Method for producing and manufacturing ultra-high-performance concave-convex concrete slab
By using polystyrene foam (EPS) filler and glass fiber injection technology in UHPC production, the problems of large amounts of premix and difficult construction in traditional UHPC concave-convex board production are solved, and a lighter and lower-cost production method is achieved. , improving construction efficiency and the compressive strength of components.
Patent Information
- Application Number
- CN202410907998.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-08
AI Technical Summary
Traditional concave-convex UHPC has problems such as large amount of premix, high production cost, and difficult construction.
Polystyrene foam (EPS) filler is used to replace part of the UHPC premix. The EPS is pre-embedded in the mold cavity to reduce the amount of premix and the weight of the components. The glass fiber spraying process is used for spraying the primer, combined with self-leveling properties. Watering and natural air-drying maintenance improve construction efficiency and safety.
It significantly reduces the production cost and weight of UHPC components, improves construction efficiency and safety, and enhances the installation convenience and compressive strength of the components.
Smart Images

Figure CN118744470A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high-performance concrete, and in particular to a method for producing an ultra-high-performance concave-convex concrete slab. Background Art
[0002] UHPC (Ultra High Performance Concrete) is a high-performance concrete with excellent strength, durability and crack resistance, and is therefore widely used in the production of building components.
[0003] 1. For example, a Chinese patent discloses an ultra-high performance concrete sandwich panel (publication number: CN217175353U), including an ultra-high performance concrete sandwich panel body, on which a transverse rib beam and a longitudinal rib beam are arranged, and the transverse rib beam and the longitudinal rib beam are arranged in multiple numbers, and the transverse rib beam and the longitudinal rib beam cross to form a matrix structure, and the middle cavity of the matrix structure is filled with thermal insulation material, and the transverse rib beam and the longitudinal rib beam are provided with steel bars. The ultra-high performance concrete sandwich panel is not only corrosion-resistant and has a high fire resistance level, reduces the later maintenance cost, and improves the fire resistance of the house, but also has high strength, light weight, easy installation, and certain thermal insulation performance.
[0004] 2. A method for preparing a UHPC premix (publication number: CN115872705B), at least all the cementitious materials and part or all of the aggregates for preparing the UHPC premix are fed into a ball mill to grind and disperse the materials, and a mixed material is obtained after exiting the ball mill; the mixed material is dry-mixed with all other raw materials for a mixing time of 0.5-3 minutes to obtain a UHPC premix. This invention can greatly shorten the wet mixing time of materials when preparing UHPC premixes by adopting short-time ball milling mixing and optimizing material formula, and can also improve the homogeneity of UHPC; even if silica fume, semi-densified silica fume, and highly densified silica fume are added, the speed of opening the wet mixed slurry during its preparation far exceeds that of UHPC premixes with ordinary mixing methods.
[0005] However, there are some problems with traditional concave-convex UHPC, such as large amount of UHPC premix, high production cost, large mass of component panels, and difficult construction.
[0006] Therefore, it is necessary to propose a method for producing ultra-high performance concave-convex concrete slabs to solve the above problems. Summary of the invention
[0007] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a lighter, lower-cost method for producing ultra-high performance concave-convex concrete panels to solve the above-mentioned problems.
[0008] A method for producing an ultra-high performance concave-convex concrete slab, the method steps are as follows:
[0009] S1. Cleaning the mold: Clean the inside of the mold to prevent particles from affecting the surface texture;
[0010] S2. Apply release agent: Apply release agent inside the mold to release the mold more effectively without damaging the product;
[0011] S3, spraying primer UHPC mixture: thickness about 2cm;
[0012] S4. Place polystyrene foam (EPS): leave two centimeters around the polystyrene foam (EPS);
[0013] S5. Grouting: Mix UHPC premix and pour it, pouring and spreading at the same time. The material itself has self-leveling properties.
[0014] S6, dry maintenance;
[0015] S7, demoulding: demoulding after standing to reach the curing strength;
[0016] S8. Air drying and curing: UHPC board is naturally air dried and cured;
[0017] S9. Finished product protection: UHPC board finished product packaging protection.
[0018] In step S1, the mold can be steel mold, wooden mold, silicone mold, resin mold or other types of molds according to the UHPC production requirements. Regardless of the type of mold, the inside should be cleaned first.
[0019] In step S3, the UHPC mixture for primer is preferably sprayed with a glass fiber mixture spraying process to prevent the steel fiber from piercing the surface layer. The primer thickness must meet the strength requirements to avoid the subsequent cracking of the plate.
[0020] The thickness of the base UHPC mixture is 20mm-30mm.
[0021] In step S4, the cut polystyrene foam (EPS) is placed in the convex UHPC groove; the shape needs to be cut in advance to facilitate placement inside the mold protrusion, and the polystyrene foam (EPS) needs to leave a gap with the surrounding primer to avoid cracking due to too thin wall thickness.
[0022] The polystyrene foam (EPS) needs to leave a gap of 18-20mm with the surrounding primer to prevent cracking and delamination due to the wall thickness being too thin.
[0023] During the pouring of the UHPC premix in step S5, another person is required to cooperate in tamping to ensure that the polystyrene foam (EPS) does not move, the premix is poured evenly, and the filling is dense. According to the size and strength requirements of the UHPC, steel bars can be added to increase the strength of the plate, and embedded sleeves can be added according to the plate installation requirements.
[0024] Among them, the air-drying maintenance in step 6 is to cover with a tarp and air-dry.
[0025] Both the air drying and demoulding curing must meet the strength requirements of the UHPC curing standards, and early demoulding, transportation and construction are not allowed.
[0026] The UHPC premix includes: 50-80 parts of silicate cement, 5-15 parts of low-heat silicate cement, 3-7 parts of ultrafine high-density terrestrial cement, 8-12 parts of high-density silica fume, 0.01-0.2 parts of nano-silicon dioxide, 0.02-0.1 parts of graphene oxide, 30-50 parts of extra-fine aggregate (limestone sand), 40-60 parts of coarse aggregate (natural crushed stone), 2.1-3 parts of admixtures, and 0.02-0.1 parts of triethanolamine.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. The present invention replaces the convex UHPC inner cavity premix by pre-embedded polystyrene foam (EPS) filler, thereby reducing the amount of premix and reducing production costs.
[0029] 2. The present invention replaces part of the UHPC premix with EPS, which greatly reduces the weight of the component, facilitates construction, improves construction efficiency, and reduces the load required for the component keel, making the keel more economical and safer.
[0030] 3. In the production process of the concave-convex UHPC components of the present invention, polystyrene foam (EPS) filler is pre-buried in the UHPC production process, thereby reducing the amount of UHPC mixture and reducing the weight of the UHPC components, significantly reducing the production cost of the UHPC components, reducing the weight of the components, and improving the efficiency and safety of on-site construction and installation. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A diagram of the production method of high performance concrete of the present invention;
[0032] Figure 2 It is a structural schematic diagram of the step of placing polystyrene foam in the present invention;
[0033] Figure 3 This is a top view of the UHPC board structure of the present invention;
[0034] Figure 4 This is a side structural diagram of the UHPC board of the present invention. DETAILED DESCRIPTION
[0035] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0036] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, but the present invention can be implemented in many different ways as defined and covered by the claims.
[0037] like Figure 1 Combined with Figures 2 to 4 As shown, a method for producing an ultra-high performance concave-convex concrete slab comprises the following steps:
[0038] S1. Cleaning the mold: Clean the inside of the mold to prevent particles from affecting the surface texture;
[0039] S2. Apply release agent: Apply release agent inside the mold to release the mold more effectively without damaging the product;
[0040] S3, spraying primer UHPC mixture: thickness about 2cm;
[0041] S4. Place polystyrene foam (EPS): leave two centimeters around the polystyrene foam (EPS);
[0042] S5. Grouting: Mix UHPC premix and pour it, pouring and spreading at the same time. The material itself has self-leveling properties.
[0043] S6. Drying and curing: Use waterproof cloth for drying and curing;
[0044] S7, demoulding: demoulding after standing to reach the curing strength;
[0045] S8, air drying and curing: natural air drying and curing;
[0046] S9. Finished product protection: Finished product packaging protection.
[0047] In step S1, the mold can be steel mold, wooden mold, silicone mold, resin mold or other types of molds according to the UHPC production requirements. Regardless of the type of mold, the inside should be cleaned first.
[0048] In step S3, the UHPC mixture for primer is preferably sprayed with a glass fiber mixture spraying process to prevent the steel fiber from piercing the surface layer. The primer thickness must meet the strength requirements to avoid the subsequent cracking of the plate.
[0049] The thickness of the base UHPC mixture is 20mm-30mm.
[0050] In step S4, the cut polystyrene foam (EPS) is placed in the convex UHPC groove; the shape needs to be cut in advance to facilitate placement inside the mold protrusion, and the polystyrene foam (EPS) needs to leave a gap with the surrounding primer to avoid cracking due to too thin wall thickness.
[0051] The polystyrene foam (EPS) needs to leave a gap of 18-20mm with the surrounding primer to prevent cracking and delamination due to the wall thickness being too thin.
[0052] During the pouring of the UHPC premix in step S5, another person is required to cooperate in tamping to ensure that the polystyrene foam (EPS) does not move, the premix is poured evenly, and the filling is dense. According to the size and strength requirements of the UHPC, steel bars can be added to increase the strength of the plate, and embedded sleeves can be added according to the plate installation requirements.
[0053] Among them, the air-drying maintenance in step 6 is to cover with a tarp and air-dry.
[0054] Both the air drying and demoulding curing must meet the strength requirements of the UHPC curing standards, and early demoulding, transportation and construction are not allowed.
[0055] The UHPC premix includes: 50-80 parts of silicate cement, 5-15 parts of low-heat silicate cement, 3-7 parts of ultrafine high-density terrestrial cement, 8-12 parts of high-density silica fume, 0.01-0.2 parts of nano-silicon dioxide, 0.02-0.1 parts of graphene oxide, 30-50 parts of extra-fine aggregate (limestone sand), 40-60 parts of coarse aggregate (natural crushed stone), 2.1-3 parts of admixtures, and 0.02-0.1 parts of triethanolamine.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] 1. The present invention replaces the convex UHPC inner cavity premix by pre-embedded polystyrene foam (EPS) filler, thereby reducing the amount of premix and reducing production costs.
[0058] 2. The present invention replaces part of the UHPC premix with EPS, which greatly reduces the weight of the component, facilitates construction, improves construction efficiency, and reduces the load required for the component keel, making the keel more economical and safer.
[0059] 3. In the production process of the concave-convex UHPC components of the present invention, polystyrene foam (EPS) filler is pre-buried in the UHPC production process, thereby reducing the amount of UHPC mixture and reducing the weight of the UHPC components, significantly reducing the production cost of the UHPC components, reducing the weight of the components, and improving the efficiency and safety of on-site construction and installation.
[0060] Embodiment 1:
[0061] Clean the mold: clean the inside of the mold to prevent particles from affecting the surface texture; apply mold release agent: apply mold release agent inside the mold to demould more effectively without damaging the product; spray primer UHPC mixture: thickness is about 2cm; place polystyrene foam (EPS): reserve two centimeters around the polystyrene foam (EPS); grouting: mix UHPC premix (wherein UHPC premix includes: 50 parts of silicate cement, 5 parts of low-heat silicate cement, 3 parts of ultrafine high-density territories, 8 parts of high-density silica fume, 0.01 parts of nano-silicon dioxide, 0.02 parts of graphene oxide, 30 parts of ultra-fine aggregate (limestone sand), 40 parts of coarse aggregate (natural crushed stone), 2.1 parts of admixtures, 0.02 parts of triethanolamine) for pouring, pouring and shoveling at the same time, the material itself has self-leveling properties; dry curing; demoulding: demoulding after standing to reach the curing strength; air drying curing; finished product packaging protection.
[0062] Embodiment 2:
[0063] Clean the mold: clean the inside of the mold to prevent particles from affecting the surface texture; apply mold release agent: apply mold release agent inside the mold to demould more effectively without damaging the product; spray primer UHPC mixture: thickness of about 2cm; place polystyrene foam (EPS): reserve two centimeters around the polystyrene foam (EPS); grouting: mix UHPC premix (wherein UHPC premix includes: 80 parts of silicate cement, 5 parts of low-heat silicate cement, 7 parts of ultrafine high-density territories, 12 parts of high-density silica fume, 0.2 parts of nano-silicon dioxide, 0.1 parts of graphene oxide, 30-50 parts of ultra-fine aggregate (limestone sand), 40-60 parts of coarse aggregate (natural crushed stone), 2.1-3 parts of admixtures, 0.02-0.1 parts of triethanolamine) for pouring, pouring and sliding at the same time, the material itself has self-leveling properties; dry curing; demoulding: demoulding after standing to reach the curing strength; air drying curing; finished product packaging protection.
[0064] Embodiment 3:
[0065] Clean the mold: clean the inside of the mold to prevent particles from affecting the surface texture; apply mold release agent: apply mold release agent inside the mold to demould more effectively without damaging the product; spray primer UHPC mixture: thickness of about 2cm; place polystyrene foam (EPS): reserve two centimeters around the polystyrene foam (EPS); grouting: mix UHPC premix (wherein UHPC premix includes: 60 parts of silicate cement, 7 parts of low-heat silicate cement, 6 parts of ultrafine high-density territories, 10 parts of high-density silica fume, 0.08 parts of nano-silicon dioxide, 0.07 parts of graphene oxide, 40 parts of ultra-fine aggregate (limestone sand), 50 parts of coarse aggregate (natural crushed stone), 2.6 parts of admixtures, 0.09 parts of triethanolamine) for pouring, pouring and shoveling at the same time, the material itself has self-leveling properties; dry curing; demoulding: demoulding after standing to reach the curing strength; air drying curing; finished product packaging protection.
[0066] Comparative experiment
[0067] The ultra-high performance concrete panels prepared by the solutions in Examples 1-3 and Comparative Documents 1-2 were selected for strength and pressure resistance tests, and the following Table 1 was obtained:
[0068] Experimental Group Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Compressive strength / Mpa 56 58 57 50 51
[0069] Comparative Analysis 1:
[0070] It can be seen from Table 1 that the strength of the concrete slabs prepared by the methods of Examples 1-3 is significantly higher than that of the concrete slabs prepared by the methods of Comparative Documents 1-2, which indicates that the ultra-high-strength concrete slabs prepared by the method of the present invention have better compressive strength.
[0071] Comparative Analysis 2:
[0072] It can be seen from Table 1 that the concrete slab of Example 2 is stronger than that of Example 1 and Example 3, which indicates that a high content of nano-silicon dioxide can improve the strength of the concrete slab.
[0073] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made by using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for producing an ultra-high performance concave-convex concrete slab, characterized in that: The method steps are: S1. Cleaning the mold: Clean the inside of the mold to prevent particles from affecting the surface texture; S2. Apply release agent: Apply release agent inside the mold to release the mold more effectively without damaging the product; S3, spraying primer UHPC mixture; S4, placing polystyrene foam; S5. Grouting: Mix UHPC premix and pour it, pouring and spreading at the same time. The material itself has self-leveling properties. S6, dry maintenance; S7, demoulding: demoulding after standing to reach the curing strength; S8. Air drying and curing: UHPC board is naturally air dried and cured; S9. Finished product protection: UHPC board finished product packaging protection.
2. The method for producing an ultra-high performance concave-convex concrete slab according to claim 1, characterized in that: The mold in step S1 can be a steel mold, a wooden mold, a silicone mold or a resin mold according to the UHPC production requirements.
3. The method for producing an ultra-high performance concave-convex concrete slab according to claim 1, characterized in that: The UHPC mixture for primer in step S3 is preferably sprayed with a glass fiber mixture spraying process.
4. The method for producing an ultra-high performance concave-convex concrete slab according to claim 1, characterized in that: The thickness of the base UHPC mixture is 20mm-30mm.
5. The method for producing an ultra-high performance concave-convex concrete slab according to claim 1, characterized in that: In step S4, the cut polystyrene foam is placed in the convex UHPC groove; a gap needs to be left between the polystyrene foam and the surrounding primer to avoid cracking due to too thin wall thickness.
6. The method for producing an ultra-high performance concave-convex concrete slab according to claim 1, characterized in that: There should be a gap of 18-20mm between the polystyrene foam and the surrounding primer to prevent the wall from being too thin and cracking and delamination.
7. The method for producing an ultra-high performance concave-convex concrete slab according to claim 1, characterized in that: During the pouring of the UHPC premix in step S5, another person is required to cooperate in tamping, so that the premix is poured evenly and filled densely. According to the size and strength requirements of the UHPC, steel bars can be added to increase the strength of the plate, and embedded sleeves can be added according to the plate installation requirements.
8. The method for producing an ultra-high performance concave-convex concrete slab according to claim 1, characterized in that: In step 6, the drying and curing is done by covering with waterproof cloth.
9. The method for producing an ultra-high performance concave-convex concrete slab according to claim 1, characterized in that: Both the air drying and demoulding curing must meet the strength requirements of the UHPC curing standards, and no demoulding, transportation or construction shall be carried out in advance.
10. The method for producing an ultra-high performance concave-convex concrete slab according to claim 1, characterized in that: The UHPC premix includes: 50-80 parts of silicate cement, 5-15 parts of low-heat silicate cement, 3-7 parts of ultrafine high-density terrestrial aggregate, 8-12 parts of high-density silica fume, 0.01-0.2 parts of nano silicon dioxide, 0.02-0.1 parts of graphene oxide, 30-50 parts of extra fine aggregate, 40-60 parts of coarse aggregate, 2.1-3 parts of admixture, and 0.02-0.1 parts of triethanolamine.