Manufacturing method for rapidly forming large shaft solid forgings by using continuous casting billets

Through the combined process of die forging extrusion and free forging, continuous casting rod-shaped blanks made of high-carbon alloy steel are used to quickly form large shaft solid forgings, which solves the problems of pass rate, cost and cycle in the traditional process, and achieves high quality and Efficient manufacturing.

CN118744219AActive Publication Date: 2024-10-08TIANJIN HEAVY EQUIP ENG RES +1

Patent Information

Application Number
CN202411033317.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-08
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The traditional process of large shaft solid forgings has shortcomings in terms of product qualification rate, production cost, production cycle and material utilization rate, and it is difficult to meet the needs of high strength and high precision.

Method used

Continuously cast rod-shaped billets made of high-carbon alloy steel are used for die forging and extrusion. By controlling the initial diameter of the billet, extrusion ratio, heating temperature and holding time, combined with free forging processing, rapid prototyping of large shaft solid forgings is achieved.

Benefits of technology

It improves the product qualification rate, reduces production costs, shortens the production cycle, improves material utilization, and ensures high-quality finished products. Especially under the conditions of high internal quality requirements, the qualification rate reaches more than 95%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744219A_ABST
    Figure CN118744219A_ABST
Patent Text Reader

Abstract

The invention relates to a manufacturing method for rapidly forming a large-scale shaft solid forge piece by using a continuous casting billet, belongs to the field of large-scale shaft forge piece manufacturing, and solves at least one of the following problems existing in a traditional process of the large-scale shaft solid forge piece: (1) the product percent of pass is difficult to meet a relatively high expected target; (2) the production cost is high; (3) the production period is relatively long; and (4) the material utilization rate is low. The manufacturing method comprises the steps that S1, a blank is prepared, specifically, a continuous casting rod-shaped blank made of high-carbon alloy steel is prepared; s2, the continuous casting rod-shaped blank is subjected to first heating number heating, die forging extrusion is adopted, the continuous casting rod-shaped blank is extruded and formed into an X-section type shaft extrusion part, and X ranges from 1 to 3; and S3, if the section number Y of the large shaft type solid forge piece is larger than 3, the shaft type extrusion piece is heated, and the roller neck except the X section is machined in a free forging mode. Through process design and parameter control, the product percent of pass is increased, the production cost is reduced, the production period is shortened, and the material utilization rate is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of manufacturing large shaft forgings, and in particular to a manufacturing method for rapidly molding large shaft solid forgings using continuous casting billets. Background Art

[0002] The traditional process of large solid shaft forgings usually uses vacuum smelting and pouring to obtain die-cast steel ingots, or under the condition of high internal quality requirements, electroslag remelting or other methods are required to produce blanks, and then a large hydraulic press or oil press is used for free forging. Generally, the steel ingot is compacted by pressing the jaws, upsetting and drawing once or multiple times, and finally the shaft forgings are completed by drawing and cutting. The process is as follows: die-cast steel ingot / electroslag ingot → free forging (pressing the jaws, upsetting + drawing, cutting and cutting).

[0003] However, the above traditional processes have shortcomings in product qualification rate, production cost, production cycle and material utilization rate. In summary, with the development of equipment manufacturing industry and the continuous improvement of green manufacturing concept, it is indeed necessary to develop new methods to manufacture large shaft solid forgings, aiming to improve product qualification rate, reduce production cost, shorten production cycle and improve material utilization rate. Summary of the invention

[0004] In view of the above analysis, the present invention aims to provide a manufacturing method for large solid shaft forgings using continuous casting billets for rapid prototyping, so as to solve at least one of the following problems existing in the traditional process of large solid shaft forgings: (1) the product qualification rate is difficult to meet the higher expected target; (2) the production cost is high; (3) the production cycle is long; (4) the material utilization rate is low.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] The present invention provides a method for manufacturing a large-scale shaft solid forging by using a continuous casting billet for rapid prototyping. The manufacturing method comprises the following steps:

[0007] S1. Prepare the billet: the billet is a continuous casting rod billet made of high carbon alloy steel;

[0008] According to the maximum diameter D1 of the large shaft solid forging to be formed and the extrusion ratio R, the initial diameter D0 of the billet is determined to satisfy: D0 = D1 × R 1 / 2 , R>2;

[0009] According to the weight M1 of the large solid shaft forging to be formed and considering the residual pressure F during die forging and extrusion and the metal oxidation loss L during each heating process, the initial weight M0 of the billet is determined to meet the following conditions: M0 = M1 × (1 + F) / (1 - L) n; Among them, F is 5% to 10%, L is 1% to 2%, and n is the number of fires;

[0010] S2, heating the continuously cast rod-shaped billet for the first time, and then extruding the continuously cast rod-shaped billet into an X-segment shaft extrusion by die forging and extrusion, removing the excess part, where X is 1 to 3;

[0011] S3, if the number of segments Y of the large shaft solid forging to be formed is greater than 3, the X-segment shaft extrusion obtained in step S2 is subjected to (n-1) heat heating, and the remaining (YX) segments of the roll neck other than the X segments are processed by free forging to obtain the large shaft solid forging;

[0012] Among them, n≥2, and the maximum diameter of the roll neck in the remaining (YX) segments is less than D1.

[0013] Further, in step S2, the main steps of the first heating include: heating the continuously cast rod-shaped billet to T1=1200~1250°C and keeping it warm, the holding time t1=D0×k1, k1=120min~150min / 100mm, and D0 is in mm.

[0014] Further, in step S3, when the number of segments Y is 4 to 7, n=2, that is, the X-segment shaft extrusion obtained in step S2 is heated for the second time.

[0015] Further, in step S3, the main steps of the second heating include: heating the X-section shaft extrusion to T2 = 1150 ~ 1200 ° C and keeping it warm, the insulation time t2 = D1 × k2, k2 = 40min ~ 55min / 100mm, D1 unit is mm.

[0016] Furthermore, the extrusion ratio R satisfies: 2.5≤R≤4.

[0017] Furthermore, in step S2, the speed of die forging extrusion is controlled at 1 mm / s to 10 mm / s, wherein the speed V1 at the initial stage of extrusion, the speed V2 at the middle stage of extrusion, and the speed V3 at the later stage of extrusion satisfy: V3>V1>V2.

[0018] Furthermore, the speed V1 in the initial stage of extrusion is 4 mm / s to 6 mm / s, the speed V2 in the middle stage of extrusion is 1 mm / s to 3 mm / s, and the speed V3 in the late stage of extrusion is 8 mm / s to 10 mm / s.

[0019] Furthermore, in step S1, chamfers are machined on the upper and lower end surfaces of the blank, wherein the chamfer of the upper end surface is an arc with a radius of 130 to 170 mm, and the chamfer of the lower end surface is an arc with a radius of 80 to 120 mm.

[0020] Furthermore, in step S2, the main steps of the die forging extrusion include: firstly coating the inner surface of the die forging extrusion mold with glass powder for lubrication, then placing the heated blank into the mold, and then using a large press to apply pressure to the mold. The mold will transfer this pressure to the blank, so that the blank is formed under the action of three-way compressive stress and the inside of the blank is effectively pressed.

[0021] Further, in step S1, the chemical composition of the high carbon alloy steel includes, by mass percentage, C: 0.8-0.9%, Si: 0.65-0.75%, Mn: 0.35-0.45%, P: 0.010-0.015%, S: 0.001-0.005%, Cr: 4.95-5.05%, Ni: 0.30-0.35%, Mo: 0.20-0.25%, V: 0.10-0.15%, N: 0.003-0.005%, and the remainder is Fe and unavoidable impurities.

[0022] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0023] (1) The present invention uses continuous casting billets as forging raw materials, which greatly reduces manufacturing costs. The continuous casting billets are directly extruded into shaft extrusions of 3 sections or less by die forging and extrusion. If necessary, free forging is combined to process the remaining parts exceeding 3 sections. Through process design and parameter control, the product qualification rate is improved, which can meet higher expected goals, reduce production costs, shorten production cycles, and improve material utilization.

[0024] (2) In the present invention, when calculating the initial diameter of the billet, by controlling the extrusion ratio R to be greater than 2, it is helpful to ensure that the loose cracks in the core of the continuous casting billet can be effectively pressed together under extrusion in the mold, which effectively solves the problem that the existing continuous casting billet cannot be used to manufacture large shaft solid forgings due to defects in the core. The product obtained by the present invention has good overall quality, especially the core can be guaranteed to be free of defects. Even under the condition of high internal quality requirements, the product qualification rate of the present invention can reach more than 95%. Compared with the existing process, the product obtained by the present invention has higher dimensional accuracy, especially the roller body with the largest diameter and the roller neck with a larger diameter.

[0025] (3) In the present invention, when calculating the initial mass of the billet, by controlling the residual pressure F and the metal oxidation loss L during each heating process to be within an appropriate numerical range, it can be ensured that the expected residual pressure and oxidation loss are closer to the actual situation, thereby improving material utilization, reducing material costs, and avoiding unnecessary processing allowance waste. Compared with the traditional free forging process using die-cast steel ingots or electroslag ingots, the present invention uses the "continuous casting billet → die forging extrusion forming" near-net forming method to complete the manufacture of large-scale shaft-type solid forgings of 3 sections or less in one fire, thereby improving production efficiency and shortening production cycle, because the die forging extrusion of 3 sections or less including the maximum diameter part is much shorter than the cycle of free forging with multiple heating and gradual forming, and has higher forming accuracy. For the remaining parts exceeding 3 sections, since the defects in the core have been effectively pressed together during die forging extrusion, the overall quality of the product, especially the core, is better than that of the existing process.

[0026] (4) In some preferred embodiments, when performing the first heating before die forging and extrusion, by selecting a suitable heating temperature and holding time, it is helpful to better eliminate the core defects of the continuous casting billet during in-die extrusion, promote the homogenization of the internal structure of the material, improve the uniformity of the material, reduce the resistance during the die forging and extrusion process, and reduce the required forging force without wasting energy due to too long a holding time. This can further improve the processing efficiency, shorten the production cycle, and reduce the cost as a whole. It can also reduce the residual pressure in the die forging and extrusion and the metal oxidation loss in the heating while ensuring the product quality and processing performance, which is beneficial to improving the material utilization rate.

[0027] (5) In some preferred embodiments, when the number of segments Y of the shaft-type solid forgings to be formed is 4 to 7, it is only necessary to heat the second time to ensure that the parts other than the 3 segments have good processing performance during free forging. By controlling the process parameters of the second time, that is, selecting appropriate heating temperature and holding time, it is possible to ensure product quality, improve the overall performance of the product, and achieve an optimal balance between production cost, production cycle and material utilization.

[0028] (6) In some preferred embodiments, during die forging extrusion, the extrusion ratio is controlled between 2.5 and 4, which can not only ensure that the central defect of the continuous casting billet is fully pressed by the three-dimensional compressive stress and has the best microstructural uniformity, but also achieve the optimal balance between forging quality and production cycle, production cost, and material utilization.

[0029] (7) In some preferred embodiments, by controlling the extrusion speed within a suitable range (1 to 10 mm / s), it is possible to ensure that the metal flows more evenly and reduce defects when filling the die; during the die forging extrusion process, by adopting a variable extrusion speed strategy, that is, a medium speed at the initial stage of extrusion, a slow speed in the middle stage of extrusion, and the fastest speed at the late stage of extrusion, it is helpful to improve product quality and overall performance, further shorten the production cycle, reduce production costs, and improve material utilization.

[0030] (8) In some preferred embodiments, by controlling the speeds of different stages of die forging extrusion to be within corresponding appropriate ranges, for example, the initial extrusion speed V1 is 4 mm / s to 6 mm / s, the mid-extrusion speed V2 is 1 mm / s to 3 mm / s, and the late extrusion speed V3 is 8 mm / s to 10 mm / s, which helps to obtain the best product quality and overall performance, while achieving the optimal balance among production cycle, production cost, and material utilization.

[0031] (9) In some preferred embodiments, by providing appropriately sized arc chamfers on the upper and lower end faces of the prepared billet before die forging and extrusion, it is possible to maximize material utilization while facilitating the positioning of the billet and its entry into the die, thereby reducing extrusion contamination at the die gap and helping to improve the surface quality of the formed product.

[0032] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0034] Figure 1 A schematic flow chart of the manufacturing method provided by the present invention;

[0035] Figure 2 A schematic diagram of the structure from a billet to a product provided in an embodiment of the present invention, wherein (a) is a billet; (b) is a three-section shaft extrusion; (c) is a five-section shaft solid forging;

[0036] Figure 3 The photographs of the continuous casting rod-shaped billet made of high carbon alloy steel provided in the embodiment of the present invention, wherein (a) is a cross-sectional photograph; (b) is an enlarged view of the A portion including the core crack in (a);

[0037] Figure 4 This is a cross-sectional photo of a shaft solid forging obtained by the preparation method of an embodiment of the present invention;

[0038] Figure 5 This is a partially enlarged photograph of the cross section of a shaft solid forging obtained by the preparation method of Comparative Example 1;

[0039] Figure 6 This is a partial enlarged photograph of the cross section of a shaft solid forging obtained by the preparation method of Comparative Example 2 after color flaw detection;

[0040] Figure 7 This is a partial enlarged photograph of the cross section of a solid shaft forging obtained by the preparation method of Comparative Example 6 after color flaw detection. DETAILED DESCRIPTION

[0041] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0042] The traditional process of large shaft solid forgings has shortcomings in product qualification rate, production cost, production cycle and material utilization rate. During the free forging process, the flow direction and speed of the metal are difficult to control accurately, which easily leads to uneven microstructure and local cracks. For large free forging presses, the accuracy and control ability of the equipment limit the accuracy of the size and shape of large shaft forgings to a certain extent, especially the forming accuracy of the largest diameter roller body and the larger diameter roller neck, which makes it difficult for the product qualification rate to meet the higher expected target; the production cost of die-cast ingots / electroslag ingots is high, which increases the cost of raw materials. At least 3 fires are required during the free forging process, which consumes a lot of energy and increases the production cost; the production cycle of die-cast ingots or electroslag ingots is long, the production efficiency of free forging is relatively low, the cycle of each forging is long, and in order to maintain the processing plasticity, it needs to be reheated many times, which increases the production time; material utilization rate: die-cast ingots or electroslag ingots will produce more risers and trimmings during the casting process, resulting in low material utilization rate, usually only about 50% to 70%.

[0043] Compared with the die-cast steel ingots / electroslag ingots used in the traditional process of large shaft solid forgings, continuous casting billets have the advantages of low cost, short forming cycle, and high material utilization rate. However, due to the easy generation of shrinkage holes, microcracks and other defects during the continuous casting process, the core quality is poor, which limits the application of continuous casting billets in high-strength requirements. At present, the application of continuous casting billets in shaft forgings is limited to hollow shaft forgings, or small low-carbon alloy shaft forgings with low strength requirements; for large shaft solid forgings with high strength requirements, how to use continuous casting billets to successfully manufacture products with high product qualification rate is still blank in this field. There are many technical difficulties to overcome, such as how to overcome the problem of core defects through reasonable process and parameter control. Moreover, for the manufacture of large shaft forgings, how to shorten the production cycle as much as possible, reduce costs, and improve material utilization while ensuring product quality is also a multi-faceted challenge.

[0044] Based on this, the present invention provides a method for manufacturing large-scale shaft solid forgings by using continuous casting billets for rapid prototyping, the manufacturing method comprising the following steps:

[0045] S1. Prepare the billet: the billet is a continuous casting rod billet made of high carbon alloy steel;

[0046] According to the maximum diameter D1 of the large shaft solid forging to be formed and the extrusion ratio R, the initial diameter D0 of the billet is determined to satisfy: D0 = D1 × R 1 / 2 , R>2;

[0047] According to the weight M1 of the large solid shaft forging to be formed and considering the residual pressure F during die forging and extrusion and the metal oxidation loss L during each heating process, the initial weight M0 of the billet is determined to meet the following conditions: M0 = M1 × (1 + F) / (1 - L) n ; Among them, F is 5% to 10%, L is 1% to 2%, and n is the number of fires;

[0048] S2, heating the continuously cast rod-shaped billet for the first time, and then extruding the continuously cast rod-shaped billet into an X-segment shaft extrusion by die forging and extrusion, removing the excess part, where X is 1 to 3;

[0049] S3, if the number of segments Y of the large shaft solid forging to be formed is greater than 3, the X-segment shaft extrusion obtained in step S2 is subjected to (n-1) heat heating, and the remaining (YX) segments of the roll neck other than the X segments are processed by free forging to obtain the large shaft solid forging;

[0050] Among them, n≥2, and the maximum diameter of the roll neck in the remaining (YX) segments is less than D1.

[0051] Compared with the prior art, the present invention uses continuous casting billets as forging raw materials, which greatly reduces the manufacturing cost. The continuous casting billets are directly extruded into shaft extrusions of 3 sections or less by die forging extrusion. If necessary, the remaining parts exceeding 3 sections are processed by free forging. Through process design and parameter control, the product qualification rate is improved, which can meet higher expected goals, reduce production costs, shorten production cycles, and improve material utilization. Specifically, when calculating the initial diameter of the billet, by controlling the extrusion ratio R to be greater than 2, it is helpful to ensure that the loose cracks in the core of the continuous casting billet can be effectively pressed together under die extrusion, which effectively solves the problem that the existing continuous casting billet cannot be used to manufacture large shaft solid forgings due to defects in the core. The product obtained by the present invention has good overall quality, especially the core can be guaranteed to be free of defects. Even under the condition of high internal quality requirements, the product qualification rate of the present invention can reach more than 95%. Compared with the existing process, the product obtained by the present invention has higher dimensional accuracy, especially the roller body with the largest diameter and the roller neck part with a larger diameter; when calculating the initial mass of the billet, by controlling the pressure margin F and the metal oxidation loss L in each heating process to be in a suitable numerical range, it can be ensured that the pre- The pressure residue and oxidation loss during the period are closer to the actual situation, thereby improving material utilization, reducing material costs, and avoiding unnecessary processing allowance waste. Compared with the traditional free forging process using die-cast steel ingots or electroslag ingots, the present invention uses the "continuous casting billet → die forging extrusion forming" near-net forming method to complete the manufacture of large-scale shaft solid forgings of 3 sections or less in one fire, thereby improving production efficiency and shortening production cycle, because the die forging extrusion of 3 sections or less including the maximum diameter part is much shorter than the multi-fire heating and gradual forming cycle of free forging and has higher forming accuracy. For the remaining parts exceeding 3 sections, since the defects in the core have been effectively pressed together during die forging extrusion, the overall quality of the product, especially the core, is better than that of the existing process.

[0052] It can be understood that the "large shaft solid forging" described in the present invention refers to: the maximum diameter D1 ≥ 400mm, illustratively, D1 = 450mm. The "extrusion ratio R" refers to: R = A0 / A1, A0 is the cross-sectional area of ​​the billet before forming, and A1 is the maximum cross-sectional area of ​​the large shaft solid forging after forming. As long as the ratio A0 / A1 is greater than 2, the extrusion ratio of other sections of the large shaft solid forging is also greater than 2.

[0053] Exemplarily, in step S1, the diameter D0 of the "continuously cast rod-shaped billet" is ≥ 640 mm. For example, D0 is 800 mm to 1600 mm.

[0054] Specifically, in step S2, the main steps of the first heating include: heating the continuously cast rod-shaped billet to T1=1200-1250°C and keeping the temperature, the holding time t1=D0×k1, k1=120min-150min / 100mm, D0 is in mm. For example, k1=125min / 100mm, 130min / 100mm, 135min / 100mm, 140min / 100mm, 145min / 100mm. Before die forging and extrusion, selecting the appropriate heating temperature and holding time has the following benefits in terms of eliminating core defects of continuous casting billets, improving material uniformity, processing efficiency, reducing costs and improving material utilization: (1) Eliminating core defects: The appropriate heating temperature can promote element diffusion and recrystallization inside the metal material, which helps to eliminate core defects of the continuous casting billet during in-die extrusion, such as shrinkage holes and cracks. The appropriate holding time can ensure uniform temperature inside the material, reduce internal stress concentration, and reduce the risk of defects such as cracks and holes during in-die extrusion. (2) Improving material uniformity: The appropriate heating temperature and holding time can promote the homogenization of the internal structure of the material, which helps to achieve more uniform deformation in the subsequent die forging and extrusion process. shape, improving the overall quality and processing performance of the material; (3) Improving processing efficiency: Appropriate heating temperature and holding time can reduce the resistance during die forging and extrusion, reduce the required forging force, but not too long to waste energy, and improve processing efficiency as a whole; (4) Reducing costs: By optimizing the heating temperature and holding time, energy consumption and production time can be reduced while ensuring product quality and processing performance, thereby reducing overall production costs; (5) Improving material utilization: Appropriate heating temperature and holding time can reduce the pressure surplus in die forging and extrusion and the metal oxidation loss during heating while ensuring product quality and processing performance, reduce processing allowance and subsequent processing requirements, and thus improve material utilization.

[0055] It can be understood that the number of segments (i.e., the number of step diameter segments) and the changing pattern of the step diameter of large shaft forgings will vary according to specific production requirements. In actual production, the number of step diameter segments of shaft forgings is usually between 2 and 5, and usually does not exceed 7.

[0056] For example, the step diameter may decrease from the middle to both ends. Figure 2 (c); or, decreasing from one end to the other.

[0057] In view of this, in step S3, when the number of segments Y is 4 to 7, n=2, that is, the X-segment shaft extrusion obtained in step S2 is subjected to a second heating. It can be seen that for large-scale solid shaft forgings in most cases, the method of the present invention can quickly form a roller body and roller neck containing a continuous X segment of maximum diameter, which greatly shortens the production cycle compared to free forging with multiple heating steps. The remaining roller necks can be obtained by free forging after the second heating. Since the remaining (YX) sections of the roller necks are relatively small, free forging does not require multiple heating steps. The processability can be maintained by controlling the process parameters of the second heating step, and the forming of all roller necks can be completed with fewer heating times, saving energy and reducing costs. The overall quality of the resulting product is excellent, and there are no defects in the core. Figure 4 .

[0058] Specifically, in step S3, the main steps of the second heating include: heating the X-section shaft extrusion to T2 = 1150 ~ 1200 ° C and keeping it warm, the insulation time t2 = D1 × k2, k2 = 40min ~ 55min / 100mm, D1 unit is mm. More preferably, k2 = 40min ~ 50min / 100mm. Exemplarily, k2 = 42min / 100mm, 45min / 100mm, 47min / 100mm. After die forging and before free forging, by selecting the appropriate heating temperature and insulation time, product quality can be guaranteed, overall performance can be improved, and the optimal balance between production cost, production cycle and material utilization can be achieved. If the temperature is too high or the holding time is too long, the grains may grow excessively, resulting in a decrease in the overall performance of the product (such as strength and hardness), while increasing energy consumption and production costs, and increasing oxidation losses on the surface of shaft extrusions, thereby reducing material utilization. If the temperature is too low or the holding time is too short, shaft extrusions cannot achieve ideal processing performance, which will increase the force requirements for free forging, lengthen the production cycle, and increase costs. At the same time, due to insufficient plasticity, residual stress in the product may not be fully released, affecting the dimensional stability, overall quality and performance of the product.

[0059] Exemplarily, in step S1, the chemical composition of the high carbon alloy steel includes, by mass percentage: C: 0.8-0.9%, Si: 0.65-0.75%, Mn: 0.35-0.45%, P: 0.010-0.015%, S: 0.001-0.005%, Cr: 4.95-5.05%, Ni: 0.30-0.35%, Mo: 0.20-0.25%, V: 0.10-0.15%, N: 0.003-0.005%, and the remainder is Fe and unavoidable impurities.

[0060] In some preferred embodiments, the extrusion ratio R satisfies: 2.5≤R≤4. During die forging extrusion, the extrusion ratio is controlled between 2.5 and 4, which can not only ensure that the central defect of the continuous casting billet is fully pressed through die forging extrusion and has the best microstructure uniformity, but also achieve the optimal balance between forging quality and production cycle, production cost, and material utilization. Controlling the extrusion ratio between 2.5 and 4 is particularly suitable for the chemical composition of high-carbon alloy steel as described above. When the extrusion ratio R is large, more material will be extruded during the die forging extrusion process, increasing the pressure surplus F, reducing the material utilization rate, increasing the power and energy consumption of the required press, lengthening the production cycle, and increasing the cost. Exemplarily, R = 2.8, 3.0, 3.2, 3.5, 3.8.

[0061] In some preferred embodiments, in step S2, the speed of the die forging extrusion is controlled at 1 mm / s to 10 mm / s, wherein the speed V1 at the initial stage of extrusion, the speed V2 at the middle stage of extrusion, and the speed V3 at the later stage of extrusion satisfy: V3>V1>V2. In the die forging extrusion process, controlling the extrusion speed is an important means to improve product quality and achieve the optimal balance among production cycle, production cost, and material utilization. Specifically, (1) by controlling the extrusion speed within a suitable range (1 to 10 mm / s), it can ensure that the metal flows more evenly and reduces defects such as bubbles and cracks when filling the mold. If the extrusion speed is too slow, it will cause the metal to overheat, increase the risk of oxidation and heat loss, extend the production cycle, and increase the overall cost; if the extrusion speed is too fast, it may cause uneven metal flow and filling defects, affecting product quality. (2) By adopting a variable extrusion speed strategy during the die forging extrusion process, that is, a medium speed at the initial extrusion stage, a slow speed in the middle extrusion stage, and the fastest speed in the later extrusion stage, it is helpful to improve product quality and overall performance, improve production efficiency, reduce production costs, and improve material utilization; for example, the initial medium speed helps to start the flow of metal and perform preliminary compression of core defects; reducing the speed in the middle stage can further compact the metal and ensure that the core defects are more fully filled and compressed. Appropriate speed changes can help obtain a more uniform microstructure and help improve the overall performance of the product, such as mechanical properties and dimensional stability; rapid extrusion in the later stage can shorten the time to fill the mold and improve production efficiency. By reasonably controlling the extrusion speed at different stages, it is possible to improve production efficiency and reduce production costs as a whole while ensuring product quality.

[0062] In some possible designs, the die for die forging extrusion includes an upper die column, an extrusion barrel and a lower die mechanism, the lower die mechanism includes a first lower die and a second lower die, the upper extrusion port of the extrusion barrel is connected to the forming cavity in the upper die column, and the outer wall of the upper die column is tightly slidably connected to the inner wall of the extrusion barrel, the lower extrusion port of the extrusion barrel is connected to the forming cavity of the first lower die or the second lower die, and the lower end of the extrusion barrel is seated on a step groove opened at the upper end of the first lower die or the second lower die; illustratively, the forming process of the blank in the die includes the following possibilities:

[0063] (1) When the large solid shaft forging to be formed is a one-section type, the accommodation space of the forming cavity of the upper die mechanism is 0, and the billet is squeezed from the lower extrusion port of the extrusion cylinder into the cylindrical forming cavity of the lower die mechanism to form the required one-section shape.

[0064] (2) When the large shaft-type solid forging to be formed is a two-section type, the accommodating space of the forming cavity of the upper die mechanism is 0, and the billet is extruded from the lower extrusion port of the extrusion barrel into the cylindrical forming cavity of the first lower die to form the shape of the first section. The first lower die is replaced with the second lower die, and the billet continues to be extruded from the lower extrusion port of the extrusion barrel into the cylindrical forming cavity of the second lower die to form the shape of the second section.

[0065] (3) When the large shaft-type solid forging to be formed is a three-section type, the blank is extruded from the upper and lower extrusion ports of the extrusion barrel into the cylinders of the upper die and the first lower die to form a cavity and fill it up, forming the roll necks at both ends. The first lower die is replaced with the second lower die, and the blank continues to be extruded from the lower extrusion port into the cylinder of the second lower die to form a cavity, forming the roll body of the middle section.

[0066] For example, in the initial stage of extrusion, when the heated billet is placed in the extrusion barrel of the mold and the large press applies pressure to the mold, the billet will be subjected to three-dimensional compressive stress and undergo plastic deformation in the extrusion barrel, which is called upsetting. When the billet completes the filling in the extrusion barrel, it enters the middle stage of extrusion. At this stage, the billet begins to extrude from the extrusion port of the extrusion barrel into the forming cavity to form the desired shape while continuing to be subjected to three-dimensional compressive stress. After the middle stage of extrusion, when the billet begins to stably extrude from the extrusion barrel and the extruded roller neck or roller body reaches a stable state, it reaches the late stage of extrusion.

[0067] More preferably, the speed V1 at the initial stage of extrusion is 4mm / s to 6mm / s, the speed V2 at the middle stage of extrusion is 1mm / s to 3mm / s, and the speed V3 at the later stage of extrusion is 8mm / s to 10mm / s, which helps to obtain the best product quality and overall performance, while achieving the optimal balance among production cycle, production cost and material utilization.

[0068] In some preferred embodiments, in step S1, chamfers are processed on the upper and lower end faces of the blank, wherein the chamfer of the upper end face is an arc with a radius of 130 to 170 mm, and the chamfer of the lower end face is an arc with a radius of 80 to 120 mm; using arcs of appropriate radius as chamfers of the upper and lower end faces can maximize material utilization while facilitating blank positioning and entry into the mold, and a larger chamfer of the upper end face helps to reduce extrusion skinning of the mold gap, and the principle is as follows: In some possible designs, in the initial stage of extrusion (i.e., the blank is upset to fill the extrusion barrel in the mold), the lower end face of the blank first completes the extrusion barrel. During filling, the lower billet will begin to change diameter and be extruded from the lower extrusion port of the die, regardless of whether there is a cavity in the upper die column that the upper end face of the billet contacts (if so, the upper roll neck can be formed). At this time, the filling of the lower end face of the billet is almost completed, while the chamfer of the upper end face is large and has not been fully filled. If the pressurization continues, the billet of the lower end face will continue to be extruded from the lower extrusion port of the die to form a roll neck, or the upper and lower end face billets are extruded from the upper and lower extrusion ports of the die respectively to form the upper and lower roll necks. A larger chamfer of the upper end face can make the upper end face complete the filling later than the lower end face, so that the billet of the upper end face can be effectively controlled not to be extruded from the gap between the upper die column and the extrusion barrel, thereby reducing the flash here.

[0069] It should be noted that in step S2, the main steps of the die forging extrusion include: first coating the inner surface of the die forging extrusion mold with glass powder for lubrication, then placing the heated billet into the mold, and then using a large press to apply pressure to the mold. The mold will transfer this pressure to the billet, so that the billet is formed under the action of three-dimensional compressive stress and the inside of the billet is effectively pressed together, especially the loose cracks in the core of the continuous casting billet can be efficiently and effectively pressed together under the three-dimensional compressive stress.

[0070] The "three-dimensional compressive stress" in the present invention refers to the fact that during the die forging extrusion process, the pressure applied to the billet is usually omnidirectional, that is, there is pressure in three directions. For example, a rod-shaped billet will be subjected to compressive stress toward the inside of the billet in the axial direction, and will also be subjected to compressive stress toward the inside of the billet in any two perpendicular directions in the radial plane.

[0071] The method of the present invention can successfully manufacture high-quality large-scale solid shaft forgings of high-carbon alloy steel. The non-destructive testing detection of the absence of equivalent defects greater than 2 mm in diameter inside the forgings is used as the main evaluation index for the pass rate. The pass rate of the products obtained in this embodiment can reach more than 95%. Compared with the existing method, the production cycle is shortened by more than 30 to 50%, the production cost is reduced by at least 20%, and the material utilization rate is increased by at least 10 to 25%.

[0072] It is understood that the size of internal defects is a key evaluation indicator in the manufacturing and quality control of metal forgings. The absence of equivalent defects greater than 2 mm in diameter inside the forging is generally considered to be an expected goal for higher quality requirements.

[0073] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and comparative examples.

[0074] Embodiment 1:

[0075] This embodiment provides a method for manufacturing a large shaft solid forging by using a continuous casting billet for rapid prototyping, comprising the following steps:

[0076] S1. Prepare the blank: Figure 2 As shown in (a), the billet is a continuous casting rod billet made of high carbon alloy steel. The chemical composition of the high carbon alloy steel is shown in Table 1 below:

[0077] Table 1: Chemical composition of high carbon alloy steel (by mass %)

[0078]

[0079] See also Figure 2 (c) The large solid shaft forging to be formed is of 5 sections, with the roller body with the largest diameter in the middle, the maximum diameter D1 = 450mm, and the diameters decreasing from the middle to the two ends, that is, the roller body with the largest diameter in the middle is the first section, and the diameters of the second and third sections to the left and right ends are 380mm, and the diameters of the fourth and fifth sections are 280mm respectively; the weight of the large solid shaft forging to be formed can be determined to be M1 = 3100Kg according to its volume and density;

[0080] (1) Determine the initial diameter D0 of the blank:

[0081] According to the maximum diameter D1 = 450 mm and the extrusion ratio R = 2.4 of the large solid shaft forging to be formed, the initial diameter of the billet D0 = D1 × R 1 / 2 =450×2.4 1 / 2 =700mm;

[0082] (2) According to the pressure surplus F = 10% during die forging and extrusion and the metal oxidation loss L = 2% during each heating, the initial weight of the billet M0 = M1 × (1 + F) / (1 - L) is determined n =3100×(1+10%) / (1-2%) 2 =3550Kg; the density of the alloy based on Table 1 is 7.85g / cm 3 , the initial length of the blank L0 is calculated to be 1175mm;

[0083] (3) According to the alloy chemical composition and size (initial diameter D0 and length L0) of the above-mentioned billet, a continuous casting rod-shaped billet is prepared by a vertical casting machine, and a circular arc chamfer with a radius of 150 mm is processed on the upper end surface of the billet, and a circular arc chamfer with a radius of 100 mm is processed on the lower end surface of the billet;

[0084] S2, heating the continuous casting rod-shaped billet prepared in step S1 for the first time, that is, heating to T1 = 1230°C and keeping the temperature, and the holding time t1 = 700mm × 120min / 100mm = 14h;

[0085] Then, the continuous casting rod-shaped billet is extruded into a three-section shaft extrusion by die forging and extrusion, such as Figure 2 (b) shows that the maximum diameter of the middle section is D1=450mm. Specifically, before die forging and extrusion, glass powder is first coated on the inner surface of the mold for lubrication, and then the heated blank is placed in the mold. A large press is used to apply pressure to the mold, and the mold will transfer this pressure to the blank, so that the blank is formed under the action of three-dimensional compressive stress and the inside of the blank is effectively pressed. The speed V1 at the beginning of the extrusion is 5mm / s, the speed V2 in the middle of the extrusion is 2mm / s, and the speed V3 at the end of the extrusion is 9mm / s; after the die forging and extrusion is completed, the excess pressure is removed by shearing with a chopper.

[0086] S3, heating the three-section shaft extrusion obtained in step S2 for the second time, that is, heating to 1170° C. and keeping the temperature for a holding time of t2=450mm×40min / 100mm=3h;

[0087] Keep as Figure 2 The diameter of the middle section (i.e., the first section) of the three-section shaft extrusion shown in (b) is 450 mm and remains unchanged. Then, the roll necks of the remaining sections 2 to 5 are processed on a free forging press. The roll necks of the second and third sections located on the left and right sides of the first section are pressed from 450 mm to 380 mm, and the forging ratio of this fire is 1.4; the diameters of the fourth and fifth sections located on the left and right ends are pressed from 450 mm to 280 mm, and the forging ratio of this fire is 2.6, thus obtaining a five-section shaft solid forging, as shown in FIG. Figure 2 (c) as shown.

[0088] The method of this embodiment successfully manufactures a large-scale 5-section shaft solid forging of high-carbon alloy steel with high quality. The overall quality is excellent, especially the core part has good quality and no defects such as cracks. Figure 4 As shown; based on the non-destructive testing detection of the forgings without defects larger than 2 mm in diameter as the main evaluation index of the qualified rate, the qualified rate of the products obtained in this embodiment can reach more than 95%; compared with the existing method, the production cycle is shortened by at least 30%, and the production cost is reduced by at least 20%.

[0089] If the die-cast steel ingots or electroslag ingots in the traditional process are used as raw materials, the material utilization rate is usually only 50% to 75%. According to the higher 65% to 75%, if you want to form the 5-section shaft solid forgings in this embodiment, the required die-cast steel ingot or electroslag ingot billet weight is 3100Kg / 0.75 to 3100Kg / 0.65, that is, about 4130kg to 4770kg; and the weight of the continuous casting billet in this embodiment is M0 = 3550Kg, which can save 580kg to 1220kg of materials in comparison. It can be seen that compared with the existing process, this embodiment saves at least 12 to 25% of raw materials and improves material utilization.

[0090] Example 2

[0091] The difference between this embodiment and embodiment 1 is that in step S1, the extrusion ratio R=3.2, the initial diameter of the billet D0=D1×R 1 / 2 =450×3.2 1 / 2 =805mm, initial length of blank L0 =889mm, and the remaining steps and parameters are similar to those in Example 1.

[0092] This embodiment adopts a more preferred extrusion ratio R (2.5-4.0), and uses the absence of equivalent defects greater than 2 mm in diameter inside the forgings detected by non-destructive testing as the main evaluation indicator for the pass rate. The pass rate of the products obtained in this embodiment can reach more than 97%.

[0093] Comparative Example 1

[0094] The difference between this comparative example and Example 1 is that in step S1, the extrusion ratio R=1.9, the initial diameter of the billet D0=D1×R 1 / 2 =450×1.9 1 / 2 =620mm, initial length of blank L0 =1500mm, and the remaining steps and parameters are similar to those in Example 1.

[0095] Since the preferred range of the extrusion ratio R provided by the present invention (R>2) is not adopted in this comparative example, the core cracks of the obtained 5-section shaft solid forgings still remain. Figure 5 The qualified rate of forging products in the portion B indicated in the figure is reduced by at least 25% compared with that in Example 1.

[0096] Comparative Example 2

[0097] The difference between this comparative example and Example 1 is that: in step S2, the insulation time t1 = D0×105min / 100mm=700mm×105min / 100mm=12.25h; the remaining steps and parameters are similar to those in Example 1.

[0098] Since the preferred range of holding time in the first heating provided by the present invention (t1=D0×k1, k1=120min~150min / 100mm) is not adopted in this comparative example, the core cracks of the obtained 5-section shaft solid forgings still remain, see Figure 6 The C portion indicated in the middle is inspected by dye flaw detection on the cross section of the forging, and the colored trace of the C portion is a crack; the qualified rate of the forging products is reduced by at least 20% compared with Example 1.

[0099] Comparative Example 3

[0100] The difference between this comparative example and Example 1 is that: in step S2, the insulation time t1 = D0×165min / 100mm=700mm×165min / 100mm=19.25h; the remaining steps and parameters are similar to those in Example 1.

[0101] Since this comparative example does not adopt the preferred range of holding time in the first heating provided by the present invention (t1=D0×k1, k1=120min~150min / 100mm), the resulting 5-section solid shaft forgings have an increased risk of internal defects due to reasons such as excessively coarse local grains, and the qualified rate of forging products is reduced by at least 15% compared with Example 1.

[0102] Comparative Example 4

[0103] The difference between this comparative example and Example 1 is that in step S3, the insulation time t2 = D1×30min / 100mm=450mm×30min / 100mm=2.25h; the remaining steps and parameters are similar to those in Example 1.

[0104] Since this comparative example does not adopt the preferred range of holding time in the second heating provided by the present invention (t2=D1×k2, k2=40min~55min / 100mm), the resulting 5-section solid shaft forgings have an increased risk of internal defects due to local structural unevenness and thermal stress cracks, and the qualified rate of forging products is reduced by at least 10% compared with Example 1.

[0105] Comparative Example 5

[0106] The difference between this comparative example and Example 1 is that: in step S3, the insulation time t2 = D1×60min / 100mm=450mm×60min / 100mm=4.5h; the remaining steps and parameters are similar to those in Example 1.

[0107] Since this comparative example does not adopt the preferred range of holding time in the second heating provided by the present invention (t2=D1×k2, k2=40min~55min / 100mm), the resulting 5-section solid shaft forgings have an increased risk of internal defects due to local structural unevenness and excessively coarse grains, and the qualified rate of forging products is reduced by at least 10% compared with Example 1.

[0108] Comparative Example 6

[0109] The difference between this comparative example and Example 1 is that: in step S2, the extrusion speed of the entire die forging extrusion process is 11 mm / s; the remaining steps and parameters are similar to those of Example 1.

[0110] Since the preferred range of die forging extrusion speed (1 mm / s to 10 mm / s) provided by the present invention is not adopted in this comparative example, cracks still remain in the core of the obtained 5-section shaft solid forging. Figure 7 The D portion indicated in the middle is inspected by dye flaw detection on the cross section of the forging, and the colored trace of the D portion is a crack; the qualified rate of the forging products is reduced by at least 25% compared with Example 1.

[0111] Comparative Example 7

[0112] The difference between this comparative example and Example 1 is that in step S2, the speed V1 at the initial extrusion stage is 2 mm / s, the speed V2 at the middle extrusion stage is 5 mm / s, and the speed V3 at the late extrusion stage is 9 mm / s; the remaining steps and parameters are similar to those in Example 1.

[0113] Since the comparative example does not adopt the preferred relationship of speeds at different stages of die forging extrusion (V3>V1>V2) provided by the present invention, the qualified rate of forging products is reduced by about 5-10% compared with Example 1.

[0114] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for manufacturing large shaft-type solid forgings by using continuous casting billets for rapid prototyping. It is characterized in that The manufacturing method comprises the following steps: S1. Prepare the billet: the billet is a continuous casting rod billet made of high carbon alloy steel; According to the maximum diameter D of the large shaft solid forgings to be formed 1 and extrusion ratio R, determine the initial billet diameter D 0 , satisfied: D 0 =D 1 ×R 1 / 2 , R>2; According to the weight M of the large shaft solid forging to be formed 1 Considering the residual pressure F during die forging and extrusion and the metal oxidation loss L during each heating, the initial weight M of the billet is determined. 0 , satisfying: M 0 =M 1 ×(1+F) / (1-L) n ; Among them, F is 5% to 10%, L is 1% to 2%, and n is the number of fires; S2, heating the continuously cast rod-shaped billet for the first time, and then extruding the continuously cast rod-shaped billet into an X-segment shaft extrusion by die forging and extrusion, removing the excess part, where X is 1 to 3; S3, if the number of segments Y of the large shaft solid forging to be formed is greater than 3, the X-segment shaft extrusion obtained in step S2 is subjected to (n-1) heat heating, and the remaining (YX) segments of the roll neck other than the X segments are processed by free forging to obtain the large shaft solid forging; Among them, n ≥ 2, the maximum diameter of the roll neck in the remaining (YX) segments is less than D 1 .

2. The manufacturing method according to claim 1, It is characterized in that In step S2, the main steps of the first heating include: heating the continuously cast rod-shaped billet to T 1 = 1200~1250℃ and keep warm, holding time t 1 =D 0 ×k 1 , k 1 =120min~150min / 100mm, D 0 The unit is mm.

3. The manufacturing method according to claim 1, It is characterized in that In step S3, when the number of segments Y is 4 to 7, n=2, that is, the X-segment shaft extrusion obtained in step S2 is heated for the second time.

4. The manufacturing method according to claim 3, It is characterized in that In step S3, the main steps of the second heating include: heating the X-section shaft extrusion to T 2 = 1150~1200℃ and keep warm, holding time t 2 =D 1 ×k 2 , k 2 =40min~55min / 100mm, D 1 The unit is mm.

5. The manufacturing method according to claim 1, It is characterized in that The extrusion ratio R satisfies: 2.5≤R≤4.

6. The manufacturing method according to claim 1, It is characterized in that In step S2, the speed of die forging extrusion is controlled at 1 mm / s to 10 mm / s, wherein the initial speed V 1 , the speed V in the middle of the squeeze 2 , the speed V at the later stage of extrusion 3 Satisfaction: V 3 >V 1 >V 2 .

7. The manufacturing method according to claim 6, It is characterized in that The initial extrusion speed V 1 The speed V in the middle of the extrusion is 4 mm / s to 6 mm / s. 2 The speed V in the later stage of extrusion is 1 mm / s to 3 mm / s. 3 8mm / s~10mm / s.

8. The manufacturing method according to claim 1, It is characterized in that In step S1, chamfers are machined on the upper and lower end surfaces of the blank, wherein the chamfer of the upper end surface is an arc with a radius of 130 to 170 mm, and the chamfer of the lower end surface is an arc with a radius of 80 to 120 mm.

9. The manufacturing method according to claim 1, It is characterized in that In step S2, the main steps of the die forging extrusion include: first coating the inner surface of the die forging extrusion mold with glass powder for lubrication, then placing the heated blank into the mold, and then using a large press to apply pressure to the mold. The mold will transfer this pressure to the blank, so that the blank is formed under the action of three-way compressive stress and the inside of the blank is effectively pressed.

10. The manufacturing method according to claim 1, It is characterized in that In step S1, the chemical composition of the high carbon alloy steel includes, by mass percentage, C: 0.8-0.9%, Si: 0.65-0.75%, Mn: 0.35-0.45%, P: 0.010-0.015%, S: 0.001-0.005%, Cr: 4.95-5.05%, Ni: 0.30-0.35%, Mo: 0.20-0.25%, V: 0.10-0.15%, N: 0.003-0.005%, and the remainder is Fe and unavoidable impurities.

Citation Information

Patent Citations

  • Forging die for stepped shaft type forging piece and forging method

    CN112475180A

  • Manufacture of hot extruded alloy material

    JP1993212434A

  • Extrusion method of magnesium alloy with zinc and ytrium

    KR101392480B1

  • METHOD FOR MANUFACTURING SEAMLESS HOT-DEFORMED PIPES OF LARGE AND MEDIUM DIAMETERS AT PIPE ROLLING PLANTS WITH PILGRIM MILLS FOR STEAM BOILERS, STEAM PIPELINES AND MANIFOLDS OF INSTALLATIONS WITH HIGH AND SUPERCRITICAL STEAM PARAMETERS

    RU2005114094A

  • Forging method for high-efficiency closing of porous defects in steel ingots or billets

    WO2013041043A1

Cited By

  • A forging process for producing a solid sun gear shaft from a continuous casting billet

    CN123039274A