Preparation method of hundred-micron self-doped spherical porous carbon material

By carbonizing hundreds of micron-sized spherical chitosan to prepare self-doped spherical porous carbon materials, the problems of complicated doping process, high reagent consumption and high energy consumption in the existing technology are solved, and materials with high strength and high specific surface area are realized. Preparation, suitable for many field applications.

CN118744988AActive Publication Date: 2024-10-08NANKAI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410732617.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-08
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

The existing spherical porous carbon doping process is complex, consumes a lot of reagents, and consumes a lot of energy, resulting in poor material strength and is only suitable for fields with low strength requirements.

Method used

Hundred-micron-level spherical chitosan is used as the precursor, and hundreds-micron-level self-doped spherical porous carbon materials are prepared through carbonization. Chitosan itself is used to provide N source to avoid additional template agents and activators. Suspension polymerization processing method is used to optimize Carbonization process to increase specific surface area and N content.

Benefits of technology

A hundred-micron level self-doped spherical porous carbon material with high specific surface area and high strength is prepared, which is suitable for a wider range of application fields, reduces energy consumption and waste generation, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744988A_ABST
    Figure CN118744988A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a hundred-micron self-doped spherical porous carbon material, and relates to the technical field of carbon materials. According to the preparation method disclosed by the invention, the hundred-micron-grade spherical chitosan is used as a precursor, and the hundred-micron-grade self-doped spherical porous carbon material is obtained through carbonization, so that the prepared hundred-micron-grade self-doped spherical porous carbon material has the advantages of high specific surface area, high strength and large size; meanwhile, the problems of complex doping process, high reagent consumption, high energy consumption and the like of the existing spherical porous carbon are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon materials, and in particular to a method for preparing a hundred-micron-level self-doped spherical porous carbon material. Background Art

[0002] Chitosan, as a nitrogen-containing polysaccharide of natural origin, is a widely distributed renewable resource and can be used to prepare N-doped porous carbon by in-situ method. The difficulty limiting its application is the lack of effective processing methods. Therefore, exploring simple, fast, environmentally friendly and low-cost processing methods is more conducive to the development and large-scale application of materials (MONTEMBAULTA, et al. (2005). Rheometric study of the gelation of chitosan in aqueous solution without cross-linking agent. Biomacromolecules.). The traditional processing method is to use natural polysaccharide powder as a carbon source, directly carbonize it to obtain activated carbon powder, and then mix it with additives such as adhesives to granulate. However, the material prepared in this way has poor strength and can only be used in fields with low strength requirements such as water treatment (Lan, J., et al. (2023). Progress on fabrication and application of activated carbon sphere in recent decade. Journal of Industrial and Engineering Chemistry.). Summary of the invention

[0003] In view of this, the purpose of the present invention is to provide a method for preparing a hundred-micron-level self-doped spherical porous carbon material. The present invention uses hundred-micron-level spherical chitosan as a precursor and obtains a hundred-micron-level self-doped spherical porous carbon material through carbonization. The hundred-micron-level self-doped spherical porous carbon material prepared by the present invention has the advantages of high specific surface area, high strength and large size, and at the same time solves the problems of complex doping process of existing spherical porous carbon, high reagent consumption and high energy consumption.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing a 100-micron-level self-doped spherical porous carbon material, comprising the following steps:

[0006] The hundred-micrometer-scale spherical chitosan precursor is carbonized to obtain a hundred-micrometer-scale self-doped spherical porous carbon material.

[0007] Preferably, the method for preparing the hundred-micrometer-scale spherical chitosan precursor comprises:

[0008] Dissolving chitosan in an acetic acid aqueous solution to obtain a dispersed phase; mixing butyl acetate and span 80 to obtain a continuous phase;

[0009] The dispersed phase and the continuous phase are mixed and suspended to obtain droplets of 100 micrometers; NaOH solution is added to perform precipitation reaction to obtain a spherical chitosan precursor of 100 micrometers.

[0010] Preferably, the deacetylation degree of the chitosan is 75-95%.

[0011] Preferably, the suspension dispersion is carried out under stirring conditions; the stirring speed is 100-500 r / min; and the suspension dispersion temperature is 10-40°C.

[0012] Preferably, the particle size of the 100-micrometer-level spherical chitosan precursor is 400-600 μm; the crystallinity of the 100-micrometer-level spherical chitosan precursor is 37-52%, and the average crystal size is

[0013] Preferably, the carbonization conditions include: first heating to 200-500° C. under a protective atmosphere, and performing a first heat preservation for 1-5 hours; second heating to 600-1000° C., and performing a second heat preservation for 2-5 hours; and naturally cooling to room temperature.

[0014] Preferably, the heating rate of the first heating is 3-10°C / min; the heating rate of the second heating is 3-10°C / min.

[0015] Preferably, the particle size of the 100-micrometer self-doped spherical porous carbon material is 100-600 μm; the specific surface area is 269-2100 m 2 / g; the average pore size is 2-4nm; the micropore size is 0.6-0.8nm.

[0016] Preferably, the N content of the hundred-micrometer-scale self-doped spherical porous carbon material is 1 to 4 at %.

[0017] Preferably, the single particle crushing strength of the hundred-micrometer-level self-doped spherical porous carbon material is 1.78-3.13N.

[0018] The present invention provides a method for preparing a 100-micron self-doped spherical porous carbon material, comprising the following steps: carbonizing a 100-micron spherical chitosan precursor to obtain a 100-micron self-doped spherical porous carbon material. The present invention uses 100-micron spherical chitosan as a precursor, does not use an additional template agent and an activator, uses chitosan itself to provide a nitrogen source, and obtains a 100-micron self-doped spherical porous carbon material through carbonization. The results of the embodiment show that the 100-micron self-doped spherical porous carbon material prepared by the present invention contains 1 to 4 at% of nitrogen elements. Figure 3 The results show that it contains pyridine N, graphite N, and oxide N. The appearance of the 100-micron self-doped spherical porous carbon material is black with a metallic luster, the single particle crushing strength is 1.78-3.13N, and the specific surface area is 269-2100m 2 / g, the average pore size is 2-4nm; the micropore size is 0.6-0.8nm, and the particle size is 100-600μm.

[0019] As a preferred solution, the present invention uses suspension polymerization processing to prepare a large amount of 100-micron-sized, highly cross-linked 100-micron-level spherical chitosan precursors, thereby improving the utilization efficiency of reagents, avoiding the use of more reagents, especially toxic reagents, and making the precursor preparation process more environmentally friendly.

[0020] As a preferred solution, for the carbonization process, the present invention makes corresponding adjustments and optimizations according to the properties of the precursor to achieve the preparation of spherical porous carbon materials with high specific surface area and N content, reduce the energy consumption of the carbonization process, reduce the generation of waste, and be more suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is an optical microscope photo of the hundred-micrometer-scale self-doped spherical porous carbon material C-1 prepared in Example 1;

[0022] Figure 2 This is a SEM image of the hundred-micrometer-scale self-doped spherical porous carbon material C-1 prepared in Example 1;

[0023] Figure 3 This is the XPS spectrum of the N1s orbital of the 100-micrometer self-doped spherical porous carbon material C-1 prepared in Example 1;

[0024] Figure 4 The XRD spectrum of the 100-micrometer self-doped spherical porous carbon material C-1 prepared in Example 1;

[0025] Figure 5 The pore distribution curve of the 100-micrometer self-doped spherical porous carbon material C-1 prepared in Example 1;

[0026] Figure 6The N of the 100-micrometer self-doped spherical porous carbon material C-1 prepared in Example 1 2 Adsorption-desorption curve;

[0027] Figure 7 This is the XRD spectrum of the hundred-micrometer-scale spherical chitosan precursor SC-1 prepared in Example 1. DETAILED DESCRIPTION

[0028] The present invention provides a method for preparing a 100-micron-level self-doped spherical porous carbon material, comprising the following steps:

[0029] The hundred-micrometer-scale spherical chitosan precursor is carbonized to obtain a hundred-micrometer-scale self-doped spherical porous carbon material.

[0030] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.

[0031] In the present invention, the method for preparing the hundred-micrometer-scale spherical chitosan precursor preferably comprises:

[0032] Dissolving chitosan in an acetic acid aqueous solution to obtain a dispersed phase; mixing butyl acetate and span 80 to obtain a continuous phase;

[0033] The dispersed phase and the continuous phase are mixed and suspended to obtain droplets of 100 micrometers; NaOH solution is added to perform precipitation reaction to obtain a spherical chitosan precursor of 100 micrometers.

[0034] The present invention preferably dissolves chitosan in an acetic acid aqueous solution to obtain a dispersed phase. In the present invention, the deacetylation degree of the chitosan is preferably 75-95%, more preferably 85-90%. In the present invention, the concentration of acetic acid in the dispersed phase is preferably 1-6wt%, more preferably 3-4wt%; the concentration of chitosan in the dispersed phase is preferably 3-6wt%, more preferably 4-5wt%.

[0035] In the present invention, butyl acetate and span 80 are mixed to obtain a continuous phase. In the present invention, the volume ratio of butyl acetate to span 80 is preferably 1:0.005-0.1, more preferably 1:0.02-0.05.

[0036] After obtaining the dispersed phase and the continuous phase, the present invention preferably mixes the dispersed phase and the continuous phase, performs suspension dispersion, and obtains 100-micrometer droplets; adds NaOH solution, performs precipitation reaction, and obtains 100-micrometer spherical chitosan precursor. In the present invention, the volume ratio of the dispersed phase and the continuous phase is preferably 1:2-4, more preferably 1:3-3.5. In the present invention, the mixing of the dispersed phase and the continuous phase preferably includes adding the dispersed phase to the continuous phase.

[0037] In the present invention, the suspension dispersion is preferably carried out under stirring conditions; the stirring speed is preferably 100-500 r / min, more preferably 250-300 r / min; the suspension dispersion temperature is preferably 10-40°C, more preferably 25-30°C.

[0038] In the present invention, the particle size of the 100-micron droplets is preferably 400-600 μm. In the present invention, the concentration of the NaOH solution is preferably 20-50 wt%, more preferably 40-50 wt%; the amount ratio of the NaOH solution to chitosan is preferably 4-50 mL:5 g, more preferably 8-20 mL:5 g. In the present invention, the beads are gradually transformed from transparent viscous droplets to turbid gel beads by adding NaOH solution.

[0039] In the present invention, the precipitation reaction time is preferably 1 to 10 hours, more preferably 4 to 8 hours; the precipitation reaction temperature is preferably 10 to 40°C, more preferably 20 to 30°C. The present invention uses precipitation reaction to make the beads have a certain strength, and will not cause obvious changes in shape under mild extrusion. The present invention uses precipitation reaction to slow down the speed of molecular chain stacking, and obtains spherical chitosan with high crystallinity and uniform crystal area distribution.

[0040] In the present invention, after the precipitation reaction, the obtained spherical chitosan is preferably washed to obtain a 100-micron-level spherical chitosan precursor. In the present invention, the washing is preferably water washing, more preferably deionized water immersion washing. In the present invention, the filtrate is preferably washed until it is neutral.

[0041] In the present invention, the particle size of the 100-micrometer-level spherical chitosan precursor is 400-600 μm. In the present invention, the crystallinity of the 100-micrometer-level spherical chitosan precursor is preferably 37-52%, and the average crystal size is preferably The 100-micron-scale spherical chitosan precursor prepared by the present invention has a uniform structure, a 100-micron-scale particle size and high cross-linking. The present invention controls the crystallization of the 100-micron-scale spherical chitosan precursor to obtain N-doped spherical carbon with a high specific surface area after carbonization. In the present invention, the precursor with high crystallinity and small crystal area size has a complete spherical shape, large particle size and high strength after carbonization.

[0042] After obtaining the 100-micron spherical chitosan precursor, the present invention carbonizes the 100-micron spherical chitosan precursor to obtain a 100-micron self-doped spherical porous carbon material. In the present invention, the carbonization conditions preferably include: first heating to 200-500°C under a protective atmosphere, and a first insulation for 1-5h; second heating to 600-1000°C, and a second insulation for 2-5h; naturally cooling to room temperature. In the present invention, the carbonization conditions more preferably include: first heating to 410-450°C under a protective atmosphere, and a first insulation for 2-4h; second heating to 660-900°C, and a second insulation for 2-3h; naturally cooling to room temperature. In the present invention, the heating rate of the first heating is preferably 3-10°C / min, more preferably 6-8°C / min; the heating rate of the second heating is preferably 3-10°C / min, more preferably 6-8°C / min. In the present invention, the carbonization is preferably carried out in a quartz boat in a tube furnace. In the present invention, the first heat preservation, the second heat preservation and the natural cooling are preferably all carried out under a protective atmosphere. In the present invention, the protective atmosphere is preferably a nitrogen atmosphere. The present invention adopts the above carbonization conditions, which is conducive to increasing the specific surface area of ​​the carbon material.

[0043] In the present invention, the particle size of the 100-micrometer self-doped spherical porous carbon material is preferably 100-600 μm, more preferably 300-400 μm; the specific surface area is preferably 269-2100 m 2 / g, more preferably 1000 to 1772 m 2 / g; the micropore diameter is preferably 0.6-0.8nm; the average pore diameter is preferably 2-4nm; the N content of the 100-micron self-doped spherical porous carbon material is preferably 1-4at%, more preferably 1.90-2.56at%; the single particle crushing strength of the 100-micron self-doped spherical porous carbon material is preferably 1.78-3.13N, more preferably 2.52-3.12N. In the present invention, the appearance of the 100-micron self-doped spherical porous carbon material is a black sphere with a metallic luster.

[0044] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] Example 1

[0046] Take 5g of chitosan powder with a deacetylation degree of 75%, add 120mL of 4wt% acetic acid aqueous solution to fully dissolve it as the dispersed phase in the suspension polymerization; transfer it to 480mL of continuous phase, which is a butyl acetate solution containing 5wt% span 80. Use overhead stirring, and obtain spherical droplets under the action of shear force (speed of 250r / min, temperature of 25°C). After the droplet size is uniform and stable at 400-600μm, add 12mL of 50wt% NaOH solution, and the beads gradually change from transparent viscous droplets to turbid gel beads. After the reaction is carried out for 4h, the chitosan beads have a certain strength, and will not cause obvious changes in shape under mild extrusion, and stop stirring. Then soak and wash the spherical chitosan with a large amount of deionized water, wash to neutrality, and obtain a 100-micron spherical chitosan precursor SC-1.

[0047] The 100-micron-sized spherical chitosan precursor SC-1 prepared above was transferred to a quartz boat, which was placed in a tube furnace and heated at N 2 Under the protection of the atmosphere, the temperature was raised to 410°C at a rate of 6°C / min, maintained at this temperature for 2 h, and then raised to 900°C at a rate of 6°C / min, and maintained at this temperature for 2 h; maintained under N 2 The mixture was naturally cooled to room temperature under an atmosphere, and then taken out to obtain a hundred-micron-scale self-doped spherical porous carbon material C-1.

[0048] Figure 1 This is an optical microscope photo of the 100-micrometer self-doped spherical porous carbon material C-1 prepared in Example 1, and the appearance and particle size of the spherical carbon can be observed; Figure 2 This is a SEM image of the 100-micrometer self-doped spherical porous carbon material C-1 prepared in Example 1, from which the appearance, particle size and surface structure of the spherical carbon can be observed; Figure 3 The XPS spectrum of the N1s orbital of the 100-micrometer self-doped spherical porous carbon material C-1 prepared in Example 1, from which the N element content of the spherical carbon and the chemical state of the N element can be obtained, including pyridinic N, graphitic N, and oxidized N; Figure 4 This is the XRD spectrum of the 100-micrometer self-doped spherical porous carbon material C-1 prepared in Example 1, and it can be seen that the crystal structure of the spherical carbon is composed of a graphite phase; Figure 5 The pore distribution curve of the 100-micron self-doped spherical porous carbon material C-1 prepared in Example 1 can be used to obtain the pore size distribution of the spherical carbon; Figure 6 The N of the 100-micrometer self-doped spherical porous carbon material C-1 prepared in Example 1 2 The adsorption-desorption curve can be used to obtain the specific surface area of ​​spherical carbon; Figure 7 This is the XRD spectrum of the 100-micrometer-scale spherical chitosan precursor SC-1 prepared in Example 1, and the crystal structure information of the precursor can be obtained.

[0049] The 100-micrometer-level spherical chitosan precursor SC-1 obtained in this example has a crystallinity of 45% and an average crystal size of

[0050] The 100-micron self-doped spherical porous carbon material C-1 obtained in this example has a black metallic spherical appearance, a particle size of 300-500 μm, a nitrogen content of 2.27 at%, a single particle crushing strength of 3.12 N, and a specific surface area of ​​1439 m 2 / g, and the micropore diameter is 0.8nm.

[0051] Example 2

[0052] Take 5g of chitosan powder with a deacetylation degree of 95%, add 120mL of 4wt% acetic acid aqueous solution to fully dissolve it as the dispersed phase in the suspension polymerization; transfer it to 480mL of continuous phase, which is a butyl acetate solution containing 5wt% span80. Use overhead stirring, and obtain spherical droplets under the action of shear force (speed of 250r / min, temperature of 25°C). After the droplet size is uniform and stable at 400-600μm, add 12mL of 50wt% NaOH solution, and the beads gradually change from transparent viscous droplets to turbid gel beads. After the reaction is carried out for 4h, the chitosan beads have a certain strength, and will not cause obvious changes in shape under mild extrusion, and stop stirring. Soak and wash the spherical chitosan with a large amount of deionized water, wash to neutrality, and obtain a 100-micron spherical chitosan precursor SC-2.

[0053] The 100-micron-sized spherical chitosan precursor SC-2 prepared above was transferred to a quartz boat, which was placed in a tube furnace and heated at N 2 Under the protection of the atmosphere, the temperature was raised to 410°C at a rate of 6°C / min, maintained at this temperature for 2 h, and then raised to 900°C at a rate of 6°C / min, and maintained at this temperature for 2 h; maintained under N 2 The mixture was naturally cooled to room temperature under an atmosphere, and then taken out to obtain a self-doped spherical porous carbon material C-2 of 100 micrometers.

[0054] The 100-micrometer-level spherical chitosan precursor SC-2 obtained in this example has a crystallinity of 52% and an average crystal size of

[0055] The 100-micron self-doped spherical porous carbon material C-2 obtained in this example has the appearance of black flaky particles with metallic luster, a particle size of 200-400 μm, a nitrogen content of 2.56 at%, a single particle crushing strength of 3.01 N, and a specific surface area of ​​2076 m 2 / g, and the micropore diameter is 0.6nm.

[0056] Example 3

[0057] The 100-micron-scale spherical chitosan precursor SC-1 prepared in Example 1 was transferred to a quartz boat, which was placed in a tube furnace and heated at N 2 Under the protection of the atmosphere, the temperature was raised to 410°C at a rate of 6°C / min, maintained at this temperature for 2 h, and then raised to 660°C at a rate of 6°C / min, and maintained at this temperature for 3 h; maintained under N 2 The mixture was naturally cooled to room temperature under an atmosphere, and then taken out to obtain a self-doped spherical porous carbon material C-3 of 100 micrometers.

[0058] The 100-micron self-doped spherical porous carbon material C-3 obtained in this example has a black metallic spherical appearance, a particle size of preferably 300-500 μm, a nitrogen content of 1.90 at%, a single particle crushing strength of 3.07 N, and a specific surface area of ​​269 m 2 / g, and the micropore diameter is 0.8nm.

[0059] Example 4

[0060] The 100-micron-scale spherical chitosan precursor SC-1 prepared in Example 1 was transferred to a quartz boat, which was placed in a tube furnace and heated at N 2 Under the protection of the atmosphere, the temperature was raised to 410°C at a heating rate of 6°C / min, maintained at this temperature for 2 h, and then raised to 900°C at a heating rate of 8°C / min, and maintained at this temperature for 3 h; maintained under N 2 The mixture was naturally cooled to room temperature under an atmosphere, and then taken out to obtain a hundred-micron-scale self-doped spherical porous carbon material C-4.

[0061] The 100-micron self-doped spherical porous carbon material C-4 obtained in this example has a gray-black metallic spherical appearance, a particle size of 200-400 μm, a nitrogen content of 2.02 at%, a single particle crushing strength of 2.87 N, and a specific surface area of ​​1515 m 2 / g, and the micropore diameter is 0.7nm.

[0062] Example 5

[0063] Take 5g of chitosan powder with a deacetylation degree of 85%, add 120mL of 4wt% acetic acid aqueous solution to fully dissolve it as the dispersed phase in the suspension polymerization; transfer it to 480mL of continuous phase, which is a butyl acetate solution containing 5wt% span 80. Use overhead stirring, and obtain spherical droplets under the action of shear force (speed of 250r / min, temperature of 25°C). After the droplet size is uniform and stable at 400-600μm, add 12mL of 50wt% NaOH solution, and the beads gradually change from transparent viscous droplets to turbid gel beads. After the reaction is carried out for 4h, the chitosan beads have a certain strength, and will not cause obvious changes in shape under mild extrusion, and stop stirring. Soak and wash the spherical chitosan with a large amount of deionized water, wash to neutrality, and obtain a 100-micron spherical chitosan precursor SC-5.

[0064] The 100-micron-sized spherical chitosan precursor SC-5 prepared above was transferred to a quartz boat, which was placed in a tube furnace and heated at N 2 Under the protection of the atmosphere, the temperature was raised to 410°C at a rate of 6°C / min, maintained at this temperature for 2 h, and then raised to 900°C at a rate of 6°C / min, and maintained at this temperature for 2 h; maintained under N 2 The mixture was naturally cooled to room temperature under an atmosphere, and then taken out to obtain a hundred-micron-scale self-doped spherical porous carbon material C-5.

[0065] The 100-micron-sized spherical chitosan precursor SC-5 obtained in this example has a crystallinity of 46% and an average crystal size of

[0066] The 100-micron self-doped spherical porous carbon material C-5 obtained in this example has the appearance of black irregular particles, with a particle size of 200-400 μm, a nitrogen content of 2.31 at%, a single particle crushing strength of 2.98 N, and a specific surface area of ​​1772 m 2 / g, and the micropore diameter is 0.7nm.

[0067] Example 6

[0068] Take 5g of chitosan powder with a deacetylation degree of 75%, add 120mL of 3wt% acetic acid aqueous solution to fully dissolve it as the dispersed phase in the suspension polymerization; transfer it to 480mL of continuous phase, which is a butyl acetate solution containing 5wt% span80. Use overhead stirring, and obtain spherical droplets under the action of shear force (speed of 250r / min, temperature of 25°C). After the droplet size is uniform and stable at 400-600μm, add 12mL of 50wt% NaOH solution, and the beads gradually change from transparent viscous droplets to turbid gel beads. After the reaction is carried out for 1h, stop stirring. Soak and wash the spherical chitosan with a large amount of deionized water, wash it to neutrality, and obtain a 100-micron spherical chitosan precursor SC-6.

[0069] The 100-micron-sized spherical chitosan precursor SC-6 prepared above was transferred to a quartz boat, which was placed in a tube furnace and heated at N 2 Under the protection of the atmosphere, the temperature was raised to 410°C at a rate of 6°C / min, maintained at this temperature for 2 h, and then raised to 900°C at a rate of 6°C / min, and maintained at this temperature for 2 h; maintained under N 2 The mixture was naturally cooled to room temperature under an atmosphere, and then taken out to obtain a self-doped spherical porous carbon material C-6 of 100 micrometers.

[0070] The 100-micrometer-level spherical chitosan precursor SC-6 obtained in this example has a crystallinity of 37% and an average crystal size of

[0071] The 100-micron self-doped spherical porous carbon material C-6 obtained in this example has the appearance of black flaky particles, a particle size of 100-300 μm, a nitrogen content of 2.30 at%, a single particle crushing strength of 2.05 N, and a specific surface area of ​​1602 m 2 / g, and the micropore diameter is 0.7nm.

[0072] Example 7

[0073] Take 5g of chitosan powder with a deacetylation degree of 75%, add 100mL of 3wt% acetic acid aqueous solution to fully dissolve it as the dispersed phase in the suspension polymerization; transfer it to 480mL of continuous phase, which is a butyl acetate solution containing 5wt% span80. Use overhead stirring, and obtain spherical droplets under the action of shear force (speed of 250r / min, temperature of 25°C). After the droplet size is uniform and stable at 400-600μm, add 18mL of 50wt% NaOH solution, and the beads gradually change from transparent viscous droplets to turbid gel beads. After the reaction is carried out for 1h, stop stirring. Soak and wash the spherical chitosan with a large amount of deionized water, wash it to neutrality, and obtain a 100-micron-level spherical chitosan precursor SC-7.

[0074] The 100-micron-sized spherical chitosan precursor SC-7 prepared above was transferred to a quartz boat, which was placed in a tube furnace and heated at N 2 Under the protection of the atmosphere, the temperature was raised to 410°C at a rate of 6°C / min, maintained at this temperature for 2 h, and then raised to 900°C at a rate of 6°C / min, and maintained at this temperature for 2 h; maintained under N 2 The mixture was naturally cooled to room temperature under an atmosphere, and then taken out to obtain a self-doped spherical porous carbon material C-7 of 100 micrometers.

[0075] The 100-micrometer-level spherical chitosan precursor SC-7 obtained in this example has a crystallinity of 40% and an average crystal size of

[0076] The 100-micron self-doped spherical porous carbon material C-7 obtained in this example has the appearance of black ellipsoidal particles, a particle size of 100-600 μm, a nitrogen content of 2.20 at%, a single particle crushing strength of 1.78 N, and a specific surface area of ​​1202 m 2 / g, and the micropore diameter is 0.7nm.

[0077] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a 100-micron self-doped spherical porous carbon material, comprising the following steps: The hundred-micrometer-scale spherical chitosan precursor is carbonized to obtain a hundred-micrometer-scale self-doped spherical porous carbon material.

2. The preparation method according to claim 1, characterized in that: The preparation method of the 100-micron-scale spherical chitosan precursor comprises: Dissolving chitosan in an acetic acid aqueous solution to obtain a dispersed phase; mixing butyl acetate and span 80 to obtain a continuous phase; The dispersed phase and the continuous phase are mixed and suspended to obtain droplets of 100 micrometers; NaOH solution is added to perform precipitation reaction to obtain a spherical chitosan precursor of 100 micrometers.

3. The preparation method according to claim 2, characterized in that: The deacetylation degree of the chitosan is 75-95%.

4. The preparation method according to claim 2, characterized in that: The suspension dispersion is carried out under stirring conditions; the stirring speed is 100-500 r / min; and the suspension dispersion temperature is 10-40°C.

5. The preparation method according to claim 1 or 2, characterized in that: The particle size of the 100-micron-scale spherical chitosan precursor is 400-600 μm; the crystallinity of the 100-micron-scale spherical chitosan precursor is 37-52%, and the average crystal area size is 6. The preparation method according to claim 1, characterized in that: The carbonization conditions include: first heating to 200-500° C. under a protective atmosphere, and performing a first heat preservation for 1-5 hours; second heating to 600-1000° C., and performing a second heat preservation for 2-5 hours; and naturally cooling to room temperature.

7. The preparation method according to claim 6, characterized in that: The first heating rate is 3-10°C / min; the second heating rate is 3-10°C / min.

8. The preparation method according to claim 1, characterized in that: The particle size of the 100-micron self-doped spherical porous carbon material is 100-600 μm; the specific surface area is 269-2100 m 2 / g; the average pore size is 2-4nm; the micropore size is 0.6-0.8nm.

9. The preparation method according to claim 1, characterized in that: The N content of the hundred-micrometer-scale self-doped spherical porous carbon material is 1 to 4 at %.

10. The preparation method according to claim 1, characterized in that: The single particle crushing strength of the 100-micron self-doped spherical porous carbon material is 1.78-3.13N.

Citation Information

Patent Citations

  • Microporous granular carbon and preparation method thereof

    CN112169756A

  • High-strength chitosan ligand exchange resin and preparation method thereof

    CN113980154A