Composite hydrogel as well as preparation method and application thereof

By preparing zinc nanoparticles in hydrogel and combining them with epigallocatechin gallate to form a composite hydrogel, the problem of zinc release and poor mechanical properties when the hydrogel is loaded with zinc is solved, achieving better results. Biocompatibility and mechanical properties, suitable for drug delivery and tissue engineering.

CN118745257AInactive Publication Date: 2024-10-08SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410749731.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When loading zinc, existing hydrogels have problems such as zinc release and migration, resulting in reduced loading rate, poor mechanical properties, and poor biocompatibility.

Method used

Zinc nanoparticles are prepared by dissolving zinc salt and 2-methylimidazole in organic solvents, combined with gelatin for cross-linking reaction, and combined with epigallocatechin gallate in a photoinitiator for ultraviolet irradiation to form a composite hydrogel, which enhances its mechanical properties.

Benefits of technology

It significantly improves the tensile strength, elongation at break and toughness of the hydrogel, enhances biocompatibility and mechanical stability, and is suitable for drug delivery and tissue engineering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745257A_ABST
    Figure CN118745257A_ABST
Patent Text Reader

Abstract

The invention discloses composite hydrogel as well as a preparation method and application thereof, and belongs to the technical field of medical hydrogel. The preparation method comprises the following steps: respectively dissolving zinc salt and 2-methylimidazole in an organic solvent to obtain a zinc salt solution and a 2-methylimidazole solution; mixing, stirring, centrifuging, washing and drying to obtain zinc nanoparticles; gelatin is dissolved in a buffer solution, methacrylic acid is added for a cross-linking reaction, dialysis and freeze-drying are carried out, and a methacrylic acid precursor is obtained; the preparation method comprises the following steps: sequentially adding a mixture of a methacrylic acid precursor, zinc nanoparticles and epigallocatechin gallate into a photoinitiator aqueous solution, uniformly mixing, putting into a mold, and performing ultraviolet irradiation to obtain the composite hydrogel. The invention also discloses the composite hydrogel prepared by the method and application of the composite hydrogel. The composite hydrogel prepared by the invention has better biocompatibility and mechanical property, and the preparation method is simple, lower in cost and wide in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of medical hydrogels, and in particular relates to a composite hydrogel and a preparation method and application thereof. Background Art

[0002] As a hydrophilic polymer material with a three-dimensional network structure, medical hydrogels have important application value in biomedical research fields such as drug transport and tissue engineering due to their unique water absorption and swelling properties, biocompatibility and controllable drug release properties. For example, they can be used as carriers of regenerative drugs, media for sustained drug release, and for peritoneal adhesion and hemostasis.

[0003] Hydrogels play a key role in the field of drug delivery. Technicians can accurately control the release rate, release time and release accuracy of drugs encapsulated in hydrogels by adjusting the cross-linking degree and preparation method of hydrogels, thereby meeting different treatment needs. This characteristic gives hydrogels unique advantages in treating chronic diseases, reducing drug side effects and improving patients' quality of life.

[0004] In recent years, researchers have been trying to compound hydrogels with other materials to improve the comprehensive performance of hydrogels. For example, zinc compounds are mixed with hydrogel raw materials to prepare composite hydrogels to achieve zinc loading on hydrogels. Zinc itself is a bioactive element, and loading it on hydrogels can achieve the multifunctionality of hydrogels. However, there are still many problems with directly loading zinc on hydrogels. During the placement of zinc-loaded hydrogels, zinc will gradually release or migrate from the hydrogel network, resulting in a decrease in loading rate and loss of functionality. In addition, most zinc-loaded hydrogels have poor mechanical properties, which can cause deformation or rupture of hydrogels in external pressure or stress environments. At the same time, when the concentration of zinc loading is too high, it may irritate and toxicize surrounding tissues and cells, making the biocompatibility of hydrogels poor. How to effectively unify the tensile strength, elongation at break and biophilicity of hydrogels is one of the technical difficulties that has not yet been solved. Summary of the invention

[0005] The problem to be solved by the present invention is to provide a composite hydrogel and a preparation method and application thereof, so as to solve the problems of poor biophilicity and mechanical properties of hydrogels in the prior art.

[0006] The technical solution adopted to solve the technical problem is to provide a method for preparing a composite hydrogel, comprising the following steps:

[0007] (1) dissolving a zinc salt and 2-methylimidazole in an organic solvent respectively to obtain a zinc salt solution and a 2-methylimidazole solution;

[0008] (2) mixing the zinc salt solution and the 2-methylimidazole solution, and centrifuging, washing and drying in sequence to obtain zinc nanoparticles;

[0009] (3) dissolving gelatin in a buffer solution and adding methacrylic acid to carry out a cross-linking reaction, followed by dialysis and freeze-drying to obtain a methacrylic acid precursor;

[0010] (4) mixing the zinc nanoparticles obtained in step (2) with epigallocatechin gallate; and sequentially adding the mixture of methacrylic acid precursor, zinc nanoparticles and epigallocatechin gallate into a photoinitiator aqueous solution, mixing well and placing in a mold, and irradiating with ultraviolet light to obtain a composite hydrogel.

[0011] The beneficial effects of the technical scheme adopted in the present invention are as follows: the composite hydrogel prepared by the present invention is composed of three core materials, namely, a hydrogel matrix, zinc nanoparticles and epigallocatechin gallate; the hydrogel matrix as a main carrier has good biocompatibility, biodegradability and high plasticity, but its strength decreases significantly after absorbing water, and its mechanical properties can be significantly improved by loading zinc nanoparticles and epigallocatechin gallate; the zinc nanoparticles themselves have biophilic activity, and the zinc nanoparticles prepared by the chemical precipitation method of the present invention have a cubic structure and a nanometer size, which can play a reinforcing role when loaded on the hydrogel, significantly improving the tensile strength, elongation at break and toughness of the hydrogel, so that it exhibits better mechanical stability when subjected to external force; epigallocatechin gallate can wrap the zinc nanoparticles on the hydrogel by interacting with the polymer chains in the hydrogel network, and at the same time mutually supports the zinc nanoparticles, providing an additional protective layer for the hydrogel body, enhancing the stability of the network structure, and thus effectively improving the mechanical properties of the composite hydrogel.

[0012] Preferably, the zinc salt is zinc nitrate, zinc sulfite, zinc sulfate or zinc chloride; and the organic solvent is methanol.

[0013] More preferably, the zinc salt is zinc nitrate.

[0014] Preferably, in step (1), the material-liquid ratio of zinc salt to organic solvent is 1 g: 6-8 mL; the material-liquid ratio of 2-methylimidazole to organic solvent is 1 g: 14-15 mL.

[0015] More preferably, in step (1), the material-liquid ratio of zinc salt to organic solvent is 2.57 g:18 mL; the material-liquid ratio of 2-methylimidazole to organic solvent is 5.68 g:82 mL.

[0016] Preferably, in step (2), the volume ratio of the zinc salt solution to the 2-methylimidazole solution is 1:4-5; the mixing time is 23-25 ​​hours; the centrifugal speed is 10000-12000 rpm, and the time is 5-7 minutes; washing is performed 2-3 times with methanol; the drying temperature is 50-70°C, and the time is 12-14 hours.

[0017] More preferably, in step (2), the volume ratio of the zinc salt solution to the 2-methylimidazole solution is 18:82; the mixing time is 24 hours; the centrifugal speed is 12000 rpm, and the time is 6 minutes; washing is performed 3 times with methanol; and the drying temperature is 60° C. and the time is 13 hours.

[0018] Preferably, the buffer in step (3) is a phosphate buffer solution; the solid-liquid ratio of gelatin to buffer is 1 g:8-12 mL; and the mass concentration of methacrylic acid in the methacrylic acid precursor is 6-9%.

[0019] More preferably, the solid-liquid ratio of gelatin to buffer is 1 g:10 mL; and the mass concentration of methacrylic acid in the methacrylic acid precursor is 8%.

[0020] Preferably, in step (3), the cross-linking reaction time is 1 to 3 hours, and the dialysis time is 160 to 170 hours.

[0021] More preferably, in step (3), the cross-linking reaction time is 2 h and the dialysis time is 168 h.

[0022] Preferably, the photoinitiator aqueous solution in step (4) is a photoinitiator Irgacure 2959 aqueous solution.

[0023] Preferably, in step (4), the mass ratio of zinc nanoparticles to epigallocatechin gallate in the mixture of zinc nanoparticles and epigallocatechin gallate is 2 to 3:1; the material-liquid ratio of the mixture of methacrylic acid precursor, zinc nanoparticles and epigallocatechin gallate and the photoinitiator aqueous solution is 1 g: 0.25 to 2 mg: 9 mL.

[0024] More preferably, in the mixture of zinc nanoparticles and epigallocatechin gallate in step (4), the mass ratio of zinc nanoparticles to epigallocatechin gallate is 2:1.

[0025] Preferably, in step (4), the ultraviolet irradiation power is 15 to 25 W and the time is 4 to 7 minutes.

[0026] More preferably, in step (4), the ultraviolet irradiation power is 20 W and the time is 5 min.

[0027] The invention also provides a composite hydrogel prepared by the preparation method.

[0028] The present invention also provides application of the composite hydrogel in preparing drug delivery materials.

[0029] The present invention has the following beneficial effects:

[0030] The composite hydrogel prepared by the present invention has good biocompatibility and mechanical properties, and can regulate the degradation rate of the hydrogel by changing the content of zinc nanoparticles, so that it can be more flexibly applied to drug delivery and tissue engineering; at the same time, the preparation method of the composite hydrogel of the present invention is simple and the production cost is relatively low. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is a TEM image of the zinc nanoparticles prepared in Example 1;

[0032] Figure 2 TEM images of the composite hydrogels prepared in Examples 1 to 4; wherein (a) is a TEM image of the composite hydrogel prepared in Example 1; (b) is a TEM image of the composite hydrogel prepared in Example 2; (c) is a TEM image of the composite hydrogel prepared in Example 3; (d) is a TEM image of the composite hydrogel prepared in Example 4;

[0033] Figure 3 is a CPX diagram of the binding energy of Zn 2p orbitals in the zinc nanoparticles prepared in Example 1;

[0034] Figure 4 It is the binding energy CPX diagram of C1s orbital and O1s orbital in the composite hydrogel prepared in Example 1; wherein (a) is the binding energy CPX diagram of C1s orbital in the composite hydrogel; (b) is the binding energy CPX diagram of O 1s orbital in the composite hydrogel. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.

[0036] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0037] The features and properties of the present invention are further described in detail below in conjunction with the examples. Epigallocatechin gallate was provided by Shandong Binzhou Zhiyuan Biotechnology Co., Ltd.

[0038] Example 1

[0039] A composite hydrogel is prepared by the following steps:

[0040] (1) Dissolve 2.57 g of zinc nitrate in 18 mL of methanol to obtain a zinc salt solution; dissolve 5.68 g of 2-methylimidazole in 82 mL of methanol to obtain a 2-methylimidazole solution;

[0041] (2) 18 mL of zinc salt solution and 82 mL of 2-methylimidazole solution were mixed and stirred for 24 h, and then centrifuged at 12000 rpm for 6 min to collect the precipitate, and the precipitate was washed with methanol three times and then dried in an oven at 60° C. for 13 h to obtain zinc nanoparticles;

[0042] (3) 2 g of gelatin was dissolved in 20 mL of phosphate buffer and stirred evenly, and 1.91 g of methacrylic acid was slowly added dropwise to carry out cross-linking reaction at a constant temperature for 2 h, and then dialyzed in deionized water for 168 h and then freeze-dried to obtain a methacrylic acid precursor; the mass concentration of methacrylic acid in the methacrylic acid precursor was 8%;

[0043] (4) The zinc nanoparticles obtained in step (2) are mixed with epigallocatechin gallate, wherein the mass ratio of the zinc nanoparticles to epigallocatechin gallate in the mixture is 2:1; and 0.9 g of methacrylic acid precursor, 0.225 mg of the mixture of zinc nanoparticles and epigallocatechin gallate are sequentially added to 8.1 mL of an aqueous solution of a photoinitiator Irgacure 2959, mixed evenly, and placed in a mold, and irradiated with ultraviolet light at 20 W for 5 min to obtain a composite hydrogel.

[0044] Example 2

[0045] (1) Dissolve 2.57 g of zinc nitrate in 18 mL of methanol to obtain a zinc salt solution; dissolve 5.68 g of 2-methylimidazole in 82 mL of methanol to obtain a 2-methylimidazole solution;

[0046] (2) 18 mL of zinc salt solution and 82 mL of 2-methylimidazole solution were mixed and stirred for 24 h, and then centrifuged at 12000 rpm for 6 min to collect the precipitate, and the precipitate was washed with methanol three times and then dried in an oven at 60° C. for 13 h to obtain zinc nanoparticles;

[0047] (3) 2 g of gelatin was dissolved in 20 mL of phosphate buffer and stirred evenly, and 1.91 g of methacrylic acid was slowly added dropwise to carry out cross-linking reaction at a constant temperature for 2 h, and then dialyzed in deionized water for 168 h and then freeze-dried to obtain a methacrylic acid precursor; the mass concentration of methacrylic acid in the methacrylic acid precursor was 8%;

[0048] (4) The zinc nanoparticles obtained in step (2) are mixed with epigallocatechin gallate, wherein the mass ratio of the zinc nanoparticles to epigallocatechin gallate in the mixture is 2:1; and 0.9 g of methacrylic acid precursor, 0.45 mg of the mixture of zinc nanoparticles and epigallocatechin gallate are sequentially added to 8.1 mL of an aqueous solution of a photoinitiator Irgacure 2959, mixed evenly, and placed in a mold, and irradiated with ultraviolet light at 20 W for 5 min to obtain a composite hydrogel.

[0049] Example 3

[0050] (1) Dissolve 2.57 g of zinc nitrate in 18 mL of methanol to obtain a zinc salt solution; dissolve 5.68 g of 2-methylimidazole in 82 mL of methanol to obtain a 2-methylimidazole solution;

[0051] (2) 18 mL of zinc salt solution and 82 mL of 2-methylimidazole solution were mixed and stirred for 24 h, and then centrifuged at 12000 rpm for 6 min to collect the precipitate, and the precipitate was washed with methanol three times and then dried in an oven at 60° C. for 13 h to obtain zinc nanoparticles;

[0052] (3) 2 g of gelatin was dissolved in 20 mL of phosphate buffer and stirred evenly, and 1.91 g of methacrylic acid was slowly added dropwise to carry out cross-linking reaction at a constant temperature for 2 h, and then dialyzed in deionized water for 168 h and then freeze-dried to obtain a methacrylic acid precursor; the mass concentration of methacrylic acid in the methacrylic acid precursor was 8%;

[0053] (4) The zinc nanoparticles obtained in step (2) are mixed with epigallocatechin gallate, wherein the mass ratio of the zinc nanoparticles to epigallocatechin gallate in the mixture is 2:1; and 0.9 g of a methacrylic acid precursor, 0.9 mg of the mixture of the zinc nanoparticles and epigallocatechin gallate are sequentially added to 8.1 mL of an aqueous solution of a photoinitiator Irgacure 2959, mixed evenly, and placed in a mold, and irradiated with ultraviolet light at 20 W for 5 min to obtain a composite hydrogel.

[0054] Example 4

[0055] (1) Dissolve 2.57 g of zinc nitrate in 18 mL of methanol to obtain a zinc salt solution; dissolve 5.68 g of 2-methylimidazole in 82 mL of methanol to obtain a 2-methylimidazole solution;

[0056] (2) 18 mL of zinc salt solution and 82 mL of 2-methylimidazole solution were mixed and stirred for 24 h, and then centrifuged at 12000 rpm for 6 min to collect the precipitate, and the precipitate was washed with methanol three times and then dried in an oven at 60° C. for 13 h to obtain zinc nanoparticles;

[0057] (3) 2 g of gelatin was dissolved in 20 mL of phosphate buffer and stirred evenly, and 1.91 g of methacrylic acid was slowly added dropwise to carry out cross-linking reaction at a constant temperature for 2 h, and then dialyzed in deionized water for 168 h and then freeze-dried to obtain a methacrylic acid precursor; the mass concentration of methacrylic acid in the methacrylic acid precursor was 8%;

[0058] (4) The zinc nanoparticles obtained in step (2) are mixed with epigallocatechin gallate, wherein the mass ratio of the zinc nanoparticles to epigallocatechin gallate in the mixture is 2:1; and 0.9 g of methacrylic acid precursor, 1.8 mg of the mixture of zinc nanoparticles and epigallocatechin gallate are sequentially added to 8.1 mL of an aqueous solution of a photoinitiator Irgacure 2959, mixed evenly, and placed in a mold, and irradiated with ultraviolet light at 20 W for 5 min to obtain a composite hydrogel.

[0059] Comparative Example 1

[0060] A hydrogel is prepared by the following steps:

[0061] (1) 2 g of gelatin was dissolved in 20 mL of phosphate buffer and stirred evenly, and 1.91 g of methacrylic acid was slowly added dropwise to carry out cross-linking reaction at a constant temperature for 2 h, and then dialyzed in deionized water for 168 h and then freeze-dried to obtain a methacrylic acid precursor; the mass concentration of methacrylic acid in the methacrylic acid precursor was 8%;

[0062] (2) 0.9 g of methacrylic acid precursor was added to 8.1 mL of photoinitiator Irgacure 2959 aqueous solution, mixed evenly and placed in a mold. After irradiation with ultraviolet light at 20 W for 5 min, a hydrogel was obtained.

[0063] Comparative Example 2

[0064] A composite hydrogel is prepared by the following steps:

[0065] (1) Dissolve 2.57 g of zinc nitrate in 18 mL of methanol to obtain a zinc salt solution; dissolve 5.68 g of 2-methylimidazole in 82 mL of methanol to obtain a 2-methylimidazole solution;

[0066] (2) 18 mL of zinc salt solution and 82 mL of 2-methylimidazole solution were mixed and stirred for 24 h, and then centrifuged at 12000 rpm for 6 min to collect the precipitate, and the precipitate was washed with methanol three times and then dried in an oven at 60° C. for 13 h to obtain zinc nanoparticles;

[0067] (3) 2 g of gelatin was dissolved in 20 mL of phosphate buffer and stirred evenly, and 1.91 g of methacrylic acid was slowly added dropwise to carry out cross-linking reaction at a constant temperature for 2 h, and then dialyzed in deionized water for 168 h and then freeze-dried to obtain a methacrylic acid precursor; the mass concentration of methacrylic acid in the methacrylic acid precursor was 8%;

[0068] (4) 0.9 g of methacrylic acid precursor and 0.225 mg of zinc nanoparticles were added to 8.1 mL of photoinitiator Irgacure 2959 aqueous solution, mixed evenly and placed in a mold. After ultraviolet irradiation at 20 W for 5 min, a composite hydrogel was obtained.

[0069] Experimental example

[0070] The composite hydrogels prepared in Examples 1 to 4 were tested, and the results were as follows: Figures 1 to 4 shown.

[0071] Transmission electron microscopy (TEM) was used to characterize the morphology of zinc nanoparticles and composite hydrogels. Figures 1-2 shown; from Figure 1 It can be seen that the zinc nanoparticles prepared in the present invention have a clear cubic appearance, are uniform in size and are homogeneously distributed; Figure 2 It can be seen that the zinc nanoparticles and epigallocatechin gallate (EGCG) in the composite hydrogels prepared in Examples 1 to 4 are closely attached to the surface of the hydrogel. As the amount of the mixture of zinc nanoparticles and epigallocatechin gallate gradually increases, the zinc nanoparticles and epigallocatechin gallate on the surface of the composite hydrogel gradually increase and are evenly distributed.

[0072] The binding energy of the Zn 2p orbital in the zinc nanoparticles prepared in Example 1 and the binding energy of the C1s orbital and the O1s orbital in the composite hydrogel were detected using X-ray photoelectron spectroscopy (XPS). Figures 3-4 As shown. Figure 3 It can be seen from the figure that the binding energy of the Zn 2p orbital of the zinc nanoparticles prepared in Example 1 fits the Zn2p theoretical value corresponding to the standard spectrum, and it is preliminarily judged that the Zn nanoparticles are successfully prepared; Figure 4 It can be seen that the binding energies of the C1s orbital and the O1s orbital in the composite hydrogel prepared in Example 1 are both fitted with the theoretical values ​​corresponding to the standard spectrum, indicating that the hydrogel of the present invention has good molding degree and good strength.

[0073] The mechanical properties of the hydrogels prepared in Example 1 and Comparative Examples 1-2 were tested, and the results are shown in Table 1.

[0074] Table 1 Mechanical properties test results of hydrogel

[0075] Tensile strength / Mpa Elongation at break / % Compression strain / % Example 1 4.3 1347 99 Comparative Example 1 0.1 40 81 Comparative Example 2 1.2 122 90

[0076] As can be seen from Table 1, the tensile strength, elongation at break and compressive strain of the composite hydrogel prepared in the present application are significantly better than those of the hydrogels prepared in Comparative Examples 1 to 2, indicating that the main hydrogel matrix without any substance loaded has poor strength, and although the mechanical strength is improved to a certain extent after only loading zinc nanoparticles on the main hydrogel matrix, it still does not reach the ideal level; and the tensile strength, elongation at break and compressive strain of the composite hydrogel prepared after simultaneously loading zinc nanoparticles and epigallocatechin gallate are significantly increased, which is because the zinc nanoparticles and epigallocatechin gallate produce a synergistic effect on the matrix hydrogel, and epigallocatechin gallate interacts with the polymer chains in the hydrogel network to wrap the zinc nanoparticles on the hydrogel, and at the same time supports each other with the zinc nanoparticles, providing an additional protective layer for the hydrogel body, enhancing the stability of the network structure, thereby effectively improving the mechanical properties of the composite hydrogel.

[0077] The present invention has been described according to the above embodiments. It should be understood that the above embodiments do not limit the present invention in any form. Any technical solutions obtained by equivalent replacement or equivalent transformation shall fall within the scope of the present invention.

Claims

1. A method for preparing a composite hydrogel, It is characterized in that The following steps are involved: (1) dissolving a zinc salt and 2-methylimidazole in an organic solvent respectively to obtain a zinc salt solution and a 2-methylimidazole solution; (2) mixing the zinc salt solution and the 2-methylimidazole solution, and centrifuging, washing and drying in sequence to obtain zinc nanoparticles; (3) dissolving gelatin in a buffer solution and adding methacrylic acid to carry out a cross-linking reaction, followed by dialysis and freeze-drying to obtain a methacrylic acid precursor; (4) mixing the zinc nanoparticles obtained in step (2) with epigallocatechin gallate; and sequentially adding the mixture of methacrylic acid precursor, zinc nanoparticles and epigallocatechin gallate into a photoinitiator aqueous solution, mixing well and placing in a mold, and irradiating with ultraviolet light to obtain a composite hydrogel.

2. The method for preparing the composite hydrogel according to claim 1, It is characterized in that The zinc salt is zinc nitrate, zinc sulfite, zinc sulfate or zinc chloride; and the organic solvent is methanol.

3. A method for preparing the composite hydrogel according to claim 1 or 2, It is characterized in that In the step (1), the material-liquid ratio of the zinc salt to the organic solvent is 1 g: 6-8 mL; the material-liquid ratio of the 2-methylimidazole to the organic solvent is 1 g: 14-15 mL.

4. The method for preparing the composite hydrogel according to claim 1, It is characterized in that In the step (2), the volume ratio of the zinc salt solution to the 2-methylimidazole solution is 1:4-5; the mixing and stirring time is 23-25 ​​hours; the centrifugal speed is 10000-12000 rpm, and the time is 5-7 minutes; the washing is performed with methanol for 2-3 times; the drying temperature is 50-70°C, and the time is 12-14 hours.

5. The method for preparing the composite hydrogel according to claim 1, It is characterized in that The buffer solution in step (3) is a phosphate buffer solution; the solid-liquid ratio of the gelatin to the buffer solution is 1 g:8-12 mL; and the mass concentration of methacrylic acid in the methacrylic acid precursor is 6-9%.

6. The method for preparing the composite hydrogel according to claim 1, It is characterized in that In the step (3), the cross-linking reaction time is 1 to 3 hours, and the dialysis time is 160 to 170 hours.

7. The method for preparing the composite hydrogel according to claim 1, It is characterized in that In the step (4), the mass ratio of zinc nanoparticles to epigallocatechin gallate in the mixture of zinc nanoparticles and epigallocatechin gallate is 2 to 3:1; the material-liquid ratio of the mixture of methacrylic acid precursor, zinc nanoparticles and epigallocatechin gallate and the photoinitiator aqueous solution is 1 g: 0.25 to 2 mg: 9 mL.

8. The method for preparing the composite hydrogel according to claim 1, It is characterized in that The ultraviolet irradiation power in step (4) is 15 to 25 W, and the time is 4 to 7 minutes.

9. A composite hydrogel prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the composite hydrogel according to claim 9 in preparing drug delivery materials.