Fused deposition modeling method of continuous fiber reinforced ceramic matrix composite material

By introducing continuous fibers into ceramic matrix composite materials and combining melt deposition molding and screw extrusion processes, the problem of fiber introduction in ceramic matrix composite materials is solved, the toughness and mechanical properties of the material are improved, the manufacturing process is simplified, and suitable for complex components is suitable for The molding meets the needs of high-performance materials such as aerospace.

CN118745115APending Publication Date: 2024-10-08CHENGDU AIRCRAFT INDUSTRY GROUP

Patent Information

Application Number
CN202410971026.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing ceramic additive manufacturing technology is difficult to introduce continuous fibers into ceramic matrix composite materials, resulting in poor surface quality and mechanical properties of prepared 3D printed components. The traditional manufacturing process is costly in small batches and complex configuration structure production. Long cycle.

Method used

Using the melt deposition molding method of continuous fiber reinforced ceramic matrix composite material, the printed base material pellets are combined with continuous by blending ceramic powder and carbon source with thermoplastic resin, extrusion, drawing and granulation, and combined with screw extrusion equipment. The fiber tows are conveyed to the printing nozzle to compound and printed by the printing nozzle movement, followed by degreasing and silicone penetration to form a continuous fiber reinforced ceramic matrix composite material with the target structure.

Benefits of technology

It realizes the introduction of continuous fibers into ceramic matrix composite materials, improves the toughness and mechanical properties of the materials, simplifies the manufacturing process, reduces the demand for raw materials and molds, and is suitable for integrated molding of complex components, meeting high-performance materials such as aerospace. demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745115A_ABST
    Figure CN118745115A_ABST
Patent Text Reader

Abstract

The invention discloses a fused deposition modeling method of a continuous fiber reinforced ceramic matrix composite material, and relates to the technical field of additive manufacturing. Comprising the following steps: adding ceramic powder and a carbon source into thermoplastic resin for blending, and then performing extrusion, wire drawing and granulation to obtain printing base material granules; drawing a mathematical model according to the target structure and slicing to obtain slice data and importing the slice data into printing equipment; printing parameters and a printing path are set, the printing base material granules and the continuous fiber tows are conveyed into printing equipment through screw extrusion equipment, the printing base material granules and the continuous fiber tows are compounded at a printing spray head, printing is conducted along with movement of the printing spray head, and a printing initial blank is obtained; degreasing and sintering the printing initial blank, and cooling to obtain a continuous fiber preform; and carrying out siliconizing treatment on the continuous fiber preform, and cooling to obtain the continuous fiber reinforced ceramic matrix composite material with the target structure. According to the method, fused deposition molding and screw extrusion are combined, and the continuous fibers are introduced into an additive manufacturing component of the ceramic matrix composite, so that the problem that the continuous fiber reinforced ceramic matrix composite is difficult to mold is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of additive manufacturing technology, and in particular to a melt deposition molding method for continuous fiber reinforced ceramic matrix composite materials. Background Art

[0002] As the aerospace industry develops towards higher speeds, the requirements for materials of thermal protection devices on aircraft have been further improved. In response to this trend, ceramic materials have become thermal structural materials with good application prospects. Compared with traditional alloy materials, ceramic materials have higher heat resistance and lower density, and have replaced alloys in the application of some thermal structural parts. However, pure ceramic materials are often too brittle, and their use in parts with high requirements for mechanical properties such as thermal structural parts is limited. It is usually necessary to compound fiber materials such as carbon fiber and silicon carbide fiber into the matrix material as a reinforcement phase to improve toughness. Since continuous fibers have higher strength than short-cut fibers, continuous fiber-reinforced ceramic matrix composites have become the focus of research. Traditional continuous fiber-reinforced ceramic matrix composites are to prepare continuous fibers in advance into preforms with the required morphology and structure, and use methods such as reaction infiltration or precursor prepreg cracking to finally form continuous fiber-reinforced ceramic matrix composites with the assistance of tooling molds. However, when preparing small batches or multiple batches of structures with complex configurations, traditional manufacturing processes not only require the preparation of multiple molds, but also the need to weave continuous fibers into preforms of different shapes in advance, resulting in excessively high parts production costs and long production cycles. In addition, parts prepared using traditional manufacturing processes require a large number of machining processes to ultimately produce products of the desired configuration.

[0003] In recent years, ceramic additive manufacturing technology has been gradually applied to fiber-reinforced ceramic-based composites, but it can only solve the complex molding of some fiber-reinforced ceramic-based composites, and is limited to using nanofillers such as chopped fibers or whiskers as reinforcement phases, while it is difficult to introduce continuous fibers into ceramic-based composites. Moreover, the additive manufacturing process for continuous fiber-reinforced ceramic-based composites is often limited to the use of slurry direct writing process for manufacturing, and the obtained 3D printed components not only have poor surface quality, but also poor mechanical properties. Based on this, the present application proposes a molding method that introduces continuous fibers as reinforcement phases into ceramic-based composites and prepares them through additive manufacturing processes. Summary of the invention

[0004] The main purpose of the present application is to provide a melt deposition molding method for continuous fiber reinforced ceramic matrix composites, aiming to solve the technical problem that it is difficult to introduce continuous fibers as a reinforcement phase into ceramic matrix composites using existing molding methods.

[0005] To achieve the above objectives, the present application proposes a method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials, comprising the following steps:

[0006] The ceramic powder and the carbon source are added into the thermoplastic resin and mixed, and then extruded, drawn and granulated to obtain the printing substrate granules;

[0007] After drawing the digital model and slicing the target structure, the slice data is obtained and imported into the printing device;

[0008] Setting printing parameters and printing paths, conveying the printing substrate pellets and the continuous fiber tow into the printing device through a screw extruder, allowing the printing substrate pellets and the continuous fiber tow to be compounded at the printing nozzle, and printing is performed as the printing nozzle moves, thereby obtaining a printed blank;

[0009] Degreasing and sintering the printed preform, and obtaining a continuous fiber preform with a target structure after cooling;

[0010] The continuous fiber preform with the target structure is subjected to siliconization treatment and, after cooling, a continuous fiber reinforced ceramic matrix composite material with the target structure is obtained.

[0011] Optionally, the step of adding ceramic powder and carbon source into thermoplastic resin and blending, and then extruding, drawing and granulating to obtain printing substrate pellets comprises:

[0012] The ceramic powder and the carbon source are added into the thermoplastic resin, and mixed at 180° C. to 220° C. to obtain a mixture;

[0013] The mixture is then extruded through a twin-screw extruder at an extrusion temperature of 180°C-220°C, and converged at the end grind of the twin-screw extruder. After being straightened into filaments at a traction speed of 250mm / min-350mm / min, a pelletizer is used for granulation to obtain printing substrate pellets.

[0014] Optionally, the diameter of the printing substrate particles is 1.74 mm-1.76 mm.

[0015] Optionally, the continuous fiber tow is one of carbon fiber or silicon carbide fabric.

[0016] Optionally, the number of monofilaments in the continuous fiber bundle is 1K-3K.

[0017] Optionally, in the step of setting printing parameters and printing path, the printing parameters include:

[0018] The printing temperature is 190℃-200℃, the slice thickness is 1.2mm-1.8mm, the line width is 0.8mm-1.2mm, the print head diameter is 0.8mm-1.2mm, and the substrate temperature is 60℃-70℃.

[0019] Optionally, the step of conveying the printing substrate granules and the continuous fiber tows into the printing device through a screw extruder, compounding the printing substrate granules and the continuous fiber tows at the printing nozzle, and printing with the movement of the printing nozzle to obtain a printed blank comprises:

[0020] Add the printing substrate pellets to the feed port of a single-screw extruder, the interior of the screw of the single-screw extruder is hollow, and add a continuous fiber bundle to the interior of the screw of the single-screw extruder, convey the printing substrate pellets and the continuous fiber bundle into the printing device through the single-screw extruder and compound them at the printing nozzle, and print as the printing nozzle moves to obtain a printed blank;

[0021] The screw speed at the printing nozzle is 75rpm-85rpm, the extrusion rate is 0.6-1.0, and the pulling speed of the continuous fiber bundle is 30mm / s-40mm / s.

[0022] Optionally, the step of degreasing and sintering the printed preform and obtaining a continuous fiber preform having a target structure after cooling comprises:

[0023] The printed blank is heated from room temperature to 150°C-200°C at a heating rate of 1.1°C / min-1.4°C / min, kept warm for 0.8h-1.2h, then heated to 280°C-320°C at a heating rate of 0.8°C / min-1.2°C / min, kept warm for 1.8h-2.2h, and cooled to room temperature to obtain a continuous fiber preform with a target structure.

[0024] Optionally, the step of subjecting the continuous fiber preform having the target structure to siliconization treatment and obtaining the continuous fiber reinforced ceramic matrix composite material having the target structure after cooling comprises:

[0025] The continuous fiber preform with the target structure is placed on silicon powder, heated to 1400°C-1600°C in a vacuum environment, kept warm for 25min-35min, and then removed from excess silicon powder after cooling to room temperature to obtain a continuous fiber reinforced ceramic matrix composite material with the target structure.

[0026] Optionally, in the step of performing siliconizing treatment on the continuous fiber preform having the target structure, the mass ratio of the silicon powder to the continuous fiber preform having the target structure is (1.2-1.8):1.

[0027] The beneficial effects of this application include:

[0028] This application combines the melt deposition molding process of continuous fiber reinforced composite materials with the screw extrusion process, and introduces continuous fibers into the additive manufacturing components of ceramic matrix composite materials, which can not only make the cracks in the components propagate along the continuous fiber interface, hindering their rapid propagation inside the matrix, but also produce the phenomenon of fiber pull-out when the components are damaged, effectively increasing the toughness of the ceramic matrix composite materials, and can not only solve the problem that continuous fiber reinforced ceramic matrix composite materials are difficult to mold, but also realize the integrated molding of complex components, thereby meeting the urgent demand of the rapidly developing aerospace technology for high-performance ceramic matrix composite components;

[0029] This application adopts additive manufacturing process to prepare continuous fiber reinforced ceramic matrix composite materials. Compared with traditional subtractive manufacturing, it can not only save a lot of raw materials and tooling molds, but also avoid cumbersome weaving and post-processing machine processing steps, and can also realize the preparation of parts with complex structures;

[0030] The fused deposition modeling method of the present application can make the continuous fiber distribution parallel to the moving direction of the printing nozzle. Due to the inherent anisotropy of additive manufacturing, the directional reinforcement of the printed component can be achieved by changing the distribution of the printing path;

[0031] The present application can achieve the distribution of different matrix materials on the surface of continuous fibers by regulating the screw speed and the pulling speed of continuous fibers. When the print head prints along the slicing direction, the amount of ceramics in different parts of the same component can be regulated, thereby fine-tuning the wall thickness and adjusting the state of the continuous fibers in the composite material. According to the different performance requirements of different parts of the engineering parts, the screw speed and the continuous fiber pulling speed ratio are changed to perform personalized regulation on the performance of the composite material.

[0032] The present application introduces continuous fibers into the additive manufacturing of ceramic-based composite materials. During degreasing and sintering, the load-bearing part of the blank is transformed from thermoplastic resin to continuous fibers, which can effectively avoid the collapse of the blank caused by the melting, flow and decomposition of the thermoplastic resin, and can meet the self-forming of the component without a mold;

[0033] The continuous fiber reinforced ceramic matrix composite material prepared by the method of the present application has significantly improved mechanical properties compared to those using chopped fibers or whiskers as reinforcement phases. At the same time, since ceramic powder is used as an added phase to be compounded and cut with thermoplastic resin, there are fewer restrictions on the selection of ceramic types, which can meet the molding needs of various ceramic substrates. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0035] Figure 1 A schematic diagram of preparing printing substrate granules by compounding ceramic powder and thermoplastic resin as described in an embodiment of the present application;

[0036] Figure 2 This is a schematic diagram of the composite of the printing substrate pellets and the continuous fiber bundles described in the embodiment of the present application to generate a printing blank.

[0037] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0039] At present, although ceramic additive manufacturing technology can solve the complex molding of some fiber-reinforced ceramic-based composites, it is limited to the use of nanofillers such as chopped fibers or whiskers as reinforcement phases, and it is difficult to introduce continuous fibers into ceramic-based composites. Moreover, the additive manufacturing process for continuous fiber-reinforced ceramic-based composites is often limited to the use of slurry direct writing technology for manufacturing. The obtained 3D printed components not only have poor surface quality, but also poor mechanical properties.

[0040] Fused deposition modeling (FDM), as a type of 3D printing technology, is a process of mixing hot-melt plastic raw materials with fillers and preparing them into filaments. The materials are heated and melted by the heating device at the print head, and the materials are extruded from the print head and deposited layer by layer according to the scanning path of the part. After each layer is printed, the printing platform drops or the print head rises by a layer thickness to deposit a new layer. This process is repeated to finally achieve the deposition molding of the part. The key is to keep the temperature of the semi-fluid molding material just above the melting point. When the material leaves the nozzle, the temperature drops to the solidification temperature and begins to solidify and form, and finally forms a physical object in a three-dimensional space. This technology can introduce continuous fibers during the printing process, and the continuous fibers are transported at a constant speed through the gears at the print head. In this process, the hot-melt composite material is introduced into the print head through another wire conveying device, compounded with the fiber tow, and the matrix material is coated on the fiber tow, finally forming a continuous fiber reinforced composite material. However, ceramic materials are difficult to prepare into filaments. Ceramic powders need to be compounded with hot-melt resins and prepared into granules for printing. When printing granules, a screw is required to push them, which limits the introduction of continuous fibers. Therefore, it is still difficult to prepare continuous fiber-reinforced ceramic-based composites using fused deposition modeling technology.

[0041] In view of the technical problems existing in the prior art, an embodiment of the present application provides a method for melt deposition molding of a continuous fiber reinforced ceramic matrix composite material, comprising the following steps:

[0042] The ceramic powder and the carbon source are added into the thermoplastic resin and mixed, and then extruded, drawn and granulated to obtain the printing substrate granules;

[0043] After drawing the digital model and slicing the target structure, the slice data is obtained and imported into the printing device;

[0044] Setting printing parameters and printing paths, conveying the printing substrate pellets and the continuous fiber tow into the printing device through a screw extruder, allowing the printing substrate pellets and the continuous fiber tow to be compounded at the printing nozzle, and printing is performed as the printing nozzle moves, thereby obtaining a printed blank;

[0045] Degreasing and sintering the printed preform, and obtaining a continuous fiber preform with a target structure after cooling;

[0046] The continuous fiber preform with the target structure is subjected to siliconization treatment and, after cooling, a continuous fiber reinforced ceramic matrix composite material with the target structure is obtained.

[0047] The present application combines the melt deposition molding process of continuous fiber reinforced composite materials with the screw extrusion process, and respectively delivers the printing substrate pellets and the continuous fiber bundles into the printing device through the screw extrusion device, so that the printing substrate pellets and the continuous fiber bundles are compounded at the printing nozzle, thereby introducing the continuous fiber into the additive manufacturing component of the ceramic matrix composite material, which can not only make the cracks in the component propagate along the continuous fiber interface, hindering its rapid propagation inside the matrix, but also produce the phenomenon of fiber pull-out when the component is destroyed, effectively increasing the toughness of the ceramic matrix composite material, not only solving the problem that the continuous fiber reinforced ceramic matrix composite material is difficult to form, but also can realize the integrated molding of complex components, thereby meeting the urgent demand of the rapidly developing aerospace technology for high-performance ceramic matrix composite components, and the continuous fiber reinforced ceramic matrix composite material prepared by the method of the present application has significantly improved mechanical properties compared with the use of chopped fibers or whiskers as the reinforcing phase. Although there is still a gap compared with the woven continuous fiber reinforced ceramic composite material, it is fully capable of being used as a secondary load-bearing member.

[0048] Specifically, the carbon source may be carbon black, the thermoplastic resin may be polylactic acid resin, and the thermoplastic resin may be replaced with micro-nano fillers or functional fillers for composite reinforcement, such as absorbing fillers or conductive fillers, as required.

[0049] As an implementation method of the present application, the step of adding ceramic powder and carbon source into thermoplastic resin and blending, and then extruding, drawing and granulating to obtain printing substrate pellets includes:

[0050] The ceramic powder and the carbon source are added into the thermoplastic resin, and mixed at 180° C. to 220° C. to obtain a mixture;

[0051] The mixture is then extruded through a twin-screw extruder at an extrusion temperature of 180°C-220°C, and converged at the end grind of the twin-screw extruder. After being straightened into filaments at a traction speed of 250mm / min-350mm / min, a pelletizer is used for granulation to obtain printing substrate pellets.

[0052] As an implementation method of the present application, the diameter of the printing substrate particles is 1.74 mm-1.76 mm.

[0053] As an implementation method of the present application, the continuous fiber tow is one of carbon fiber or silicon carbide fabric.

[0054] As an implementation method of the present application, the number of monofilaments in the continuous fiber tow is 1K-3K.

[0055] As an implementable embodiment of the present application, in the step of setting printing parameters and printing path, the printing parameters include:

[0056] The printing temperature is 190℃-200℃, the slice thickness is 1.2mm-1.8mm, the line width is 0.8mm-1.2mm, the print head diameter is 0.8mm-1.2mm, and the substrate temperature is 60℃-70℃.

[0057] Specifically, the printing path can be adjusted according to actual needs, and can be calculated through finite element analysis simulation to obtain the most suitable printing path, and by changing the distribution of the printing path, directional enhancement of the printed component can be achieved.

[0058] As an implementation method of the present application, the step of conveying the printing substrate pellets and the continuous fiber tow into the printing device through a screw extruder, compounding the printing substrate pellets and the continuous fiber tow at the printing nozzle, and printing with the movement of the printing nozzle to obtain a printed blank includes:

[0059] Add the printing substrate pellets to the feed port of a single-screw extruder, the interior of the screw of the single-screw extruder is hollow, and add a continuous fiber bundle to the interior of the screw of the single-screw extruder, convey the printing substrate pellets and the continuous fiber bundle into the printing device through the single-screw extruder and compound them at the printing nozzle, and print as the printing nozzle moves to obtain a printed blank;

[0060] The screw speed at the printing nozzle is 75rpm-85rpm, the extrusion rate is 0.6-1.0, and the pulling speed of the continuous fiber bundle is 30mm / s-40mm / s.

[0061] In order to solve the problem that continuous fibers are difficult to introduce during pellet printing, this application selects a single-screw extruder to transport the printed substrate pellets and continuous fiber bundles, and designs the interior of the screw of the single-screw extruder to be a hollow structure, such as Figure 2As shown, the continuous fiber is conveyed through the inner circular hole of the screw, and the printing substrate pellets enter from the feed port of the single-screw extruder, are conveyed under the rotation of the screw, and are compounded at the nozzle to form a continuous fiber reinforced ceramic matrix composite material precursor, and then deposited and formed into the required structure as the printing nozzle moves to obtain a printed blank, thereby solving the problem of difficulty in introducing continuous fibers as a reinforcing phase into the pellet printing process. In addition, the present application can achieve the distribution amount of different matrix materials on the surface of the continuous fiber by regulating the screw speed and the pulling speed of the continuous fiber. When the printing nozzle prints along the slicing direction, the amount of ceramic in different parts of the same component can be regulated, thereby fine-tuning the wall thickness and adjusting the state of the continuous fiber in the composite material. According to the different performance requirements of different parts of the engineering parts, the screw speed and the continuous fiber pulling speed ratio are changed, thereby personalizing the performance of the composite material, wherein the ratio of the screw speed to the pulling speed is comprehensively determined by the ceramic composite material itself and actual needs.

[0062] In the specific implementation process, the continuous fiber tow needs to be treated with an interface layer to ensure that the continuous fiber will not react during the subsequent siliconization treatment.

[0063] As an implementation method of the present application, the step of degreasing and sintering the printed preform and obtaining a continuous fiber preform having a target structure after cooling includes:

[0064] The printed blank is heated from room temperature to 150°C-200°C at a heating rate of 1.1°C / min-1.4°C / min, kept warm for 0.8h-1.2h, then heated to 280°C-320°C at a heating rate of 0.8°C / min-1.2°C / min, kept warm for 1.8h-2.2h, and cooled to room temperature to obtain a continuous fiber preform with a target structure.

[0065] Specifically, during debinding and sintering, the load-bearing part of the printed blank is converted from thermoplastic resin to continuous fiber, which can effectively avoid the collapse of the printed blank caused by the melting, flow and decomposition of the thermoplastic resin. The self-forming of the component can be achieved without a mold. After debinding and sintering, the mechanical properties and densification degree of the continuous fiber preform can be enhanced, thereby obtaining a continuous fiber reinforced porous preform with target morphology and size.

[0066] As an implementation method of the present application, the step of subjecting the continuous fiber preform having the target structure to siliconization treatment and obtaining the continuous fiber reinforced ceramic matrix composite material having the target structure after cooling includes:

[0067] The continuous fiber preform with the target structure is placed on silicon powder, heated to 1400°C-1600°C in a vacuum environment, kept warm for 25min-35min, and then removed from excess silicon powder after cooling to room temperature to obtain a continuous fiber reinforced ceramic matrix composite material with the target structure.

[0068] By burying a continuous fiber preform in a certain amount of silicon powder and heating it in a vacuum environment to melt the silicon powder, liquid silicon can penetrate into the continuous fiber preform through the capillary effect, thereby obtaining a densified continuous fiber reinforced ceramic material.

[0069] As an implementation method of the present application, the mass ratio of the silicon powder to the continuous fiber preform having the target structure is (1.2-1.8):1.

[0070] Specifically, the mass of silicon powder during siliconizing treatment is determined by the mass of the continuous fiber preform, and the mass of silicon powder is preferably 1.5 times the mass of the continuous fiber preform.

[0071] The above technical solution of the present application is described in detail below in conjunction with specific embodiments.

[0072] Example 1

[0073] A method for melt deposition molding of a continuous fiber reinforced ceramic matrix composite material, taking continuous carbon fiber reinforced silicon carbide ceramic as an example, comprises the following steps:

[0074] Adding silicon carbide powder and carbon black to polylactic acid resin, mixing them by an internal mixer, heating the internal mixer at a temperature of 200° C. to obtain a mixture, wherein the mass fraction of silicon carbide is 65wt%, the mass fraction of carbon black is 15wt%, and the mass fraction of polylactic acid resin is 20wt%;

[0075] The mixture is then extruded through a twin-screw extruder, the heating nozzle temperature of the twin-screw extruder is set to 200° C., and the mixture is converged at the end grinding of the twin-screw extruder, and then straightened into filaments at a traction speed of 300 mm / min by a traction machine, such as Figure 1 As shown, a pelletizer is used for granulation to obtain printing substrate pellets, and the diameter of the printing substrate pellets is 1.75 mm;

[0076] According to the target structure, Materialise Magics software was used to model a bending performance test piece with a size of 80mm×40mm×10mm. The slicing software was used to perform path planning and slicing according to the performance enhancement requirements, and the stl format file was obtained and imported into the printing device.

[0077] The printing path and printing temperature are set to 195°C, the slice thickness is 1.5mm, the line width is 1.0mm, the print nozzle diameter is 1.0mm, and the substrate temperature is 65°C. The printing substrate pellets are added to the feed port of the single-screw extruder, the screw of the single-screw extruder is hollow, and the continuous fiber tow is added to the screw of the single-screw extruder. The printing substrate pellets and the continuous fiber tow are transported into the printing device through the single-screw extruder and compounded at the print nozzle, and printing is performed as the print nozzle moves, such as Figure 2 As shown, a printed blank is obtained;

[0078] Among them, the screw speed at the printing nozzle is 80rpm, the extrusion rate is 0.8, the pulling speed of the continuous fiber tow is 35mm / s, and the number of single filaments in the continuous fiber tow is 2K;

[0079] The printed preform was heated from room temperature to 180° C. at a heating rate of 1.25° C. / min, kept at that temperature for 1.0 h, then heated to 300° C. at a heating rate of 1.0° C. / min, kept at that temperature for 2.0 h, and cooled to room temperature to obtain a continuous fiber preform with a target structure;

[0080] Silicon powder with a mass 1.5 times that of the continuous fiber preform is spread evenly in a graphite crucible, and the continuous fiber preform is placed on the silicon powder. The temperature is raised to 1520°C in a vacuum environment and kept warm for 30 minutes. After cooling to room temperature, the excess silicon powder is removed to obtain a continuous fiber reinforced ceramic matrix composite material with a target structure.

[0081] Example 2

[0082] A method for melt deposition molding of a continuous fiber reinforced ceramic matrix composite material comprises the following steps:

[0083] Adding silicon carbide powder and carbon black to polylactic acid resin, mixing them by an internal mixer, heating the internal mixer at 180° C. to obtain a mixture, wherein the mass fraction of silicon carbide is 65wt%, the mass fraction of carbon black is 15wt%, and the mass fraction of polylactic acid resin is 20wt%;

[0084] The mixture is then extruded through a twin-screw extruder at an extrusion temperature of 180° C., and converged at the end grind of the twin-screw extruder. After being straightened into filaments at a traction speed of 250 mm / min, a pelletizer is used for granulation to obtain printing substrate pellets, and the diameter of the printing substrate pellets is 1.74 mm;

[0085] According to the target structure, Materialise Magics software was used to model a bending performance test piece with a size of 80mm×40mm×10mm. The slicing software was used to perform path planning and slicing according to the performance enhancement requirements, and the stl format file was obtained and imported into the printing device.

[0086] The printing path and the printing temperature are set to 190° C., the slice thickness is 1.2 mm, the line width is 0.8 mm, the print nozzle diameter is 0.8 mm, and the substrate temperature is 60° C. The printing substrate pellets are added to the feed port of a single-screw extruder, the screw of the single-screw extruder is hollow inside, and a continuous fiber tow is added to the screw of the single-screw extruder. The printing substrate pellets and the continuous fiber tow are transported into the printing device through the single-screw extruder and compounded at the print nozzle, and printing is performed as the print nozzle moves to obtain a printed blank;

[0087] Among them, the screw speed at the printing nozzle is 75rpm, the extrusion rate is 0.6, the pulling speed of the continuous fiber tow is 30mm / s, and the number of single filaments in the continuous fiber tow is 1K;

[0088] The printed preform was heated from room temperature to 150° C. at a heating rate of 1.1° C. / min, kept at that temperature for 0.8 h, then heated to 280° C. at a heating rate of 0.8° C. / min, kept at that temperature for 1.8 h, and cooled to room temperature to obtain a continuous fiber preform with a target structure;

[0089] Silicon powder with a mass 1.2 times that of the continuous fiber preform is spread evenly in a graphite crucible, and the continuous fiber preform is placed on the silicon powder. The temperature is raised to 1400°C in a vacuum environment and kept warm for 25 minutes. After cooling to room temperature, the excess silicon powder is removed to obtain a continuous fiber reinforced ceramic matrix composite material with a target structure.

[0090] Example 3

[0091] A method for melt deposition molding of a continuous fiber reinforced ceramic matrix composite material comprises the following steps:

[0092] Adding silicon carbide powder and carbon black to polylactic acid resin, mixing them by an internal mixer, heating the internal mixer at a temperature of 220° C. to obtain a mixture, wherein the mass fraction of silicon carbide is 65wt%, the mass fraction of carbon black is 15wt%, and the mass fraction of polylactic acid resin is 20wt%;

[0093] The mixture is then extruded through a twin-screw extruder at an extrusion temperature of 220° C., and converged at the end grind of the twin-screw extruder. After being straightened into filaments at a traction speed of 350 mm / min, a pelletizer is used for granulation to obtain printing substrate pellets, and the diameter of the printing substrate pellets is 1.76 mm;

[0094] According to the target structure, Materialise Magics software was used to model a bending performance test piece with a size of 80mm×40mm×10mm. The slicing software was used to perform path planning and slicing according to the performance enhancement requirements, and the stl format file was obtained and imported into the printing device.

[0095] The printing path and the printing temperature are set to 200° C., the slice thickness is 1.8 mm, the line width is 1.2 mm, the print nozzle diameter is 1.2 mm, and the substrate temperature is 70° C. The printing substrate pellets are added to the feed port of a single-screw extruder, the screw of the single-screw extruder is hollow, and a continuous fiber bundle is added to the screw of the single-screw extruder. The printing substrate pellets and the continuous fiber bundle are transported into the printing device through the single-screw extruder and compounded at the print nozzle. Printing is performed as the print nozzle moves to obtain a printed blank.

[0096] Among them, the screw speed at the printing nozzle is 85rpm, the extrusion rate is 1.0, the pulling speed of the continuous fiber tow is 40mm / s, and the number of single filaments in the continuous fiber tow is 3K;

[0097] The printed preform was heated from room temperature to 200° C. at a heating rate of 1.4° C. / min, kept at that temperature for 1.2 h, then heated to 320° C. at a heating rate of 1.2° C. / min, kept at that temperature for 2.2 h, and cooled to room temperature to obtain a continuous fiber preform with a target structure;

[0098] Silicon powder with a mass 1.8 times that of the continuous fiber preform is spread evenly in a graphite crucible, and the continuous fiber preform is placed on the silicon powder. The temperature is raised to 1600°C in a vacuum environment and kept warm for 35 minutes. After cooling to room temperature, the excess silicon powder is removed to obtain a continuous fiber reinforced ceramic matrix composite material with a target structure.

[0099] The above description is only an optional embodiment of the present application, and does not limit the patent scope of the present application. All equivalent structural transformations made by using the contents of the present application specification and drawings under the inventive concept of the present application, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present application.

Claims

1. A method for melt deposition molding of a continuous fiber reinforced ceramic matrix composite material, comprising the following steps: The ceramic powder and the carbon source are added into the thermoplastic resin and mixed, and then extruded, drawn and granulated to obtain the printing substrate granules; After drawing the digital model and slicing the target structure, the slice data is obtained and imported into the printing device; Setting printing parameters and printing paths, conveying the printing substrate pellets and the continuous fiber tow into the printing device through a screw extruder, allowing the printing substrate pellets and the continuous fiber tow to be compounded at the printing nozzle, and printing is performed as the printing nozzle moves, thereby obtaining a printed blank; Degreasing and sintering the printed preform, and obtaining a continuous fiber preform with a target structure after cooling; The continuous fiber preform with the target structure is subjected to siliconization treatment and, after cooling, a continuous fiber reinforced ceramic matrix composite material with the target structure is obtained.

2. The method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials according to claim 1, characterized in that: The step of adding ceramic powder and carbon source into thermoplastic resin and blending, and then extruding, drawing and granulating to obtain printing substrate pellets comprises: The ceramic powder and the carbon source are added into the thermoplastic resin, and mixed at 180° C. to 220° C. to obtain a mixture; The mixture is then extruded through a twin-screw extruder at an extrusion temperature of 180°C-220°C, and converged at the end grind of the twin-screw extruder. After being straightened into filaments at a traction speed of 250mm / min-350mm / min, a pelletizer is used for granulation to obtain printing substrate pellets.

3. The method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials according to claim 1, characterized in that: The diameter of the printing substrate particles is 1.74 mm to 1.76 mm.

4. The method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials according to claim 1, characterized in that: The continuous fiber tow is one of carbon fiber or silicon carbide fabric.

5. The method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials according to claim 1, characterized in that: The number of monofilaments in the continuous fiber tow is 1K-3K.

6. The method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials according to claim 1, characterized in that: In the step of setting the printing parameters and the printing path, the printing parameters include: The printing temperature is 190℃-200℃, the slice thickness is 1.2mm-1.8mm, the line width is 0.8mm-1.2mm, the print head diameter is 0.8mm-1.2mm, and the substrate temperature is 60℃-70℃.

7. The method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials according to claim 1, characterized in that: The step of conveying the printing substrate granules and the continuous fiber bundles into the printing device through a screw extruder, compounding the printing substrate granules and the continuous fiber bundles at the printing nozzle, and printing with the movement of the printing nozzle to obtain a printed blank comprises: Add the printing substrate pellets to the feed port of a single-screw extruder, the interior of the screw of the single-screw extruder is hollow, and add a continuous fiber bundle to the interior of the screw of the single-screw extruder, convey the printing substrate pellets and the continuous fiber bundle into the printing device through the single-screw extruder and compound them at the printing nozzle, and print as the printing nozzle moves to obtain a printed blank; The screw speed at the printing nozzle is 75rpm-85rpm, the extrusion rate is 0.6-1.0, and the pulling speed of the continuous fiber bundle is 30mm / s-40mm / s.

8. The method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials according to claim 1, characterized in that: The step of degreasing and sintering the printed preform and obtaining a continuous fiber preform having a target structure after cooling comprises: The printed blank is heated from room temperature to 150°C-200°C at a heating rate of 1.1°C / min-1.4°C / min, kept warm for 0.8h-1.2h, then heated to 280°C-320°C at a heating rate of 0.8°C / min-1.2°C / min, kept warm for 1.8h-2.2h, and cooled to room temperature to obtain a continuous fiber preform with a target structure.

9. The method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials according to claim 1, characterized in that: The step of subjecting the continuous fiber preform having the target structure to siliconization treatment and, after cooling, obtaining a continuous fiber reinforced ceramic matrix composite material having the target structure comprises: The continuous fiber preform with the target structure is placed on silicon powder, heated to 1400°C-1600°C in a vacuum environment, kept warm for 25min-35min, and then removed from excess silicon powder after cooling to room temperature to obtain a continuous fiber reinforced ceramic matrix composite material with the target structure.

10. The method for melt deposition molding of continuous fiber reinforced ceramic matrix composite materials according to claim 9, characterized in that: In the step of performing siliconization treatment on the continuous fiber preform having the target structure, the mass ratio of the silicon powder to the continuous fiber preform having the target structure is (1.2-1.8):1.

Citation Information

Patent Citations

  • Preparation method of continuous fiber reinforced SiC parts based on additive manufacturing, and product

    CN110372390A

  • 3D printing device and method for continuous fiber and particle base material compounding

    CN112140533A

  • Hot auxiliary material extrusion direct-writing 3D printing method for continuous fiber reinforced ceramic

    CN116551808A

Cited By

  • Carbon fiber toughened ceramic matrix composite 3D printing equipment, printing method and application

    CN119635789A

  • Preparation method of continuous fiber reinforced SiC ceramic composite material for 3D printing

    CN119912269A