Efficient photocatalytic organic synthesis method utilizing high single photon energy of quantum dots

By constructing a ZnSe@ZnS-organic molecule hybrid system and utilizing the thermally activated delayed fluorescence mechanism, the problems of narrow absorption spectrum and low quantum efficiency of the photocatalyst are solved, and high-efficiency photocatalytic organic synthesis is achieved, with a wider selection range of substrate molecules. The excited state lifetime of quantum dots is longer, and the single photon energy is close to ultraviolet, which is suitable for the synthesis of high value-added chemicals.

CN118745190APending Publication Date: 2024-10-08HUBEI UNIV OF ARTS & SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410919650.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

In existing photocatalytic organic synthesis, common photocatalysts have narrow absorption spectra and low recombination rates of electrons and holes, resulting in low quantum efficiency. Moreover, the catalytic mechanism of specific catalysts is unknown, making it difficult to achieve efficient high single-photon energy applications.

Method used

Design a ZnSe@ZnS-organic molecule hybrid system. By controlling the particle size of ZnSe core quantum dots and ZnS shell thickness, a thermally activated delayed fluorescence system is constructed, and the forward triplet energy transfer and thermal activation of quantum dots are used to achieve Long excited state lifetime and high single photon energy are suitable for efficient photocatalytic organic synthesis.

Benefits of technology

Achieve efficient photocatalysis without coordination bonding of substrate molecules under visible light irradiation, significantly improve the quantum efficiency and conversion rate of organic synthesis, wider selection range of substrate molecules, longer quantum dot excited state lifetime, single photon energy Close to ultraviolet, suitable for the synthesis of high value-added chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745190A_ABST
    Figure CN118745190A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of application of quantum dots, in particular to an efficient photocatalytic organic synthesis method utilizing high single photon energy of quantum dots. A ZnSe (at) ZnS quantum dot-organic molecule hybrid system is used as a photocatalyst, and a quantum dot excited state with high single photon energy and long service life is realized through a thermal activation delayed fluorescence mechanism of the ZnSe (at) ZnS quantum dot-organic molecule hybrid system, so that substrate molecules are subjected to efficient photocatalytic organic synthesis. According to the method, the substrate molecules are subjected to photocatalysis through the quantum dot thermal activation delayed fluorescence process, compared with catalysis by directly utilizing triplet state energy of intermediate molecules, higher single photon energy is achieved, the quantum dot excited state service life is longer, meanwhile, the substrate molecules do not need to be subjected to coordination bonding with a photocatalyst, and the type selection range of the substrate molecules is wider.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of quantum dot application, and in particular to a highly efficient photocatalytic organic synthesis method utilizing the high single-photon energy of quantum dots. Background Art

[0002] Photocatalytic organic synthesis usually uses solar energy to perform photochemical synthesis of organic molecules at room temperature and pressure. It not only has loose requirements on reaction conditions and is easy to operate, but also can effectively reduce the occurrence of side reactions. Against the background of increasingly prominent energy issues, it is a low-carbon, environmentally friendly, and sustainable means of organic synthesis, which is especially important for the synthesis of high value-added chemicals. However, with the deepening of research, the shortcomings of photocatalytic organic synthesis are becoming more and more recognized by people, such as the narrow absorption spectrum of common photocatalysts resulting in low light energy utilization, the high recombination probability of electrons and holes resulting in low quantum efficiency, and the unclear catalytic mechanism of specific catalysts.

[0003] Semiconductor colloidal quantum dots have the advantages of simple synthesis method, adjustable band gap with size, large light absorption coefficient, short transmission distance of photogenerated electrons and holes to the surface of quantum dots, etc. They are very beneficial to photocatalytic organic synthesis reactions and have become a hot material in the field of photocatalytic organic synthesis in recent years. Under light, the excited state lifetime of pure quantum dots is generally short, in the nanosecond order. In order to achieve effective catalysis, there are currently two main schemes for photocatalytic organic synthesis based on quantum dots. One is to coordinate the substrate molecules on the surface of quantum dots through groups, and improve the catalytic efficiency by reducing the transmission distance of charge or energy transfer, but it also inevitably limits the selection range of substrate molecules; the other scheme is to introduce intermediate molecules coordinated on the surface of quantum dots. After light excitation, the quantum dots transfer the excited state energy to the intermediate molecules through triplet energy transfer. Since the triplet lifetime of the intermediate molecules is long, usually in the microsecond order, it can photocatalyze the substrate molecules freely dispersed in the solvent, and at the same time, it can also broaden the selection range of substrate molecules. However, the disadvantage of this scheme is that there is a large energy loss in the process of transferring the excited state energy of quantum dots to the intermediate molecules, which is not conducive to the application of photocatalytic organic synthesis with high single-photon energy requirements.

[0004] Thermally activated delayed fluorescence in quantum dot-organic molecule hybrid systems can significantly extend the excited state lifetime of quantum dots through forward triplet energy transfer from quantum dots to molecules and reverse triplet energy transfer from molecules to quantum dots under thermal activation. Since the final excited state energy is determined by the band edge energy level of quantum dots, its single photon energy is almost lossless, which makes this type of thermally activated delayed fluorescence system have both high single photon energy and long excited state lifetime. In theory, it can achieve 100% exciton utilization, which is very beneficial for efficient or thermodynamically difficult photocatalytic organic synthesis processes and has promising application prospects. However, although a small number of literatures have reported the thermally activated delayed fluorescence phenomenon of several quantum dot-organic molecule hybrid systems, their single photon energy is lower than that of blue light emission, and quantum dot systems with single photon energy up to 3.0 eV, which have more thermodynamic advantages in chemical reactions, have not been reported in the field of photocatalytic organic synthesis.

[0005] In view of this, the present invention designs a ZnSe@ZnS-organic molecule hybrid system with a long thermally activated delayed fluorescence lifetime and a single photon energy close to ultraviolet (~3.0eV), and performs efficient photocatalytic organic synthesis on specific substrate molecules based on the thermally activated delayed fluorescence mechanism. The present invention first achieves energy level matching between quantum dots and BCA intermediate molecules by controlling the particle size of ZnSe core quantum dots and the thickness of ZnS shell, constructs a ZnSe@ZnS-BCA thermally activated delayed fluorescence system, and further uses the system as a photocatalyst to perform ring closure and polymerization reactions on DAE and ACN substrate molecules, respectively. When the first exciton absorption peak of ZnSe@ZnS quantum dots is located at 405nm, under irradiation with 405nm continuous light with a power of 5mW, the quantum efficiency of the DAE molecule ring closure reaction is higher than 28.7% in the first 10s, and is as high as 60% in the initial reaction. The quantum efficiency of the ACN molecular polymerization reaction is higher than 13.5% in the first 10 seconds under the irradiation of a 405nm laser with a power of 110mW; the conversion rate can reach more than 70% in ~60 seconds. This scheme uses the quantum dot thermally activated delayed fluorescence process to photocatalyze the substrate molecules. Compared with directly using the triplet energy of the intermediate molecule for catalysis, it has higher single-photon energy and longer lifetime of the quantum dot excited state. At the same time, the substrate molecules do not need to be coordinated and bonded with the photocatalyst, and the selection range of substrate molecules is wider. Summary of the invention

[0006] The purpose of the present invention is to provide an efficient photocatalytic organic synthesis method utilizing the high single-photon energy of quantum dots. The thermally activated delayed fluorescence of quantum dots is achieved through the forward triplet energy transfer from quantum dots to molecules and the reverse triplet energy transfer from molecules to quantum dots under thermal activation. It has high single-photon energy and long excited state lifetime, and the reaction substrate is freely dispersed in the solvent without the need for coordination bonding with the photocatalyst, and can adapt to similar application scenarios requiring high single-photon energy and long excited state lifetime.

[0007] The scheme adopted by the present invention to achieve the purpose is: a method for efficient photocatalytic organic synthesis using the high single photon energy of quantum dots. Under visible light irradiation, a ZnSe@ZnS quantum dot-organic molecule hybrid system is used as a photocatalyst to achieve a high single photon energy and long-life excited state of quantum dots through its thermally activated delayed fluorescence mechanism, thereby performing efficient photocatalytic organic synthesis on substrate molecules.

[0008] Preferably, the thermally activated delayed fluorescence mechanism involves the triplet energy transfer from ZnSe@ZnS quantum dots to organic molecules in the ZnSe@ZnS quantum dot-organic molecule hybrid system under visible light and the reverse triplet energy transfer from organic molecules to quantum dots under thermal activation. Through the thermally activated delayed fluorescence mechanism, long exciton lifetimes of hundreds of microseconds or even milliseconds and high single-photon energies can be obtained, thereby catalyzing photochemical reactions of substrate molecules freely dispersed in the solvent.

[0009] Preferably, the ZnSe@ZnS quantum dots are of a core-shell structure, and the first exciton absorption peak thereof is at 405nm-430nm, corresponding to a ZnSe core particle size of 3.4nm-5.6nm; and the ZnS shell thickness is between 0.3nm-0.65nm.

[0010] Preferably, the triplet energy level of the organic molecule and the singlet energy level of the ZnSe@ZnS quantum dots differ by less than 0.3 eV.

[0011] Preferably, the organic molecule is a 4-biphenylcarboxylic acid (BCA) molecule, 9-fluorenone-2-carboxylic acid (FCA) or 9-phenanthrolinecarboxylic acid (9-PTA).

[0012] Preferably, the substrate molecule includes at least one of 1,2-bis(2,4-dimethyl-5-phenyl-thienyl)-3,3,4,4,5,5-hexafluoro-1-cyclopentene, acenaphthylene and derivatives thereof.

[0013] Preferably, the photocatalytic organic synthesis includes at least one of a ring-closing reaction, a ring-opening reaction, a polymerization reaction or a dehalogenation reaction of a substrate molecule.

[0014] Preferably, the photocatalytic organic synthesis is carried out in a non-polar organic solvent environment, and the non-polar organic solvent is at least one of n-hexane, toluene, cyclohexane and n-decane.

[0015] Preferably, the visible light wavelength range is 400nm-450nm.

[0016] In the present invention, by regulating the ZnSe particle size, ZnSe@ZnS and organic molecules form a reasonable energy level match, and by regulating the ZnS shell thickness to passivate the surface defects of ZnSe quantum dots, the ZnSe@ZnS-organic molecule system has the maximum single photon energy, the longest thermally activated delayed fluorescence lifetime and a higher fluorescence quantum yield, thereby achieving efficient photocatalytic organic synthesis. When the ZnSe particle size is 3.4nm and the ZnS shell thickness is 0.3nm, the quantum dot fluorescence lifetime is extended from 10ns to ~80μs, the single photon energy reaches ~3.0ev, and the fluorescence quantum yield is ~63%, which is the optimal solution for thermally activated delayed fluorescence of the ZnSe@ZnS-BCA system in the present invention. If the ZnSe particle size increases, the single photon energy of the quantum dots decreases, and the thermally activated delayed fluorescence efficiency decreases, thereby reducing the efficiency of photocatalytic organic synthesis; if the ZnS shell thickness increases, the efficiency of energy transfer between quantum dots and molecules will be reduced, and the efficiency of photochemical organic synthesis will also be reduced.

[0017] The present invention has the following advantages and beneficial effects:

[0018] The present invention photocatalyzes substrate molecules through the process of quantum dot thermally activated delayed fluorescence. Compared with directly utilizing the triplet energy of intermediate molecules for catalysis, it has higher single photon energy and longer lifetime of quantum dot excited state. At the same time, substrate molecules do not need to be coordinated and bonded with the photocatalyst, and the selection range of substrate molecules is wider.

[0019] The present invention realizes a long-life excited state with single photon energy close to ultraviolet (up to 3.0 eV) in a ZnSe@ZnS-organic molecule hybrid system based on the mechanism of thermally activated delayed fluorescence, and performs efficient photocatalytic organic synthesis on specific substrate molecules. Under the preferred embodiment, when the first exciton absorption peak of ZnSe@ZnS quantum dots is located at 405nm, under the irradiation of 405nm continuous light with a power of 5mW, the quantum efficiency of the DAE molecular ring-closing reaction is higher than 28.7% in the first 10s, and as high as 60% in the initial reaction. Under the irradiation of 405nm laser with a power of 110mW, the quantum efficiency of the ACN molecular polymerization reaction is higher than 13.5% in the first 10s; the conversion rate can reach more than 70% in 60s. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The schematic diagram of the thermally activated delayed fluorescence of the high single-photon energy ZnSe@ZnS-BCA system and its photocatalytic organic synthesis; where: TET is triplet energy transfer (or intersystem crossing); RTET is reverse triplet energy transfer (or reverse intersystem crossing); S0 is the ground state; S1 is the singlet excited state of the quantum dot; T1 is the triplet excited state of the BCA molecule;

[0021] Figure 2TEM images and size distribution of ZnSe core (a) and ZnSe@ZnS (b) in Example 1;

[0022] Figure 3 (a) Steady-state absorption spectra of ZnSe@ZnS quantum dots and BCA molecules under aerobic conditions and ZnSe@ZnS-BCA system under anaerobic conditions in Example 1; (b) Steady-state fluorescence spectra of ZnSe@ZnS quantum dots under aerobic conditions and ZnSe@ZnS-BCA system under aerobic and anaerobic conditions;

[0023] Figure 4 The time-resolved fluorescence of (a) ZnSe@ZnS quantum dots under aerobic conditions and ZnSe@ZnS-BCA system under anaerobic conditions in Example 1; (b) long-lived thermally activated delayed fluorescence of ZnSe@ZnS-BCA system under anaerobic conditions;

[0024] Figure 5 Steady-state absorption spectra of (a) ZnSe@ZnS-BCA / / DAE under 405nm excitation at 5mW and (b) ZnSe@ZnS-BCA / / ACN under 405nm excitation at 110mw after deducting the absorption of ZnSe@ZnS-BCA in Example 1, which vary with time; (c, d) quantum efficiency and conversion rate of photocatalytic organic synthesis of ZnSe@ZnS-BCA / / DAE and (e, f) ZnSe@ZnS-BCA / / ACN (including comparison with CsPbBr3-PTA system);

[0025] Figure 6 The single DAE (5 mW) and ACN (110 mW) substrate molecules did not react under 405 nm light. DETAILED DESCRIPTION

[0026] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0027] The preparation method of ZnSe@ZnS core-shell structure quantum dots is as follows:

[0028] (1) degassing a zinc source, oleic acid, oleylamine and octadecene and mixing them uniformly, injecting a diphenylphosphine solution of selenium powder Se-DPP into the mixture in an inert atmosphere at a certain temperature for several times and reacting the mixture for a certain time to obtain a solution containing ZnSe core quantum dots;

[0029] (2) After uniformly mixing the zinc stearate octadecene solution ZnSt2-ODE and the sulfur powder trioctylphosphine solution S-TOP, a syringe pump is used to inject the solution containing ZnSe core quantum dots obtained in step (1) at a rate of 2-4 mL / hour, and the reaction is carried out at a certain temperature to form a shell. After the reaction is completed, the supernatant is separated and precipitated multiple times to obtain the ZnSe@ZnS quantum dots.

[0030] In the step (1), the zinc source is at least one of Zn(Ac)2, ZnSt2, and ZnO, and the mixing temperature is 100-150°C.

[0031] In the step (1), the reaction temperature is 280-320° C. and the reaction time is 7-15 min.

[0032] The concentration range of Se-DPP is 80-110 mg / mL, the concentration of ZnSt2-ODE is 50-75 mg / mL, the concentration of S-TOP is 25-45 mg / mL, and the dosage ratio of the zinc source, oleic acid, oleylamine, octadecene, Se-DPP, ZnSt2-ODE, and S-TOP is 0.4588 g: 3 mL: 1 mL: 15 mL: 0.5 mL: 4-8 mL: 1-4 mL.

[0033] In the step (2), the reaction temperature is 260-310°C.

[0034] In the step (2), the precipitation step is to mix the supernatant, ethanol or acetone, ethyl acetate or methyl acetate in a volume ratio of 0.5-1:1:1 and then centrifuge to obtain a precipitate, and precipitate the supernatant after centrifugation multiple times according to the above method, and combine the obtained precipitates to obtain the ZnSe@ZnS quantum dots.

[0035] Using the high-efficiency photocatalytic organic synthesis method of quantum dots with high single-photon energy, the concentration of BCA intermediate molecules is controlled at an average bonding number of 400-600 per quantum dot, and the concentration of substrate molecules such as DAE and ACN are controlled at 1 to 2 mmol / L. DAE molecules and ACN substrate molecules undergo ring closure and polymerization reactions respectively.

[0036] In order to verify the efficient photocatalytic organic synthesis of the above thermally activated delayed fluorescence system under visible light irradiation, the verification scheme adopted by the present invention is as follows;

[0037] The particle size and shell thickness of ZnSe@ZnS quantum dots were determined by transmission electron microscopy, and the light absorption and emission properties of ZnSe@ZnS and its molecular hybrid system were characterized by steady-state absorption and fluorescence emission spectroscopy.

[0038] The thermally activated delayed fluorescence process in the ZnSe@ZnS-organic molecule system was characterized by time-resolved fluorescence and transient absorption spectroscopy.

[0039] The ring closure or polymerization reaction of the ZnSe@ZnS-organic molecule system to the reaction substrate molecules was characterized by steady-state absorption spectroscopy.

[0040] Figure 1 The figure shows the principle diagram of thermally activated delayed fluorescence of high single-photon energy ZnSe@ZnS-BCA system and its photocatalytic organic synthesis; among them: TET is triplet energy transfer (or intersystem crossing); RTET is reverse triplet energy transfer (or reverse intersystem crossing); S0 is the ground state; S1 is the singlet excited state of quantum dots; T1 is the triplet excited state of BCA molecules.

[0041] Example 1

[0042] The preparation and testing process of ZnSe@ZnS core-shell structure quantum dots is as follows:

[0043] 0.4588g Zn(Ac)2, 3mL oleic acid, 1mL oleylamine and 15mL octadecene (ODE) were added to a three-necked flask, and the temperature was raised to 120°C and maintained for 60 minutes under vacuum degassing conditions. Nitrogen was introduced into the flask and the solution was heated to 303°C, followed by rapid injection of 0.5mL Se-DPP (0.1888g Se powder and 2mL DPP were added to a 5mL glass bottle, and the glass bottle containing the reagents was ultrasonically placed on a hot plate at 100°C until the red solution became clear) in several times and the reaction was continued for about 9 minutes (the particle size of the obtained ZnSe core quantum dots was about 3.4nm measured by transmission electron microscopy); 4mL ZnSt2-ODE (0.2588g ZnSt2 and 4mL ODE were added to a 5mL glass bottle and ultrasonicated for 5 minutes to fully mix) and 1mL S-TOP (0.0385g S powder and 1ml TOP solution was added to a 5ml glass bottle, and ultrasonicated for 5 minutes to completely dissolve the yellow S powder to present a colorless solution) a total of 5mL of solution was mixed evenly in the glass bottle, and slowly injected into the solution containing ZnSe core quantum dots at a rate of 2.5mL / hour through a syringe pump. The temperature during the injection process was maintained at 280°C for reaction encapsulation. After the reaction was completed, the heater power was turned off, the heating jacket was removed, and the temperature was naturally cooled to below 60°C. Then the original solution in the flask was poured into a centrifuge tube, the centrifuge tube was placed in a centrifuge and centrifuged at 3000 rpm for 4 minutes, the supernatant was taken, and the supernatant: ethanol: ethyl acetate = 1:1:1 was added to the centrifuge tube, shaken well, and continued to be centrifuged at 10000 rpm for 3 minutes. The obtained precipitate was dissolved with 5mL of n-hexane, and the obtained The clear solution was centrifuged by adding the same amount of ethanol and ethyl acetate, and the obtained precipitate was added with 5 mL of n-hexane solvent. This operation was repeated 3 times. The obtained solution was the ZnSe@ZnS quantum dot solution (the particle size of the obtained ZnSe@ZnS quantum dot was about 4.0 nm and the ZnS shell thickness was about 0.3 nm measured by transmission electron microscopy). The ZnSe@ZnS quantum dot solution obtained above was placed in a 1 mm quartz cuvette to test the UV-visible absorption spectrum. The concentration of the quantum dots was determined by comparing the UV absorption spectrum. The first exciton absorption peak was located at 405 nm. When the concentration of the quantum dots was 1 umol / L, the absorbance at 380 nm was 0.5. According to the Lambert-Beer law, the concentration of the prepared quantum dots can be calculated to be 200 uM. The sample fluorescence emission spectrum and lifetime were tested by FLS980 fluorescence spectrometer, with an excitation wavelength of 380 nm and a detection wavelength of 413 nm. Under aerobic conditions, the fluorescence lifetime of the ZnSe@ZnS quantum dots was 10 ns.

[0044] The preparation and testing process of the ZnSe@ZnS-BCA thermally activated delayed fluorescence system is as follows:

[0045] Take 1ml of ZnSe@ZnS with an absorption value of about 0.2 in a 1mm cuvette and put it in a 2ml glass bottle, then add excess BCA (4-biphenylcarboxylic acid) powder, and filter after ultrasonication for 1min to obtain a ZnSe@ZnS-BCA system solution, then take 0.3ml of ZnSe@ZnS-BCA solution in a 5ml glass bottle. Add 2.7ml of n-hexane to the glass bottle, seal it and put it in a glove box filled with nitrogen under dark conditions, fully deoxygenate it for 20 minutes, and then put the solution into a 10mm cuvette. Put the sealed cuvette into the FLS980 fluorescence spectrometer, and test the fluorescence lifetime of the sample under anaerobic conditions, with 380nm excitation and 413nm detection wavelength. It is concluded that the thermally activated delayed fluorescence lifetime of ZnSe@ZnS quantum dots is ~80μs.

[0046] The process of photocatalytic organic synthesis and its spectral testing using ZnSe@ZnS-BCA system thermally activated delayed fluorescence (TADF) is as follows:

[0047] Ring-closing reaction of DAE (1,2-bis(2,4-dimethyl-5-phenyl-thienyl)-3,3,4,4,5,5-hexafluoro-1-cyclopentene) molecule (ZnSe@ZnS-BCA / / DAE): Take 1 ml of ZnSe@ZnS with an absorption value of about 0.2 in a 1 mm cuvette and put it in a 2 ml glass bottle, then add excess BCA powder, ultrasonicate for 1 min and filter to obtain the ZnSe@ZnS-BCA system solution, then take 0.3 ml of ZnSe@ZnS-BCA solution in a 5 ml glass bottle. After adding 1.7 ml of n-hexane to the glass bottle, add 1 ml of DAE solution (a mixed solution of 12 mg of DAE and 4.3 ml of n-hexane) under dark conditions. After sealing, put it in a glove box filled with nitrogen under dark conditions and deoxygenate it for 20 minutes. Then put the solution into a 10 mm cuvette and excite it with a 405 nm laser under dark conditions. The power of the excitation light is adjusted to 5 mW after passing through a cylindrical mirror. The duration of each irradiation is recorded in seconds. After each irradiation, shake the solution in the cuvette evenly and test the absorption spectrum.

[0048] Polymerization reaction of ACN (acenaphthylene) molecules (ZnSe@ZnS-BCA / / ACN): Take 1ml ZnSe@ZnS with an absorption value of about 0.2 in a 1mm cuvette and put it in a 2ml glass bottle, then add excess BCA powder, and filter after ultrasonication for 1min to obtain a ZnSe@ZnS-BCA system solution. Then take 0.2ml ZnSe@ZnS-BCA solution in a 1ml glass bottle, add 270ul n-hexane to the glass bottle, and add 30ul ACN solution (ACN 42mg and 8ml n-hexane mixed solution) into it under dark conditions. After sealing, put it in a glove box filled with nitrogen under dark conditions, deoxygenate it for 20 minutes, then put the solution into a 1mm cuvette, excite it with a 405nm laser under dark conditions, and adjust the power of the excitation light to 110mW after passing through a cylindrical mirror. The duration of each irradiation is recorded in seconds. After each illumination, shake the solution in the cuvette evenly and test the absorption spectrum.

[0049] Embodiment 2:

[0050] Except for the preparation of ZnSe@ZnS core-shell structure quantum dots, the remaining steps are the same as those in Example 1.

[0051] The preparation and testing process of ZnSe@ZnS core-shell structure quantum dots is as follows:

[0052] 0.4588g Zn(Ac)2, 3mL oleic acid, 1mL oleylamine and 15mL octadecene (ODE) were added to a three-necked flask, and the temperature was raised to 120°C and maintained for 60 minutes under vacuum degassing conditions. Nitrogen was introduced into the flask and the solution was heated to 303°C, followed by rapid injection of 0.5mL Se-DPP (0.1888g Se powder and 2mL DPP were added to a 5mL glass bottle, and the glass bottle containing the reagents was ultrasonically placed on a hot plate at 100°C until the red solution became clear) in several times and the reaction was continued for about 35 minutes (the particle size of the obtained ZnSe core quantum dots was about 4.4nm measured by transmission electron microscopy); 4mL ZnSt2-ODE (0.2588g ZnSt2 and 4mL ODE were added to a 5mL glass bottle and ultrasonicated for 5 minutes to fully mix) and 1mL S-TOP (0.0385g S powder and 1ml TOP solution was added to a 5ml glass bottle, and ultrasonicated for 5 minutes to completely dissolve the yellow S powder to present a colorless solution) a total of 5mL of solution was mixed evenly in the glass bottle, and slowly injected into the solution containing ZnSe core quantum dots at a rate of 2.5mL / hour through a syringe pump. The temperature during the injection process was maintained at 280°C for reaction encapsulation. After the reaction was completed, the heater power was turned off, the heating jacket was removed, and the temperature was naturally cooled to below 60°C. Then the original solution in the flask was poured into a centrifuge tube, the centrifuge tube was placed in a centrifuge and centrifuged at 3000 rpm for 4 minutes, the supernatant was taken, and the supernatant: ethanol: ethyl acetate = 1:1:1 was added to the centrifuge tube, shaken well, and continued to be centrifuged at 10000 rpm for 3 minutes. The obtained precipitate was dissolved with 5mL of n-hexane, and the obtained The clear solution was centrifuged by adding the same amount of ethanol and ethyl acetate, and the obtained precipitate was added with 5 mL of n-hexane solvent. This operation was repeated 3 times, and the obtained solution was the ZnSe@ZnS quantum dot solution (the particle size of the obtained ZnSe@ZnS quantum dot was about 5.0 nm and the ZnS shell thickness was about 0.3 nm measured by transmission electron microscopy). The ZnSe@ZnS quantum dot solution obtained above was placed in a 1 mm quartz cuvette to test the UV-visible absorption spectrum. The concentration of the quantum dots was determined by comparing the UV absorption spectrum. The first exciton absorption peak was located at 415 nm, and the absorbance at 380 nm was 0.5 when the concentration of the quantum dots was 1 umol / L. According to the Lambert-Beer law, the concentration of the prepared quantum dots can be calculated to be 200 uM. The fluorescence emission spectrum and lifetime of the sample were tested by FLS980 fluorescence spectrometer, with an excitation wavelength of 380 nm and a detection wavelength of 421 nm. It was concluded that the thermally activated delayed fluorescence lifetime of the ZnSe@ZnS quantum dots was ~70 μs.

[0053] Embodiment 3:

[0054] Except for the preparation of ZnSe@ZnS core-shell structure quantum dots, the remaining steps are the same as those in Example 1.

[0055] The preparation and testing process of ZnSe@ZnS core-shell structure quantum dots is as follows:

[0056] 0.4588g Zn(Ac)2, 3mL oleic acid, 1mL oleylamine and 15mL octadecene (ODE) were added to a three-necked flask, and the temperature was raised to 120°C and maintained for 60 minutes under vacuum degassing conditions. Nitrogen was introduced into the flask and the solution was heated to 303°C, followed by rapid injection of 0.5mL Se-DPP (0.1888g Se powder and 2mL DPP were added to a 5mL glass bottle, and the glass bottle containing the reagents was ultrasonically placed on a hot plate at 100°C until the red solution became clear) in several times and the reaction was continued for about 9 minutes (the particle size of the obtained ZnSe core quantum dots was about 3.4nm measured by transmission electron microscopy); 8mL ZnSt2-ODE (0.5176g ZnSt2 and 8mL ODE were added to a 10mL glass bottle and ultrasonicated for 5 minutes to fully mix) and 2mL S-TOP (0.077g S powder and 2ml TOP solution was added to a 5ml glass bottle, and ultrasonicated for 5 minutes to completely dissolve the yellow S powder to present a colorless solution) a total of 10mL of solution was mixed evenly in the glass bottle, and slowly injected into the solution containing ZnSe core quantum dots at a rate of 3.5mL / hour through a syringe pump. The temperature during the injection process was maintained at 280°C for reaction encapsulation. After the reaction was completed, the heater power was turned off, the heating jacket was removed, and the temperature was naturally cooled to below 60°C. Then the original solution in the flask was poured into a centrifuge tube, the centrifuge tube was placed in a centrifuge and centrifuged at 3000 rpm for 4 minutes, the supernatant was taken, and the supernatant: ethanol: ethyl acetate = 1:1:1 was added to the centrifuge tube, shaken well, and continued to be centrifuged at 10000 rpm for 3 minutes. The obtained precipitate was dissolved with 5mL of n-hexane, and the obtained The clear solution was centrifuged by adding the same amount of ethanol and ethyl acetate, and the obtained precipitate was added with 5 mL of n-hexane solvent. This operation was repeated 3 times, and the obtained solution was the ZnSe@ZnS quantum dot solution (the particle size of the obtained ZnSe / ZnS quantum dots was about 4.7 nm and the ZnS shell thickness was about 0.65 nm measured by transmission electron microscopy). The ZnSe@ZnS quantum dot solution obtained above was placed in a 1 mm quartz cuvette to test the UV-visible absorption spectrum. The concentration of the quantum dots was determined by comparing the UV absorption spectrum. The first exciton absorption peak was located at 405 nm, and the absorbance at 380 nm was 0.5 when the concentration of the quantum dots was 1 umol / L. According to the Lambert-Beer law, the concentration of the prepared quantum dots can be calculated to be 200 uM. The fluorescence emission spectrum and lifetime of the sample were tested by FLS980 fluorescence spectrometer, with an excitation wavelength of 380 nm and a detection wavelength of 413 nm. It was concluded that the thermally activated delayed fluorescence lifetime of the ZnSe@ZnS quantum dots was ~80 μs.

[0057] Comparative Example 1

[0058] This comparative example synthesizes the CsPbBr3-PTA system by the same method as the patent CN 117402026 A (a method for molecular isomerization based on perovskite nanocrystal sensitization), and uses the same parameters as the photocatalytic organic synthesis test in Example 1 to compare the efficiency of photocatalytic organic synthesis based on thermally activated delayed fluorescence of the ZnSe@ZnS-BCA system and photocatalytic organic synthesis based on triplet energy transfer of the CsPbBr3-PTA system. The quantum efficiency and conversion rate of the DAE molecule ring-closing reaction and the ACN molecule polymerization reaction using the thermally activated delayed fluorescence mechanism of the ZnSe@ZnS-BCA system in the present invention are higher than those of the CsPbBr3-PTA system ( Figure 5 ).

[0059] Figure 2 Shown are the transmission electron microscope images and size distribution of the ZnSe core (a) and ZnSe@ZnS (b) in Example 1; it can be seen from the figure that the size distribution of the quantum dots is relatively uniform; the particle size of the ZnSe core with the first exciton absorption at 405nm is about 3.4nm, and the size after being coated with the ZnS shell is about 4.0nm, and the thickness of the ZnS shell is about 0.3nm.

[0060] Figure 3 The following are the steady-state absorption spectra of (a) ZnSe@ZnS quantum dots, BCA molecules under aerobic conditions and ZnSe@ZnS-BCA system under anaerobic conditions in Example 1; (b) steady-state fluorescence spectra of ZnSe@ZnS quantum dots under aerobic conditions and ZnSe@ZnS-BCA system under aerobic and anaerobic conditions. It can be seen from Figure (a) that the absorption peak of quantum dots is at 405nm, and the absorption peak of BCA molecules is in the deep ultraviolet region. After ZnSe@ZnS quantum dots bridge BCA molecules, the absorption spectrum changes only in the deep ultraviolet region, indicating that the absorption characteristics of the ZnSe@ZnS-BCA system can be simply understood as ZnSe@ZnS. The superposition of the absorption characteristics of nSe@ZnS quantum dots and BCA molecules did not cause changes in other physical properties; in addition, according to the reference method, the fluorescence quantum yield of ZnSe@ZnS quantum dots was about 63%; as can be seen from Figure (b), the steady-state fluorescence of ZnSe@ZnS-BCA under aerobic conditions was significantly quenched compared with ZnSe@ZnS, while the steady-state fluorescence quenching of ZnSe@ZnS-BCA under anaerobic conditions was significantly weakened. The same fluorescence peak position indicates that the luminescent substance in the ZnSe@ZnS-BCA system is ZnSe@ZnS quantum dots, that is, there is a thermally activated delayed fluorescence process, and the fluorescence quantum yield of this process is ~19%.

[0061] Figure 4Shown are (a) the time-resolved fluorescence of ZnSe@ZnS quantum dots under aerobic conditions and ZnSe@ZnS-BCA system under anaerobic conditions in Example 1; (b) the long-lived thermally activated delayed fluorescence of ZnSe@ZnS-BCA system under anaerobic conditions. It can be seen from the figure that within 100ns, the fluorescence lifetime of ZnSe@ZnS-BCA under anaerobic conditions is significantly shortened compared with that under aerobic conditions, and at a delay time of the order of microseconds, long-lived fluorescence is only observed under anaerobic conditions, which proves the TET process between ZnSe@ZnS and BCA molecules and the RTET process between BCA and ZnSe@ZnS.

[0062] Figure 5 Shown are the steady-state absorption spectra of (a) ZnSe@ZnS-BCA / / DAE under 405nm excitation of 5 mW and (b) ZnSe@ZnS-BCA / / ACN changing with time under 405nm excitation of 110 mw after deducting the absorption of ZnSe@ZnS-BCA in Example 1; (c, d) quantum efficiency and conversion rate of photocatalytic organic synthesis of ZnSe@ZnS-BCA / / DAE and (e, f) ZnSe@ZnS-BCA / / ACN (including comparison diagrams with the CsPbBr3-PTA system in Comparative Example 1). It can be seen from the figure that under the optimal experimental conditions, the quantum efficiency and conversion rate of the photocatalytic reaction of DAE and ACN molecules by the ZnSe@ZnS-BCA system in Example 1 of the present invention are higher than those in Comparative Example 1, thereby achieving efficient photocatalytic organic synthesis.

[0063] Figure 6 It is shown that the single DAE (5 mW) and ACN (110 mW) substrate molecules do not react under 405 nm light.

[0064] Table 1 shows the spectrum and photocatalytic test results in Examples 1-3 and Comparative Example 1.

[0065] Table 1 Spectrum and photocatalytic test

[0066]

[0067]

[0068] The data in Table 1 show that the particle size and shell thickness of quantum dots in the ZnSe@ZnS-BCA system are the main factors affecting their single photon energy and photocatalytic organic synthesis efficiency. Comparing Examples 1 and 2, there is no significant difference in the intrinsic exciton lifetime of quantum dots and the thermally activated delayed fluorescence lifetime of the ZnSe@ZnS-BCA with the same ZnS shell thickness and different ZnSe particle sizes, but the thermally activated delayed fluorescence quantum yield of Example 1 with a small ZnSe particle size is significantly higher due to the higher single photon energy, and the photocatalytic organic synthesis efficiency is significantly higher than that of Example 2; Comparing Example 1 and Example 3, since the ZnS shell thickness in Example 3 is significantly increased, it has a significant hindering effect on the TET and RTET processes required to complete the thermally activated delayed fluorescence process, resulting in a significant decrease in the thermally activated delayed fluorescence quantum yield and photocatalytic organic synthesis efficiency in Example 3; Comparing Example 1 and Comparative Example 1, under the optimal experimental conditions, since the thermally activated delayed fluorescence of the ZnSe@ZnS-BCA system in Example 1 of the present invention is emitted by quantum dots (~3.0 eV), it has a higher single photon energy than the molecular triplet energy (~2.7 eV) in Comparative Example 1, and its fluorescence quantum yield and the quantum efficiency of the photocatalytic reaction for DAE and ACN molecules are both higher.

[0069] Under the above optimal scheme, under the irradiation of 405nm continuous light with a power of 5mW, the quantum efficiency of DAE molecular ring closure reaction is higher than 28.7% in the first 10s, and as high as 60% in the initial reaction. Under the irradiation of 405nm laser with a power of 110mW, the quantum efficiency of ACN molecular polymerization reaction is higher than 13.5% in the first 10s; the conversion rate can reach more than 70% in ~60s, and other parameters are better than those of comparative example 1.

[0070] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.

Claims

1. A highly efficient photocatalytic organic synthesis method using high single-photon energy of quantum dots, characterized in that: Under visible light irradiation, the ZnSe@ZnS quantum dot-organic molecule hybrid system is used as a photocatalyst to achieve high single-photon energy and long-life excited state of quantum dots through its thermally activated delayed fluorescence mechanism, thereby performing efficient photocatalytic organic synthesis of substrate molecules.

2. The method for efficient photocatalytic organic synthesis using high single-photon energy of quantum dots according to claim 1, characterized in that: The thermally activated delayed fluorescence mechanism involves the triplet energy transfer from ZnSe@ZnS quantum dots to organic molecules in the ZnSe@ZnS quantum dot-organic molecule hybrid system under visible light and the reverse triplet energy transfer from organic molecules to quantum dots under thermal activation. Through the thermally activated delayed fluorescence mechanism, long exciton lifetimes of hundreds of microseconds or even milliseconds and high single-photon energies can be obtained, thereby catalyzing photochemical reactions of substrate molecules freely dispersed in the solvent.

3. The method for efficient photocatalytic organic synthesis using high single-photon energy of quantum dots according to claim 1, characterized in that: The ZnSe@ZnS quantum dots are of a core-shell structure, and the first exciton absorption peak thereof is at 405nm-430nm, corresponding to a ZnSe core particle size of 3.4nm-5.6nm; and the ZnS shell thickness is between 0.3nm-0.65nm.

4. The method for efficient photocatalytic organic synthesis using high single-photon energy of quantum dots according to claim 1, characterized in that: The triplet energy level of the organic molecule and the singlet energy level of the ZnSe@ZnS quantum dot are less than 0.3 eV.

5. The method of highly efficient photocatalytic organic synthesis using high single photon energy of quantum dots according to claim 1, characterized in that: The organic molecule is a 4-biphenylcarboxylic acid molecule, 9-fluorenone-2-carboxylic acid or 9-phenanthrolinecarboxylic acid.

6. The method of highly efficient photocatalytic organic synthesis using high single photon energy of quantum dots according to claim 1, characterized in that: The substrate molecule includes at least one of 1,2-bis(2,4-dimethyl-5-phenyl-thienyl)-3,3,4,4,5,5-hexafluoro-1-cyclopentene, acenaphthylene and derivatives thereof.

7. The method for efficient photocatalytic organic synthesis using high single-photon energy of quantum dots according to claim 1, characterized in that: The photocatalytic organic synthesis includes at least one of a ring-closing reaction, a ring-opening reaction, a polymerization reaction or a dehalogenation reaction of substrate molecules.

8. The method of highly efficient photocatalytic organic synthesis using high single photon energy of quantum dots according to claim 1, characterized in that: The photocatalytic organic synthesis is in a non-polar organic solvent environment, and the non-polar organic solvent is at least one of n-hexane, toluene, cyclohexane, and n-decane.

9. The method of highly efficient photocatalytic organic synthesis using high single photon energy of quantum dots according to claim 1, characterized in that: The visible light wavelength range is 400nm-450nm.