Corrosion-resistant crosslinked polyethylene insulated power cable and production process thereof
By using a specific combination of materials and processes in the cable sheath layer, the problem of poor corrosion resistance of the cable is solved, the tensile strength and corrosion resistance of the cable are improved, the service life is extended and the safety is improved.
Patent Information
- Application Number
- CN202411130348.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-08
AI Technical Summary
During the use of power cables, due to the influence of environmental factors, the sheath layer is easily thinned or damaged, resulting in a decrease in the mechanical properties of the cable, affecting the service life and causing safety hazards.
Using a sheath layer material composed of polyethylene resin, ethylene-vinyl acetate copolymer, inorganic fillers, cross-linking agents, antioxidants and dispersants (containing carbonyl compounds and sodium methyl lauroyl taurate), through specific Mass ratio and process treatment improve the tensile strength, elongation at break and corrosion resistance of the cable.
It effectively improves the corrosion resistance of the cable, extends its service life, improves safety, and reduces maintenance costs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of power cables, and in particular to a corrosion-resistant cross-linked polyethylene insulated power cable and a production process thereof. Background Art
[0002] Electricity is the cornerstone of today's society. With the continuous development of social economy, the demand for electricity is also increasing. In the process of power transmission, power cables are one of the infrastructures connecting power stations, substations and end users. Cross-linked polyethylene insulation material has a high dielectric constant and dielectric strength, exhibits good electrical properties in power cables, and is widely used in the manufacture of power cables. However, during the use of power cables, due to the influence of soil properties, humidity and chemicals in the environment, the sheath layer of the power cable will become thinner or damaged, resulting in a decrease in the mechanical properties of the cable, affecting the service life of the power cable and bringing safety hazards. Therefore, it is necessary to provide a corrosion-resistant cross-linked polyethylene insulated power cable. Summary of the invention
[0003] The invention provides a corrosion-resistant cross-linked polyethylene insulated power cable and a production process thereof, which solves the problem of poor corrosion resistance of the power cable in the related art.
[0004] The technical solution of the present invention is as follows: The invention provides a corrosion-resistant cross-linked polyethylene insulated power cable, which comprises a cable core, an insulating layer and a sheath layer from the inside to the outside, wherein the sheath layer comprises the following raw materials in parts by weight: 100 parts of polyethylene resin, 40-50 parts of ethylene-vinyl acetate copolymer, 20-25 parts of inorganic filler, 1.5-2.5 parts of cross-linking agent, 1-2 parts of antioxidant, 1-3 parts of plasticizer, and 6-8 parts of dispersant, wherein the dispersant consists of a carbonyl compound and sodium methyl lauroyl taurate.
[0005] As a further technical solution, the carbonyl-containing compound includes one of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and oxidized polyethylene wax.
[0006] As a further technical solution, the mass ratio of the carbonyl-containing compound to sodium methyl lauroyl taurate is 1:1-5.
[0007] As a further technical solution, the mass ratio of the carbonyl-containing compound to sodium methyl lauroyl taurate is 1:2.
[0008] As a further technical solution, the carbonyl-containing compound is 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride.
[0009] As a further technical solution, the polyethylene resin consists of a first polyethylene resin and a second polyethylene resin, and the first polyethylene resin and the second polyethylene resin have different melt flow rates.
[0010] As a further technical solution, the melt flow rate of the first polyethylene resin is 25.7 g / 10 min, and the melt flow rate of the second polyethylene resin is 7 g / 10 min.
[0011] In the present invention, the polyethylene resin is composed of two polyethylene resins with different melt flow rates. The composite material formed by the combination is superior to the addition of a single polyethylene resin and can further improve the tensile strength, elongation at break and corrosion resistance of the cable.
[0012] As a further technical solution, the mass ratio of the first polyethylene resin to the second polyethylene resin is 1:8-12.
[0013] The present invention finds that by limiting the mass ratio of the first polyethylene resin to the second polyethylene resin to 1:8-12, the processing performance of the cable sheath layer can be better improved, and the tensile strength, elongation at break and corrosion resistance of the cable can be further improved.
[0014] As a further technical solution, the mass ratio of the first polyethylene resin to the second polyethylene resin is 1:10.
[0015] As a further technical solution, the inorganic filler includes one or both of silicon dioxide and talc.
[0016] As a further technical solution, the particle size of the inorganic filler is 600-1200 mesh.
[0017] As a further technical solution, the cross-linking agent includes one or more of dicumyl peroxide, benzoyl peroxide and dicumyl hydroperoxide.
[0018] As a further technical solution, the plasticizer includes one or more of dibutyl phthalate, dioctyl phthalate, and triphenyl phosphate.
[0019] As a further technical solution, the antioxidant includes one or more of antioxidant 1010, antioxidant 264 and antioxidant B215.
[0020] The present invention also proposes a production process for a corrosion-resistant cross-linked polyethylene insulated power cable, comprising the following steps: S1. Wrapping the insulating layer on the cable core to obtain a semi-finished power cable; S2. After the raw materials of the sheath layer are evenly mixed, they are extruded and coated on the outside of the semi-finished power cable to obtain the power cable.
[0021] The working principle and beneficial effects of the present invention are: In the present invention, polyethylene and ethylene-vinyl acetate copolymer are used as base materials, both of which have excellent electrical properties, physical properties and chemical stability. The two are matched with each other to better improve the mechanical properties and corrosion resistance of the sheath layer, and a dispersant composed of a carbonyl compound and sodium methyl lauroyl taurate is added to further improve the mechanical properties and corrosion resistance of the sheath layer, effectively improve the situation that the mechanical properties of the cable are reduced due to the thinning or damage of the sheath layer caused by the poor corrosion resistance of the power cable, resulting in a reduction in the service life of the power cable, improve the safety of the power cable, better protect the safety of people and property, and reduce maintenance costs. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In the following examples and comparative examples: LF2700 polyethylene resin, melt flow rate 25.7g / 10min, Shanghai Petrochemical; 955 polyethylene resin, melt flow rate 7.0g / 10min, Hanwha, South Korea; LD608 polyethylene resin, melt flow rate 6.0g / 10min, Yanshan Petrochemical; 868-000 polyethylene resin, melt flow rate 49.3g / 10min, Maoming Petrochemical; Ethylene-vinyl acetate copolymer, model 2050, Hanwha, South Korea; Oxidized polyethylene wax, model AC316A, Honeywell, USA.
[0024] Example 1 A method for preparing a corrosion-resistant cross-linked polyethylene insulated power cable comprises the following steps: S1. Wrapping the insulating layer on the cable core to obtain a semi-finished power cable; S2. Mix 100 parts of 955 polyethylene resin, 40 parts of ethylene-vinyl acetate copolymer, 20 parts of talc (particle size 600 mesh), 1.5 parts of diisopropyl peroxide, 1 part of antioxidant 1010, 1 part of dibutyl phthalate and 4 parts of dispersant evenly, extrude and coat the mixture on the outside of a semi-finished power cable to obtain a power cable; wherein the dispersant is composed of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate in a mass ratio of 2:1.
[0025] Example 2 A method for preparing a corrosion-resistant cross-linked polyethylene insulated power cable comprises the following steps: S1. Wrapping the insulating layer on the cable core to obtain a semi-finished power cable; S2. Mix 100 parts of 955 polyethylene resin, 45 parts of ethylene-vinyl acetate copolymer, 22 parts of talc (particle size 800 mesh), 2 parts of benzoyl peroxide, 1.5 parts of antioxidant 264, 2 parts of dioctyl phthalate and 5 parts of dispersant evenly, extrude and coat the mixture on the outside of a semi-finished power cable to obtain a power cable; wherein the dispersant is composed of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate in a mass ratio of 2:1.
[0026] Example 3 A method for preparing a corrosion-resistant cross-linked polyethylene insulated power cable comprises the following steps: S1. Wrapping the insulating layer on the cable core to obtain a semi-finished power cable; S2. After uniformly mixing 100 parts of 955 polyethylene resin, 50 parts of ethylene-vinyl acetate copolymer, 25 parts of talc (particle size 1200 mesh), 2.5 parts of diisopropylbenzene hydroperoxide, 2 parts of antioxidant B215, 3 parts of triphenyl phosphate and 6 parts of dispersant, the mixture is extruded and coated on the outside of a semi-finished power cable to obtain a power cable; wherein the dispersant is composed of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate in a mass ratio of 2:1.
[0027] Example 4 The only difference between this embodiment and embodiment 1 is that the dispersant is composed of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate in a mass ratio of 1:6.
[0028] Example 5 The only difference between this embodiment and embodiment 1 is that the dispersant is composed of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate in a mass ratio of 1:1.
[0029] Example 6 The only difference between this embodiment and embodiment 1 is that the dispersant is composed of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate in a mass ratio of 1:2.
[0030] Example 7 The only difference between this embodiment and embodiment 1 is that the dispersant is composed of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate in a mass ratio of 1:5.
[0031] Example 8 The only difference between this embodiment and embodiment 1 is that the 955 polyethylene resin is replaced by an equal amount of LF2700 polyethylene resin.
[0032] Example 9 The only difference between this embodiment and embodiment 1 is that the 955 polyethylene resin is replaced with equal amounts of LF2700 polyethylene resin and 955 polyethylene resin in a mass ratio of 1:8.
[0033] Example 10 The only difference between this embodiment and embodiment 1 is that the 955 polyethylene resin is replaced with equal amounts of LF2700 polyethylene resin and 955 polyethylene resin in a mass ratio of 1:10.
[0034] Embodiment 11 The only difference between this embodiment and embodiment 1 is that the 955 polyethylene resin is replaced with equal amounts of LF2700 polyethylene resin and 955 polyethylene resin in a mass ratio of 1:12.
[0035] Example 12 The only difference between this embodiment and embodiment 9 is that the 955 polyethylene resin is replaced by an equal amount of LD608 polyethylene resin.
[0036] Embodiment 13 The only difference between this embodiment and embodiment 9 is that the LF2700 polyethylene resin is replaced by an equal amount of 868-000 polyethylene resin.
[0037] Embodiment 14 The only difference between this embodiment and embodiment 1 is that 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride is replaced by an equal amount of oxidized polyethylene wax.
[0038] Comparative Example 1 The only difference between this comparative example and Example 1 is that the dispersant is 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride.
[0039] Comparative Example 2 The only difference between this comparative example and Example 1 is that the dispersant is sodium methyl lauroyl taurate.
[0040] Test example The sheath layer of the power cable prepared in Examples 1 to 14 and Comparative Examples 1 to 2 was tested for tensile strength and elongation at break according to GB / T 2951.11-2008 "General test methods for insulation and sheath materials of electric and optical cables Part 11: General test methods - Thickness and dimensions measurement - Mechanical properties test", and a corrosion resistance test was performed. The specific test method is as follows: the sample is placed in a 50wt% sulfuric acid aqueous solution and immersed at 25°C for 30d, and the tensile strength and elongation at break after immersion are measured, and the change rate of tensile strength and the change rate of elongation at break are calculated, wherein the change rate of tensile strength = (tensile strength after test / tensile strength before test-1) × 100%, and the change rate of elongation at break = (elongation at break after test / elongation at break before test-1) × 100%. The measurement results are shown in Table 1.
[0041] Table 1 Performance measurement results of power cables of Examples 1 to 14 and Comparative Examples 1 to 2
[0042] Compared with Example 1, Example 14 replaces 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride with an equal amount of oxidized polyethylene wax, the dispersant in Comparative Example 1 is 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride, and the dispersant in Comparative Example 2 is sodium methyl lauroyl taurate. As a result, the tensile strength, elongation at break and corrosion resistance of the cable sheath layer in Example 14 and Comparative Examples 1~2 are lower than those in Example 1, indicating that when the dispersant is composed of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate, the tensile strength, elongation at break and corrosion resistance of the cable can be further improved.
[0043] Compared with Example 1, the mass ratio of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate was changed in Examples 4 to 7. As a result, the tensile strength, elongation at break and corrosion resistance of the cables in Examples 5 to 7 were better than those in Example 4 and Example 1, indicating that when the mass ratio of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and sodium methyl lauroyl taurate was 1:1 to 5, the tensile strength, elongation at break and corrosion resistance of the cable could be further improved.
[0044] Compared with Example 1, Example 8 changes the model of polyethylene resin, and the polyethylene resins in Examples 9 to 13 are composed of polyethylene resins with different melt flow rates. As a result, the tensile strength, elongation at break and corrosion resistance of the cables in Examples 9 to 11 are better than those in Example 1, Example 8, and Examples 12 to 13, indicating that when the polyethylene resin is composed of LF2700 polyethylene resin and 955 polyethylene resin, the tensile strength, elongation at break and corrosion resistance of the cable can be further improved.
[0045] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A corrosion-resistant cross-linked polyethylene insulated power cable, characterized in that: From the inside to the outside, there are cable core, insulation layer and sheath layer. The sheath layer includes the following raw materials in parts by weight: 100 parts of polyethylene resin, 40-50 parts of ethylene-vinyl acetate copolymer, 20-25 parts of inorganic filler, 1.5-2.5 parts of cross-linking agent, 1-2 parts of antioxidant, 1-3 parts of plasticizer, 6-8 parts of dispersant, and the dispersant is composed of carbonyl compound and sodium methyl lauroyl taurate.
2. A corrosion-resistant cross-linked polyethylene insulated power cable according to claim 1, characterized in that: The carbonyl-containing compound includes one of 3-(2-chlorocarbonyl-ethyldisulfonyl)-propionyl chloride and oxidized polyethylene wax.
3. The corrosion-resistant cross-linked polyethylene insulated power cable according to claim 1, characterized in that: The polyethylene resin consists of a first polyethylene resin and a second polyethylene resin, and the first polyethylene resin and the second polyethylene resin have different melt flow rates.
4. The corrosion-resistant cross-linked polyethylene insulated power cable according to claim 3, characterized in that: The melt flow rate of the first polyethylene resin is 25.7 g / 10 min, and the melt flow rate of the second polyethylene resin is 7 g / 10 min.
5. The corrosion-resistant cross-linked polyethylene insulated power cable according to claim 4, characterized in that: The mass ratio of the first polyethylene resin to the second polyethylene resin is 1:8-12.
6. The corrosion-resistant cross-linked polyethylene insulated power cable according to claim 1, characterized in that: The inorganic filler includes one or both of silicon dioxide and talc.
7. The corrosion-resistant cross-linked polyethylene insulated power cable according to claim 1, characterized in that: The particle size of the inorganic filler is 800-1000 mesh.
8. The corrosion-resistant cross-linked polyethylene insulated power cable according to claim 1, characterized in that: The cross-linking agent includes one or more of dicumyl peroxide, benzoyl peroxide and dicumyl hydroperoxide.
9. The corrosion-resistant cross-linked polyethylene insulated power cable according to claim 1, characterized in that: The antioxidant includes one or more of antioxidant 1010, antioxidant 264 and antioxidant B215.
10. The production process of a corrosion-resistant cross-linked polyethylene insulated power cable according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Wrapping the insulating layer on the cable core to obtain a semi-finished power cable; S2. After the raw materials of the sheath layer are evenly mixed, they are extruded and coated on the outside of the semi-finished power cable to obtain the power cable.
Citation Information
Cited By
Corrosion-resistant crosslinked polyethylene insulated power cable
CN121122822A