaction chamber 36 to 50° C. After stirring for 6 hours, the heating plate 17 is turned off, and the centrifugal pump 29 is started to filter the waste liquid in the main reaction chamber 36 and discharge it through the polytetrafluoroethylene drainage pipe 32 to obtain the cross-linked CT-SPL; the mass ratio of epichlorohydrin to the CT-SPL obtained in step ④ is 3:100 based on the absolute dry mass.
[0047] ⑥ Repeatedly wash the cross-linked CT-SPL obtained in step ⑤, add deionized water through the deionized water inlet 13 until the water level covers the solid sample, start the pH sensor 15 and the motor 23, turn off the heating plate 17, stir for 15 minutes, start the centrifugal pump 29, filter out the waste liquid in the main reaction chamber 36, and discharge it through the polytetrafluoroethylene drainage pipe 32. Repeat the operation until the pH value of the solution is 6, start the hot air heating furnace 7, the motor 23 and the temperature sensor 16, and maintain the temperature in the main reaction chamber 36 at 60°C until the CT-SPL is dried for use.
[0048] ⑦ By controlling the metering pump 6, 10000mL of dodecyltriethoxysilane ethanol aqueous solution is introduced from the dodecyltriethoxysilane hydrolysis chamber 5 into the main reaction chamber 36, and the dodecyltriethoxysilane ethanol aqueous solution reacts with the dry CT-SPL obtained in step ⑥, and the motor 23 is started. After stirring for 24 hours, the centrifugal pump 29 is started to filter out the waste liquid in the main reaction chamber 36 and discharge it through the polytetrafluoroethylene drainage pipe 32 to obtain a DS-CT-SPL wet sample; when preparing the dodecyltriethoxysilane ethanol aqueous solution, an ethanol aqueous solution with a ratio of V (anhydrous ethanol): V (deionized water) = 4:1 is used; the volume of dodecyltriethoxysilane in the dodecyltriethoxysilane ethanol aqueous solution is 1% of the total volume of the solution; the dodecyltriethoxysilane ethanol aqueous solution needs to be hydrolyzed for 48 hours before being added to the main reaction chamber 36; the usage ratio of the dry CT-SPL obtained in step ⑥ to the dodecyltriethoxysilane ethanol aqueous solution is 1g:10mL.
[0049] ⑧ Dry the wet sample DS-CT-SPL obtained in step ⑦, start the hot air heating furnace 7, the motor 23 and the temperature sensor 16, maintain the temperature in the main reaction chamber 36 at 60°C, until the solid sample is dry, and obtain the surface lipophilic aluminum electrolysis waste refractory material, recorded as DS-CT-SPL, and take out the dry DS-CT-SPL sample through the reaction chamber discharge port 11 for use.
[0050] 2) No. 70 road petroleum asphalt, diabase and DS-CT-SPL were weighed in a mass ratio of 5:96:4, and heated in an oven at 180°C for 4 hours. Then, No. 70 road petroleum asphalt, diabase and DS-CT-SPL were mixed in an asphalt mixture mixer. After mixing for 2 minutes, an asphalt mixture of aluminum electrolysis waste refractory materials was obtained.
[0051] Example 2
[0052] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture, using the harmless treatment device for waste refractory materials from aluminum electrolysis, the method has the following steps:
[0053] 1) Preparation of surface lipophilic aluminum electrolysis waste refractory (DS-CT-SPL):
[0054] ① 1000g of aluminum electrolysis waste refractory powder (SPL), 2000g of calcium hypochlorite solid and 5000g of calcium chloride are added into the main reaction chamber 36 through the solid material feeding port 26, 20000mL of deionized water is added through the deionized water inlet 13, the motor 23 is started, the heating plate 17 and the pH sensor 15 are turned off, the stirring magnetic coupler 20 drives the stirring blade 18 to stir, and the motor 23 is stopped after the reaction for more than 48 hours, the centrifugal pump 29 is started, the waste liquid in the main reaction chamber 36 is filtered out, and discharged through the polytetrafluoroethylene drainage pipe 32; the SPL powder is obtained by grinding with a vibrating sieve machine, and the particle size of the SPL powder satisfies the following conditions at the same time: the proportion of less than 0.6mm is 100%, the proportion of less than 0.15mm is 90-100%, and the proportion of less than 0.075mm is 90-100%.
[0055] ② Wash the wet sample SPL obtained in step ① repeatedly, add deionized water through the deionized water inlet 13 until the water level covers the solid sample, start the pH sensor 15 and the motor 23, turn off the heating plate 17, stir for 15 minutes, start the centrifugal pump 29, filter out the waste liquid in the main reaction chamber 36, and discharge it through the polytetrafluoroethylene drainage pipe 32. Repeat the operation until the pH value of the solution is 7, start the hot air heating furnace 7, the motor 23 and the temperature sensor 16, maintain the temperature in the main reaction chamber 36 at 60°C, until the solid sample is dry, and the obtained dry SPL is ready for use.
[0056] ③ By controlling the electric three-way reversing valve 9 and the metering pump 6, 5000mL of chitosan acetic acid solution is introduced from the glacial acetic acid storage bin 3 into the main reaction bin 36, and the chitosan acetic acid solution reacts with the dry SPL obtained in step ②, the motor 23, the heating plate 17 and the temperature sensor 16 are started, and the temperature in the main reaction bin 36 is controlled to be 60°C. After stirring for 6 hours, the heating plate 17 is turned off, and the electric three-way reversing valve 9 is controlled to allow sodium hydroxide solution (2mol / L) to enter the main reaction bin 36 from the sodium hydroxide solution bin 1. The speed is controlled to be 50 rpm. After stirring for 5 minutes, the centrifugal pump 29 is started to filter out the waste liquid in the main reaction bin 36 and discharge it through the polytetrafluoroethylene drainage pipe 32 to obtain a wet sample CT-SPL; the volume concentration of the acetic acid solution used in preparing the chitosan acetic acid solution is 5%; the mass ratio of the dry SPL obtained in step ② to the absolute dry chitosan is 50:1.
[0057] ④ Repeatedly wash the wet sample CT-SPL obtained in step ③, add deionized water through the deionized water inlet 13 until the water level covers the solid sample, start the pH sensor 15 and the motor 23, turn off the heating plate 17, stir for 15 minutes, start the centrifugal pump 29, filter out the waste liquid in the main reaction chamber 36, and discharge it through the polytetrafluoroethylene drainage pipe 32. Repeat the operation until the pH of the solution is 7, and the obtained CT-SPL is ready for use.
[0058] ⑤ By controlling the electric three-way reversing valve 9 and the metering pump 6, 25.4 mL of epichlorohydrin is introduced from the epichlorohydrin bin 2 into the main reaction bin 36, and 3000 mL of deionized water is added through the deionized water inlet 13. The epichlorohydrin aqueous solution reacts with the CT-SPL obtained in step ④, and the motor 23, the heating plate 17 and the temperature sensor 16 are started to control the temperature of the main reaction bin 36 to 50° C. After stirring for 6 hours, the heating plate 17 is turned off, and the centrifugal pump 29 is started to filter the waste liquid in the main reaction bin 36 and discharge it through the polytetrafluoroethylene drainage pipe 32 to obtain the cross-linked CT-SPL; the mass ratio of epichlorohydrin to the CT-SPL obtained in step ④ is 3:100 based on the absolute dry mass.
[0059] ⑥ Repeatedly wash the cross-linked CT-SPL obtained in step ⑤, add deionized water through the deionized water inlet 13 until the water level covers the solid sample, start the pH sensor 15 and the motor 23, turn off the heating plate 17, stir for 15 minutes, start the centrifugal pump 29, filter out the waste liquid in the main reaction chamber 36, and discharge it through the polytetrafluoroethylene drainage pipe 32. Repeat the operation until the pH of the solution is 7, start the hot air heating furnace 7, the motor 23 and the temperature sensor 16, and keep the temperature in the main reaction chamber 36 at 60°C until the CT-SPL is dried for use.
[0060] ⑦ By controlling the metering pump 6, 10000mL of dodecyltriethoxysilane ethanol aqueous solution is introduced from the dodecyltriethoxysilane hydrolysis chamber 5 into the main reaction chamber 36, and the dodecyltriethoxysilane ethanol aqueous solution reacts with the dry CT-SPL obtained in step ⑥, and the motor 23 is started. After stirring for 24 hours, the centrifugal pump 29 is started to filter out the waste liquid in the main reaction chamber 36 and discharge it through the polytetrafluoroethylene drainage pipe 32 to obtain a DS-CT-SPL wet sample. The dodecyltriethoxysilane ethanol aqueous solution is prepared by using an ethanol aqueous solution with a ratio of V (anhydrous ethanol): V (deionized water) = 4:1; the dodecyltriethoxysilane volume in the dodecyltriethoxysilane ethanol aqueous solution is 1% of the total volume of the solution; the dodecyltriethoxysilane ethanol aqueous solution needs to be hydrolyzed for 48 hours before being added to the main reaction chamber 36; the amount ratio of the dry CT-SPL obtained in step ⑥ to the dodecyltriethoxysilane ethanol aqueous solution is 1g: 10mL.
[0061] ⑧ Dry the wet sample DS-CT-SPL obtained in step ⑦, start the hot air heating furnace 7, the motor 23 and the temperature sensor 16, maintain the temperature in the main reaction chamber 36 at 60°C, until the solid sample is dry, and obtain the surface lipophilic aluminum electrolysis waste refractory material, recorded as DS-CT-SPL, and take out the dry DS-CT-SPL sample through the reaction chamber discharge port 11 for use.
[0062] 2) The preparation of asphalt mixture of waste refractory materials from aluminum electrolysis is the same as in Example 1.
[0063] Example 3
[0064] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture, using the harmless treatment device for waste refractory materials from aluminum electrolysis, the method has the following steps:
[0065] 1) Preparation of surface lipophilic aluminum electrolysis waste refractory (DS-CT-SPL):
[0066] ① 1000g of aluminum electrolysis waste refractory powder (SPL), 2000g of calcium hypochlorite solid and 5000g of calcium chloride are added into the main reaction chamber 36 through the solid material feeding port 26, 20000mL of deionized water is added through the deionized water inlet 13, the motor 23 is started, the heating plate 17 and the pH sensor 15 are turned off, the stirring magnetic coupler 20 drives the stirring blade 18 to stir, and the motor 23 is stopped after the reaction for more than 48 hours, the centrifugal pump 29 is started, the waste liquid in the main reaction chamber 36 is filtered out, and discharged through the polytetrafluoroethylene drainage pipe 32; the SPL powder is obtained by grinding with a vibrating sieve machine, and the particle size of the SPL powder satisfies the following conditions at the same time: the proportion of less than 0.6mm is 100%, the proportion of less than 0.15mm is 90-100%, and the proportion of less than 0.075mm is 90-100%.
[0067] ② Wash the wet sample SPL obtained in step ① repeatedly, add deionized water through the deionized water inlet 13 until the water level covers the solid sample, start the pH sensor 15 and the motor 23, turn off the heating plate 17, stir for 15 minutes, start the centrifugal pump 29, filter out the waste liquid in the main reaction chamber 36, and discharge it through the polytetrafluoroethylene drainage pipe 32. Repeat the operation until the pH value of the solution is 8, start the hot air heating furnace 7, the motor 23 and the temperature sensor 16, maintain the temperature in the main reaction chamber 36 at 60°C, until the solid sample is dry, and the obtained dry SPL is ready for use.
[0068] ③ By controlling the electric three-way reversing valve 9 and the metering pump 6, 5000mL of chitosan acetic acid solution is introduced from the glacial acetic acid storage bin 3 into the main reaction bin 36, and the chitosan acetic acid solution reacts with the dry SPL obtained in step ②, the motor 23, the heating plate 17 and the temperature sensor 16 are started, and the temperature of the main reaction bin 36 is controlled to be 60°C. After stirring for 6 hours, the heating plate 17 is turned off, and the electric three-way reversing valve 9 is controlled to allow sodium hydroxide solution (2mol / L) to enter the main reaction bin 36 from the sodium hydroxide solution bin 1. The speed is controlled to be 50 rpm. After stirring for 5 minutes, the centrifugal pump 29 is started to filter out the waste liquid in the main reaction bin 36 and discharge it through the polytetrafluoroethylene drainage pipe 32 to obtain a wet sample CT-SPL; the volume concentration of the acetic acid solution used in preparing the chitosan acetic acid solution is 5%; the mass ratio of the dry SPL obtained in step ② to the absolute dry chitosan is 50:1.
[0069] ④ Repeatedly wash the wet sample CT-SPL obtained in step ③, add deionized water through the deionized water inlet 13 until the water level covers the solid sample, start the pH sensor 15 and the motor 23, turn off the heating plate 17, stir for 15 minutes, start the centrifugal pump 29, filter out the waste liquid in the main reaction chamber 36, and discharge it through the polytetrafluoroethylene drainage pipe 32. Repeat the operation until the pH of the solution is 8, and the obtained CT-SPL is ready for use.
[0070] ⑤ By controlling the electric three-way reversing valve 9 and the metering pump 6, 25.4 mL of epichlorohydrin is introduced from the epichlorohydrin bin 2 into the main reaction bin 36, and 3000 mL of deionized water is added through the deionized water inlet 13. The epichlorohydrin aqueous solution reacts with the CT-SPL obtained in step ④, and the motor 23, the heating plate 17 and the temperature sensor 16 are started to control the temperature of the main reaction bin 36 to 50° C. After stirring for 6 hours, the heating plate 17 is turned off, and the centrifugal pump 29 is started to filter the waste liquid in the main reaction bin 36 and discharge it through the polytetrafluoroethylene drainage pipe 32 to obtain the cross-linked CT-SPL; the mass ratio of epichlorohydrin to the CT-SPL obtained in step ④ is 3:100 based on the absolute dry mass.
[0071] ⑥ Repeatedly wash the cross-linked CT-SPL obtained in step ⑤, add deionized water through the deionized water inlet 13 until the water level covers the solid sample, start the pH sensor 15 and the motor 23, turn off the heating plate 17, stir for 15 minutes, start the centrifugal pump 29, filter out the waste liquid in the main reaction chamber 36, and discharge it through the polytetrafluoroethylene drainage pipe 32. Repeat the operation until the pH of the solution is 8, start the hot air heating furnace 7, the motor 23 and the temperature sensor 16, and keep the temperature in the main reaction chamber 36 at 60°C until the CT-SPL is dried for use.
[0072] ⑦ By controlling the metering pump 6, 10000mL of dodecyltriethoxysilane ethanol aqueous solution is introduced from the dodecyltriethoxysilane hydrolysis chamber 5 into the main reaction chamber 36, and the dodecyltriethoxysilane ethanol aqueous solution reacts with the dry CT-SPL obtained in step ⑥, and the motor 23 is started. After stirring for 24 hours, the centrifugal pump 29 is started to filter out the waste liquid in the main reaction chamber 36 and discharge it through the polytetrafluoroethylene drainage pipe 32 to obtain a DS-CT-SPL wet sample. The dodecyltriethoxysilane ethanol aqueous solution is prepared by using an ethanol aqueous solution with a ratio of V (anhydrous ethanol): V (deionized water) = 4:1; the dodecyltriethoxysilane volume in the dodecyltriethoxysilane ethanol aqueous solution is 1% of the total volume of the solution; the dodecyltriethoxysilane ethanol aqueous solution needs to be hydrolyzed for 48 hours before being added to the main reaction chamber 36; the amount ratio of the dry CT-SPL obtained in step ⑥ to the dodecyltriethoxysilane ethanol aqueous solution is 1g: 10mL.
[0073] ⑧ Dry the wet sample DS-CT-SPL obtained in step ⑦, start the hot air heating furnace 7, the motor 23 and the temperature sensor 16, maintain the temperature in the main reaction chamber 36 at 60°C, until the solid sample is dry, and obtain the surface lipophilic aluminum electrolysis waste refractory material, recorded as DS-CT-SPL, and take out the dry DS-CT-SPL sample through the reaction chamber discharge port 11 for use.
[0074] 2) The preparation of asphalt mixture of waste refractory materials from aluminum electrolysis is the same as in Example 1.
[0075] Example 4
[0076] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture, using the harmless treatment device for waste refractory materials from aluminum electrolysis, the method has the following steps:
[0077] 1) The preparation of surface lipophilic aluminum electrolysis waste refractory material (DS-CT-SPL) is the same as in Example 1;
[0078] 2) SBS modified asphalt, diabase and DS-CT-SPL were weighed in a mass ratio of 5:96:4, and heated in an oven at 180°C for 4 hours. Then, the SBS modified asphalt, diabase and DS-CT-SPL were mixed in an asphalt mixture mixer. After mixing for 2 minutes, an asphalt mixture of aluminum electrolysis waste refractory materials was obtained.
[0079] Example 5
[0080] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture, using the harmless treatment device for waste refractory materials from aluminum electrolysis, the method has the following steps:
[0081] 1) The preparation of surface oleophilic aluminum electrolysis waste refractory material (DS-CT-SPL) is the same as in Example 2;
[0082] 2) The preparation of asphalt mixture of waste refractory materials from aluminum electrolysis is the same as in Example 4.
[0083] Example 6
[0084] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture, comprising the following steps:
[0085] 1) The preparation of surface lipophilic aluminum electrolysis waste refractory material (DS-CT-SPL) is the same as in Example 3;
[0086] 2) The preparation of asphalt mixture of waste refractory materials from aluminum electrolysis is the same as in Example 4.
[0087] Comparative Example 1:
[0088] Replace DS-CT-SPL with limestone powder in the same proportion. Other materials and preparation processes are as follows:
[0089] Road petroleum asphalt No. 70, diabase and limestone powder are weighed in a mass ratio of 5:96:4, placed in an oven at 180°C for heating for 4 hours, and then placed in an asphalt mixture mixer for mixing. After mixing for 2 minutes, the asphalt mixture is obtained.
[0090] Comparative Example 2:
[0091] Replace DS-CT-SPL with limestone powder in the same proportion. Other materials and preparation processes are as follows:
[0092] SBS modified asphalt, diabase and limestone powder were weighed in a mass ratio of 5:96:4, heated in an oven at 180°C for 4 hours, and then mixed in an asphalt mixer. After mixing for 2 minutes, the asphalt mixture was obtained.
[0093] The asphalt mixture prepared by the above method was tested for performance according to the current domestic standards "Test Procedure for Asphalt and Asphalt Mixture for Highway Engineering" (JTGE20-2011) and "Solid Waste Leaching Method - Horizontal Oscillation Method" (HJ557-2010):
[0094] Test items:
[0095]
[0096]
[0097] The standard rutting test, the Marshall test and the freeze-thaw splitting test were all tested in accordance with the "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTGE20-2011). In order to further verify the effect of DS-CT-SPL on the high-temperature performance of asphalt concrete, and considering the long-term hot and humid climate conditions in the southern region, on the basis of the standard rutting test, the test wheel contact pressure was kept at 0.7MPa, and the test temperature was increased from 60℃ to 70℃, and the asphalt mixture was subjected to a high-temperature rutting test. At the same time, combined with the current situation of the increasing number of automobiles in my country, the continuous development of the transportation industry, and the increase in the average load of freight trucks or even overloading, on the basis of the standard rutting test, the test temperature was kept at 60℃, and the test wheel contact pressure was increased from 0.7MPa to 1.0MPa, and the asphalt mixture was subjected to a heavy-load rutting test.
[0098] The fluoride ion leaching experiment of asphalt mixture is carried out according to the "Solid Waste Leaching Reading Leaching Method Horizontal Oscillation Method" HJ557-2010, and the fluoride ion concentration test in the leachate is carried out according to the method of "Hazardous Waste Identification Standard Toxic Substance Content Identification" GB5085.6-2007.
[0099] In addition, to further verify the effect of DS-CT-SPL on the water stability of asphalt concrete, a water rutting test was conducted on the basis of the standard rutting test. The test temperature was kept at 60°C and the test wheel contact pressure was kept at 0.7 MPa. The rutting specimens that had been formed and placed at room temperature for 48 hours were placed in a stainless steel high-temperature resistant basin together with the test mold. A sufficient amount of 60°C water was injected to completely immerse the specimens and the test mold. The basin containing the specimens and 60°C water was then transferred to an oven set at 60°C for 5 hours, followed by a rutting test to explore the effect of DS-CT-SPL on the anti-rutting performance of asphalt concrete under pavement immersion conditions.
[0100] The test results are as follows:
[0101] 1. High temperature stability study:
[0102]
[0103]
[0104] It can be seen from the test results and comparison results that due to the addition of DS-CT-SPL, the standard dynamic stability of the matrix asphalt mixture reached a maximum of 6062 times / mm, and the standard dynamic stability of the SBS asphalt mixture reached a maximum of 7721 times / mm, which can enhance the anti-rutting performance of the asphalt mixture and to a certain extent improve and maintain the ability of the asphalt mixture to resist rutting damage.
[0105] 2. Water stability study:
[0106] (I) Immersion Marshall test:
[0107] Test Project Standard stability (kN) Standard flow value (mm) Water immersion stability (kN) Residual stability (%) Example 1 12.54 4.46 11.32 90.27 Example 2 12.89 4.22 11.22 87.04 Example 3 11.45 4.97 10.21 89.17 Comparative Example 1 9.98 5.36 8.07 80.86 Example 4 15.13 4.09 13.88 91.74 Example 5 14.06 4.26 12.68 90.18 Example 6 16.13 3.91 14.60 90.51 Comparative Example 2 10.6 5.46 8.87 83.68
[0108] It can be seen from the test results and comparison results that due to the addition of DS-CT-SPL, the residual stability of the matrix asphalt mixture after immersion in water reached up to 90.27%, and the residual stability of the SBS asphalt mixture after immersion in water reached up to 91.74%. Compared with mineral powder fillers, DS-CT-SPL can effectively improve the water stability of asphalt mixtures.
[0109] (II) Freeze-thaw splitting test:
[0110]
[0111]
[0112] From the test results and comparison results, it can be seen that due to the addition of DS-CT-SPL, the freeze-thaw splitting tensile strength ratio of the matrix asphalt mixture reached a maximum of 88.41%, and the freeze-thaw splitting tensile strength ratio of the SBS asphalt mixture reached a maximum of 91.62%. Compared with mineral powder filler, DS-CT-SPL improves and maintains the water stability of asphalt mixture to a certain extent.
[0113] (III) Water rutting test:
[0114] Test Project Dynamic stability under water immersion (times / mm) Example 1 3399 Example 2 3264 Example 3 3044 Comparative Example 1 2449 Example 4 4174 Example 5 3990 Example 6 4413 Comparative Example 2 3322
[0115] It can be seen from the test results and comparative results that due to the addition of DS-CT-SPL, the dynamic stability of the matrix asphalt mixture under water immersion has increased to 3399 times / mm at most, and the dynamic stability of the SBS asphalt mixture under water immersion has increased to 4413 times / mm at most. Compared with mineral powder filler, the addition of DS-CT-SPL can also improve and maintain the ability of the asphalt mixture to resist rutting disease to a certain extent, and also improve and maintain the ability of the asphalt mixture to resist water damage to a certain extent.
[0116] (V) Fluoride ion leaching test
[0117] Test Project Fluoride ion concentration of leachate (mg / L) Example 1 1.76 Example 2 1.41 Example 3 1.58 Example 4 0.99 Example 5 0.91 Example 6 1.34
[0118] It can be seen from the test results and comparative results that the maximum fluoride ion leaching liquid of asphalt mixture is only 1.76 mg / L (<100 mg / L), which is far less than the requirement of the specification (GB5085.6-2007). After the surface lipophilicity modification treatment, SPL is more compatible with asphalt. There is a barrier of asphalt molecules between water molecules and inorganic fluorides in SPL, which effectively reduces the ionization of inorganic fluorides in water and effectively inhibits the leaching of fluoride ions.
Claims
1. A harmless treatment device for aluminum electrolysis waste refractory materials, characterized by: It includes a sodium hydroxide solution bin, an acetic acid storage bin, an epichlorohydrin bin, a main reaction bin and a dodecyltriethoxysilane hydrolysis bin; a stirring blade and a stirring magnetic coupler are installed in the main reaction bin, the stirring magnetic coupler is installed on the inner base of the main reaction bin, and the stirring magnetic coupler is connected to the stirring blade through a connecting rod; a main reaction bin control box is arranged at the bottom of the main reaction bin; a motor, a control operating system, a filter screen, a filter bucket, a centrifugal pump, a transmission shaft and a polytetrafluoroethylene drainage pipe are installed in the reaction bin control box; the motor is connected to the transmission shaft; the filter screen is connected to the upper part of the filter bucket, the centrifugal pump is connected to the lower part of the filter bucket, and the centrifugal pump is connected to the polytetrafluoroethylene drainage pipe; the sodium hydroxide solution bin, the acetic acid storage bin and the epichlorohydrin bin are respectively connected to the electric three-way reversing valve through a polytetrafluoroethylene pipe, and the polytetrafluoroethylene pipe is connected to the electric The three-way reversing valve and the metering pump are connected to the reaction solution inlet; the dodecyltriethoxysilane hydrolysis chamber is connected to the metering pump through a polytetrafluoroethylene pipe, and the polytetrafluoroethylene pipe is connected to the metering pump and then connected to the reaction solution inlet; the top of the main reaction chamber is connected to the hot air heating furnace through a polytetrafluoroethylene hot air conveying pipe; a heating plate, a pH sensor and a temperature sensor are also installed in the main reaction chamber, and the control operating system is respectively connected to the heating plate, the hot air heating furnace, the pH sensor and the temperature sensor; the top of the main reaction chamber is covered by the main reaction chamber upper panel, and a solid material feeding port is provided on the top of the main reaction chamber, and the solid material feeding port is covered by the main reaction chamber upper panel, and the main reaction chamber upper panel is connected through a rotating shaft; a deionized water inlet is provided near the reaction solution inlet; a reaction chamber discharge port is provided at the lower end of the side wall of the main reaction chamber.
2. The harmless treatment device for aluminum electrolysis waste refractory materials according to claim 1 is characterized by: The filter has a pore size of 400 mesh and is replaceable.
3. The harmless treatment device for aluminum electrolysis waste refractory materials according to claim 1 is characterized by: The side walls of the main reaction chamber are wrapped with a heat-insulating outer layer.
4. The harmless treatment device for aluminum electrolysis waste refractory materials according to claim 1 is characterized by: The upper panel of the main reaction bin and the solid material feeding port are sealed by a polytetrafluoroethylene rubber ring; the main reaction bin and the reaction bin discharge port are sealed by a polytetrafluoroethylene rubber ring.
5. A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture, characterized in that: The method comprises the following steps: 1) Preparation of surface lipophilic aluminum electrolysis waste refractory materials: ① Add aluminum electrolysis waste refractory powder, calcium hypochlorite solid and calcium chloride into the main reaction chamber through the solid material feeding port, add deionized water through the deionized water inlet, the volume of deionized water is 10 times the mass of calcium hypochlorite solid, start the motor, turn off the heating plate and pH sensor, stir the stirring blades with the stirring magnetic coupler, turn off the motor after reacting for more than 48 hours, start the centrifugal pump, filter out the waste liquid in the main reaction chamber, and discharge it through the polytetrafluoroethylene drainage pipe to obtain the wet sample SPL; ② Wash the wet SPL obtained in step ① repeatedly, add deionized water through the deionized water inlet until the water level covers the solid sample, start the pH sensor and the motor, turn off the heating plate, stir for 15 minutes, start the centrifugal pump, filter out the waste liquid in the main reaction chamber, and discharge it through the polytetrafluoroethylene drainage pipe. Repeat the operation until the pH of the solution is 6-8, start the hot air heating furnace, the motor and the temperature sensor, and maintain the temperature in the main reaction chamber at 60°C until the solid sample is dry. The obtained dry SPL is ready for use; ③ The chitosan acetic acid solution is introduced into the main reaction chamber from the glacial acetic acid storage chamber by controlling the electric three-way reversing valve, the volume of the chitosan acetic acid solution is determined by the metering pump, the chitosan acetic acid solution reacts with the dry SPL obtained in step ②, the motor, the heating plate and the temperature sensor are started, the temperature in the main reaction chamber is controlled to be 60°C, after stirring for 6 hours, the heating plate is turned off, the electric three-way reversing valve is controlled to allow the sodium hydroxide solution to enter the main reaction chamber from the sodium hydroxide solution chamber, the speed is controlled to be 50 rpm, after stirring for 5 minutes, the centrifugal pump is started, the waste liquid in the main reaction chamber is filtered out, and discharged through the polytetrafluoroethylene drainage pipe to obtain the wet sample CT-SPL; ④ Wash the wet sample CT-SPL obtained in step ③ repeatedly, add deionized water through the deionized water inlet until the water level covers the solid sample, start the pH sensor and the motor, turn off the heating plate, stir for 15 minutes, start the centrifugal pump, filter out the waste liquid in the main reaction chamber, and discharge it through the polytetrafluoroethylene drainage pipe. Repeat the operation until the pH of the solution is 6 to 8, and the obtained CT-SPL is ready for use; ⑤ By controlling the electric three-way reversing valve, epichlorohydrin is introduced from the epichlorohydrin bin into the main reaction bin, the volume of epichlorohydrin is determined by the metering pump, deionized water is added through the deionized water inlet, the epichlorohydrin aqueous solution reacts with the CT-SPL obtained in step ④, the motor, the heating plate and the temperature sensor are started, the temperature in the main reaction bin is controlled to be 50° C., after stirring for 6 hours, the heating plate is turned off, the centrifugal pump is started, the waste liquid in the main reaction bin is filtered out, and discharged through the polytetrafluoroethylene drainage pipe 32 to obtain the CT-SPL after cross-linking treatment; ⑥ Repeatedly wash the cross-linked CT-SPL obtained in step ⑤, add deionized water through the deionized water inlet until the water level covers the solid sample, start the pH sensor and the motor, turn off the heating plate, stir for 15 minutes, start the centrifugal pump, filter out the waste liquid in the main reaction chamber, and discharge it through the polytetrafluoroethylene drainage pipe. Repeat the operation until the pH of the solution is 6 to 8, start the hot air heating furnace, the motor and the temperature sensor, and keep the temperature in the main reaction chamber at 60°C until the CT-SPL is dried for use; ⑦ The dodecyltriethoxysilane ethanol aqueous solution is introduced into the main reaction chamber from the dodecyltriethoxysilane hydrolysis chamber by controlling the metering pump, and the dodecyltriethoxysilane ethanol aqueous solution reacts with the dry CT-SPL obtained in step ⑥, and the motor is started. After stirring for 24 hours, the centrifugal pump is started to filter out the waste liquid in the main reaction chamber and discharge it through the polytetrafluoroethylene drainage pipe to obtain a DS-CT-SPL wet sample; ⑧ Dry the wet sample DS-CT-SPL obtained in step ⑦, start the hot air heating furnace, the motor and the temperature sensor, and maintain the temperature in the main reaction chamber at 60° C. until the solid sample is dry, and obtain the surface lipophilic aluminum electrolysis waste refractory material, which is recorded as DS-CT-SPL, and take out the dry DS-CT-SPL sample through the discharge port of the reaction chamber for use; 2) Take asphalt, coarse and fine aggregates and DS-CT-SPL, place them in an oven at 180°C and heat them for 4 hours, then place the asphalt, DS-CT-SPL and coarse and fine aggregates in an asphalt mixture mixer for mixing, and after mixing for 2 minutes, an asphalt mixture of aluminum electrolysis waste refractory materials is obtained.
6. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 5, characterized in that: The mass ratio of the aluminum electrolysis waste refractory material, calcium hypochlorite and calcium chloride in step ① is 1:2:5; the aluminum electrolysis waste refractory material is obtained by grinding with a vibrating screen machine, and the aluminum electrolysis waste refractory material simultaneously satisfies the requirements that the proportion of less than 0.6 mm is 100%, the proportion of less than 0.15 mm is 90-100%, and the proportion of less than 0.075 mm is 90-100%.
7. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture according to claim 5, characterized in that: The mass ratio of the dry SPL obtained in step ② to chitosan is 50:
1.
8. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture according to claim 5, characterized in that: The mass ratio of epichlorohydrin in step ⑤ to CT-SPL obtained in step ④ is 3:100 based on absolute dry mass.
9. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 5, characterized in that: The dodecyltriethoxysilane ethanol aqueous solution has a dodecyltriethoxysilane content of 1% by volume of the total volume of the solution; the dodecyltriethoxysilane ethanol aqueous solution needs to be hydrolyzed for 48 hours before being added to the main reaction chamber; the ratio of the dried CT-SPL obtained in step ⑥ to the dodecyltriethoxysilane ethanol aqueous solution is 1g:10mL.
10. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying the waste refractory materials to prepare asphalt mixture according to claim 5, characterized in that: The mass ratio of the asphalt, coarse and fine aggregates and DS-CT-SPL is 5:96:4; the asphalt is one of road petroleum asphalt No. 70 and SBS modified asphalt; and the coarse and fine aggregates are diabase.
Citation Information
Patent Citations
Conversion method and system of sodium-containing and fluorine-containing compounds in aluminum electrolysis overhaul slag
CN109108050A
Recycled asphalt mixture and preparation method thereof
CN109678397A
Online monitoring early-warning device and method for anaerobic fermentation process
CN110361551A
Efficient harmless method for fluoride and cyanide in waste refractory material
CN112692029A
Process for preparing a bituminous mix, device for storing hot aggregates, process and device for maintaining the hot aggregate storage temperature
WO2017103505A1