Process for preparing superfine copper powder from DMAC cuprous bromide hazardous waste and application
By optimizing the process of cuprous bromide hazardous waste, high-purity ultra-fine copper powder is prepared, which solves the recycling and environmental pollution problems in the treatment of cuprous bromide hazardous waste, and achieves efficient resource utilization and catalysis of copper powder. The recycling of non-toxic metals is suitable for many fields.
Patent Information
- Application Number
- CN202410935918.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-08
AI Technical Summary
The existing technology cannot effectively handle hazardous wastes of cuprous bromide, especially in terms of recycling, which has problems of low efficiency and environmental pollution. It also fails to consider the impact of other organic matter on copper powder and does not realize the recovery of bromine element.
The process of preparing ultrafine copper powder from DMAC cuprous bromide hazardous waste includes preliminary sorting, grinding and pretreatment, reduction reaction, separation and purification, as well as methanol washing and vacuum low-temperature drying. By optimizing process nodes and steps, high-quality copper powder can be achieved. The production of pure ultra-fine copper powder and the formation of thin film materials through the condensation of formaldehyde and methanol to reduce the oxidation of copper powder.
It realizes the production of high-purity ultra-fine copper powder, improves the utilization rate of raw materials, solves the problem of environmental pollution, creates economic value, and is suitable for the fields of electronics, metallurgy and catalysts, and realizes the recovery of catalytic metals.
Smart Images

Figure CN118744237A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hazardous waste treatment, and specifically relates to a production process for preparing ultrafine copper powder by utilizing DMAC (dimethylacetamide) cuprous bromide hazardous waste, and application of the production process. Background Art
[0002] In the context of industrial development, the generation and treatment of cuprous bromide hazardous waste has become an urgent issue. Cuprous bromide hazardous waste mainly comes from waste catalysts in organic synthesis reactions, which are widely used in alkylation reactions of brominated acyl chlorides, coupling nitrogen reactions, and photosensitizer components in the photographic industry. In addition, cuprous bromide is also used in catalytic reactions in other organic chemistry research.
[0003] Traditional methods for treating cuprous bromide hazardous waste include landfill and incineration, but these methods are inefficient and may cause secondary pollution to the environment. Specifically:
[0004] 1. Landfill method: It involves the safe landfill of cuprous bromide hazardous waste. It is necessary to select a suitable site and follow relevant standards for design and construction to reduce the impact on the environment.
[0005] 2. Incineration method: Through high-temperature decomposition and deep oxidation processes, cuprous bromide hazardous waste is converted into harmless substances, reducing the waste volume and removing toxicity, but attention should be paid to the treatment of waste gas and waste residue generated by incineration.
[0006] 3. Chemical method: Use chemical reactions to convert cuprous bromide hazardous waste into harmless end products, such as through acid-base neutralization, oxidation-reduction or precipitation.
[0007] 4. Recycling: Consider using appropriate technologies to recover valuable components from cuprous bromide hazardous waste and achieve resource recycling.
[0008] At present, there are no specific cases of cuprous bromide hazardous waste recycling in China, but scientific research institutions and environmental protection companies are researching and developing related technologies. Existing literature provides different methods for preparing copper powder, but does not consider the impact of other organic matter on copper powder, and does not achieve the recovery of bromine. Therefore, it is of great practical significance to develop an environmentally friendly and efficient method for treating cuprous bromide hazardous waste. Summary of the invention
[0009] In view of the above-mentioned shortcomings and deficiencies in the existing cuprous bromide hazardous waste recycling and treatment, the present invention provides a process for preparing ultrafine copper powder using DMAC cuprous bromide hazardous waste.
[0010] The process for preparing ultrafine copper powder by using DMAC cuprous bromide hazardous wastes specifically comprises the following steps:
[0011] Step 1: Raw material preparation
[0012] Collect cuprous bromide hazardous waste (derived from but not limited to the residue produced by falling film evaporation of the filtrate after neutralization and precipitation filtration in the tetrafluorobutadiene production process after zincation, the copper content in the hazardous waste is about 15%, mainly in the form of cuprous (I) precipitation, and a small part in the form of copper (II), and the hazardous waste contains about 35% DMAC, so the hazardous waste is partially dissolved in water, but the aqueous solution still exists in the form of solid precipitation), and perform preliminary sorting on it to remove impurities and pollutants;
[0013] Step 2: Grinding and pretreatment
[0014] The cuprous bromide hazardous waste is ground and sieved, and then cleaned with 2-16% methanol-containing ethyl acetate cleaning solution; the ratio of hazardous waste to cleaning solution is 1:1-1:3, and the cleaning time is 30-150 minutes; after cleaning, the solid is stored for use in subsequent processes;
[0015] Step 3: Reduction reaction
[0016] Add the pretreated cuprous bromide hazardous waste solids into the reaction tank, disperse them in water at a ratio of 1:1, add the reducing agent after stirring for reaction, and the stirring speed is 200~1600rps; the reducing agent formula is zinc powder, aluminum powder or reducing iron powder, the reaction temperature is 80~90℃, and the reaction time is 1~8h; during the reaction, spray isomeric tridecanol, propylene glycol, n-butanol or phenylethanol dispersant (first, to make the copper powder production process uniform and control the particle size at the micron level, and second, to play a defoaming role);
[0017] Step 4: Separation and purification
[0018] After the reduction reaction is completed, the reaction product is separated from the unreacted substances by filtering or centrifuging to obtain a crude ultrafine copper powder solid;
[0019] Step 5: Ultrafine copper powder processing
[0020] 0.1~3.0% methanol is used to wash and remove organic matter adsorbed on the surface, and then vacuum low-temperature drying is performed to obtain ultrafine copper powder; the vacuum degree of vacuum drying is -0.1mPa and the drying temperature is 30~90℃;
[0021] Step 6: Product Testing
[0022] The prepared ultrafine copper powder is quality tested to ensure that the product meets relevant standards.
[0023] On the basis of the above technical solution, in order to minimize the loss rate of cuprous bromide and obtain ultrafine copper powder with a suitable particle size, etc., the present invention optimizes and limits the nodes and steps of the preparation process, specifically including the following three aspects:
[0024] 1. In the grinding and pretreatment of step 2, it is preferred to use 8% methanol in ethyl acetate cleaning solution to clean the cuprous bromide hazardous waste, the ratio of hazardous waste to cleaning solution is preferably 1:1 to 1:1.5, and the cleaning time is preferably 120 min.
[0025] 2. In the reduction reaction of step 3, zinc powder is used as the reducing agent; the stirring speed is preferably 1400-1600 rps; the reaction time is preferably 4 h; and 1.5-2.5% of isotridecyl alcohol is sprayed during the reaction.
[0026] 3. In the ultrafine copper powder treatment of step 5, 1.0% methanol is preferably used for washing to remove organic matter adsorbed on the surface; the vacuum drying temperature is preferably 50°C.
[0027] In addition, the present invention also provides an application of the process for preparing ultrafine copper powder: applied to an organic solvent system of a halogen compound containing a catalytic metal to recover the catalytic metal; the catalytic metal includes nickel, copper, silver, gold, platinum or palladium.
[0028] Beneficial effects of the present invention:
[0029] The present invention uses an innovative process to prepare high-purity ultrafine copper powder from cuprous bromide hazardous waste, realizing resource utilization of hazardous waste, effectively solving environmental pollution problems, and creating significant economic value. The prepared ultrafine copper powder has uniform particle size and high purity, exhibits excellent electrical conductivity and thermal conductivity, and is suitable for multiple fields such as electronics, metallurgy, and catalysts.
[0030] At the same time, the pharmaceutical reduction method adopted by the present invention can efficiently reduce cuprous bromide to copper element, and produce copper powder with a purity greater than 99.5% by precisely controlling the reaction conditions. In the drying and storage process of the copper powder, the present invention adopts innovative technology to form a thin film material through the condensation of formaldehyde and methanol, thereby reducing the oxidizability of the copper powder and greatly solving the oxidation problem.
[0031] In summary, the present invention not only improves the utilization rate of raw materials, but also realizes the efficient recovery of various substances, has good application prospects and promotion value, is suitable for treating organic solvent systems containing catalytic metal halogen compounds, and realizes the recovery of catalytic metals and halogen elements. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention is a flow chart of the preparation process. DETAILED DESCRIPTION
[0033] In order to make the above and other purposes, features, and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with specific embodiments. The test materials, reagents, etc. used in the following examples can be obtained through commercial channels or known experimental methods.
[0034] The following are specific embodiments of the present invention, but are not limited thereto:
[0035] 1. Implementation methods of hazardous waste pretreatment:
[0036] 1.1. Choice of cleaning agent
[0037] The solvents that are more effective for dissolving DMAC are generally dichloromethane, ethyl acetate, methanol and acetone. Take 100g of solid waste (residue produced by falling film evaporation of the filtrate after zincification and precipitation filtration in the tetrafluorobutadiene production process), wash it with 1:1 pure solvent for 30 minutes, detect the bromine content in the liquid after washing and the DMAC content in the solid after washing, calculate the cuprous bromide loss rate and DMAC removal rate, and the washing effect is as follows:
[0038] Cleaning agent Dichloromethane Ethyl acetate Methanol acetone Cuprous bromide loss rate 41.34% 5.88% 37.52% 73.26% DMAC removal rate 77.59% 41.23% 94.31% 56.43% Difficulty of the process Volatile and difficult to clean Easy to clean Easier to clean Easy to clean
[0039] Dichloromethane and acetone have high cuprous bromide loss rates. Dichloromethane and acetone can be excluded according to actual conditions. Ethyl acetate and methanol need to be combined in proportion to achieve the maximum cleaning effect. According to the above experimental results, it is believed that ethyl acetate should be used as the base liquid. The effect of the amount of methanol added on the cleaning effect is as follows:
[0040] Methanol addition amount 2% 4% 6% 8% 10% 12% 14% 16% Cuprous bromide loss rate% 4.56 5.28 6.01 6.38 7.53 9.86 13.26 18.96 DMAC removal rate% 65.69 73.87 80.13 85.12 84.66 83.27 84.79 85.31
[0041] Through the above implementation, when the amount of methanol added reaches 8%, the removal rate of DMAC stabilizes at about 85%, but continued addition will lead to the loss of cuprous bromide, so the optimal addition amount is 8%.
[0042] 1.2.Choice of cleaning ratio
[0043] Different cleaning ratios have a great influence on the cleaning effect. Therefore, we designed cleaning ratios of 1:1, 1:1.5, 1:2, 1:2.5, and 1:3. The cleaning results after 30 minutes of cleaning with 8% methanol addition are as follows:
[0044] Cleaning ratio 1:1 1:1.5 1:2 1:2.5 1:3 Cuprous bromide loss rate% 6.42 7.38 11.67 18.92 24.44 DMAC removal rate% 85.49 90.31 92.27 93.14 94.26
[0045] As the cleaning ratio increases, the cuprous bromide loss rate increases rapidly, and the DMAC removal rate does not change significantly. Therefore, the greatest economic benefit is achieved under a 1:1.5 cleaning ratio.
[0046] 1.3.Choice of cleaning time
[0047] The cleaning time will affect the removal rate of DMAC, so we implemented cleaning for 30min, 60min, 90min, 120min, and 150min. The results of the addition of 8% methanol and a dosing ratio of 1:1.5 are as follows:
[0048] Cleaning time 30min 60min 90min 120min 150min Cuprous bromide loss rate% 7.53 7.66 7.78 7.75 8.02 DMAC removal rate% 90.26 92.55 94.18 96.47 95.83
[0049] Through the above implementation, the maximum DMAC removal rate and the lower cuprous bromide loss rate were achieved when the cleaning time was 120 min.
[0050] In summary, using ethyl acetate with 8% methanol added as the cleaning agent and cleaning for 120 minutes at a cleaning ratio of 1:1.5 has the best effect on the pretreatment of hazardous waste.
[0051] 2. Preparation of ultrafine copper powder
[0052] The reducing agents for reducing copper include metal reducing agents (zinc powder, aluminum powder, reducing iron powder), hydrazine hydrate, formaldehyde, etc. The reaction routes are solid-solid reaction route and solid-liquid reaction route. The specific implementation process is as follows:
[0053] 2.1. Principle of solid-solid reaction route
[0054] Reaction principle: The active metal replaces the inert metal. The chemical reaction formula is as follows:
[0055] Zinc powder: Zn+CuBr2=Cu+ZnBr2 Zn+2CuBr=2Cu+ZnBr2
[0056] Aluminum powder: 2Al+3CuBr2=3Cu+2AlBr3 Al+3CuBr=3Cu+AlBr3
[0057] Reducing iron powder: 2Fe+3CuBr2=3Cu+2FeBr3 Fe+3CuBr=3Cu+FeBr3
[0058] In order to ensure sufficient reaction, a little excess reducing agent was added. However, in order to ensure that the particle size of the copper powder was at the micron level, 100g of solid waste was reduced by zinc powder, aluminum powder, and reducing iron powder respectively. The reaction temperature was room temperature and the reaction was carried out in a 500rps water dispersion system for 1h. During the process, the corresponding reducing agent was slowly added to detect the particle size of the reduced copper powder. The specific implementation results are as follows:
[0059] reducing agent Zinc powder Aluminum powder Reduced iron powder Copper powder particle size / μm 48.23 75.97 92.46
[0060] The more active the metal is, the smaller the particle size of the copper powder will be. In this embodiment, zinc powder is used as a reducing agent to reduce the particle size of the copper powder.
[0061] 2.2. Effect of reaction temperature on particle size
[0062] In order to make the reaction fully contact, 100g of the pretreated solid was dispersed in 100g of water at a ratio of 1:1. Because the reaction is an exothermic reaction, it was first stirred and dispersed at a stirring speed of 500rps. Zinc powder was slowly added during the process. The reaction was continued for 1h. The particle size of the reduced copper powder was detected. The results of the implementation at different temperatures are described as follows:
[0063] Reaction temperature / ℃ 20 30 40 50 60 70 80 90 Copper powder particle size / μm 55.78 48.34 44.67 40.19 36.83 31.26 28.15. 27.32
[0064] As the reaction temperature increases, the particle size of the copper powder tends to shrink, and it shrinks rapidly and then slowly. Considering the actual energy consumption problem, the reaction temperature in the range of 80-90℃ can meet the requirements.
[0065] 2.3. Effect of stirring speed on particle size
[0066] Stirring speed is the main influencing parameter affecting the particle size of copper powder. During the implementation process, the particle size distribution under different stirring speeds was explored. Specifically, 100g of pre-treated hazardous waste was used, the reaction temperature range was 80-90℃, the reaction time was 1h, and the particle size of the reduced copper powder was detected. The following are the implementation results:
[0067] Stirring speed / rps 200 400 600 800 1000 1200 1400 1600 Copper powder particle size / μm 33.28 30.59 27.27 23.86 20.18 18.21 16.84 16.87
[0068] The faster the stirring speed, the smaller the copper powder particle size. When the stirring speed reaches 1400rps, the copper powder particle size does not change much. Therefore, the stirring speed should reach 1400-1600rps, and the copper powder particle size will reach a smaller size.
[0069] 2.4. Effect of reaction time on particle size
[0070] Reaction time affects the copper recovery rate and copper powder quality. It is very important to control the reaction time during the implementation process. Specifically, 100g of pre-treated hazardous waste was used, the reaction temperature range was 80-90℃, the stirring speed was 1400-1600rps, and the particle size of the reduced copper powder and the copper powder yield were detected. The following are the implementation results:
[0071] Reaction time / h 1h 2h 3h 4h 5h 6h 7h 8h Copper powder particle size / μm 16.38 16.83 17.10 17.44 18.98 19.33 20.37 21.64 Copper powder yield / % 81.78 94.68 98.91 99.58 99.65 99.74 99.84 99.86
[0072] As the reaction time increases, the copper powder particle size tends to increase, and the yield of copper powder becomes higher and higher. According to the maximum yield and the smaller copper powder particle size, the reaction time of 4 hours is the best reaction condition.
[0073] 2.5. Effect of dispersant on particle size
[0074] As the copper particles grow, they become heavier and heavier, and gradually become difficult to disperse by stirring. They tend to settle at the bottom of the reaction tank. Therefore, adding a dispersant to suspend the copper powder is beneficial to uniform particle size.
[0075] The dispersant is mainly alcohol, which can disperse and grow the copper powder and defoam the reaction process. The more suitable alcohols are mainly isomeric tridecanol, propylene glycol, n-butanol and phenylethanol. The specific implementation uses 100g of pre-treated hazardous waste, 80-90℃ reaction temperature range, stirring speed 1400-1600rps, reaction time 4h, and 2.0% dispersant is sprayed during the process. The following is the implementation result:
[0076] Dispersants Isotridecyl alcohol Glycerol n-Butanol Phenylethyl alcohol Copper powder particle size / μm 10.38 13.27 15.63 14.15
[0077] Dispersants can significantly reduce the particle size of copper powder, among which isotridecyl alcohol has the most obvious effect. The particle size of copper powder can be controlled at about 10μm. After multiple implementations, stable production can be achieved. Therefore, this research and development result has very important production guidance.
[0078] 3. Separation and purification implementation methods
[0079] After the reduction reaction is completed, the reaction product is separated from the unreacted substance by filtering or centrifuging, etc. The obtained solid is a crude ultrafine copper powder, and the liquid is a solution containing sodium bromide.
[0080] 4. Copper powder treatment implementation method
[0081] Due to the particle surface effect, ultrafine copper powder is easily oxidized during drying and storage, and further treatment is required for ultrafine copper powder. Methanol washing is used to remove organic matter adsorbed on the surface and oxidation of copper powder during the process. Spraying 1% formaldehyde solution before drying can effectively reduce copper powder oxidation during vacuum low-temperature drying. The oxidation rate of copper powder is less than 0.1%, thereby improving the purity and quality of copper powder. The following are the implementation results:
[0082] Methanol cleaning + vacuum low-temperature drying, the vacuum degree is -0.1mPa, and the temperature gradient is as follows:
[0083] Drying temperature / ℃ 30 40 50 60 70 80 90 Copper powder oxidation rate / % 1.08 1.41 1.94 2.56 3.87 4.44 5.12
[0084] As the drying temperature increases, the oxidizability of the copper powder increases. Vacuum drying at 50°C is used. Formaldehyde solution is used for mixing before drying. The results of the formaldehyde addition are as follows:
[0085] Formaldehyde addition / % 0.1 0.5 1.0 1.5 2.0 2.5 3.0 Copper powder oxidation rate / % 0.88 0.15 0.08 0.07 0.07 0.06 0.06
[0086] Adding formaldehyde can significantly reduce the oxidation of copper powder, not only because formaldehyde itself has reducing properties, but also because under the catalytic effect of ultrafine copper powder, formaldehyde and methanol condense to form an organic film. Excess formaldehyde and methanol will be evaporated, forming a reducing atmosphere in the drying box, preventing copper powder from contacting with oxygen, effectively avoiding oxidation of copper powder, and providing advantages for subsequent transportation and storage.
[0087] 5. Product quality
[0088] Ultrafine copper powder: Cu purity ≥ 99.50%, O content ≤ 0.5%
[0089] product D50 (μm) <![CDATA[Bulk density (g / cm 3 )]]> <![CDATA[Tap density (g / cm 3 )]]> 1 7.0-11.0 2.8-3.6 4.0-4.8 2 12.0-18.0 2.5-3.3 3.8-4.6
[0090] The applicant declares that, based on the above embodiments, technicians in the relevant technical field combine the specific content point value of a component in the above embodiments with the technical solutions in the content of the invention to produce a new numerical range, which is also one of the recorded ranges of the present invention. In order to make the specification concise, the present application no longer lists these numerical ranges.
Claims
1. A process for preparing ultrafine copper powder using DMAC cuprous bromide hazardous waste, characterized in that: The steps include: Step 1: Raw material preparation Collect cuprous bromide hazardous waste and conduct preliminary sorting to remove impurities and pollutants; Step 2: Grinding and pretreatment The cuprous bromide hazardous waste is ground and passed through a 60-mesh sieve, and then cleaned with a special organic solvent cleaning solution containing 2-16% methanol; the ratio of hazardous waste to cleaning solution is 1:1-1:3, and the cleaning time is 30-150 minutes; after cleaning, the solid is stored for use in subsequent processes; Step 3: Reduction reaction The pretreated cuprous bromide hazardous waste solid is added to the reaction tank, dispersed in water at a ratio of 1:1, stirred and then added with a reducing agent for reaction, with a stirring speed of 200-1600rps; the reducing agent formula is zinc powder, aluminum powder or reducing iron powder, the reaction temperature is 80-90°C, and the reaction time is 1-8h; during the reaction, an alcohol dispersant such as isotridecyl alcohol, n-butanol or phenylethyl alcohol is sprayed; Step 4: Separation and purification After the reduction reaction is completed, the reaction product is separated from the unreacted substances by filtering or centrifuging to obtain a crude ultrafine copper powder solid; Step 5: Ultrafine copper powder processing 0.1~3.0% methanol is used to wash and remove organic matter adsorbed on the surface, and then vacuum low-temperature drying is performed to obtain ultrafine copper powder; the vacuum degree of vacuum drying is -0.1mPa and the drying temperature is 30~90℃; Step 6: Product Testing The prepared ultrafine copper powder is quality tested to ensure that the product meets relevant standards.
2. A process for preparing ultrafine copper powder using DMAC cuprous bromide hazardous waste as claimed in claim 1, characterized in that: In the grinding and pretreatment of step 2, a special organic solvent cleaning solution of 8% methanol is used to clean the cuprous bromide hazardous waste, the ratio of hazardous waste to cleaning solution is 1:1~1:1.5, and the cleaning time is 120 minutes.
3. A process for preparing ultrafine copper powder using DMAC cuprous bromide hazardous waste as claimed in claim 1, characterized in that: In the reduction reaction of step 3, zinc powder is used as the reducing agent; the stirring speed is 1400-1600 rps; the reaction time is 4 h; and 1.5-2.5% of isotridecyl alcohol is sprayed during the reaction.
4. A process for preparing ultrafine copper powder using DMAC cuprous bromide hazardous waste as claimed in claim 1, characterized in that: In the ultrafine copper powder treatment of step 5, 1.0% methanol is used to wash and remove organic matter adsorbed on the surface; the vacuum drying temperature is 50°C.
5. The application of the process for preparing ultrafine copper powder as claimed in claim 1, characterized in that: The preparation process is applied to an organic solvent system of a halogen compound containing a catalytic metal to recover the catalytic metal; the catalytic metal includes nickel, copper, silver, gold, platinum or palladium.