PVC (polyvinyl chloride) waterproof coiled material

By using fluorine-containing resin and PVC refrigeration layer combined with high-efficiency hydrophobic particles in PVC waterproof membranes, the solar reflectivity and atmospheric window emissivity are improved, which solves the problem that ordinary waterproof membranes cannot effectively cool down and achieves a temperature control within the building. and energy consumption, while improving the weather resistance and self-cleaning properties of the material.

CN118744577AActive Publication Date: 2024-10-08NINGBO RADI COOL ADVANCED ENERGY TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410820940.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-08
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

Ordinary waterproof membranes cannot effectively reflect solar radiation, causing the temperature inside the building to rise and increasing air conditioning energy consumption.

Method used

It adopts PVC waterproof membrane composed of fluororesin refrigeration layer, PVC refrigeration layer and fiber layer. Both fluororesin refrigeration layer and PVC refrigeration layer contain efficient hydrophobic refrigeration particles to improve solar reflectivity and 8μm-13μm atmospheric window. Emissivity, combined with the fiber layer, improves the weather resistance and self-cleaning properties of the material.

Benefits of technology

Significantly lower the indoor temperature of the building, reduce the use of air conditioning, reduce energy consumption, and improve the weather resistance and self-cleaning properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744577A_ABST
    Figure CN118744577A_ABST
Patent Text Reader

Abstract

The invention relates to a PVC waterproof roll which comprises a fluorine-containing resin refrigeration layer, a PVC refrigeration layer, a fiber layer and a PVC layer which are sequentially arranged from top to bottom, the fluorine-containing resin refrigeration layer comprises, by weight, 20-60 parts of fluorine-containing resin and 5-20 parts of hydrophobic first refrigeration particles, and the sunlight reflectivity of the hydrophobic first refrigeration particles is larger than or equal to 85%; the 8-13 [mu] m atmosphere window emissivity is greater than or equal to 90%; the PVC refrigeration layer comprises 100 parts by weight of PVC resin, 20-60 parts by weight of a plasticizer, 1-2 parts by weight of a stabilizer, 0.2-0.5 part by weight of a mildew preventive, 5-8 parts by weight of a flame retardant, 5-10 parts by weight of a cold-resistant agent, 0.05-0.1 part by weight of an ultraviolet light absorber, 10-60 parts by weight of second refrigeration particles and 10-30 parts by weight of light calcium carbonate; the sunlight reflectivity of the second refrigeration particles is greater than or equal to 85%, and the 8-13 [mu] m atmosphere window emissivity is greater than or equal to 90%; the D90 particle size of the second refrigeration particles is 2-100 times of the D90 particle size of the hydrophobic first refrigeration particles. The PVC waterproof coiled material disclosed by the invention has excellent refrigeration effect, weather resistance and self-cleaning property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof coiled materials, in particular to a PVC waterproof coiled material. Background Art

[0002] Waterproof membranes are mainly used on the outer surface of building walls to provide waterproofing. However, ordinary waterproof membranes can only reflect a small amount of solar radiation, and most of the solar radiation will be absorbed by the building walls, causing the internal temperature of the building to rise and increasing air conditioning energy consumption. Summary of the invention

[0003] Based on this, it is necessary to provide a PVC waterproof membrane to address the above problems. The PVC waterproof membrane has excellent sunlight reflectivity and 8μm-13μm atmospheric window emissivity, can achieve excellent cooling effect, and has excellent weather resistance and self-cleaning properties.

[0004] A PVC waterproof coiled material, comprising a fluorine-containing resin refrigeration layer, a PVC refrigeration layer, a fiber layer and a PVC layer arranged in sequence from top to bottom, wherein the fluorine-containing resin refrigeration layer comprises 20 parts by weight to 60 parts by weight of fluorine-containing resin and 5 parts by weight to 20 parts by weight of hydrophobic first refrigeration particles, and the solar reflectivity of the hydrophobic first refrigeration particles is greater than or equal to 85%, and the 8μm-13μm atmospheric window emissivity is greater than or equal to 90%;

[0005] The PVC refrigeration layer comprises 100 parts by weight of PVC resin, 20 parts by weight to 60 parts by weight of plasticizer, 1 part by weight to 2 parts by weight of stabilizer, 0.2 parts by weight to 0.5 parts by weight of mildewproof agent, 5 parts by weight to 8 parts by weight of flame retardant, 5 parts by weight to 10 parts by weight of cold-resistant agent, 0.05 parts by weight to 0.1 parts by weight of ultraviolet absorber, 10 parts by weight to 60 parts by weight of second refrigeration particles and 10 parts by weight to 30 parts by weight of light calcium carbonate, and the solar reflectivity of the second refrigeration particles is greater than or equal to 85%, and the 8μm-13μm atmospheric window emissivity is greater than or equal to 90%;

[0006] The D90 particle size of the second refrigerant particles is 2 to 100 times the D90 particle size of the hydrophobic first refrigerant particles.

[0007] In one embodiment, the D90 particle size of the hydrophobic first refrigerant particles is 0.01 μm-5 μm;

[0008] And / or, the D90 particle size of the second refrigerant particles is 0.05 μm-20 μm.

[0009] In one embodiment, the D90 particle size of the hydrophobic first refrigerant particles is 0.02 μm-1 μm;

[0010] And / or, the D90 particle size of the second refrigerant particles is 0.1 μm-10 μm.

[0011] In one embodiment, the hydrophobic angle of the hydrophobic first refrigerant particles is greater than 150°;

[0012] And / or, the sliding angle of the hydrophobic first refrigerant particles is less than or equal to 6°.

[0013] In one embodiment, the thickness of the fluorine-containing resin refrigeration layer is 1 μm-100 μm;

[0014] And / or, the thickness of the PVC refrigeration layer is 20 μm-2000 μm;

[0015] And / or, the thickness of the fiber layer is 100 μm-2000 μm;

[0016] And / or, the thickness of the PVC layer is 100 μm-2000 μm.

[0017] In one embodiment, the fluorine-containing resin is selected from at least one of polyvinylidene fluoride resin, ethylene-tetrafluoroethylene copolymer or polytetrafluoroethylene resin;

[0018] And / or, the hydrophobic first refrigerant particles are selected from at least one of hydrophobic barium sulfate, hydrophobic titanium dioxide, hydrophobic silicon nitride, hydrophobic aluminum oxide, hydrophobic silicon oxide, hydrophobic calcium fluoride, hydrophobic magnesium phosphate or hydrophobic zinc oxide;

[0019] And / or, the second cooling particles are selected from at least one of barium sulfate, titanium dioxide, silicon nitride, aluminum oxide, silicon oxide, calcium fluoride, magnesium phosphate or zinc oxide.

[0020] In one of the embodiments, the surface of the fluorine-containing resin refrigeration layer facing away from the PVC refrigeration layer has a micron-scale and / or nano-scale concavo-convex structure.

[0021] In one embodiment, the fiber layer is selected from at least one of a polyester fiber layer and a glass fiber layer.

[0022] In one embodiment, the number of the PVC refrigeration layers is more than two, and the D90 particle size of the second refrigeration particles in each PVC refrigeration layer is different.

[0023] In one of the embodiments, a first adhesive layer is further included between the PVC refrigeration layer and the fiber layer;

[0024] And / or, a second adhesive layer is further included between the PVC layer and the fiber layer.

[0025] The present invention cooperates with a fluorine-containing resin refrigeration layer and a PVC refrigeration layer of a specific formula, so that the PVC waterproof membrane has excellent solar reflectivity and atmospheric window emissivity of 8μm-13μm wavelength, thereby having an excellent refrigeration effect. When the PVC waterproof membrane of the present invention is applied to the surface of a building or the like, the indoor temperature of the building can be effectively reduced.

[0026] In addition, the fluorine-containing resin refrigeration layer of the present invention has excellent weather resistance and self-cleaning ability, thereby making the PVC waterproof coiled material also have excellent weather resistance and self-cleaning ability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 It is a schematic structural diagram of the PVC waterproofing coiled material of the present invention, wherein 10, PVC layer; 20, fiber layer; 30, PVC refrigeration layer; 40, fluorine-containing resin refrigeration layer; 50, first adhesive layer; 60, second adhesive layer. DETAILED DESCRIPTION

[0029] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0031] like Figure 1 As shown, the PVC waterproof coiled material provided by the present invention includes a fluorine-containing resin refrigeration layer 40, a PVC refrigeration layer 30, a fiber layer 20 and a PVC layer 10 arranged in sequence from top to bottom.

[0032] Specifically, the fluorine-containing resin refrigeration layer 40 includes 20-60 parts by weight of fluorine-containing resin and 5-20 parts by weight of hydrophobic first refrigeration particles, and the solar reflectivity of the hydrophobic first refrigeration particles is greater than or equal to 85%, and the 8μm-13μm atmospheric window emissivity is greater than or equal to 90%; the PVC refrigeration layer 30 includes 100 parts by weight of PVC resin, 20-60 parts by weight of plasticizer, 1-2 parts by weight of stabilizer, 0.2-0.5 parts by weight of mildewproof agent, 5-8 parts by weight of flame retardant, 5-10 parts by weight of cold-resistant agent, 0.05-0.1 parts by weight of ultraviolet absorber, 10-60 parts by weight of second refrigeration particles and 10-30 parts by weight of light calcium carbonate, and the solar reflectivity of the second refrigeration particles is greater than or equal to 85%, and the 8μm-13μm atmospheric window emissivity is greater than or equal to 90%.

[0033] The D90 particle size of the second refrigerant particles is 2 to 100 times the D90 particle size of the hydrophobic first refrigerant particles.

[0034] The present invention can effectively improve the solar reflectivity and emissivity of the PVC waterproof membrane by cooperating with the fluorine-containing resin refrigeration layer 40 and the PVC refrigeration layer 30 of a specific formula, so that the solar reflectivity of the PVC waterproof membrane can be as high as 87% or more, and the atmospheric window emissivity of 8μm-13μm wavelength can reach more than 94%, with excellent cooling effect. When the PVC waterproof membrane of the present invention is applied to the surface of a building, it can not only effectively reduce the indoor temperature of the building and improve the living comfort, but also help to reduce the use of air conditioning, reduce CO2 emissions, and reduce energy consumption.

[0035] In addition, since the fluorine-containing resin refrigeration layer 40 has excellent weather resistance, and the hydrophobic first refrigeration particles contained in the fluorine-containing resin refrigeration layer 40 have excellent hydrophobicity, it can effectively improve the self-cleaning property of the PVC waterproof membrane. Therefore, the PVC waterproof membrane of the present invention also has excellent weather resistance and self-cleaning ability.

[0036] Preferably, the D90 particle size of the hydrophobic first cooling particles is 0.01μm-5μm, and more preferably 0.02μm-1μm; and / or, the D90 particle size of the second cooling particles is 0.05μm-20μm, and more preferably 0.1μm-10μm, so that by regulating the particle size, the fluorine-containing resin cooling layer 40 and the PVC cooling layer 30 can better cooperate to improve the reflectivity of sunlight and the emissivity of the atmospheric window, thereby improving the cooling effect of the PVC waterproof membrane.

[0037] Preferably, the hydrophobic angle of the hydrophobic first cooling particles is greater than 150°; and / or the rolling angle of the hydrophobic first cooling particles is less than or equal to 6°, so that the hydrophobic first cooling particles have excellent super hydrophobicity, which is beneficial to improving the self-cleaning property of the fluorine-containing resin cooling layer 40.

[0038] More preferably, the surface of the fluorine-containing resin refrigeration layer 40 facing away from the PVC refrigeration layer 30 has a micron-scale and / or nano-scale concavo-convex structure, which is beneficial to further improve the self-cleaning property of the PVC waterproof membrane.

[0039] Preferably, the thickness of the fluorine-containing resin refrigeration layer 40 is 1 μm-100 μm, more preferably 5 μm-20 μm, and / or the thickness of the PVC refrigeration layer 30 is 20 μm-2000 μm, more preferably 100 μm-800 μm, and / or the thickness of the fiber layer 20 is 100 μm-2000 μm, and / or the thickness of the PVC layer 10 is 100 μm-2000 μm, so that the coordination of the corresponding thicknesses of different layers is conducive to improving the solar reflectivity and the 8 μm-13 μm atmospheric window emissivity, thereby improving the refrigeration effect of the PVC waterproof membrane.

[0040] The fluorine-containing resin of the present invention is selected from at least one of polyvinylidene fluoride resin, ethylene-tetrafluoroethylene copolymer or polytetrafluoroethylene resin, and is more preferably polyvinylidene fluoride resin, which is beneficial to improving the weather resistance of the PVC waterproof membrane.

[0041] The hydrophobic first cooling particles of the present invention are selected from at least one of hydrophobic barium sulfate, hydrophobic titanium dioxide, hydrophobic silicon nitride, hydrophobic aluminum oxide, hydrophobic silicon oxide, hydrophobic calcium fluoride, hydrophobic magnesium phosphate or hydrophobic zinc oxide, and / or, the second cooling particles are selected from at least one of barium sulfate, titanium dioxide, silicon nitride, aluminum oxide, silicon oxide, calcium fluoride, magnesium phosphate or zinc oxide.

[0042] It is understood that the refrigerant particles may be subjected to a hydrophobic treatment to obtain the hydrophobic first refrigerant particles of the present invention.

[0043] In one embodiment, the number of the PVC refrigeration layer 30 of the present invention is preferably two or more layers, such as two layers, three layers, four layers, etc., and the D90 particle size of the second refrigeration particles in each layer of the PVC refrigeration layer 30 is different, thereby improving the refrigeration effect of the PVC waterproof membrane by combining the PVC refrigeration layer 30 containing the second refrigeration particles of different particle sizes.

[0044] The plasticizer, stabilizer, mildewproof agent, ultraviolet absorber, flame retardant and cold-resistant agent in the PVC refrigeration layer of the present invention are conventionally selected in the art, and the present invention does not impose specific restrictions on this. Preferably, the plasticizer is selected from at least one of phthalate resins, epoxy soybean oil, epoxy stearate, tricresyl phosphate (TCP), triphenyl phosphate (TPP), and diisooctyl phthalate (DPOP). The phthalate resin is preferably at least one of diisononyl phthalate (DINP), dioctyl phthalate (DOP), and diisodecyl phthalate (DIDP); the stabilizer is selected from a single stabilizer and / or a composite stabilizer, and the single stabilizer is selected from basic lead salts, gold The invention relates to a novel nanostructured carbon foam, wherein the nanostructured carbon foam comprises at least one of a soap, an organic tin, an epoxy compound, a phosphite, and a polyol; the composite stabilizer is selected from at least one of a barium zinc stabilizer, a calcium barium stabilizer, and a barium cadmium stabilizer; the mildew inhibitor is selected from at least one of pentachlorophenol, sodium pentachlorophenol, and salicylanilide; the ultraviolet absorber is selected from at least one of UV-531 and UV-990; the flame retardant is selected from at least one of magnesium hydroxide, aluminum hydroxide, antimony trioxide, and zinc hydroxystannate; the cold-resistant agent is selected from at least one of dioctyl sebacate (DOS) and rubber.

[0045] It is understandable that the fluorine-containing resin refrigeration layer 40 may also include the above-mentioned plasticizer, stabilizer, mildewproof agent, ultraviolet absorber, flame retardant, cold-resistant agent and other auxiliary agents.

[0046] Preferably, the fiber layer 20 is selected from at least one of a polyester fiber layer and a glass fiber layer, which is beneficial to improving the mechanical properties of the PVC waterproof membrane.

[0047] In one embodiment, the PVC waterproof roll material of the present invention further includes an adhesive layer. Specifically, a first adhesive layer 50 is included between the PVC refrigeration layer 30 and the fiber layer 20, and / or a second adhesive layer 60 is included between the PVC layer 10 and the fiber layer 20. Thus, the adhesive layer can effectively improve the adhesion between the layers, thereby improving the stability of the PVC waterproof roll material, so that it can more stably play the role of cooling and refrigeration.

[0048] It can be understood that the PVC waterproof membrane of the present invention is a layered structure, wherein the fluorine-containing resin refrigeration layer 40, the PVC refrigeration layer 30 and the PVC layer 10 can be formed into a film layer by coating or by calendering.

[0049] The preparation method of the PVC waterproof coiled material of the present invention preferably adopts the following steps:

[0050] S1, PVC resin, plasticizer, stabilizer, mildewproof agent, flame retardant, cold-resistant agent, ultraviolet absorber, second refrigeration particles and light calcium carbonate are mixed evenly and calendered to obtain a PVC refrigeration layer, and an adhesive is provided on any surface of the PVC refrigeration layer.

[0051] S2, dispersing the fluorine-containing resin and the hydrophobic first refrigeration particles in an organic solvent to obtain a fluorine-containing resin dispersion, and applying the fluorine-containing resin dispersion to a surface away from the PVC refrigeration layer binder to form a fluorine-containing resin refrigeration layer.

[0052] S3, calendering to obtain a PVC layer, and providing a fiber layer, setting an adhesive on any surface of the PVC layer, and respectively laminating the surface of the PVC layer provided with the adhesive and the surface of the PVC refrigeration layer provided with the adhesive to the upper and lower surfaces of the fiber layer, and obtaining the PVC waterproof coiled material after cooling and shaping.

[0053] In the step of dispersing the fluorine-containing resin and the hydrophobic first refrigerant particles in the organic solvent, the amount of the fluorine-containing resin is 20 parts by weight to 60 parts by weight, the amount of the hydrophobic first refrigerant particles is 5 parts by weight to 20 parts by weight, and the amount of the organic solvent is 30 parts by weight to 70 parts by weight.

[0054] Hereinafter, the PVC waterproof membrane will be further described through the following specific embodiments.

[0055] Example 1

[0056] Take 100 parts by weight of PVC resin, 20 parts by weight of plasticizer DINP, 2 parts by weight of stabilizer barium zinc 205, 0.2 parts by weight of mildewproofing agent pentachlorophenol, 6 parts by weight of flame retardant antimony trioxide, 8 parts by weight of cold-resistant agent DOS, 0.1 parts by weight of ultraviolet absorber UV-531, 30 parts by weight of aluminum oxide and 20 parts by weight of light calcium carbonate, wherein the D90 particle size of the aluminum oxide is 5 μm, the solar reflectivity is 92.5%, and the 8 μm-13 μm atmospheric window emissivity is 95%. After mixing the above raw materials in a high-speed mixer, put them into a screw extruder for plasticization and extrusion, and then calender them through a calender to obtain a PVC refrigeration layer with a thickness of 100 μm. Then print polyurethane glue on any surface of the PVC refrigeration layer.

[0057] 50 parts by weight of polyvinylidene fluoride resin, 10 parts by weight of hydrophobic alumina and 0.2 parts by weight of ultraviolet absorber UV-531 are dispersed in an organic solvent, dimethylformamide, and then coated on the surface of the PVC refrigeration layer away from the polyurethane glue to form a 10 μm fluorine-containing resin refrigeration layer, wherein the D90 particle size of the hydrophobic alumina is 0.5 μm, the solar reflectivity is 93.5%, the 8 μm-13 μm atmospheric window emissivity is 95%, the hydrophobic angle is 155°, and the rolling angle is 5°.

[0058] A 200-μm PVC layer and a 300-μm polyester fiber layer are provided, and polyurethane glue is printed on one surface of the PVC layer. Then, the surface of the PVC layer printed with the polyurethane glue and the surface of the PVC refrigeration layer printed with the polyurethane glue are hot-pressed and bonded to the upper and lower surfaces of the polyester fiber layer at 120° C., and then cooled and formed to obtain a PVC waterproof roll.

[0059] Example 2

[0060] Take 100 parts by weight of PVC resin, 20 parts by weight of plasticizer DINP, 2 parts by weight of stabilizer barium zinc 205, 0.2 parts by weight of mildewproof pentachlorophenol, 6 parts by weight of flame retardant antimony trioxide, 8 parts by weight of cold-resistant agent DOS, 0.1 parts by weight of ultraviolet absorber UV-531, 50 parts by weight of aluminum oxide and 10 parts by weight of light calcium carbonate, wherein the D90 particle size of aluminum oxide is 10 μm, the solar reflectivity is 91.2%, and the 8 μm-13 μm atmospheric window emissivity is 94%. After mixing the above raw materials in a high-speed mixer, put them into a screw extruder for plasticization and extrusion, and then calender them through a calender to obtain a PVC refrigeration layer with a thickness of 100 μm. Then print polyurethane glue on any surface of the PVC refrigeration layer.

[0061] 50 parts by weight of polyvinylidene fluoride resin, 20 parts by weight of hydrophobic alumina and 0.2 parts by weight of ultraviolet absorber UV531 are dispersed in an organic solvent, dimethylformamide, and then coated on the surface of the PVC refrigeration layer away from the polyurethane glue to form a 10 μm fluorine-containing resin refrigeration layer, wherein the D90 particle size of the hydrophobic alumina is 0.5 μm, the solar reflectivity is 93.5%, the 8 μm-13 μm atmospheric window emissivity is 95%, the hydrophobic angle is 160°, and the rolling angle is 3°.

[0062] A 200-μm PVC layer and a 300-μm polyester fiber layer are provided, and polyurethane glue is printed on one surface of the PVC layer. Then, the surface of the PVC layer printed with the polyurethane glue and the surface of the PVC refrigeration layer printed with the polyurethane glue are hot-pressed and bonded to the upper and lower surfaces of the polyester fiber layer at 120° C., and then cooled and formed to obtain a PVC waterproof roll.

[0063] Example 3

[0064] Take 100 parts by weight of PVC resin, 20 parts by weight of plasticizer DINP, 2 parts by weight of stabilizer barium zinc 205, 0.2 parts by weight of mildewproof pentachlorophenol, 6 parts by weight of flame retardant antimony trioxide, 8 parts by weight of cold-resistant agent DOS, 0.1 parts by weight of ultraviolet absorber UV531, 20 parts by weight of titanium oxide and 30 parts by weight of light calcium carbonate, wherein the D90 particle size of titanium oxide is 0.3 μm, the solar reflectivity is 95.1%, and the 8 μm-13 μm atmospheric window emissivity is 94%. After mixing the above raw materials in a high-speed mixer, put them into a screw extruder for plasticization and extrusion, and then calender them through a calender to obtain a PVC refrigeration layer with a thickness of 100 μm. Then print polyurethane glue on any surface of the PVC refrigeration layer.

[0065] 50 parts by weight of polyvinylidene fluoride resin, 10 parts by weight of hydrophobic alumina and 0.2 parts by weight of ultraviolet absorber UV-531 are dispersed in an organic solvent dimethylformamide, and then coated on the surface of the PVC refrigeration layer away from the polyurethane glue to form a 10 μm fluorine-containing resin refrigeration layer, wherein the surface of the fluorine-containing resin refrigeration layer has a micron-scale and / or nano-scale concave-convex structure, the D90 particle size of the hydrophobic alumina is 0.05 μm, the solar reflectivity is 92%, the 8 μm-13 μm atmospheric window emissivity is 95%, the hydrophobic angle is 153°, and the rolling angle is 6°.

[0066] A 200-μm PVC layer and a 300-μm polyester fiber layer are provided, and polyurethane glue is printed on one surface of the PVC layer. Then, the surface of the PVC layer printed with the polyurethane glue and the surface of the PVC refrigeration layer printed with the polyurethane glue are hot-pressed and bonded to the upper and lower surfaces of the polyester fiber layer at 120° C., and then cooled and formed to obtain a PVC waterproof roll.

[0067] Example 4

[0068] Take 100 parts by weight of PVC resin, 20 parts by weight of plasticizer DOP, 2 parts by weight of stabilizer barium zinc 205, 0.1 parts by weight of mildewproof pentachlorophenol, 6 parts by weight of flame retardant antimony trioxide, 8 parts by weight of cold-resistant agent DOS, 0.1 parts by weight of ultraviolet absorber UV531, 80 parts by weight of titanium oxide and 20 parts by weight of light calcium carbonate, wherein the D90 particle size of titanium oxide is 1 μm, the solar reflectivity is 93.5%, and the atmospheric window emissivity of 8 μm-13 μm is 95%. After the above raw materials are mixed by a high-speed mixer, they are put into a screw extruder for plasticization and extrusion, and then calendered by a calender to obtain a first PVC refrigeration layer with a thickness of 50 μm, and then a second PVC refrigeration layer is prepared by the same preparation method, wherein the D90 particle size of titanium oxide in the second PVC refrigeration layer is 0.3 μm, the solar reflectivity is 95.1%, and the atmospheric window emissivity of 8 μm-13 μm is 94%. Then, polyurethane glue is printed on any surface of the first PVC refrigeration layer and both surfaces of the second PVC refrigeration layer, and the first PVC refrigeration layer and the second PVC refrigeration layer are hot-pressed and laminated.

[0069] 50 parts by weight of polyvinylidene fluoride resin, 10 parts by weight of hydrophobic silica and 0.2 parts by weight of ultraviolet absorber are dispersed in an organic solvent of dimethylformamide, and then coated on the surface of the PVC refrigeration layer away from the polyurethane glue to form a 10 μm fluorine-containing resin refrigeration layer, wherein the surface of the fluorine-containing resin refrigeration layer has a micron-scale and / or nano-scale concave-convex structure, the D90 particle size of the hydrophobic aluminum oxide is 0.025 μm, the solar reflectivity is 92%, the 8 μm-13 μm atmospheric window emissivity is 95%, the hydrophobic angle is 154°, and the rolling angle is 4.5°.

[0070] A 200 μm PVC layer and a 300 μm polyester fiber layer are provided, and polyurethane glue is printed on one surface of the PVC layer. Then, the surface of the PVC layer printed with the polyurethane glue and the surface of the second PVC cooling layer printed with the polyurethane glue are hot-pressed and bonded to the upper and lower surfaces of the polyester fiber layer at 120° C., and then cooled and formed to obtain a PVC waterproof roll.

[0071] Comparative Example 1

[0072] The difference between Comparative Example 1 and Example 1 is that no fluorine-containing resin refrigeration layer is provided.

[0073] Comparative Example 2

[0074] The difference between Comparative Example 2 and Example 1 is that no PVC refrigeration layer is provided.

[0075] Comparative Example 3

[0076] The difference between Comparative Example 3 and Example 1 is that the D90 particle size of the hydrophobic alumina in the fluorine-containing resin refrigeration layer is 0.02 μm, and the D90 particle size of the alumina in the PVC refrigeration layer is 3 μm, that is, the particle size of the alumina is 150 times that of the hydrophobic alumina.

[0077] Comparative Example 4

[0078] The difference between Comparative Example 4 and Example 1 is that the D90 particle size of the hydrophobic alumina in the fluorine-containing resin refrigeration layer is 2 μm, and the D90 particle size of the alumina in the PVC refrigeration layer is 2 μm, that is, the particle size of the alumina is 1 times the particle size of the hydrophobic alumina.

[0079] Comparative Example 5

[0080] The difference between Comparative Example 5 and Example 1 is that the hydrophobic first cooling particles are ceramic microbeads, whose solar reflectivity is 81% and whose 8μm-13μm atmospheric window emissivity is 93%; the second cooling particles are mica powder, whose solar reflectivity is 78% and whose 8μm-13μm atmospheric window emissivity is 85%.

[0081] The reflectivity, atmospheric window emissivity, weather resistance and self-cleaning property of the PVC waterproof membranes in the above-mentioned embodiments and comparative examples were tested, and the results are shown in Table 1.

[0082] Reflectivity test method: Tested in accordance with GB / T2680-2021 method.

[0083] Atmospheric window emissivity test method: Test in accordance with T / ZZB 2304-2021 method.

[0084] Weather resistance test method: Test according to cycle number 1 conditions in Table 3 of GB / T1622.2-2022.

[0085] Self-cleaning test method: PVC waterproofing membrane is polluted by common pollution sources such as coal slag, waste oil, cooking oil, tea stains, red wine, etc. The pollution source stays on the surface of the PVC waterproofing membrane for 2 hours, and then wiped with a dust-free cloth soaked in water, and the surface pollution source is observed to remove the pollution source, and the pollution resistance level is obtained. Among them, the higher the level of 1-5, the better the pollution resistance, level 1 represents severe, level 2 represents medium, level 3 represents slight, level 4 represents very slight, and level 5 represents no pollution.

[0086] Table 1

[0087]

[0088]

[0089] From Examples 1-4 and Comparative Examples 1-5 in Table 1, it can be seen that the reflectivity and atmospheric window emissivity of the PVC waterproofing membranes of Examples 1-4 are both high, so that they can effectively reflect sunlight and effectively transfer heat to outer space in the form of infrared radiation in the atmospheric window band, indicating that the PVC waterproofing membrane of the present invention has an excellent cooling effect and can significantly reduce the indoor temperature of the building. In addition, the PVC waterproofing membranes of Examples 1-4 also have excellent weather resistance and self-cleaning properties.

[0090] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0091] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A PVC waterproof coiled material, characterized in that: The invention comprises a fluorine-containing resin refrigeration layer, a PVC refrigeration layer, a fiber layer and a PVC layer which are sequentially arranged from top to bottom, wherein the fluorine-containing resin refrigeration layer comprises 20 parts by weight to 60 parts by weight of fluorine-containing resin and 5 parts by weight to 20 parts by weight of hydrophobic first refrigeration particles, and the solar reflectivity of the hydrophobic first refrigeration particles is greater than or equal to 85%, and the 8μm-13μm atmospheric window emissivity is greater than or equal to 90%; The PVC refrigeration layer includes 100 parts by weight of PVC resin, 20 parts by weight to 60 parts by weight of plasticizer, 1 part by weight to 2 parts by weight of stabilizer, 0.2 parts by weight to 0.5 parts by weight of mildewproofing agent, 5 parts by weight to 8 parts by weight of flame retardant, 5 parts by weight to 10 parts by weight of cold-resistant agent, 0.05 parts by weight to 0.1 parts by weight of ultraviolet absorber, 10 parts by weight to 60 parts by weight of second refrigeration particles and 10 parts by weight to 30 parts by weight of light calcium carbonate, and the solar reflectivity of the second refrigeration particles is greater than or equal to 85%, and the 8μm-13μm atmospheric window emissivity is greater than or equal to 90%; wherein the D90 particle size of the second refrigeration particles is 2 times to 100 times the D90 particle size of the hydrophobic first refrigeration particles.

2. The PVC waterproofing membrane according to claim 1, characterized in that: The D90 particle size of the hydrophobic first refrigerant particles is 0.01 μm-5 μm; And / or, the D90 particle size of the second refrigerant particles is 0.05 μm-20 μm.

3. The PVC waterproofing membrane according to claim 2, characterized in that: The D90 particle size of the hydrophobic first refrigerant particles is 0.02 μm-1 μm; And / or, the D90 particle size of the second refrigerant particles is 0.1 μm-10 μm.

4. The PVC waterproofing membrane according to claim 1, characterized in that: The hydrophobic angle of the hydrophobic first refrigerant particles is greater than 150°; And / or, the sliding angle of the hydrophobic first refrigerant particles is less than or equal to 6°.

5. The PVC waterproofing membrane according to claim 1, characterized in that: The thickness of the fluorine-containing resin refrigeration layer is 1 μm-100 μm; And / or, the thickness of the PVC refrigeration layer is 20 μm-2000 μm; And / or, the thickness of the fiber layer is 100 μm-2000 μm; And / or, the thickness of the PVC layer is 100 μm-2000 μm.

6. The PVC waterproofing membrane according to claim 1, characterized in that: The fluorine-containing resin is selected from at least one of polyvinylidene fluoride resin, ethylene-tetrafluoroethylene copolymer or polytetrafluoroethylene resin; And / or, the hydrophobic first refrigerant particles are selected from at least one of hydrophobic barium sulfate, hydrophobic titanium dioxide, hydrophobic silicon nitride, hydrophobic aluminum oxide, hydrophobic silicon oxide, hydrophobic calcium fluoride, hydrophobic magnesium phosphate or hydrophobic zinc oxide; And / or, the second cooling particles are selected from at least one of barium sulfate, titanium dioxide, silicon nitride, aluminum oxide, silicon oxide, calcium fluoride, magnesium phosphate or zinc oxide.

7. The PVC waterproofing membrane according to claim 1, characterized in that: The surface of the fluorine-containing resin refrigeration layer away from the PVC refrigeration layer has a micron-scale and / or nano-scale concavo-convex structure.

8. The PVC waterproofing membrane according to claim 1, characterized in that: The fiber layer is selected from at least one of a polyester fiber layer and a glass fiber layer.

9. The PVC waterproofing membrane according to any one of claims 1 to 8, characterized in that: The number of the PVC refrigeration layers is more than two, and the D90 particle size of the second refrigeration particles in each PVC refrigeration layer is different.

10. The PVC waterproofing membrane according to any one of claims 1 to 8, characterized in that: A first adhesive layer is also included between the PVC refrigeration layer and the fiber layer; And / or, a second adhesive layer is further included between the PVC layer and the fiber layer.

Citation Information

Patent Citations

  • Radiation cooling film and preparation method thereof

    CN110128688A

  • Refrigeration coating and application thereof

    CN113354989A

  • Impervious covering, processes for the joining or fixing thereof and apparatus employing such processes

    EP0314548A2

  • Radiative cooling functional coating material and application thereof

    IN202024018781A

  • Radiative cooling fabrics and products

    US20230158786A1