Low-temperature sintered silver paste for flexible circuit board printing and preparation method thereof

By using low-temperature sintering silver paste in flexible circuit boards, combined with nano-silver powder and micron silver powder and other additives, the problem of copper foil materials being unable to meet miniaturization requirements and high temperature damage to insulating substrates is solved, achieving high conductivity and good adhesion. The strong silver layer reduces the sintering temperature and square resistance value.

CN118841204APending Publication Date: 2024-10-25NANO TOP ELECTRONICS TECH
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202410844365.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

In existing flexible circuit boards, copper foil materials cannot meet the requirements for miniaturization and integration of electronic components, and high-temperature sintering causes damage to the insulating substrate, resulting in insufficient density and adhesion of the conductive layer.

Method used

Low-temperature sintering silver paste is used. By mixing nano silver powder and micron silver powder, combined with metal salt additives, organic additives and glass powder, specific process steps are used to prepare conductive silver paste, which improves the density and adhesion of the silver layer and reduces sintering. temperature.

Benefits of technology

The conductivity and bending resistance of the silver layer are improved, the square resistance value and sintering temperature of the silver layer are reduced, and the adhesion between the silver layer and the insulating substrate is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841204A_ABST
    Figure CN118841204A_ABST
Patent Text Reader

Abstract

The invention provides low-temperature sintered silver paste for printing a flexible circuit board and a preparation method, the low-temperature sintered silver paste comprises the following raw materials in parts by weight: 70-90 parts of micro-nano silver powder, 20-40 parts of a metal salt additive, 1-5 parts of a polymer auxiliary agent, 15-19 parts of an organic solvent, 1-5 parts of an organic auxiliary agent and 30-50 parts of glass powder, and the micro-nano silver powder comprises nano silver powder and micron silver powder; the nano silver powder and the micron silver powder are mixed and matched for use, and the closest powder packing theory is utilized, so that the packing density of the silver powder is greatly improved, the porosity among the silver powder is reduced, the square resistance of a silver layer is greatly reduced, and the electric conductivity of the silver layer after sintering is improved; and secondly, the metal salt additive, the thixotropic agent, the organic solvent, the dispersing agent and the like are matched for use, and the synergistic effect among the components is fully exerted, so that the conductive silver paste is relatively high in silver content, relatively low in temperature in the sintering process, relatively high in adhesion with an insulating base material and good in bending resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive silver paste, and in particular to a low-temperature sintered silver paste for printing on a flexible circuit board and a preparation method thereof. Background Art

[0002] Flexible Printed Circuit, or FPC for short, is generally made of deformable materials such as polyimide or polyester film as a substrate. It is a highly reliable and extremely flexible printed circuit board. It has the advantages of high wiring density, light weight, thin thickness, and free bending and folding, and is widely valued.

[0003] In a flexible circuit board, the circuit board includes: an insulating substrate, a metal conductive layer, an adhesive, etc. Among them, the electrical properties of the metal conductive layer and the adhesion between the metal conductive layer and the insulating substrate are the key to determining the electrical properties of the flexible circuit board. With the miniaturization and integration of electronic components, the existing copper foil material as the metal conductive layer of the flexible circuit board can no longer meet the requirements of FPC. Therefore, the present invention proposes a low-temperature sintered silver paste for printing on a flexible circuit board and a preparation method to solve the problems existing in the prior art. Summary of the invention

[0004] In view of the above problems, the purpose of the present invention is to propose a low-temperature sintered silver paste for printing flexible circuit boards and a preparation method. The low-temperature sintered silver paste for printing flexible circuit boards and the preparation method have the advantages of improving the density of the silver layer after sintering the conductive silver paste, enhancing the adhesion between the silver layer and the insulating substrate, being suitable for screen printing process, and reducing the sintering temperature to prevent high temperature from damaging the insulating substrate, and can solve the problems existing in the prior art.

[0005] To achieve the purpose of the present invention, the present invention is implemented by the following technical scheme: a low-temperature sintered silver paste for flexible circuit board printing and a preparation method thereof, comprising the following raw materials in parts by weight:

[0006] 70-90 parts of micro-nano silver powder, 20-40 parts of metal salt additives, 1-5 parts of polymer additives, 15-19 parts of organic solvents, 1-5 parts of organic additives and 30-50 parts of glass powder. The micro-nano silver powder includes nano silver powder and micron silver powder.

[0007] A further improvement is that the following raw materials are included in parts by weight:

[0008] 70 parts of micro-nano silver powder, 40 parts of metal salt additives, 1 part of polymer additives, 15 parts of organic solvents, 1 part of organic additives and 50 parts of glass powder.

[0009] A further improvement is that the following raw materials are included in parts by weight:

[0010] 90 parts of micro-nano silver powder, 20 parts of metal salt additives, 5 parts of polymer additives, 19 parts of organic solvents, 5 parts of organic additives and 30 parts of glass powder.

[0011] A further improvement is that the mass ratio of the nano silver powder to the micron silver powder is 6-18:1-10.

[0012] A further improvement is that the metal salt additive includes one or more of aluminum oxide, zinc oxide, nickel oxide, silicon oxide, bismuth oxide, copper oxide, aluminum isooctanoate, zinc isooctanoate, nickel isooctanoate, bismuth isooctanoate, and copper isooctanoate.

[0013] A further improvement is that the organic auxiliary agent includes one or more of a thixotropic agent, a leveling agent, a dispersant, a thickener, and a wetting agent.

[0014] A further improvement is that the polymer auxiliary agent includes a resin and a curing agent.

[0015] A further improvement is that the organic solvent is ethanol.

[0016] A method for preparing a low-temperature sintered silver paste for printing on a flexible circuit board comprises the following steps:

[0017] Step 1: Preparation of primary polymer carrier

[0018] Add the polymer additive and the organic solvent into a mixer and mix them at a mixing temperature of 90 to 100°C for 3 to 6 hours. Filter the mixture to obtain a primary polymer carrier.

[0019] Step 2: Preparation of secondary polymer carrier

[0020] Then, glass powder, metal salt additive, organic additive and primary polymer carrier are mixed at a mixing temperature of 80-120° C. for a mixing time of 3-6 hours, and then ground and dispersed to obtain the preparation of secondary polymer carrier;

[0021] Step 3: Preparation of Conductive Silver Paste

[0022] The primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder are mixed, and then ground and dispersed to obtain a conductive silver paste.

[0023] A further improvement is that in step three, the weight ratio of the primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder is 5-20:2.5-5.0:0.5-1.0:70-90.

[0024] The beneficial effects of the present invention are as follows: the low-temperature sintered silver paste and preparation method for flexible circuit board printing provided by the present invention adopt a mixture of nano silver powder and micron silver powder, and utilize the closest packing theory of powder to greatly improve the packing density of the silver powder, reduce the porosity between the silver powders, greatly reduce the square resistance of the silver layer, and improve the conductivity of the silver layer after sintering; secondly, by using a metal salt additive, a thixotropic agent, an organic solvent, a dispersant, etc. in combination, the synergistic effect between them is fully exerted, so that the silver content of the conductive silver paste is higher, the temperature during the sintering process is lower, the density of the silver layer after sintering is higher, the adhesion between the silver layer and the insulating substrate is higher, and the bending resistance is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the preparation method steps of the present invention. DETAILED DESCRIPTION

[0026] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0027] The raw materials used in the following examples are all obtained through conventional commercial routes. In the following examples, the thixotropic agent is an organic bentonite thixotropic agent, the leveling agent is a polyether-modified siloxane leveling agent, the dispersant is a polyvinyl pyrrolidone dispersant, the thickener is a fumed silica thickener, the wetting agent is a polyethylene glycol wetting agent, the resin is an epoxy resin, and the curing agent is a polyamide curing agent.

[0028] Embodiment 1

[0029] according to Figure 1 As shown, this embodiment provides a low-temperature sintering silver paste for printing a flexible circuit board, comprising the following raw materials in parts by weight:

[0030] 70 parts of micro-nano silver powder, 40 parts of metal salt additives, 1 part of polymer additives, 15 parts of organic solvents, 1 part of organic additives and 50 parts of glass powder, wherein the micro-nano silver powder includes nano silver powder and micron silver powder, and the mass ratio of nano silver powder to micron silver powder is 6:1.

[0031] The metal salt additives include aluminum oxide, zinc oxide, nickel oxide, silicon oxide, bismuth oxide, copper oxide, aluminum isooctanoate, zinc isooctanoate, nickel isooctanoate, bismuth isooctanoate and copper isooctanoate. In the metal salt additives, each additive is mixed in equal proportions.

[0032] The organic additives include thixotropic agents, leveling agents, dispersants, thickeners, and wetting agents. In this embodiment, the various additives of the organic additives are mixed in equal proportions.

[0033] Furthermore, the polymer auxiliary agent includes a resin and a curing agent, the ratio of the resin to the curing agent is 10:2 (weight ratio), and the organic solvent is ethanol.

[0034] A method for preparing a low-temperature sintered silver paste for printing on a flexible circuit board comprises the following steps:

[0035] Step 1: Preparation of primary polymer carrier

[0036] Add the polymer additive and the organic solvent into a mixer and mix them at a mixing temperature of 90°C for 6 hours. Filter them after mixing to obtain a primary polymer carrier.

[0037] Step 2: Preparation of secondary polymer carrier

[0038] Then, glass powder, metal salt additive, organic additive and primary polymer carrier are mixed at a mixing temperature of 80° C. and a mixing time of 6 hours, and then ground and dispersed to obtain the preparation of secondary polymer carrier;

[0039] Step 3: Preparation of Conductive Silver Paste

[0040] The primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder are mixed, and then ground and dispersed to obtain a conductive silver paste.

[0041] In step three, the weight ratio of the primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder is 5:2.5:0.5:90.

[0042] Embodiment 2

[0043] according to Figure 1 As shown, this embodiment provides a low-temperature sintering silver paste for printing a flexible circuit board, comprising the following raw materials in parts by weight:

[0044] 90 parts of micro-nano silver powder, 20 parts of metal salt additives, 5 parts of polymer additives, 19 parts of organic solvents, 5 parts of organic additives and 30 parts of glass powder, the micro-nano silver powder includes nano silver powder and micron silver powder, the mass ratio of nano silver powder to micron silver powder is 18:10, the metal salt additive is aluminum oxide, the organic additive includes a thixotropic agent, the polymer additive includes a resin and a curing agent, the ratio of the resin to the curing agent is 10:2 (weight ratio), and the organic solvent is ethanol.

[0045] A method for preparing a low-temperature sintered silver paste for printing on a flexible circuit board comprises the following steps:

[0046] Step 1: Preparation of primary polymer carrier

[0047] Add the polymer additive and the organic solvent into a mixer and mix them at a mixing temperature of 100°C for 3 hours. Filter the mixture after mixing to obtain a primary polymer carrier.

[0048] Step 2: Preparation of secondary polymer carrier

[0049] Then, glass powder, metal salt additive, organic additive and primary polymer carrier are mixed at a mixing temperature of 120° C. for 3 hours, and then ground and dispersed to obtain the preparation of secondary polymer carrier;

[0050] Step 3: Preparation of Conductive Silver Paste

[0051] The primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder are mixed, and then ground and dispersed to obtain a conductive silver paste, wherein the weight ratio of the primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder is 20:5.0:1.0:90.

[0052] Embodiment 3

[0053] according to Figure 1 As shown, this embodiment provides a low-temperature sintering silver paste for printing a flexible circuit board, comprising the following raw materials in parts by weight:

[0054] 80 parts of micro-nano silver powder, 30 parts of metal salt additives, 3 parts of polymer additives, 17 parts of organic solvents, 3 parts of organic additives and 40 parts of glass powder, the micro-nano silver powder includes nano silver powder and micron silver powder, the mass ratio of nano silver powder to micron silver powder is 10:6, the metal salt additives are aluminum oxide, zinc oxide and nickel oxide, the ratio is 1:1:1, the organic additives include thixotropic agent, leveling agent, dispersant and thickener, the ratio is 1:1:1:1, the polymer additives include resin and curing agent, the ratio of resin to curing agent is 10:2 (weight ratio), and the organic solvent is ethanol.

[0055] A method for preparing a low-temperature sintered silver paste for printing on a flexible circuit board comprises the following steps:

[0056] Step 1: Preparation of primary polymer carrier

[0057] Add the polymer additive and the organic solvent into a mixer and mix them at a mixing temperature of 100°C, a mixing time of 6 hours, a mixer speed of 400 r / min, and filter them after mixing to obtain a primary polymer carrier;

[0058] Step 2: Preparation of secondary polymer carrier

[0059] Then, glass powder, metal salt additive, organic additive and primary polymer carrier are mixed at a mixing temperature of 110° C., a mixing time of 5 h, a mixer speed of 800 / min, and then ground and dispersed to obtain a secondary polymer carrier;

[0060] Step 3: Preparation of Conductive Silver Paste

[0061] The primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder are mixed at a mixer speed of 800 / min and a temperature of 100°C. After mixing, they are ground and dispersed to obtain a conductive silver paste, wherein the weight ratio of the primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder is 15:3:0.7:80.

[0062] Embodiment 4

[0063] according to Figure 1 As shown, this embodiment provides a low-temperature sintering silver paste for printing a flexible circuit board, comprising the following raw materials in parts by weight:

[0064] 80 parts of micro-nano silver powder, 30 parts of metal salt additives, 3 parts of polymer additives, 17 parts of organic solvents, 3 parts of organic additives and 40 parts of glass powder, the micro-nano silver powder includes nano silver powder and micron silver powder, the mass ratio of nano silver powder to micron silver powder is 10:6, wherein the metal salt additives are bismuth oxide, copper oxide and aluminum isooctanoate, and their ratio is 1:1:1, the organic additives include thixotropic agent, leveling agent, dispersant, thickener and wetting agent, and their ratio is 1:1:1:1:1, the polymer additives include resin and curing agent, the ratio of resin to curing agent is 10:3 (weight ratio), and the organic solvent is ethanol.

[0065] A method for preparing a low-temperature sintered silver paste for printing on a flexible circuit board comprises the following steps:

[0066] Step 1: Preparation of primary polymer carrier

[0067] Add the polymer additive and the organic solvent into a mixer and mix them at a mixing temperature of 100°C, a mixing time of 6 hours, a mixer speed of 400 r / min, and filter them after mixing to obtain a primary polymer carrier;

[0068] Step 2: Preparation of secondary polymer carrier

[0069] Then, glass powder, metal salt additive, organic additive and primary polymer carrier (part) are mixed at a mixing temperature of 120° C., a mixing time of 4 h, a mixer speed of 1000 / min, and then ground and dispersed to obtain the preparation of secondary polymer carrier;

[0070] Step 3: Preparation of Conductive Silver Paste

[0071] The primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder are mixed at a mixer speed of 1000 / min and a temperature of 120°C. After mixing, they are ground and dispersed to obtain a conductive silver paste, wherein the weight ratio of the primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder is 20:3:0.7:90.

[0072] In combination with Example 1, Example 2, Example 3 and Example 4, the present invention adopts a mixture of nano silver powder and micron silver powder in a specific ratio range, and utilizes the theory of the densest packing of powders to greatly increase the packing density of the silver powder, reduce the porosity between the silver powders, greatly reduce the sheet resistance of the silver layer, and improve the conductivity of the silver layer after sintering.

[0073] Furthermore, an organic additive is introduced, which includes one or more of a thixotropic agent, a leveling agent, a dispersant, a thickener and a wetting agent. Correspondingly, the thixotropic agent can improve the thixotropy of the conductive silver paste, that is, the property that the viscosity of the silver paste changes under the action of shear force. The thixotropic agent can help the silver paste maintain good fluidity and stability during the printing process, and can quickly recover to a higher viscosity after printing is completed to prevent the silver paste from flowing or diffusing before sintering.

[0074] Leveling agent is an additive used to improve the spreading and leveling performance of silver paste on the substrate. Leveling agent can help silver paste form a smooth and uniform film during the sintering process and reduce surface defects such as orange peel effect and fish eyes.

[0075] Dispersants are substances used to improve the dispersibility of silver powder in silver paste and prevent the aggregation of silver powder particles. Dispersants can improve the uniformity and stability of silver paste, thereby affecting the conductive and mechanical properties after sintering.

[0076] Thickeners can increase the viscosity of silver paste and improve its thixotropy, ensuring that the silver paste can maintain its shape after printing and will not flow due to gravity.

[0077] Wetting agents are used to improve the wettability between the silver paste and the substrate and promote the uniform spreading and adhesion of the silver paste on the substrate.

[0078] Therefore, the present invention uses silver powder, metal salt additives, thixotropic agents, organic solvents, dispersants and the like within a specific range in combination, giving full play to the synergistic effect between each other, so that the silver content of the conductive silver paste is higher, the temperature during the sintering process is lower, the density of the silver layer after sintering is higher, the adhesion between the silver layer and the insulating substrate is higher, and the overall performance is good. At the same time, nano silver powder and micron silver powder within a specific ratio range are mixed and used, and the closest packing theory of powder is used to greatly improve the packing density of the silver powder, reduce the porosity between the silver powders, greatly reduce the square resistance of the silver layer, and improve the conductivity of the silver layer after sintering.

[0079] The conductive silver paste purchased on the market was used as a control group for the experiment. The test method was to print the conductive silver paste prepared in Examples 1 to 4 and the conductive silver paste of the control group on a substrate, respectively, and heat-treated at 240° C. in an air atmosphere. After heat preservation for 60 minutes, the square resistance was measured using a four-probe method. Furthermore, a sintering temperature test was performed. As shown in Table 1 below, the present invention can reduce the square resistance of the silver layer and also reduce the temperature during the sintering process.

[0080] Table 1 Performance test comparison results

[0081]

[0082] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the framework and scope of application of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A low-temperature sintered silver paste for printing on flexible circuit boards, characterized in that: It includes the following raw materials in parts by weight: 70-90 parts of micro-nano silver powder, 20-40 parts of metal salt additives, 1-5 parts of polymer additives, 15-19 parts of organic solvents, 1-5 parts of organic additives and 30-50 parts of glass powder. The micro-nano silver powder includes nano silver powder and micron silver powder.

2. The low-temperature sintered silver paste for flexible circuit board printing according to claim 1, characterized in that: It includes the following raw materials in parts by weight: 70 parts of micro-nano silver powder, 40 parts of metal salt additives, 1 part of polymer additives, 15 parts of organic solvents, 1 part of organic additives and 50 parts of glass powder.

3. The low-temperature sintered silver paste for printing on a flexible circuit board according to claim 1, characterized in that: It includes the following raw materials in parts by weight: 90 parts of micro-nano silver powder, 20 parts of metal salt additives, 5 parts of polymer additives, 19 parts of organic solvents, 5 parts of organic additives and 30 parts of glass powder.

4. The low-temperature sintered silver paste for printing on a flexible circuit board according to claim 1, characterized in that: The mass ratio of the nano silver powder to the micron silver powder is 6-18:1-10.

5. The low-temperature sintered silver paste for printing flexible circuit boards according to claim 1, characterized in that: The metal salt additive includes one or more of aluminum oxide, zinc oxide, nickel oxide, silicon oxide, bismuth oxide, copper oxide, aluminum isooctanoate, zinc isooctanoate, nickel isooctanoate, bismuth isooctanoate, and copper isooctanoate.

6. The low-temperature sintered silver paste for printing flexible circuit boards according to claim 1, characterized in that: The organic auxiliary agent includes one or more of a thixotropic agent, a leveling agent, a dispersant, a thickener, and a wetting agent.

7. The low-temperature sintered silver paste for printing flexible circuit boards according to claim 1, characterized in that: The polymer auxiliary agent includes resin and curing agent.

8. The low-temperature sintered silver paste for printing flexible circuit boards according to claim 1, characterized in that: The organic solvent is ethanol.

9. A method for preparing a low-temperature sintered silver paste for printing a flexible circuit board as claimed in claim 1, characterized in that: The following steps are involved: Step 1: Preparation of primary polymer carrier Add the polymer additive and the organic solvent into a mixer and mix them at a mixing temperature of 90 to 100°C for 3 to 6 hours. Filter the mixture to obtain a primary polymer carrier. Step 2: Preparation of secondary polymer carrier Then, glass powder, metal salt additive, organic additive and primary polymer carrier are mixed at a mixing temperature of 80-120° C. for a mixing time of 3-6 hours, and then ground and dispersed to obtain the preparation of secondary polymer carrier; Step 3: Preparation of Conductive Silver Paste The primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder are mixed, and then ground and dispersed to obtain a conductive silver paste.

10. The low-temperature sintered silver paste for printing flexible circuit boards according to claim 9, characterized in that: In the step three, the weight ratio of the primary polymer carrier, the secondary polymer carrier, the organic additive and the micro-nano silver powder is 5-20:2.5-5.0:0.5-1.0:70-90.

Citation Information

Cited By

  • Flexible circuit board made of weldable low-temperature silver paste and preparation process of flexible circuit board

    CN120692753A

  • Weldable low-temperature sintered silver paste

    CN120809326A

  • A solderable low temperature sintering silver paste

    CN120809326B

  • Nano sintered silver paste and preparation method thereof

    CN121662482A

  • Nanosintered silver paste and preparation method thereof

    CN121662482B