Nano-porous elemental metal Co catalytic material as well as preparation method and application thereof

Activation of peroxymonosulfate through a nanoporous elemental metal Co catalyst solves the problem of efficient degradation of bisphenol A and phenol in wastewater, achieves low-cost, simple catalyst preparation and efficient degradation effects, and provides important environmental protection and resource recycling Take advantage of support.

CN118744238APending Publication Date: 2024-10-08QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410731670.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing technology is difficult to efficiently degrade bisphenol A and phenol in wastewater. Traditional methods have problems such as high energy consumption, high cost, poor controllability, or complex catalyst preparation. There is no research and application of elemental metal catalysts.

Method used

Using nanoporous elemental metal Co catalytic materials, through alloy strip preparation and chemical dealloying methods, a nanoporous Co catalyst with high specific surface area and strong magnetism was prepared for activating permonosulfate (PMS) to degrade bisphenol A. and phenol.

Benefits of technology

It achieves low-cost and simple catalyst preparation, has excellent catalytic activity and stability, can efficiently degrade BPA and phenol, and has broad application prospects in the field of wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744238A_ABST
    Figure CN118744238A_ABST
Patent Text Reader

Abstract

The invention provides a nano-porous elemental metal Co catalytic material as well as a preparation method and application thereof. The preparation method of the catalytic material comprises the following steps: preparing an Al-Co alloy strip by taking metal Al and Co as raw materials; and immersing the Al-Co alloy strip in the corrosive liquid, and carrying out chemical dealloying, cleaning and drying to obtain the Al-Co alloy strip. The preparation method disclosed by the invention is simple, convenient and rapid to operate, easy in implementation of reaction conditions, low in required cost and easy for large-scale production, and has a good practical prospect. The prepared porous elemental metal Co catalytic material has excellent performance of activating PMS to degrade BPA and phenol, and has good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wastewater treatment, and in particular relates to a nano porous single-substance metal Co catalytic material and a preparation method and application thereof. Background Art

[0002] From the perspective of sustainable development, wastewater treatment is gradually becoming one of the focuses of world attention. Among them, bisphenol A (BPA) is a typical organic pollutant, which is often used in the synthesis of polycarbonate, epoxy resin and various daily consumer products. However, due to its stable chemical properties, bisphenol A is difficult to degrade in the daily environment and has obvious lipophilicity. It is very easy to enrich in organisms, causing serious harm to human health and the environment. Phenol (C 6 H 5 OH) is one of the main representatives of phenolic compounds. It is a compound with a special smell, highly toxic and corrosive. It is an important raw material for the industrial production of certain resins, bactericides, preservatives and medicines. However, phenol has a low biodegradability, and its discharge into the environment will cause serious and continuous pollution, which is extremely harmful to aquatic organisms and humans. Therefore, how to simultaneously and effectively degrade bisphenol A and phenol in wastewater is of great research significance.

[0003] There are many methods for treating organic pollutants in wastewater, including traditional physical methods, chemical methods and biological methods. Physical methods mainly remove pollutants from wastewater through physical processes such as separation, filtration and adsorption. However, this method only transfers the pollutants out and does not achieve the effect of degradation. Chemical methods convert pollutants into harmless or easier to handle substances through chemical reactions such as oxidation, reduction, neutralization and precipitation to purify wastewater. However, this method has the disadvantages of high energy consumption and the generation of harmful wastes that easily cause environmental pollution. Biological methods use the metabolic activities of microorganisms to degrade organic matter in wastewater into simpler substances to achieve purification. These microorganisms can grow and reproduce under suitable environmental conditions, and then complete the treatment of wastewater by adsorbing, engulfing or decomposing organic matter, such as biofiltration, biofilm reactors, biological treatment tanks, activated sludge methods, etc., but the production cycle is long, the cost is high and the controllability is poor. In contrast, advanced oxidation technology (AOPs) has become one of the most effective methods for treating difficult-to-degrade organic pollutants due to its high efficiency and non-selectivity, and has received widespread attention in recent years. Among them, the production of sulfate free radicals (SO 4 ·- Compared with traditional water treatment technologies, the advanced oxidation technology with ) as the core has the advantages of strong oxidizing ability, fast reaction rate, mild reaction conditions, wide applicability, simple equipment and easy operation. This technology mainly activates persulfate to produce highly active SO by ultraviolet light, ultrasound, heat or homogeneous / heterogeneous catalysts. 4 ·-, OH, O 2 ·- Free radicals and 1 O 2 However, since ultraviolet light, ultrasound and heat all require higher energy, the activation cost becomes higher, so it is very important to develop catalysts with high catalytic activity and high stability.

[0004] Among the common transition metals, Co can 2+ With Co 3+ The persulfate is activated multiple times to produce SO 4 ·- , so it has a high catalytic activation for persulfate, and it has good corrosion resistance in wastewater, so it has attracted much attention. For example, Chinese patent document CN117599794A discloses a magnetic single-atom cobalt catalyst and a method for catalyzing the degradation of antibiotics with peracetic acid; first, Zn / Co ZIFs are synthesized by an improved MOF-derived spatial confinement strategy, and then calcined and pyrolyzed to generate a magnetic single-atom Co catalyst; it has a high efficiency activation effect on peracetic acid, and utilizes the strong oxidizing active substances generated in situ during the activation process to enhance the oxidative degradation of sulfonamide antibiotics in sewage. However, the preparation method of the catalyst is relatively complicated, and there may be disadvantages such as unstable ligands and easy detachment of metal ions, and it does not involve catalytic degradation of BPA and phenol by PMS. Chinese patent document CN114904530A discloses a method for preparing a cobalt-based porous amorphous catalyst based on dealloying, first preparing a Co-Fe-Mo-Si-B amorphous alloy strip, and then preparing a cobalt-based porous amorphous catalyst with a porous structure through dealloying treatment, and applying it to the degradation of azo dyes. However, this patent does not involve the research and preparation of elemental metals, and does not involve the degradation of bisphenol A and phenol.

[0005] Therefore, how to efficiently prepare a catalyst that can effectively catalyze the degradation of bisphenol A (BPA) and phenol by peroxymonosulfate (PMS) deserves further study. Summary of the invention

[0006] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a nanoporous single-substance metal Co catalytic material and a preparation method and application thereof. The preparation method of the present invention is simple and quick to operate, the reaction conditions are easy to implement, and the required cost is low, and it is easy to mass produce, and has good practical prospects. The porous single-substance metal Co catalytic material prepared by the present invention has excellent performance of activating PMS to degrade BPA and phenol, and has good stability.

[0007] To achieve the above object, the present invention adopts the following technical solution:

[0008] A nanoporous single-element metal Co catalytic material, the catalytic material is a Co single-element metal with a nanoporous structure, wherein the pore size of the nanoporous structure is 2-140nm, and the specific surface area is 40-50m 2 ·g -1 , which is magnetic.

[0009] The method for preparing the above-mentioned nanoporous single-element metal Co catalytic material comprises the steps of:

[0010] (1) Preparing Al-Co alloy strips using metal Al and Co as raw materials;

[0011] (2) The Al-Co alloy strip is immersed in a corrosive solution, chemically dealloyed, cleaned, and dried to obtain a nanoporous single-element metal Co catalytic material.

[0012] According to the present invention, preferably, in step (1), the atomic ratio of metal Al and Co is 88-96:4-12. The purity of metal Al and Co is above 99.9%.

[0013] According to the present invention, preferably, in step (1), the method for preparing the Al-Co alloy strip comprises the steps of: mixing metal Al and Co, and obtaining an alloy ingot by smelting; and obtaining the Al-Co alloy strip by spinning the alloy ingot.

[0014] Preferably, the smelting is carried out in a vacuum arc furnace.

[0015] Preferably, the smelting method is as follows: smelting at 650-750°C for 1-2 minutes under the protection of inert gas, cooling to room temperature; and repeating the above steps 3-6 times to obtain an alloy ingot. Preferably, the inert gas is nitrogen or argon.

[0016] Preferably, the belt spinning is carried out in a vacuum belt spinning machine. The belt spinning can be carried out according to the existing method. The alloy ingot is crushed, and a part of the crushed alloy ingot is used as a master alloy and placed in a quartz tube of the vacuum belt spinning machine; the vacuum degree of the furnace chamber of the vacuum belt spinning machine is adjusted to 4×10 -3 Pa, start the stepless speed regulating motor, when the speed of the copper roller reaches the set speed, turn on the power of the induction coil, melt the master alloy in the quartz tube to obtain the alloy melt; fill the quartz tube with high-purity argon gas instantly, so as to establish a pre-set pressure difference between the quartz tube and the furnace chamber of the vacuum belt spinning machine, under the effect of the set pressure difference, the alloy melt is ejected from the nozzle of the quartz tube, sprayed onto the surface of the copper roller, and quickly cooled into an alloy strip. The preset speed of the copper roller is 2000-3500rpm, preferably 2865rpm; the preset pressure difference formed between the quartz tube and the furnace chamber of the vacuum belt spinning machine is 0.03-0.05MPa, preferably 0.04MPa.

[0017] According to the present invention, preferably, in step (2), the etching solution is a NaOH aqueous solution with a concentration of 2-5 mol / L.

[0018] According to the present invention, preferably, in step (2), the temperature of chemical dealloying is room temperature, and the chemical dealloying is carried out until no bubbles are generated in the reaction system.

[0019] According to the present invention, preferably, in step (2), the cleaning is performed by using ultrapure water and anhydrous ethanol for 3 to 7 times respectively.

[0020] According to the present invention, preferably, in step (2), the drying is vacuum drying; the vacuum drying temperature is 40-80° C., preferably 60° C.; and the vacuum drying time is 10-14 hours.

[0021] The above-mentioned nanoporous single-element metal Co catalytic material is used in catalyzing the degradation of organic pollutants in wastewater by peroxymonosulfate (PMS).

[0022] According to the present invention, preferably, the organic pollutant is bisphenol A (BPA) and / or phenol.

[0023] The technical features and beneficial effects of the present invention are as follows:

[0024] 1. The preparation method of the present invention combines alloy design with a dealloying method, preferably using a non-consumable vacuum arc furnace to accurately control the alloy composition to obtain an alloy ingot with uniform composition, and then obtain an alloy strip after vacuum stripping, and then remove the Al element through dealloying technology, thereby converting the bulk alloy into a pure nanoporous single metal Co catalytic material. The obtained nanoporous single metal Co catalytic material has a high specific surface area and abundant active sites, which improves the activity and selectivity of the catalyst. The preparation method of the present invention is simple and efficient, the conditions are easy to implement, it is safe and environmentally friendly, the required cost is low, it can be mass-produced, and it has broad application prospects, especially in the field of wastewater treatment, and its good catalytic activity will provide important support for environmental protection and resource recycling.

[0025] 2. The nanoporous single-element metal Co catalytic material of the present invention has a nanoporous structure with small and evenly distributed pores, which effectively increases its specific surface area. This feature makes the active area of ​​the catalyst more abundant, which helps to improve the catalytic efficiency and reaction rate. Compared with traditional materials, this porous structure can more fully expose the active sites, promote effective contact between the catalyst and the reactants, and thus accelerate the reaction process.

[0026] 3. The nanoporous single-element metal Co catalytic material of the present invention has strong magnetism, so it can catalyze PMS to degrade BPA and phenol while also being able to recover them well. Its high catalytic activity, stability and high recovery bring broad application prospects to the field of wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The X-ray diffraction patterns of the catalytic materials prepared in Examples 1-4 and Comparative Examples 1-4 of the present invention are shown.

[0028] Figure 2 The scanning electron microscope photograph (a) and particle size distribution histogram (b) of the nanoporous single-element metal Co catalytic material prepared in Example 1 of the present invention.

[0029] Figure 3 This is the hysteresis loop diagram of the nanoporous single-element metal Co catalytic material prepared in Example 1 of the present invention.

[0030] Figure 4 These are the nitrogen adsorption-desorption curve and pore size distribution curve of the nanoporous single-element metal Co catalytic material prepared in Example 1 of the present invention.

[0031] Figure 5 This is a comparison chart of the degradation performance of BPA by catalytic material activated PMS prepared in Examples 1-4 of the present invention and Comparative Examples 1-4.

[0032] Figure 6 This is a comparison chart of the degradation performance of BPA using the single metal Co catalyst / PMS system prepared in Example 1, using only the Co catalyst, and using only PMS.

[0033] Figure 7 The single metal Co catalytic material prepared in Example 1 of the present invention is prepared in Co catalyst / PMS, Co catalyst / PDS and Co catalyst / H 2 O 2 Comparison of the degradation performance of the system on BPA.

[0034] Figure 8 This is a comparison chart of the degradation performance of phenol by catalytic materials activated PMS prepared in Examples 1-4 of the present invention and Comparative Examples 1-4.

[0035] Fig. 9 The figure is a comparison chart of the degradation performance of phenol using the single metal Co catalyst / PMS system prepared in Example 1, using only the Co catalyst, and using only PMS.

[0036] Fig.10 The single metal Co catalytic material prepared in Example 1 of the present invention is prepared in Co catalyst / PMS, Co catalyst / PDS and Co catalyst / H 2 O 2 Comparison of the degradation performance of the systems on phenol. DETAILED DESCRIPTION

[0037] The following examples are only listed as examples of embodiments of the present invention and do not constitute any limitation to the present invention. It can be understood by those skilled in the art that modifications within the scope of the essence and concept of the present invention fall within the scope of protection of the present invention. Unless otherwise specified, the reagents and instruments used in the following examples are commercially available products.

[0038] Example 1

[0039] A nanoporous single-element metal Co catalytic material is prepared by the following method:

[0040] (1) mixing raw metals Al and Co with a purity of more than 99.9% in an atomic ratio of 88:12;

[0041] The mixed raw metals are loaded into a graphite crucible, and then the graphite crucible is placed in the melting pit of a vacuum arc furnace;

[0042] Mechanical pump rough pumping and molecular pump fine pumping are used to exhaust air. -1 Pa, high-purity argon was injected; the vacuum was again evacuated to 1×10 -1 Pa, and then inject high-purity argon gas; finally evacuate to 1×10 -1 Pa, turn on the molecular pump and evacuate to 4×10 -3 Pa, and high-purity argon gas is injected again;

[0043] Under the protection of high-purity argon, the mixture was smelted at 655°C for 2 minutes and then cooled to room temperature. The above steps were repeated 4 times to obtain an alloy ingot.

[0044] The alloy ingot with uniform composition is placed in a vacuum belt spinning machine to spin the strips to obtain alloy strips; the alloy ingot is crushed, and a portion of the alloy ingot that has been crushed and graphite removed is placed in a quartz tube of the vacuum belt spinning machine to serve as the master alloy (the nozzle section is 0.2×3mm 2 );The vacuum degree in the vacuum belt furnace chamber is adjusted to 4×10 -3 Pa, start the stepless speed regulation motor, when the speed of the copper roller reaches 2865rpm (surface linear speed of about 30m / s), turn on the power of the induction coil to melt the master alloy in the quartz tube to obtain the alloy melt; instantly fill the quartz tube with high-purity argon gas, thereby establishing a pressure difference (0.04MPa) in the furnace chamber of the quartz tube and the vacuum belt spinning machine. Under the pressure difference, the alloy melt is ejected from the quartz tube nozzle, sprayed onto the surface of the copper roller, and quickly cooled into an alloy strip.

[0045] (2) The alloy strip was placed in a 250 mL beaker and immersed in 120 mL of a 5 mol / L NaOH aqueous solution. The strip was allowed to stand at room temperature for 24 hours until no bubbles were generated in the beaker. The supernatant was then poured out to obtain the solid. The solid was then washed with ultrapure water and anhydrous ethanol for 5 times respectively to completely remove impurities. The washed sample was placed in a vacuum drying oven at 60°C, and the air in the vacuum drying oven was evacuated by a vacuum pump. The sample was dried for 12 hours to obtain a nanoporous single-element metal Co catalytic material (abbreviated as Co 12 -5M NaOH).

[0046] After testing, the phase structure of the nanoporous single-element metal Co catalytic material prepared in this embodiment is as follows: Figure 1 As shown in a, it can be seen from the figure that only the Co phase is contained. The scanning electron microscope photo and particle size distribution of the nanoporous single metal Co catalytic material prepared in this embodiment are shown in FIG. Figure 2 As shown in the figure, the sample is a nanoporous structure with small pores and a pore size of 2-110nm. The hysteresis loop of the nanoporous single-element metal Co catalytic material prepared in this embodiment is shown in Figure 3 As shown in the figure, it can be seen that the sample is a strong magnetic material. Figure 4 The nitrogen adsorption / desorption curve and pore size distribution curve of the nanoporous single-element metal Co catalytic material prepared in this example. The specific surface area of ​​the material prepared in this example is 45.14 m 2 ·g -1 .

[0047] Example 2

[0048] A method for preparing a nanoporous single-element metal Co catalytic material is as described in Example 1, except that in step (1), the atomic ratio of the original metal Al and Co is replaced with 96:4; the other steps and conditions are the same as in Example 1. 4 -5M NaOH).

[0049] After testing, the phase structure of the nanoporous single-element metal Co catalytic material obtained in Example 2 is as follows: Figure 1 As shown in b, it can be seen from the figure that only the Co phase is contained. The nanoporous single-substance metal Co catalytic material prepared in this embodiment has a nanoporous structure with a pore size of 11-140nm.

[0050] Example 3

[0051] A method for preparing a nanoporous single-element metal Co catalytic material is as described in Example 1, except that in step (1), the atomic ratio of the original metal Al and Co is replaced with 92:8; the other steps and conditions are the same as in Example 1. 8 -5M NaOH).

[0052] After testing, the phase structure of the nanoporous single-element metal Co catalytic material obtained in Example 3 is as follows: Figure 1 As shown in c, it can be seen from the figure that only the Co phase is contained. The nanoporous single-substance metal Co catalytic material prepared in this embodiment is a nanoporous structure with a relatively regular arrangement and a pore size of 5-80nm.

[0053] Example 4

[0054] A method for preparing a nanoporous single-element metal Co catalytic material is as described in Example 1, except that in step (2), the 5 mol / L NaOH aqueous solution is replaced by a 2 mol / L NaOH aqueous solution; the other steps and conditions are the same as in Example 1. 12 -2M NaOH).

[0055] After testing, the phase structure of the nanoporous single-element metal Co catalytic material obtained in Example 4 is as follows: Figure 1 As shown in d, it can be seen from the figure that only the Co phase is contained. The nanoporous single-substance metal Co catalytic material prepared in this embodiment has a nanoporous structure, the particles are arranged densely, and the pore size is 3-80nm.

[0056] Comparative Example 1

[0057] A method for preparing a nanoporous single-element metal Fe catalytic material is as described in Example 1, except that in step (1), the original metal Co is replaced by metal Fe with a purity of more than 99.9%; the other steps and conditions are the same as in Example 1. A nanoporous single-element metal Fe catalytic material (referred to as Fe-5M NaOH) is obtained.

[0058] After testing, the phase structure of the nanoporous single-element metal Fe catalyst material obtained in this comparative example 1 is as follows Figure 1 As shown in Figure e, it can be seen that only the Fe phase is contained. The nanoporous single-element metal Fe catalytic material prepared in this comparative example is a nanoporous structure, and the pores are smaller than those in Example 1, and the structure is more compact.

[0059] Comparative Example 2

[0060] A method for preparing a nanoporous single-element metal Ni catalytic material is as described in Example 1, except that in step (1), the original metal Co is replaced by metal Ni with a purity of more than 99.9%; the other steps and conditions are the same as in Example 1. A nanoporous single-element metal Ni catalytic material (referred to as Ni-5M NaOH) is obtained.

[0061] After testing, the phase structure of the nanoporous single-element metal Ni catalyst material obtained in this comparative example 2 is as follows Figure 1 As shown in FIG. 5 , it can be seen from the figure that only Ni phase is contained. The nanoporous single-substance metal Ni catalytic material prepared in this comparative example is a nanoporous structure, which is distributed in a large number of granules, and the granules are relatively rounded and have small pores.

[0062] Comparative Example 3

[0063] A method for preparing a nanoporous single-element metal Cu catalytic material is as described in Example 1, except that in step (1), the original metal Co is replaced by metal Cu with a purity of more than 99.9%; the other steps and conditions are the same as in Example 1. A nanoporous single-element metal Cu catalytic material (abbreviated as Cu-5M NaOH) is obtained.

[0064] After testing, the phase structure of the nanoporous single-element metal Cu catalyst material obtained in this comparative example 3 is as follows Figure 1 As shown in g, it can be seen from the figure that only the Cu phase is contained. The nanoporous single-substance metal Cu catalytic material prepared in this comparative example is a nanoporous structure with a relatively regular structure distribution and larger pores than those in Example 1.

[0065] Comparative Example 4

[0066] A nanoporous metal oxide Co 3 O 4 The preparation method of the catalytic material is as described in Example 1, except that the obtained nanoporous single metal Co catalytic material is heated from room temperature to 450°C at a heating rate of 4°C / min in an air atmosphere, and then kept at this temperature for 2 hours to obtain a black powder sample, i.e., a nanoporous metal oxide Co 3 O 4 Catalytic material (Co 3 O 4 -5M NaOH).

[0067] After testing, the nanoporous metal oxide Co obtained in this comparative example 4 3 O 4 The physical structure of the catalytic material is Figure 1 h, it can be seen from the figure that it contains Co 3 O 4 Phase. The nanoporous metal oxide Co prepared in this comparative example 3O 4 The catalytic material is a nanoporous structure, distributed in the form of large particles, relatively loosely distributed, with large pores and a pore size of 15-360nm.

[0068] Application Example 1

[0069] The application of catalytic materials in catalytic activation of PMS to degrade BPA in wastewater is as follows:

[0070] The simulated wastewater sample uses bisphenol A (BPA) as the target pollutant and prepares a 20 mg / L bisphenol A aqueous solution. That is, an aqueous solution of BPA;

[0071] The catalytic materials prepared in Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, 4 were added to simulated wastewater samples, respectively, at an amount of 10 mg / L of the catalytic material. After mixing evenly, the mixture was stirred at room temperature for 30 min to bring it into an adsorption equilibrium state. Subsequently, PMS (permonosulfate) was added at room temperature (the amount of PMS added was 3.25 mM). The reaction time at room temperature was 10 min. Sampling was performed every 2 min, 1 mL of the sample solution was filtered using a 0.22 μm filter head, and then mixed with 0.5 mL of methanol for quenching. Finally, the content of organic pollutants in the sample was determined using high performance liquid chromatography.

[0072] Figure 5 The performance comparison chart of the catalytic materials prepared in Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, 4 in activating PMS and degrading BPA is shown in FIG. Figure 5 It can be seen that the single metal Co catalytic material prepared in Example 1 activated PMS to degrade 99.48% of BPA in 10 minutes. The catalytic activity of the catalytic materials prepared in Examples 1-4 is better than that of the catalytic materials prepared in Comparative Examples 1, 2, 3, and 4.

[0073] As a comparison, based on the above test method, the degradation performance test of BPA was carried out without adding PMS or without adding catalytic material (PMS acting alone), such as Figure 6 As shown. Figure 6 It can be seen that the single metal Co catalytic material and PMS prepared in Example 1 have no obvious degradation effect on BPA, while the single metal Co activated PMS shows excellent degradation performance on BPA.

[0074] As a comparison, based on the above test method, PMS was replaced by PDS (peroxydisulfate) and H 2 O 2 , to test the degradation performance of BPA, such as Figure 7 As shown. Figure 7 It can be seen that in the case of Co catalyst / PDS and Co catalyst / H 2 O2 In the system, the single metal Co catalytic material prepared in Example 1 had no significant effect on the degradation of BPA, but in the Co catalyst / PMS system, it showed excellent catalytic performance.

[0075] Application Example 2

[0076] The application of catalytic materials in catalytic activation of PMS to degrade phenol in wastewater is as follows:

[0077] The simulated wastewater sample was taken with phenol as the target pollutant, and a phenol aqueous solution with a concentration of 20 mg / L was prepared.

[0078] The catalytic materials prepared in Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, 4 were added to simulated wastewater samples, respectively, at an amount of 10 mg / L of the catalytic material. After mixing evenly, the mixture was stirred at room temperature for 30 min to bring it into an adsorption equilibrium state. Subsequently, PMS (permonosulfate) was added at room temperature (the amount of PMS added was 3.25 mM). The reaction time at room temperature was 10 min. Sampling was performed every 2 min, 1 mL of the sample solution was filtered using a 0.22 μm filter head, and then mixed with 0.5 mL of methanol for quenching. Finally, the content of organic pollutants in the sample was determined using high performance liquid chromatography.

[0079] Figure 8 The performance comparison chart of the catalytic materials prepared in Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, 4 in activating PMS to degrade phenol is shown in FIG. Figure 8 It can be seen that the elemental metal Co catalytic material prepared in Example 1 activated PMS and degraded 93.3% of phenol in 10 minutes. Its catalytic activity was slightly different from that of Examples 2, 3, and 4, but significantly better than that of the catalytic materials prepared in Comparative Examples 1, 2, 3, and 4.

[0080] As a comparison, based on the above test method, the degradation performance test of phenol was carried out without adding PMS or without adding catalytic material (PMS acting alone), such as Fig. 9 As shown. Fig. 9 It can be seen that the single metal Co catalytic material and PMS prepared in Example 1 have no obvious degradation effect on phenol, while the single metal Co activated PMS shows excellent degradation performance on phenol.

[0081] As a comparison, based on the above test method, PMS was replaced by PDS (peroxydisulfate) and H 2 O 2 , to test the degradation performance of phenol, such as Fig.10 As shown. Fig.10 It can be seen that in the case of Co catalyst / PDS and Co catalyst / H 2 O2 In the system, the single metal Co catalytic material prepared in Example 1 had no significant effect on the degradation of phenol, but in the Co catalyst / PMS system, it showed excellent catalytic performance.

[0082] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.

Claims

1. A nanoporous elemental metal Co catalytic material, characterized in that: The catalytic material is a Co elemental metal with a nanoporous structure, wherein the pore size of the nanoporous structure is 2-140 nm and the specific surface area is 40-50 m 2 ·g -1 , which is magnetic.

2. The method for preparing the nanoporous elemental metal Co catalytic material according to claim 1, comprising the steps of: (1) Al-Co alloy strips were prepared using metallic Al and Co as raw materials; (2) The Al-Co alloy strip is immersed in a corrosive solution, chemically dealloyed, cleaned, and dried to obtain a nanoporous single-element metal Co catalytic material.

3. The method for preparing the nanoporous elemental metal Co catalytic material according to claim 2, characterized in that: In step (1), the atomic ratio of metal Al and Co is 88-96:4-12.

4. The method for preparing the nanoporous elemental metal Co catalytic material according to claim 2, characterized in that: In step (1), the preparation method of the Al-Co alloy strip includes the following steps: mixing metal Al and Co, and smelting to obtain an alloy ingot; and spinning the alloy ingot to obtain an Al-Co alloy strip.

5. The method for preparing the nanoporous elemental metal Co catalytic material according to claim 4, characterized in that: Include one or more of the following conditions: i. Melting is carried out in a vacuum arc furnace; ii. The smelting method is as follows: smelting at 650-750°C for 1-2 minutes under an inert gas protection, and then cooling to room temperature; repeating the above steps 3-6 times to obtain an alloy ingot; preferably, the inert gas is nitrogen or argon; iii. The belt throwing is carried out in a vacuum belt throwing machine.

6. The method for preparing the nanoporous elemental metal Co catalytic material according to claim 2, characterized in that: In step (2), the etching solution is a NaOH aqueous solution with a concentration of 2-5 mol / L.

7. The method for preparing the nanoporous elemental metal Co catalytic material according to claim 2, characterized in that: In step (2), the temperature of chemical dealloying is room temperature, and the chemical dealloying is carried out until no bubbles are generated in the reaction system.

8. The method for preparing the nanoporous elemental metal Co catalytic material according to claim 2, characterized in that: In step (2), the cleaning is performed by using ultrapure water and anhydrous ethanol for 3-7 times respectively.

9. The method for preparing the nanoporous elemental metal Co catalytic material according to claim 2, characterized in that: In step (2), the drying is vacuum drying; the vacuum drying temperature is 40-80°C, preferably 60°C; and the vacuum drying time is 10-14 hours.

10. Use of the nanoporous elemental metal Co catalytic material according to claim 1 in catalyzing the degradation of organic pollutants in wastewater by peroxymonosulfate (PMS); Preferably, the organic pollutant is bisphenol A (BPA) and / or phenol.

Citation Information

Patent Citations

  • Modification method for preparing cobalt-based porous amorphous catalyst based on dealloying and application

    CN114904530A

  • Magnetic monatomic cobalt catalyst and method for catalyzing peracetic acid to degrade antibiotics by using magnetic monatomic cobalt catalyst

    CN117599794A