Preparation method of steel-bonded alloy particles
Through the process flow of ball milling, drying, granulation, sintering and roller separation and sieving, the problems of low production efficiency, low yield, high cost, high noise and dust in the traditional process are solved, and the efficient preparation of TiC-based materials is achieved. Steel-bonded alloy particles improve production efficiency, increase yield, and reduce costs and noise.
Patent Information
- Application Number
- CN202410835921.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-08
AI Technical Summary
The traditional process for preparing TiC-based steel alloy particles has the problems of low production efficiency, low yield, high cost, high noise, and excessive dust.
Adopting the process flow of ball milling, drying, granulation, dewaxing and sintering and roller separation and screening, the size and strength of the particles are controlled through the pressure roller and screen, reducing the crushing process, and directly making particles of corresponding sizes to avoid crushing with a powerful hammer. Use Paraffin wax is used as a molding agent to control the sintering temperature and time to achieve efficient preparation.
The production efficiency and yield rate are significantly improved, the cost and noise pollution are reduced, and dust is reduced. The production efficiency is increased to 1 ton/day, the yield rate is increased to more than 95%, and the sintering time is shortened to within 20 hours.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cemented carbide preparation, and particularly relates to a method for preparing steel-bonded alloy particles. Background Technology
[0002] TiC-based steel-bonded cemented carbide is commonly used as a wear-resistant material for the surface of composite wear-resistant equipment. The binder phase of this material has a composition similar to the base steel, enabling metallurgical bonding and resulting in better adhesion strength, making the wear-resistant layer less prone to peeling. This material is lightweight and possesses extremely high wear resistance, making it suitable for use in crushing and grinding media and wear parts in mining, cement, and coal powder grinding machinery. It helps reduce the cost of wear-resistant parts and the power consumption of individual machines, showing promising prospects for industrial application.
[0003] Traditional manufacturing processes typically follow this flow: batching – ball milling – drying – pressing (using a press) – dewaxing and sintering – crushing and sieving – finished granules. The drying process is generally spray drying or vacuum drying. Vacuum-dried mixtures require an additional granulation process to provide a mixture with better pressing performance for the pressing process. The granulated particles are small, typically tens to hundreds of micrometers in size. Crushing alloy products into granules often requires vigorous hammer crushing during the crushing process. If the product is in the form of thin flakes or discs, crushing it into granules results in low production efficiency, high undersize material, low yield, high cost, high noise, and high dust levels. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the background art above, and to provide a method for preparing steel-bonded alloy particles with high production efficiency, high yield, low cost, low noise and low dust.
[0005] To solve the above-mentioned technical problems, the technical solution proposed by this invention is as follows:
[0006] A method for preparing steel-bonded gold particles includes the following steps:
[0007] (1) The raw materials for steel-bonded alloy particles are batched, ball-milled, and dried to obtain a mixture;
[0008] (2) The mixture is granulated to obtain millimeter-sized blank particles. This granulation is carried out in a granulator, and the process is different from the roller granulation process after vacuum drying of the mixture (roller granulation is still in the state of the mixture and does not have the alloy properties and strength required by the customer). This granulation requires pressing the mixture into a strip with a certain strength after passing it through the pressure roller, and then crushing and screening it to obtain blank particles (the actual process is similar to crushing the pressed blank after pressing the mixture into shape). The material on the screen can be crushed and screened again, and the material under the screen can be pressed into a strip by the pressure roller again, crushed and screened again, and reused repeatedly.
[0009] (3) The blank particles are dewaxed and sintered to obtain sintered blanks;
[0010] (4) The sintered blank is separated by roller separation and sieve to obtain the steel-bonded alloy particles.
[0011] In the above preparation method, preferably, the steel-bonded alloy is a TiC-based steel-bonded cemented carbide.
[0012] More preferably, the TiC-based steel-bonded cemented carbide composition includes TiC and Fe, and also includes any one or more of MnFe, CrFe, Mo, and Ni.
[0013] Preferably, the ball-to-material ratio in the ball mill is 6:1-2, and the ball milling time is 24-36 hours.
[0014] Preferably, the drying is spray drying or vacuum drying.
[0015] Preferably, during the granulation process, a molding agent is added, which is paraffin wax, and the amount added is 2%-5% by mass.
[0016] Preferably, during the granulation process, the feeding speed is 1-60 rpm, the pressure roller speed is 1-60 rpm, and the screen diameter is 1-20 mm. The values of process parameters such as feeding speed, pressure roller speed, and particle size need to be determined based on the properties of the mixture and the particle size. The feeding speed and pressure roller speed can control and affect the strength of the pressed strip and particles (too fast a speed results in low strength of the pressed strip and particles, while too slow a speed leads to low production efficiency), directly affecting the properties of the alloy particles after dewaxing and sintering.
[0017] Preferably, the particle size of the blank particles is controlled between 1-20 mm. The particle size mainly meets customer needs and can be adjusted appropriately according to the operating conditions.
[0018] Preferably, the sintering temperature is 1380-1450℃, the sintering time does not exceed 20 hours, and the sintering atmosphere is vacuum sintering or 10-80 mbar low-pressure argon sintering. Compared with the traditional pressing and molding of semi-finished products, the blank particle size of the present invention is significantly reduced, and the dewaxing and sintering process time can be reduced from 30-40 hours in the traditional process to less than 20 hours, greatly reducing the sintering production cost and time.
[0019] Preferably, the roller crushing process can basically separate the particles that are stuck together during sintering by rolling them together, without the need to crush the product with heavy hammers, thus saving costs and reducing noise pollution and dust.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0021] 1. The preparation method of the present invention directly forms the desired finished product into particles of the corresponding size and sintersects them without going through the pressing, sintering and hammer crushing process. The sintering and crushing time and cost can be greatly reduced, and the actual yield of particles can be greatly improved (from 60-70% to more than 95%).
[0022] 2. The preparation method of the present invention can basically separate the particles that are stuck together during sintering by roller separation. It does not require the product to be crushed by heavy hammering, which saves costs, reduces noise pollution and dust, and greatly improves efficiency. The crushing rate has been increased from about 200 kg / day to 1 ton / day. Detailed Implementation
[0023] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below in conjunction with the specification and preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.
[0024] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0025] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0026] The granulation process of this invention is carried out in a granulator.
[0027] Example 1:
[0028] A method for preparing steel-bonded gold particles includes the following steps:
[0029] (1) The raw materials for steel-bonded alloy particles are batched, ball-milled, and spray-dried to obtain a mixture;
[0030] Raw material formula: TiC, Fe, MnFe, Ni, Mo, mixed in a certain proportion;
[0031] Ball milling parameters: alcohol as the ball milling medium, ball mill speed 65 rpm, ball-to-material ratio 6:1, ball milling time 24 h;
[0032] (2) After adding 5% mass percentage of molding agent paraffin to the mixture, granulation is carried out. During the granulation process, the feeding speed is controlled at 20 rpm, the roller speed is controlled at 20 rpm, the upper screen diameter is 7 mm, the lower screen diameter is 3 mm, and the blank particles with a particle size of about 5 mm are obtained.
[0033] (3) The blank particles are sintered under low pressure argon gas to obtain sintered blanks;
[0034] Sintering parameters: dewaxing sintering time 19.5h, final temperature 1430℃, holding time 90min, and 50mbar low-pressure argon gas filling;
[0035] (4) The sintered blank is separated by roller separation and sieve to obtain the steel-bonded alloy particles of this embodiment.
[0036] In this embodiment, 1 ton of finished pellets were produced. After being separated and sieved by rollers, the pellet weight that met the customer's requirements was 974.6 kg, with an actual yield of 97.46%.
[0037] Example 2:
[0038] A method for preparing steel-bonded gold particles includes the following steps:
[0039] (1) The raw materials for steel-bonded alloy particles are batched, ball-milled, and spray-dried to obtain a mixture;
[0040] Raw material formula: TiC, Fe, MnFe, Ni, Mo, mixed in a certain proportion;
[0041] Ball milling parameters: alcohol as the ball milling medium, ball mill speed 65 rpm, ball-to-material ratio 6:1, ball milling time 24 h;
[0042] (2) After adding 5% mass percentage of molding agent paraffin to the mixture, granulation is carried out. During the granulation process, the feeding speed is controlled at 20 rpm, the roller speed is controlled at 20 rpm, the upper screen diameter is 7 mm, the lower screen diameter is 3 mm, and the blank particles with a particle size of about 5 mm are obtained.
[0043] (3) Vacuum sintering of the blank particles to obtain sintered blank;
[0044] Sintering parameters: dewaxing sintering time 18h, final temperature 1430℃, holding time 90min, vacuum sintering;
[0045] (4) The sintered blank is separated by roller separation and sieve to obtain the steel-bonded alloy particles of this embodiment.
[0046] In this embodiment, 1 ton of finished pellets were produced. After being separated and sieved by rollers, the pellet weight that met the customer's requirements was 961.3 kg, with an actual yield of 96.13%.
[0047] Example 3:
[0048] A method for preparing steel-bonded gold particles includes the following steps:
[0049] (1) The raw materials for steel-bonded alloy particles are batched, ball-milled, and vacuum-dried to obtain a mixture;
[0050] Raw material formula: TiC, Fe, MnFe, Ni, Mo, mixed in a certain proportion;
[0051] Ball milling parameters: alcohol as the ball milling medium, ball mill speed 65 rpm, ball-to-material ratio 6:1, ball milling time 24 h;
[0052] (2) After adding 5% mass percentage of molding agent paraffin to the mixture, granulation is carried out to obtain blank particles. During the granulation process, the feeding speed is controlled at 40 rpm, the roller speed is controlled at 40 rpm, the upper screen diameter is 7 mm, the lower screen diameter is 3 mm, and blank particles with a particle size of about 5 mm are obtained.
[0053] (3) The blank particles are sintered under low pressure argon gas to obtain sintered blanks;
[0054] Sintering parameters: dewaxing sintering time 19h, final temperature 1430℃, holding time 90min, and 50mbar low-pressure argon gas filling;
[0055] (4) The sintered blank is separated by roller separation and sieve to obtain the steel-bonded alloy particles of this embodiment.
[0056] In this embodiment, 1 ton of finished granules was produced. After being separated and sieved by rollers, the granules that met the customer's requirements weighed 965.2 kg, with an actual yield of 96.52%.
[0057] Example 4:
[0058] A method for preparing steel-bonded gold particles includes the following steps:
[0059] (1) The raw materials for steel-bonded alloy particles are batched, ball-milled, and vacuum-dried to obtain a mixture;
[0060] Raw material formula: TiC, Fe, MnFe, Ni, Mo, mixed in a certain proportion;
[0061] Ball milling parameters: alcohol as the ball milling medium, ball mill speed 65 rpm, ball-to-material ratio 6:1, ball milling time 24 h;
[0062] (2) After adding 5% mass percentage of molding agent paraffin to the mixture, granulation is carried out. During the granulation process, the feeding speed is controlled at 50 rpm, the roller speed is controlled at 50 rpm, the upper screen diameter is 12 mm, and the lower screen diameter is 8 mm to obtain blank particles with a particle size of about 10 mm.
[0063] (3) Vacuum sintering of the blank particles to obtain sintered blank;
[0064] Sintering parameters: dewaxing sintering time 18h, final temperature 1430℃, holding time 90min, vacuum sintering;
[0065] (4) The sintered blank is separated by roller separation and sieve to obtain the steel-bonded alloy particles of this embodiment.
[0066] In this embodiment, 1 ton of finished granules was produced. After being separated and sieved by rollers, the granules that met the customer's requirements weighed 958.4 kg, with an actual yield of 95.84%.
[0067] Example 5:
[0068] A method for preparing steel-bonded gold particles includes the following steps:
[0069] (1) The raw materials for steel-bonded alloy particles are batched, ball-milled, and vacuum-dried to obtain a mixture;
[0070] Raw material formula: TiC, Fe, MnFe, Ni, Mo, mixed in a certain proportion;
[0071] Ball milling parameters: alcohol as the ball milling medium, ball mill speed 65 rpm, ball-to-material ratio 6:1, ball milling time 24 h;
[0072] (2) After adding 5% mass percentage of molding agent paraffin to the mixture, granulation is carried out. During the granulation process, the feeding speed is controlled at 30 rpm, the roller speed is controlled at 30 rpm, the upper screen diameter is 12 mm, and the lower screen diameter is 8 mm to obtain blank particles with a particle size of about 10 mm.
[0073] (3) Vacuum sintering of the blank particles to obtain sintered blank;
[0074] Sintering parameters: dewaxing sintering time 17h, final temperature 1430℃, holding time 90min, vacuum sintering;
[0075] (4) The sintered blank is separated by roller separation and sieve to obtain the steel-bonded alloy particles of this embodiment.
[0076] In this embodiment, 2 tons of finished pellets were produced. After being separated and sieved by rollers, the weight of pellets meeting customer requirements was 1944.5 kg, with an actual yield of 97.23%.
[0077] Comparative Example 1:
[0078] Traditional methods for producing steel-bonded alloy particles include the following steps:
[0079] (1) Same as Example 1;
[0080] (2) The mixture is pressed into sheet blanks using a press.
[0081] (3) The sheet blank is sintered, and the sintering process is the same as in Example 1, to obtain a sintered blank;
[0082] (4) The sintered blank is crushed by hammer crusher (low production efficiency, high noise, high dust, high cost), and then sieved to obtain finished particles.
[0083] The traditional production process produces 2 tons of sintered finished products. After crushing and sieving, the weight of particles that meet the customer's size requirements is 1364 kg, with an actual yield of only 68.2%. The remaining screened material weighs 632.2 kg and is difficult to process.
[0084] Comparative Example 2:
[0085] Traditional methods for producing steel-bonded alloy particles include the following steps:
[0086] (1) Same as Example 2;
[0087] (2) Add the mixture to the molding agent to granulate and obtain particles with a particle size of about 60 micrometers (the purpose is to improve the pressing performance of the mixture). Then press the mixture with a press to obtain a sheet blank.
[0088] (3) Vacuum sintering is performed on the sheet blank at a temperature of 1430℃ and a holding time of 90min to obtain the sintered blank.
[0089] (4) The sintered blank is crushed by hammer crusher (low production efficiency, high noise, high dust, high cost), and then sieved to obtain finished particles.
[0090] The traditional production process produces 2 tons of sintered finished products. After crushing and sieving, the weight of particles that meet the customer's size requirements is 1391 kg, with an actual yield of only 69.55%. The remaining 609 kg of undersize material is difficult to process.
Claims
1. A method for preparing steel-bonded alloy particles, characterized in that: The steps include: (1) mixing raw materials of steel-bonded alloy particles, ball milling, and drying to obtain a mixed material; (2) granulating the mixture to obtain millimeter-sized blank particles; (3) sintering the blank particles to obtain a sintered blank; (4) The sintered blank is subjected to roller separation and screening to obtain the steel-bonding alloy particles.
2. The method for preparing the steel-bonded alloy particles according to claim 1, characterized in that: The steel bonding alloy is TiC-based steel-bonded hard alloy.
3. The method for preparing the steel-bonded alloy particles according to claim 2, characterized in that: The TiC-based steel-bonded hard alloy contains TiC and Fe, and further contains any one or more of MnFe, CrFe, Mo and Ni.
4. The method for preparing the steel-bonded alloy particles according to claim 1, characterized in that: The ball-to-material ratio of the ball milling is 6:1-2, and the ball milling time is 24-36h.
5. The method for preparing the steel-bonded alloy particles according to claim 1, characterized in that: The drying is spray drying or vacuum drying.
6. The method for preparing steel-bonded alloy particles according to claim 1, characterized in that: During the granulation process, the molding agent is paraffin, and the added amount is 2%-5% by mass.
7. The method for preparing steel-bonded alloy particles according to claim 1, characterized in that: During the granulation process, the feeding speed is 1-60 rpm, and the speed of the pressing roller is 1-60 rpm.
8. The method for preparing steel-bonded alloy particles according to claim 1, characterized in that: The particle size of the blank particles is controlled within a range of 1-20 mm.
9. The method for preparing steel-bonded alloy particles according to claim 1, characterized in that: The sintering temperature is 1380-1450° C., and the dewaxing sintering time does not exceed 20 hours.
10. The method for preparing the steel-bonded alloy particles according to any one of claims 1 to 9, characterized in that: The sintering atmosphere is vacuum sintering or 10-80 mbar low-pressure argon sintering.