SiC fiber reinforced metal matrix composite pipe structure and preparation method thereof
By designing SiC fiber-reinforced metal matrix composite tube structures in aircraft tubular structural parts, and using chemical vapor deposition and hot isostatic pressing processes, the problem of traditional metal materials being difficult to meet lightweight requirements and fiber breakage has been solved, and an efficient shaft has been achieved. Towards load carrying capacity and weight reduction.
Patent Information
- Application Number
- CN202410883040.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-03
AI Technical Summary
In the aerospace field, traditional metal materials are difficult to meet the lightweight needs of aircraft tubular structural parts, and SiC fiber-reinforced metal matrix composites are prone to fiber breakage in tubular structural parts, making preparation difficult.
Design a SiC fiber-reinforced metal matrix composite tube structure. Composite material layers are formed by coaxial compounding between the inner and outer metal matrix. Continuous single-filament SiC fibers are prepared using chemical vapor deposition method, using ladder-shaped arrangement and thermal etc. Static pressing process ensures uniform fiber distribution and connection strength.
It significantly improves the axial load-bearing capacity of tubular structural parts, reduces weight, avoids fiber breakage and local defects, and improves the lightweight performance of the aircraft.
Smart Images

Figure CN118744568A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of composite material structure design and manufacturing, and in particular to a SiC fiber reinforced metal matrix composite material pipe structure and a preparation method thereof. Background Art
[0002] In recent years, with the continuous development of the aerospace field, in order to further improve the performance of aircraft, the demand for lightweight aircraft structural parts has been increasing. The relevant theories and preparation processes of traditional metal materials such as high-strength steel, aluminum alloy, and titanium alloy have become mature. Under the premise of ensuring the mechanical properties such as stiffness and strength of structural parts, it is difficult to further meet the weight reduction needs of structural parts. Therefore, using lightweight and high-strength materials to replace traditional metal materials has gradually become the most important and effective way to achieve lightweighting of advanced aircraft.
[0003] SiC fiber reinforced metal matrix composites are usually a composite material with SiC fiber filaments as reinforcement and metal material as matrix. SiC fiber filaments have the characteristics of high strength, high modulus, and low density. As a reinforcement, they can effectively improve the specific strength, specific stiffness, creep resistance, and high temperature durability of metal materials. Using SiC fiber reinforced metal matrix composites to replace the original metal materials to prepare aircraft structural parts can ensure the performance requirements of the structural parts and achieve a weight reduction effect of 20% to 60%.
[0004] Tubular structural parts are an important type of load-bearing structural parts in advanced aircraft, and are usually subjected to large tensile and compressive loads. Due to the characteristics of thin walls and large aspect ratio, when SiC fiber-reinforced metal matrix composites are used to replace traditional metal materials to prepare tubular structural parts, fiber breakage and other problems are prone to occur, making the preparation of structural parts difficult. Therefore, a reasonable and effective SiC fiber-reinforced metal matrix composite tubular structure and its preparation method are proposed, which has great significance and application prospects in the field of aerospace. Summary of the invention
[0005] In response to the demand for weight reduction of tubular structural parts of advanced aircraft, the present invention proposes a SiC fiber reinforced metal matrix composite tubular structure and a preparation method thereof. The SiC fiber reinforced metal matrix composite tubular structural parts prepared based on the present invention can improve the axial bearing capacity and significantly reduce the weight of the tubular structural parts compared with the tubular structural parts prepared with matrix metal materials.
[0006] The present invention is achieved through the following technical solutions:
[0007] A SiC fiber reinforced metal matrix composite material pipe structure is a tubular structure formed by coaxially compounding an inner metal matrix, a composite material layer and an outer metal matrix in sequence. The outer shape of the pipe structure is a cylinder with equal outer diameters. The SiC fiber reinforced metal matrix composite material layer is arranged in a metal matrix pipe wall composed of an inner metal matrix and an outer metal matrix. In the composite material layer, SiC fibers with metal coatings deposited on the surface are arranged in the metal matrix pipe wall as reinforcements, and the two ends of the composite material layer are arranged in a stepped manner at the joints with the pipe structure. The pipe structure is divided into a central section and a joint section. The joint section is a part where the two ends of the composite material layer are connected to the pipe structure. The central section is a non-joint section part of the SiC fiber reinforced metal matrix composite material pipe structure where SiC fibers are uniformly arranged. The wall thickness of the joint section of the pipe structure is greater than that of the central section.
[0008] The SiC fiber reinforced metal matrix composite material tube structure is a continuous monofilament SiC fiber, which is prepared by chemical vapor deposition with tungsten wire or carbon fiber as a deposition substrate. The SiC fiber has a diameter range of 50 to 160 μm, a tensile strength range of 3000 to 4000 MPa, and a density range of 2.80 to 3.50 g / cm 3 .
[0009] The SiC fiber reinforced metal matrix composite material tube structure has a metal matrix tube wall thickness ranging from 4 to 8 mm, and the metal matrix tube wall material is a light alloy such as aluminum alloy, titanium alloy or titanium aluminum alloy.
[0010] The SiC fiber reinforced metal matrix composite material tube structure has a composite material layer thickness ranging from 2 to 4 mm, the composite material layer is equidistant from the inner and outer walls of the tube structure, no SiC fibers are exposed above or below the tube structure, the SiC fiber axial direction is consistent with the axial direction of the tube structure, the SiC fibers are arranged in layers along the radial direction of the tube structure, the number of SiC fiber layers ranges from 4 to 8 layers, and the SiC fibers between layers are densely arranged in an interlaced manner, that is, the SiC fibers in the cross section of the tube structure are approximately hexagonally densely packed.
[0011] The SiC fiber reinforced metal matrix composite tube structure has a length of each layer of SiC fiber that decreases from inside to outside, and the single-side decreasing range of each layer is 0.5 to 2.5 mm, so that the angle α between the bottom edge connection line or the top edge connection line of the composite layer and the axial edge is in the range of 5 to 20 degrees.
[0012] The SiC fiber reinforced metal matrix composite material pipe structure has a thickness of the inner metal matrix in the pipe structure joint section that is greater than the thickness of the inner metal matrix in the center section, and the thickness is greater by 50 to 100% of the thickness of the inner metal matrix in the center section. The end of the thickened portion of the inner metal matrix is flush with the end of the outermost SiC fiber of the composite material layer, and chamfers are used to connect different thickness regions of the inner metal matrix.
[0013] The method for preparing the SiC fiber reinforced metal matrix composite material tube structure comprises the following steps:
[0014] (1) Designing and processing a composite material tube structure mold: The composite material tube structure mold consists of a tube structure mold liner, a tube structure mold outer sleeve, and two tube structure mold mouth covers. The tube structure mold liner is an equal-diameter cylinder made of a metal matrix material, and the tube structure mold outer sleeve is a cylinder made of a metal matrix material with a circular cross-section. The tube structure mold liner and the tube structure mold outer sleeve are coaxially arranged relative to each other. The tube structure mold mouth covers are respectively a left cover and a right cover of the tube structure mold. The left cover and the right cover of the tube structure mold are coaxially symmetrically arranged at the two ends of the tube structure mold liner and the tube structure mold outer sleeve; the four tube structure mold components are assembled in close contact and matched in size, and a cavity for arranging the composite material is formed;
[0015] (2) preparing composite precursor fibers: depositing a metal coating on the surface of SiC fibers by physical vapor deposition to obtain composite precursor fibers, wherein the volume fraction of SiC fibers ranges from 40 to 80%;
[0016] (3) preparing a composite material prefabricated tape: arranging composite material precursor wires and bonding them with organic adhesive to form a single-layer composite material prefabricated tape, and cutting the prefabricated tape according to the size of the inner lining of the pipe structure mold and the stepped size of the composite material layer of the pipe structure joint section;
[0017] (4) Laying composite material prefabricated tapes: Then, the composite material prefabricated tapes are stacked and pasted on the outer wall of the inner lining of the pipe structure mold in order from long to short, and the left cover of the pipe structure mold, the outer sleeve of the pipe structure mold, and the right cover of the pipe structure mold are assembled and fixed in order;
[0018] (5) Heat treatment of the composite material pipe structure mold: vacuum heat treatment is performed on the composite material pipe structure mold to remove the organic glue used in the process of preparing the composite material prefabricated tape, the temperature range is 200 to 400° C., and the heating time range is 60 to 120 min;
[0019] (6) Sealing the composite tube structure mold: using an electron beam vacuum welding process to seal the gap between the four tube structure mold components and the composite prefabricated belt;
[0020] (7) Composite tube structure molding: The vacuum-sealed composite tube structure mold is processed by hot isostatic pressing to completely close the gaps between the composite precursor wires and the composite preformed tapes to form a dense SiC reinforced metal matrix composite preform;
[0021] (8) Composite material tube structure processing: The excess metal matrix of the SiC reinforced metal matrix composite preform is removed by mechanical processing to obtain a SiC fiber reinforced metal matrix composite tube structure.
[0022] The preparation method of the SiC fiber reinforced metal matrix composite material tube structure, the tube structure mold outer sleeve includes an outer sleeve equal-diameter inner bore surface and an outer sleeve positioning groove, the outer sleeve positioning grooves are respectively an outer sleeve left positioning groove and an outer sleeve right positioning groove, the outer sleeve left positioning groove and the outer sleeve right positioning groove are respectively coaxially opened at the two ends of the outer sleeve equal-diameter inner bore surface.
[0023] In the method for preparing the SiC fiber reinforced metal matrix composite tube structure, the tube structure mold cover is a stepped rotating body whose diameters are respectively consistent with the diameters of the outer sleeve positioning groove and the diameters of the outer sleeve equal-diameter inner bore surface, wherein:
[0024] The left cover of the pipe structure mold is provided with a left cover positioning step, a contact surface between the left cover and the inner bore surface of the outer sleeve, and a contact surface between the left cover and the precursor wire. The outer diameter of the left cover positioning step matches the diameter of the left positioning groove of the outer sleeve. The outer diameter of the contact surface between the left cover and the inner bore surface of the outer sleeve matches the diameter of the equal-diameter inner bore surface of the outer sleeve. The contact surface between the left cover and the precursor wire is a truncated cone-shaped surface corresponding to the inner side of the contact surface between the left cover and the inner bore surface of the outer sleeve. The edge size of the contact surface between the left cover and the precursor wire is consistent with the stepped arrangement size of the composite material layer at the pipe structure joint.
[0025] The right cover of the tube structure mold is provided with a right cover positioning step, a contact surface between the right cover and the inner bore surface of the outer sleeve, and a contact surface between the right cover and the pioneer wire. The outer diameter of the right cover positioning step matches the diameter of the right positioning groove of the outer sleeve, the outer diameter of the contact surface between the right cover and the inner bore surface of the outer sleeve matches the diameter of the equal-diameter inner bore surface of the outer sleeve, the contact surface between the right cover and the pioneer wire is a truncated cone-shaped surface corresponding to the inner side of the contact surface between the right cover and the inner bore surface of the outer sleeve, and the edge size of the contact surface between the right cover and the pioneer wire is consistent with the stepped arrangement size of the composite material layer at the tube structure joint.
[0026] In the method for preparing the SiC fiber reinforced metal matrix composite material tube structure, in step (7), the hot isostatic pressing temperature ranges from 400 to 1200° C., the hot isostatic pressing pressure ranges from 25 to 300 MPa, and the hot isostatic pressing time ranges from 60 to 120 min.
[0027] The design idea of the present invention is:
[0028] According to the common service conditions of the pipe structure, continuous single-filament SiC fiber is used to unidirectionally reinforce the pipe structure axially, so as to improve the service performance of the pipe structure in a targeted manner. Based on the calculation formula of interface shear strength and the stepped lap theory, the arrangement of SiC fiber composite material layer in the metal matrix is designed to improve the connection performance of the joint between the composite material layer and the metal matrix, so as to avoid the failure of the SiC fiber reinforced metal matrix composite pipe structure at the weak connection under the service conditions. For this composite pipe structure, the three-step method of fiber filament-pioneer filament-prefabricated tape is used to prepare the composite material layer, simplify the fiber laying process, accurately control the volume fraction of the reinforcement, ensure the uniform distribution of fiber filaments in the composite material layer, and avoid local defects such as fiber breakage and fiber interlacing during the fiber laying process; the composite material preform is made by using metal matrix mold, electron beam vacuum welding, hot isostatic pressing and other integrated molding processes to ensure the density of the material in the pipe structure.
[0029] The advantages and beneficial effects of the present invention include:
[0030] The present invention proposes a SiC fiber metal matrix composite material tube structure and a preparation method thereof. The composite material tube structure uses continuous monofilament SiC fiber as a reinforcement, and uses a stepped arrangement to improve the connection strength between the reinforcement and the metal matrix. It is suitable for a variety of light alloy metal matrices such as aluminum alloy, titanium alloy, and titanium aluminum alloy. Compared with the tube structure of the same specification prepared using only a metal matrix, the axial bearing capacity of the tube structure can be improved and the weight of the tube structure can be reduced, which is of great significance in the lightweight technology of high-performance aircraft. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the SiC fiber reinforced metal matrix composite tube structure proposed by the present invention. Among them, (a) is a stereoscopic view, (b) is a cross-sectional view of the central section perpendicular to the axial direction, and (c) is a cross-sectional view of the joint section parallel to the axial direction.
[0032] Figure 2 The SiC fiber reinforced metal matrix composite material pipe structure mold and assembly diagram proposed in the present invention have been shortened in length in the axial direction.
[0033] Figure 3 This is a schematic diagram of the outer sleeve of the SiC fiber reinforced metal matrix composite material tube structure mold proposed in the present invention, which has been shortened in length in the axial direction.
[0034] Figure 4 Schematic diagram of the left cover (a) and the right cover (b) of the SiC fiber reinforced metal matrix composite material tube structure mold proposed in the present invention.
[0035] Figure 5 This is a schematic diagram of the assembly process of the SiC fiber reinforced metal matrix composite material tube structure mold proposed in the present invention.
[0036] In the figure, 1 is the inner metal matrix, 2 is the composite material layer, 3 is the outer metal matrix, 4 is the SiC fiber, 5 is the inner lining of the tube structure mold, 6 is the outer sleeve of the tube structure mold, 6.1 is the equal-diameter inner bore surface of the outer sleeve, 6.2 is the left positioning groove of the outer sleeve, 6.3 is the right positioning groove of the outer sleeve, 7 is the left cover of the tube structure mold, 7.1 is the left cover positioning step, 7.2 is the contact surface between the left cover and the inner bore surface of the outer sleeve, 7.3 is the contact surface between the left cover and the precursor wire, 8 is the right cover of the tube structure mold, 8.1 is the right cover positioning step, 8.2 is the contact surface between the right cover and the inner bore surface of the outer sleeve, 8.3 is the contact surface between the right cover and the precursor wire, 9 is the center section, 10 is the joint section, and 11 is the composite material prefabricated belt. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0038] like Figure 1 As shown in FIG. 1 , the SiC fiber reinforced metal matrix composite tube structure is a tubular structure formed by coaxially compounding an inner metal matrix 1, a composite material layer 2, and an outer metal matrix 3 in sequence. Figure 1 As shown in (a), the outer shape of the tube structure is a cylinder of equal outer diameter, and a SiC fiber reinforced metal matrix composite material layer is provided in the tube wall; wherein, the outer shape of the metal matrix tube structure is a cylinder of equal outer diameter, and the tube wall thickness ranges from 4 to 8 mm, and the material includes but is not limited to aluminum alloy, titanium alloy or titanium aluminum alloy, etc.; in the composite material layer 2, SiC fibers 4 with metal coating deposited on the surface are arranged in the metal matrix tube wall as reinforcement. The tube structure is divided into a central section 9 and a joint section 10. The joint section 10 is the part where the two ends of the composite material layer 2 are connected to the tube structure. The central section 9 is the part of the SiC fiber reinforced metal matrix composite tube structure where the SiC fibers 4 are evenly arranged, and is not the joint section 10. The cross-sectional view of the central section 9 perpendicular to the axial direction is shown in FIG. Figure 1 As shown in (b), the SiC fiber reinforced metal matrix composite material layer 2 is arranged in the metal matrix tube wall composed of the inner metal matrix 1 and the outer metal matrix 3. The thickness of the composite material layer 2 ranges from 2 to 4 mm. The composite material layer 2 is equidistant from the inner and outer walls of the tube structure. No SiC fibers 4 are exposed above or below the tube structure. The axial direction of the SiC fibers 4 is consistent with the axial direction of the tube structure. The SiC fibers 4 are arranged in layers along the radial direction of the tube structure. The number of SiC fiber layers ranges from 4 to 8 layers. The SiC fibers between the layers are densely arranged in an interlaced manner, that is, the SiC fibers in the cross section of the tube structure are approximately hexagonally densely packed. The cross section of the joint segment 10 parallel to the axial direction is as follows: Figure 1As shown in (c), the two ends of the composite material layer 2 are arranged in a step-like manner at the joint of the pipe structure, and the length of each layer of SiC fiber 4 decreases from the inside to the outside layer by layer, and the single-side decreasing range of each layer is 0.5-2.5 mm, so that the angle α between the bottom edge connection line or the top edge connection line of the composite material layer 2 and the axial edge is in the range of 5-20°. The wall thickness of the pipe structure joint section 10 is greater than the wall thickness of the central section 9, and the thickness of the inner metal matrix 1 of the pipe structure joint section 10 is greater than the thickness of the inner metal matrix 1 of the central section 9, and the range is greater than 50-100% of the thickness of the inner metal matrix 1 of the central section 9. The end of the thickened part of the inner metal matrix 1 is flush with the end of the outermost layer of SiC fiber 4 of the composite material layer 2, and the different thickness areas of the inner metal matrix 1 are connected by chamfering.
[0039] SiC fiber is a continuous single-filament SiC fiber, which is prepared by chemical vapor deposition with tungsten wire or carbon fiber as the deposition substrate. The diameter of SiC fiber ranges from 50 to 160 μm, the tensile strength ranges from 3000 to 4000 MPa, and the density ranges from 2.80 to 3.50 g / cm 3 .
[0040] The method for preparing the SiC fiber reinforced metal matrix composite material tube structure comprises the following steps:
[0041] (1) Design and process composite material pipe structure molds: Figure 2 As shown, the composite material tube structure mold is composed of a tube structure mold liner 5, a tube structure mold outer sleeve 6, and two tube structure mold covers (tube structure mold left cover 7, tube structure mold right cover 8). The tube structure mold liner 5 is an equal diameter cylinder made of a metal matrix material, and the tube structure mold outer sleeve 6 is a cylinder made of a metal matrix material with a circular cross section. The tube structure mold liner 5 and the tube structure mold outer sleeve 6 are coaxially arranged inside and outside, and the tube structure mold left cover 7 and the tube structure mold right cover 8 are coaxially symmetrically arranged at both ends of the tube structure mold liner 5 and the tube structure mold outer sleeve 6. The four tube structure mold components can be assembled to be in close contact and size matching, and form a cavity for arranging composite materials.
[0042] like Figure 3 As shown, the outer sleeve 6 of the tube structure mold includes an outer sleeve equal-diameter inner bore surface 6.1 and outer sleeve positioning grooves (outer sleeve left positioning groove 6.2 and outer sleeve right positioning groove 6.3). The outer sleeve left positioning groove 6.2 and the outer sleeve right positioning groove 6.3 are coaxially arranged at the two ends of the outer sleeve equal-diameter inner bore surface 6.1.
[0043] like Figure 4 As shown, the pipe structure mold mouth cover is a stepped rotating body with diameters consistent with the diameters of the outer sleeve positioning groove and the diameter of the outer sleeve equal diameter inner bore surface 6.1, wherein:
[0044] The left cover 7 of the pipe structure mold is provided with a left cover positioning step 7.1, a contact surface 7.2 between the left cover and the inner bore surface of the outer sleeve, and a contact surface 7.3 between the left cover and the precursor wire. The outer diameter of the left cover positioning step 7.1 matches the diameter of the left positioning groove 6.2 of the outer sleeve. The outer diameter of the contact surface 7.2 between the left cover and the inner bore surface of the outer sleeve matches the diameter of the equal-diameter inner bore surface 6.1 of the outer sleeve. The contact surface 7.3 between the left cover and the precursor wire is a truncated cone-shaped surface corresponding to the inner side of the contact surface 7.2 between the left cover and the inner bore surface of the outer sleeve. The edge size of the contact surface 7.3 between the left cover and the precursor wire is consistent with the stepped arrangement size of the composite material layer 2 at the pipe structure joint.
[0045] The right mouth cover 8 of the tube structure mold is provided with a right mouth cover positioning step 8.1, a contact surface 8.2 between the right mouth cover and the inner bore surface of the outer sleeve, and a contact surface 8.3 between the right mouth cover and the pioneer wire. The outer diameter of the right mouth cover positioning step 8.1 matches the diameter of the right positioning groove 6.3 of the outer sleeve, the outer diameter of the contact surface 8.2 between the right mouth cover and the inner bore surface of the outer sleeve matches the diameter of the equal-diameter inner bore surface 6.1 of the outer sleeve, the contact surface 8.3 between the right mouth cover and the pioneer wire is a truncated cone-shaped surface corresponding to the inner side of the contact surface 8.2 between the right mouth cover and the inner bore surface of the outer sleeve, and the edge size of the contact surface 8.3 between the right mouth cover and the pioneer wire is consistent with the stepped arrangement size of the composite material layer 2 at the tube structure joint.
[0046] (2) preparing composite precursor fibers: depositing a metal coating on the surface of SiC fibers by physical vapor deposition to obtain composite precursor fibers, wherein the volume fraction of SiC fibers ranges from 40 to 80%;
[0047] (3) Preparing composite material prefabricated tape: Arranging composite material precursor wires and bonding them through organic glue (such as polyvinyl alcohol (PVA) or polymethyl methacrylate (PMMA) etc.) to form a single-layer composite material prefabricated tape, and cutting the prefabricated tape according to the size of the inner lining of the pipe structure mold and the stepped size of the composite material layer of the pipe structure joint section;
[0048] (4) Laying composite material prefabricated tapes: Then, the composite material prefabricated tapes 11 are stacked and pasted on the outer wall of the inner lining 5 of the pipe structure mold in order from long to short, and the left cover 7 of the pipe structure mold, the outer sleeve 6 of the pipe structure mold, and the right cover 8 of the pipe structure mold are assembled and fixed in order. The assembly sequence is shown in FIG. Figure 2 and Figure 5 ;
[0049] (5) Heat treatment of the composite material pipe structure mold: vacuum heat treatment is performed on the composite material pipe structure mold to remove the organic glue used in the process of preparing the composite material prefabricated tape, the temperature range is 200 to 400° C., and the heating time range is 60 to 120 min;
[0050] (6) Sealing the composite tube structure mold: using an electron beam vacuum welding process to seal the gap between the four tube structure mold components and the composite prefabricated belt;
[0051] (7) Composite material tube structure molding: The composite material tube structure mold after vacuum sealing is processed by hot isostatic pressing and other processes to completely close the gaps between the composite material precursor wires and the composite material preformed belts to form a dense SiC reinforced metal matrix composite material preform. The hot isostatic pressing temperature range is 400 to 1200 °C, the hot isostatic pressing pressure range is 25 to 300 MPa, and the hot isostatic pressing time range is 60 to 120 min.
[0052] (8) Composite material tube structure processing: Use turning and other mechanical processing methods to remove the excess metal matrix of the SiC reinforced metal matrix composite preform to obtain a SiC fiber reinforced metal matrix composite tube structure. Figure 1-Figure 2 As shown, the outer sheath 6 of the tube structure mold corresponds to the outer metal matrix 3 after processing, the inner lining 5 of the tube structure mold corresponds to the inner metal matrix 1 after processing, and the composite material prefabricated belt 11 corresponds to the composite material layer 2 after hot isostatic pressing.
[0053] The implementation results show that compared with metal matrix tube structures with the same appearance, the SiC fiber reinforced metal matrix composite tube structure of the present invention improves the bearing capacity of structural parts and reduces the weight of structural parts, and has great application prospects in lightweighting of high-performance aircraft.
[0054] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.
Claims
1. A SiC fiber reinforced metal matrix composite pipe structure, characterized in that: The SiC fiber reinforced metal matrix composite material tube structure is a tubular structure formed by coaxially compounding an inner metal matrix, a composite material layer, and an outer metal matrix in sequence. The outer shape of the tube structure is a cylinder of equal outer diameter. The SiC fiber reinforced metal matrix composite material layer is arranged in the metal matrix tube wall composed of the inner metal matrix and the outer metal matrix. In the composite material layer, SiC fibers with metal coatings deposited on the surface are arranged in the metal matrix tube wall as reinforcements, and the two ends of the composite material layer and the tube structure joint are arranged in a stepped manner. The tube structure is divided into a central section and a joint section. The joint section is the part where the two ends of the composite material layer are connected to the tube structure. The central section is the non-joint section part of the SiC fiber reinforced metal matrix composite material tube structure where SiC fibers are uniformly arranged. The wall thickness of the tube structure joint section is greater than the wall thickness of the central section.
2. The SiC fiber reinforced metal matrix composite material tube structure according to claim 1, characterized in that: SiC fiber is a continuous single-filament SiC fiber, which is prepared by chemical vapor deposition with tungsten wire or carbon fiber as the deposition substrate. The diameter of SiC fiber ranges from 50 to 160 μm, the tensile strength ranges from 3000 to 4000 MPa, and the density ranges from 2.80 to 3.50 g / cm 3 .
3. The SiC fiber reinforced metal matrix composite material tube structure according to claim 1, characterized in that: The thickness of the metal matrix tube wall ranges from 4 to 8 mm, and the metal matrix tube wall material is a light alloy such as aluminum alloy, titanium alloy or titanium aluminum alloy.
4. The SiC fiber reinforced metal matrix composite material pipe structure according to claim 1, characterized in that: The thickness of the composite material layer ranges from 2 to 4 mm, the composite material layer is equidistant from the inner and outer walls of the tube structure, no SiC fibers are exposed above and below the tube structure, the SiC fiber axial direction is consistent with the axial direction of the tube structure, the SiC fibers are arranged in layers along the radius of the tube structure, the number of SiC fiber layers ranges from 4 to 8 layers, and the SiC fibers between layers are densely arranged in an alternating manner, that is, the SiC fibers in the cross section of the tube structure are approximately hexagonally densely packed.
5. The SiC fiber reinforced metal matrix composite material tube structure according to claim 1, characterized in that: The length of each layer of SiC fiber decreases from inside to outside, and the single-side decreasing range of each layer is 0.5-2.5 mm, so that the angle α between the bottom edge connection line or the top edge connection line of the composite material layer and the axial edge is in the range of 5-20 degrees.
6. The SiC fiber reinforced metal matrix composite material pipe structure according to claim 1, characterized in that: The thickness of the inner metal matrix of the joint section of the pipe structure is greater than the thickness of the inner metal matrix of the central section, and is greater than 50% to 100% of the thickness of the inner metal matrix of the central section. The end of the thickened part of the inner metal matrix is flush with the end of the outermost SiC fiber of the composite material layer, and chamfers are used to connect different thickness areas of the inner metal matrix.
7. A method for preparing a SiC fiber reinforced metal matrix composite tube structure according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Designing and processing a composite material tube structure mold: The composite material tube structure mold consists of a tube structure mold liner, a tube structure mold outer sleeve, and two tube structure mold mouth covers. The tube structure mold liner is an equal-diameter cylinder made of a metal matrix material, and the tube structure mold outer sleeve is a cylinder made of a metal matrix material with a circular cross-section. The tube structure mold liner and the tube structure mold outer sleeve are coaxially arranged relative to each other. The tube structure mold mouth covers are respectively a left cover and a right cover of the tube structure mold. The left cover and the right cover of the tube structure mold are coaxially symmetrically arranged at the two ends of the tube structure mold liner and the tube structure mold outer sleeve; the four tube structure mold components are assembled in close contact and matched in size, and a cavity for arranging the composite material is formed; (2) preparing composite precursor fibers: depositing a metal coating on the surface of SiC fibers by physical vapor deposition to obtain composite precursor fibers, wherein the volume fraction of SiC fibers ranges from 40 to 80%; (3) preparing a composite material prefabricated tape: arranging composite material precursor wires and bonding them with organic adhesive to form a single-layer composite material prefabricated tape, and cutting the prefabricated tape according to the size of the inner lining of the pipe structure mold and the stepped size of the composite material layer of the pipe structure joint section; (4) Laying composite material prefabricated tapes: Then, the composite material prefabricated tapes are stacked and pasted on the outer wall of the inner lining of the pipe structure mold in order from long to short, and the left cover of the pipe structure mold, the outer sleeve of the pipe structure mold, and the right cover of the pipe structure mold are assembled and fixed in order; (5) Heat treatment of the composite material pipe structure mold: vacuum heat treatment is performed on the composite material pipe structure mold to remove the organic glue used in the process of preparing the composite material prefabricated tape, the temperature range is 200 to 400° C., and the heating time range is 60 to 120 min; (6) Sealing the composite tube structure mold: using an electron beam vacuum welding process to seal the gap between the four tube structure mold components and the composite prefabricated belt; (7) Composite tube structure molding: The vacuum-sealed composite tube structure mold is processed by hot isostatic pressing to completely close the gaps between the composite precursor wires and the composite preformed tapes to form a dense SiC reinforced metal matrix composite preform; (8) Composite material tube structure processing: The excess metal matrix of the SiC reinforced metal matrix composite preform is removed by mechanical processing to obtain a SiC fiber reinforced metal matrix composite tube structure.
8. The method for preparing a SiC fiber reinforced metal matrix composite material tube structure according to claim 7, characterized in that: The outer sleeve of the tube structure mold includes an outer sleeve equal-diameter inner bore surface and an outer sleeve positioning groove. The outer sleeve positioning grooves are respectively an outer sleeve left positioning groove and an outer sleeve right positioning groove. The outer sleeve left positioning groove and the outer sleeve right positioning groove are coaxially arranged at the two ends of the outer sleeve equal-diameter inner bore surface.
9. The method for preparing a SiC fiber reinforced metal matrix composite material tube structure according to claim 8, characterized in that: The pipe structure mold mouth cover is a stepped rotating body with diameters consistent with the outer sleeve positioning groove diameter and the outer sleeve equal diameter inner bore surface diameter, wherein: The left cover of the pipe structure mold is provided with a left cover positioning step, a contact surface between the left cover and the inner bore surface of the outer sleeve, and a contact surface between the left cover and the precursor wire. The outer diameter of the left cover positioning step matches the diameter of the left positioning groove of the outer sleeve. The outer diameter of the contact surface between the left cover and the inner bore surface of the outer sleeve matches the diameter of the equal-diameter inner bore surface of the outer sleeve. The contact surface between the left cover and the precursor wire is a truncated cone-shaped surface corresponding to the inner side of the contact surface between the left cover and the inner bore surface of the outer sleeve. The edge size of the contact surface between the left cover and the precursor wire is consistent with the stepped arrangement size of the composite material layer at the pipe structure joint. The right cover of the tube structure mold is provided with a right cover positioning step, a contact surface between the right cover and the inner bore surface of the outer sleeve, and a contact surface between the right cover and the pioneer wire. The outer diameter of the right cover positioning step matches the diameter of the right positioning groove of the outer sleeve, the outer diameter of the contact surface between the right cover and the inner bore surface of the outer sleeve matches the diameter of the equal-diameter inner bore surface of the outer sleeve, the contact surface between the right cover and the pioneer wire is a truncated cone-shaped surface corresponding to the inner side of the contact surface between the right cover and the inner bore surface of the outer sleeve, and the edge size of the contact surface between the right cover and the pioneer wire is consistent with the stepped arrangement size of the composite material layer at the tube structure joint.
10. The method for preparing a SiC fiber reinforced metal matrix composite material tube structure according to claim 7, characterized in that: In step (7), the hot isostatic pressing temperature ranges from 400 to 1200° C., the hot isostatic pressing pressure ranges from 25 to 300 MPa, and the hot isostatic pressing time ranges from 60 to 120 min.
Citation Information
Patent Citations
Engineered SIC-SIC composite and monolithic SIC layered structures
CN109564786A
Sleeving structure of SiC fiber reinforced metal matrix composite variable-diameter pipe shaft part and precursor wire laying method
CN115838905A
Sleeve structure for preparing fiber reinforced metal matrix composite pipe shaft part
CN218489153U
Fiber-reinforced plastic pipe with step and its manufacturing method
JP2009279769A
Lattice fin for missiles or other fluid-born bodies and method for producing same
US20030173459A1
Cited By
Optimization method and system for improving connection performance of continuous fiber reinforced metal matrix composite thin-walled pipe
CN122413872A
An optimization method and system for improving the connection performance of a continuous fiber reinforced metal matrix composite thin-walled pipe