Cloakroom wooden door filler, preparation method thereof and wooden door using filler

By using acrylic emulsion, calcium carbonate, areca fiber and mullite composition in the coating layer on the cloakroom wooden door, the problem of solid wood filler deformation in a humid environment is solved, achieving high strength and durability of the wooden door, and extending extended service life.

CN118745304APending Publication Date: 2024-10-08GUANGDONG GUANGZHOU DEWEIER FURNITURE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410983743.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Solid wood fillers are easily affected by changes in ambient humidity, causing wooden doors to expand and crack in humid environments, affecting their service life and aesthetics. Especially in high-height cloakrooms, the problem of deformation caused by uneven stress is more serious.

Method used

The coating layer is composed of acrylic emulsion, calcium carbonate, areca fiber and mullite to form a network structure, which enhances the overall stability and adhesion of the coating layer, prevents water vapor penetration, and improves the overall strength and deformation resistance of the wood core.

Benefits of technology

It effectively isolates water vapor, enhances the mechanical properties of wooden doors, reduces damage to the wooden core by external forces, extends the service life of wooden doors, and improves the quality and deformation resistance of wooden doors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956805700000071
    Figure BDA0004956805700000071
  • Figure BDA0004956805700000082
    Figure BDA0004956805700000082
  • Figure BDA0004956805700000091
    Figure BDA0004956805700000091
Patent Text Reader

Abstract

The invention relates to the field of wooden doors, in particular to a cloakroom wooden door filler, a preparation method of the cloakroom wooden door filler and a wooden door using the cloakroom wooden door filler. The cloakroom wooden door filler comprises a wooden core and a coating layer, and the coating layer is arranged on the outer surface of the wooden core; the coating layer is prepared from a coating material, and the coating material is prepared from the following components in percentage by mass: 45 to 55 percent of acrylic emulsion, 20 to 30 percent of calcium carbonate, 0.1 to 1 percent of coalescing agent, 0.1 to 1 percent of dispersing agent, 0.1 to 1 percent of defoaming agent, 0.1 to 1 percent of pH regulator, 0.1 to 1 percent of thickening agent, 3 to 10 percent of betel nut fiber, 1 to 5 percent of mullite and the balance of water. The cloakroom wooden door filling material can effectively enhance the water vapor blocking capacity, and the strength of the cloakroom wooden door filling material is remarkably improved; the wooden door filled with the cloakroom wooden door filling material is not prone to deformation and has a longer service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of wooden doors, and more specifically, to a cloakroom wooden door filler and a preparation method thereof, and a wooden door using the filler. Background Art

[0002] As an important part of the building, wooden doors not only bear the basic protection and partition functions, but also become an important element to show the style and taste of interior decoration due to its unique material and craftsmanship. With the improvement of people's living standards and the change of aesthetic concepts, the requirements for wooden doors have gradually changed from single practicality to the pursuit of dual standards of practicality and beauty.

[0003] In the process of making wooden doors, the choice of filler has a crucial impact on the performance of wooden doors. At present, the common wooden door fillers on the market mainly include solid wood filler, MDF board filler, hollow particle board filler and other types. Among them, solid wood filler is favored by consumers for its natural, environmentally friendly, strong and durable characteristics.

[0004] Although solid wood fillers have many advantages, they still face some problems in practical applications. Because wood is hygroscopic, it is easily affected by changes in environmental humidity and deformed. Especially in a humid environment, wooden doors filled with solid wood are prone to expansion and cracking, which seriously affects their service life and appearance. For wooden doors in cloakrooms, due to their high height, they are prone to deformation due to uneven force over time.

[0005] Therefore, there is room for improvement. Summary of the invention

[0006] In order to prevent a wooden door from being easily deformed, the present application provides a filler for a cloakroom wooden door, a preparation method thereof, and a wooden door using the filler.

[0007] In the first aspect, the present application provides a cloakroom wooden door filling material, which adopts the following technical solution: A filling material for a cloakroom wooden door comprises a wood core and a coating layer, wherein the coating layer is arranged on the outer surface of the wood core; the coating layer is prepared from a coating material, and the coating material comprises the following components by mass percentage: 45-55% acrylic emulsion, 20-30% calcium carbonate, 0.1-1% film-forming aid, 0.1-1% dispersant, 0.1-1% defoamer, 0.1-1% pH regulator, 0.1-1% thickener, 3-10% betel nut fiber, 1-5% mullite, and the balance is supplemented by water.

[0008] Acrylic paint is prepared by using betel nut fiber and mullite together. It is applied on the surface of the wood core to form a coating layer, which can effectively isolate water vapor and improve the overall strength of the wood core. When the wooden door is subjected to force, it can quickly transfer the force as a filler to reduce the impact of the force causing the wooden door to deform.

[0009] Specifically, mullite is a high-quality refractory raw material with high strength, high hardness, excellent chemical stability and corrosion resistance. In the coating, mullite particles can act as a "skeleton" to provide strong support and enhance the overall strength and wear resistance of the coating. Betel nut fiber, with its excellent flexibility and tensile strength, plays the role of a "bridge" in the coating. Betel nut fiber provides a large number of attachment sites, allowing mullite particles to be firmly attached to the betel nut fiber to form a stable mixed system. This mixed system is also a network structure, which can not only enhance the overall stability of the coating, but also improve the adhesion between the coating and the wood core, ensuring that the coating can be firmly attached to the surface of the wood core.

[0010] At the same time, this mixed system not only improves the overall stability of the coating, but also enhances the bonding between the coating and the wood core surface. The fine fiber structure of betel nut fiber can well fill the tiny gaps on the surface of the wood core, thereby improving the uniformity and density of the coating. This filling effect not only enhances the adhesion between the coating and the wood core, but also effectively prevents the penetration of water vapor. In addition, due to the good hydrophilicity of betel nut fiber, the mixed system allows the coating to quickly penetrate into the wood core surface and form a tight bond.

[0011] In addition, mullite, as a mineral material with high hardness, can significantly improve the hardness and strength of the coating layer, thereby enhancing the overall mechanical properties of the filler. When the wooden door is subjected to external force, the mixed system containing betel nut fiber and mullite can effectively disperse and transmit the force, reducing the destructive effect of the force on the wood core.

[0012] The cooperation of betel nut fiber and mullite in the coating is not just a simple superposition, but also a synergistic effect. This synergistic effect significantly improves the performance of the coating layer, especially in terms of strength, integrity, and water vapor barrier.

[0013] The coating layer is evenly dispersed on the surface of the wood core to form a filler with good performance. The filler is not easily affected by water vapor, has good integrity, and high overall strength. When used in wooden doors, it is not easy to deform due to force or water vapor, thereby extending the service life of the wooden doors and improving the quality of the wooden doors.

[0014] Preferably, the mass ratio of the betel nut fiber to mullite is (1-3):1, based on the mass of the mullite.

[0015] By adopting the above technical solution, the mass ratio of betel nut fiber to mullite is further limited, so that the mullite can be more fully and firmly attached to the betel nut fiber, thereby better exerting the role of the mixed system.

[0016] Preferably, the mullite at least includes large-particle mullite with a particle size of 1-3 mm and small-particle mullite with a particle size of 50-150 μm.

[0017] Preferably, the mullite is large-size mullite with a particle size of 1-3 mm and small-size mullite with a particle size of 50-150 μm, and the mass ratio of large-size mullite to small-size mullite is (1-2):1, with the mass of small-size mullite as the basis.

[0018] By adopting the above technical solution, the particle size and dosage of mullite are further limited, so that the mullite can be more tightly embedded in the attachment site of the betel nut fiber and is not easy to fall off, thereby giving full play to the role of the mixed system, improving the water vapor barrier effect of the filler, and enhancing the integrity and strength of the filler.

[0019] Preferably, the preparation of the betel nut fiber comprises the following steps: Step 01: Remove the skin and seeds of betel nut from the short fibers and crush them to obtain fibers to be processed; Step 02: Wash and dry the treated fibers, and then ball-mill them with an alkaline solution; Step 03: The turbid liquid obtained by ball milling in step 02 is sieved, and the solid part is the semi-finished fiber; Step 04: Wash the semi-finished fiber, mix it with a KOH solution with a concentration of 10-15%, and cook it, with a material-liquid ratio of 10-15; Step 05: After the cooking is completed, wash and dry it to obtain betel nut fiber.

[0020] By adopting the above technical solution, short fiber specifications of betel nut fiber are prepared, which has many surface contact points, forms a larger friction force, and is conducive to the adhesion of mullite. In addition, the fibers can be more closely combined with each other, making the structure of the coating layer more stable, and having a better adhesion effect with the wood core, and playing a role for a long time.

[0021] Preferably, in step 04, the cooking time is 3-4 hours and the cooking temperature is 120-135°C.

[0022] By adopting the above technical solution, the cooking time and temperature are further limited, and the structure is fully destroyed to extract purer betel nut fiber.

[0023] In a second aspect, the present application provides a method for preparing a filling material for a cloakroom wooden door, using the following technical solution: A method for preparing a filling material for a cloakroom wooden door, comprising the following steps: Step 1: preparing the coating material, comprising the following steps: Step 1a: Stir water, pH adjuster, dispersant and calcium carbonate until uniform to obtain slurry; Step 1b: mixing the acrylic emulsion, the film-forming aid, the film-forming aid, the betel nut fiber, the mullite and the slurry until uniform, and then adding the defoaming agent and mixing until uniform to obtain a coating material; Step 2: Brush the coating material evenly onto the surface of the wood core, and after drying, obtain the cloakroom wooden door filling material.

[0024] By adopting the above technical solution, the raw materials are mixed in a specific order to obtain a uniform and fine coating material, so that it can be more fully matched with the wood core to obtain a filling material with good performance.

[0025] In a third aspect, the present application provides a wooden door utilizing a cloakroom wooden door filler.

[0026] In summary, this application has the following beneficial effects: 1. Use betel nut fiber and mullite together to prepare acrylic paint, which is applied on the surface of the wood core to form a coating layer, which can effectively isolate water vapor and improve the overall strength of the wood core. When the wooden door is subjected to force, it can quickly transfer the force as a filler to reduce the impact of the force on the deformation of the wooden door.

[0027] 2. In the present application, it is preferred to use mullite and betel nut fiber together to prepare the coating. Mullite serves as the skeleton and betel nut fiber serves as the bridge. A large amount of mullite is attached to the betel nut fiber to form a mixed system, so that the coating can be filled into the tiny gaps on the surface of the wood core, effectively blocking the penetration of water vapor and reducing the deformation effect of moisture on the wooden door.

[0028] 3. The combination of mullite and betel nut fiber can also improve the integrity and strength of the filling material, effectively disperse and transmit force, reduce the destructive effect of force on the wood core, and thus alleviate the deformation of the wooden door. DETAILED DESCRIPTION

[0029] The present application is further described in detail below with reference to the embodiments.

[0030] The raw materials used in the following examples and comparative examples are all commercially available products.

[0031] Preparation Example Preparation Example 1 A betel nut fiber, the preparation of which comprises the following steps: Step 01: Peel and remove the seeds of the betel nut short fibers, put them into a grinder and grind them to obtain fibers to be processed.

[0032] Step 02: Wash the treated fiber with clean water, and then dry the treated fiber in a vacuum drying oven at 55° C. for 6 hours.

[0033] After drying, the fiber to be treated is placed in a ball mill and milled with an alkaline solution at a solid-liquid ratio of 1:8 for 3 hours to obtain a turbid solution.

[0034] Step 03: The turbid liquid obtained by ball milling in step 02 is sieved, and the solid part is the semi-finished fiber.

[0035] Step 04: Wash the semi-finished fiber with clean water, and mix it with a 12% KOH solution for steaming. The steaming time is 3.5 hours, the cooking temperature is 128°C, and the material-liquid ratio is 1:12.

[0036] Step 05: Use clean water to wash the semi-finished fiber after the cooking treatment, and then dry it at 85°C for 6 hours to obtain betel nut fiber.

[0037] Preparation Example 2 A betel nut fiber, the preparation of which comprises the following steps: Step 01: Peel and remove the seeds of the betel nut short fibers, put them into a grinder and grind them to obtain fibers to be processed.

[0038] Step 02: Wash the treated fiber with clean water, and then dry the treated fiber in a vacuum drying oven at 55° C. for 6 hours.

[0039] After drying, the fiber to be treated is placed in a ball mill and milled with an alkaline solution at a solid-liquid ratio of 1:8 for 3 hours to obtain a turbid solution.

[0040] Step 03: The turbid liquid obtained by ball milling in step 02 is sieved, and the solid part is the semi-finished fiber.

[0041] Step 04: Wash the semi-finished fiber with clean water, and mix it with a 10% KOH solution for steaming. The steaming time is 4 hours, the cooking temperature is 120°C, and the material-liquid ratio is 1:10.

[0042] Step 05: Use clean water to wash the semi-finished fiber after the cooking treatment, and then dry it at 85°C for 6 hours to obtain betel nut fiber.

[0043] Preparation Example 3 A betel nut fiber, the preparation of which comprises the following steps: Step 01: Peel and remove the seeds of the betel nut short fibers, put them into a grinder and grind them to obtain fibers to be processed.

[0044] Step 02: Wash the treated fiber with clean water, and then dry the treated fiber in a vacuum drying oven at 55° C. for 6 hours.

[0045] After drying, the fiber to be treated is placed in a ball mill and milled with an alkaline solution at a solid-liquid ratio of 1:8 for 3 hours to obtain a turbid solution.

[0046] Step 03: The turbid liquid obtained by ball milling in step 02 is sieved, and the solid part is the semi-finished fiber.

[0047] Step 04: Wash the semi-finished fiber with clean water, and mix it with a 15% KOH solution for steaming. The steaming time is 3 hours, the cooking temperature is 135°C, and the material-liquid ratio is 1:15.

[0048] Step 05: Use clean water to wash the semi-finished fiber after the cooking treatment, and then dry it at 85°C for 6 hours to obtain betel nut fiber.

[0049] Preparation Example 4 A betel nut fiber, the preparation of which comprises the following steps: Step 01: Peel and remove the seeds of the betel nut short fibers, put them into a grinder and grind them to obtain fibers to be processed.

[0050] Step 02: Wash the treated fiber with clean water, and then dry the treated fiber in a vacuum drying oven at 55° C. for 6 hours.

[0051] After drying, the fiber to be treated is placed in a ball mill and milled with an alkaline solution at a solid-liquid ratio of 1:8 for 3 hours to obtain a turbid solution.

[0052] Step 03: The turbid liquid obtained by ball milling in step 02 is sieved, and the solid part is the semi-finished fiber.

[0053] Step 04: Wash the semi-finished fiber with clean water, and mix it with a 15% KOH solution for cooking. The cooking time is 3 hours, the cooking temperature is 135°C, and the material-liquid ratio is 1:8.

[0054] Step 05: Use clean water to wash the semi-finished fiber after the cooking treatment, and then dry it at 85°C for 6 hours to obtain betel nut fiber. Example

[0055] Example 1 A cloakroom wooden door filling material comprises a wood core and a coating layer, wherein the coating layer is arranged on the outer surface of the wood core. The coating layer is prepared from a coating material, and the coating material comprises: acrylic emulsion, calcium carbonate, film-forming aid, dispersant, defoamer, pH regulator, thickener, betel nut fiber, mullite, and water.

[0056] The acrylic emulsion is commercially available, and the one used in this embodiment is Acronal ECO 338ap.

[0057] Calcium carbonate is specifically heavy calcium carbonate, which is commercially available.

[0058] The film-forming aid is alcohol ester dodecahydrate, which is commercially available.

[0059] The dispersant is commercially available, and in this embodiment, it is BYK-190.

[0060] The defoaming agent is an organosilicon defoaming agent, which in this embodiment was purchased from Beijing Zhubao New Technology Co., Ltd. and has a model number of DZ-1130.

[0061] The pH adjuster was AMP95.

[0062] The thickener is hydroxyethyl cellulose.

[0063] The betel nut fiber adopts the betel nut fiber prepared in Preparation Example 1.

[0064] Mullite is commercially available and crushed into large-particle mullite with a particle size of 1-3 mm and small-particle mullite with a particle size of 50-150 μm.

[0065] The specific content of each raw material is shown in Table 1.

[0066] The present application also provides a method for preparing a filling material for a cloakroom wooden door, comprising the following steps: Step 1: preparing a coating material, comprising the following steps: Step 1a: Mix water, a pH adjuster, a dispersant and calcium carbonate, and stir at 1300 r / min until uniform to obtain a slurry.

[0067] Step 1b: Mix the acrylic emulsion, film-forming aid, film-forming aid, betel nut fiber, mullite and slurry, and stir and disperse them at a high speed of 1300 r / min for 20 minutes.

[0068] Then add the defoamer and mix, stir and disperse at 800 r / min for 5 minutes to obtain the coating material.

[0069] Step 2: Brush the coating material evenly onto the surface of the wood core, and after drying, obtain the cloakroom wooden door filling material.

[0070] The present application also provides an application of a cloakroom wooden door filling material, wherein the cloakroom wooden door filling material is used to fill the inside of a wooden door, so that the wooden door obtained is not easily deformed and has a longer service life.

[0071] Example 2 A cloakroom wooden door filling material, which is different from Example 1 in that: The betel nut fiber adopts the betel nut fiber prepared in Preparation Example 2.

[0072] The specific content of each raw material is different, see Table 1 for details.

[0073] Example 3 A cloakroom wooden door filling material, which is different from Example 1 in that: The betel nut fiber adopts the betel nut fiber prepared in Preparation Example 3.

[0074] The specific content of each raw material is different, see Table 1 for details.

[0075] Example 4 A filling material for a cloakroom wooden door, which is different from Example 1 in that the mass ratio of betel nut fiber to mullite is 1:1.

[0076] The mass ratio of large-size mullite to small-size mullite is 1:1.

[0077] The specific contents are shown in Table 1.

[0078] Example 5 A filling material for a cloakroom wooden door, which is different from Example 1 in that the mass ratio of betel nut fiber to mullite is 3:1.

[0079] The mass ratio of large-size mullite to small-size mullite is 1.5:1.

[0080] The specific contents are shown in Table 1.

[0081] Table 1 Example 6 A filling material for a cloakroom wooden door, which is different from Example 1 in that the mullite is large-diameter mullite with a particle size of 1-3 mm, that is, the large-diameter mullite is 3 kg, and the small-diameter mullite is 0 kg.

[0082] Example 7 A filling material for a cloakroom wooden door, which is different from Example 1 in that the betel nut fiber is the betel nut fiber prepared in Preparation Example 4.

[0083] Comparative Example Comparative Example 1 A filling material for a cloakroom wooden door, which is different from Example 1 in that betel nut fiber and mullite are omitted, the betel nut fiber and mullite are 0 kg, and the water is 21.2 kg.

[0084] Comparative Example 2 A cloakroom wooden door filling material, which is different from Example 1 in that the betel nut fiber is replaced by sisal fiber. The sisal fiber is commercially available and is purchased from Poyang County Changjiang Textile Co., Ltd. in this example.

[0085] Comparative Example 3 A cloakroom wooden door filling material, which is different from Example 1 in that mullite is replaced by alumina.

[0086] Comparative Example 4 A filling material for a cloakroom wooden door, which is different from Example 1 in that the amount of betel nut fiber is 1 kg and the amount of mullite is 8 kg.

[0087] The large-size mullite weighs 5.33 kg, and the small-size mullite weighs 2.67 kg.

[0088] Performance testing Test 1: Samples to be tested: The cloakroom wooden door filling materials of Examples 1-7 and Comparative Examples 1-4 were selected, wherein the size of the wooden core was 20*20*4 cm, and the thickness of the coating layer was 0.05 cm.

[0089] Weigh the initial weight of the cloakroom door filling material, record it as m1. Then immerse the cloakroom door filling material in water for 12 hours. Take out the cloakroom door filling material after immersion, and weigh it again, record it as m2.

[0090] Calculate the weight gain rate according to the following formula and record the results in Table 2. The greater the weight gain rate, the worse the water vapor resistance effect.

[0091] Test 2: According to GB / T 1938-2009 "Test Method for Tensile Strength Parallel to Grain of Wood", the tensile strength of the cloakroom wooden door filling materials of Examples 1-7 and Comparative Examples 1-4 was tested, and the results are recorded in Table 2. The thickness of the coating layer is 0.05 cm.

[0092] Test three: The cloakroom wooden door filling materials of Examples 1-7 and Comparative Examples 1-4 were placed in a room with a temperature of 45°C and a humidity of 75% for 30 days. After being taken out, the cloakroom wooden door filling materials were visually inspected for deformation, and the results were recorded in Table 2.

[0093] The size of the wood core is 60*100*4cm, and the thickness of the coating layer is 0.05cm.

[0094] Table 2 According to the test data in Table 2, after being soaked in water, the weight gain rate of the cloakroom wooden door filling materials of Examples 1-7 is significantly lower than that of Comparative Examples 1-4, indicating that the cloakroom wooden door filling materials of Examples 1-7 can well resist the entry of water vapor. In Test 2, the cloakroom wooden door filling materials of Examples 1-7 also showed higher tensile strength than Comparative Examples 1-4, indicating that the cloakroom wooden door filling materials of Examples 1-7 are better overall and have higher strength. The results of Test 3 also prove that the cloakroom wooden door filling materials of Examples 1-7 have better anti-deformation effect, with less obvious deformation, and can be well applied to wooden doors to play a filling role.

[0095] Specifically, Comparative Example 1 is based on Example 1, and betel nut fiber and mullite are omitted at the same time; Comparative Examples 2-3 are based on Example 1, and any of betel nut fiber and mullite are replaced with other raw materials; Comparative Example 4 is based on Example 1, and the specific dosage relationship of betel nut fiber and mullite in the system is destroyed. Comparative Examples 1-4 all destroy the integrity of the scheme of Example 1 to varying degrees, and Comparative Examples 1-4 also show poor results in the test. It shows that under the specific dosage of betel nut fiber and mullite, the prepared coating material can be well matched with the wood core, thereby effectively improving the performance of the cloakroom wooden door filling material.

[0096] Example 6 is based on Example 1, but mullite with large particle size is used instead. The coating material obtained by lacking the combination of large and small particle sizes has reduced the performance in terms of water vapor isolation and strength, but still maintains a good non-deformation effect. This shows that further optimizing the particle size combination of mullite is helpful to improve the performance of the cloakroom wooden door filling material.

[0097] Example 7 is based on Example 1, but the extraction conditions of the betel nut fiber are changed, which affects the coordination effect between the betel nut fiber and mullite, so that the performance of Example 7 is lower than that of Example 1.

[0098] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A cloakroom wooden door filling material, characterized in that: It comprises a wood core and a coating layer, wherein the coating layer is arranged on the outer surface of the wood core; The coating layer is prepared from a coating material, which includes the following components by mass percentage: 45-55% acrylic emulsion, 20-30% calcium carbonate, 0.1-1% film-forming aid, 0.1-1% dispersant, 0.1-1% defoaming agent, 0.1-1% pH regulator, 0.1-1% thickener, 3-10% betel nut fiber, 1-5% mullite, and the balance is supplemented by water.

2. The cloakroom wooden door filling material according to claim 1, characterized in that: The mass ratio of the betel nut fiber to mullite is (1-3):

1.

3. The cloakroom wooden door filling material according to claim 1, characterized in that: The mullite at least includes large-grained mullite with a grain size of 1-3 mm and small-grained mullite with a grain size of 50-150 μm.

4. The cloakroom wooden door filling material according to claim 3, characterized in that: The mullite comprises large-size mullite with a particle size of 1-3 mm and small-size mullite with a particle size of 50-150 μm, and the mass ratio of the large-size mullite to the small-size mullite is (1-2):

1.

5. The cloakroom wooden door filling material according to any one of claims 1 to 4, characterized in that: The preparation of the betel nut fiber comprises the following steps: Step 01: Remove the skin and seeds of betel nut from the short fibers and crush them to obtain fibers to be processed; Step 02: Wash and dry the treated fibers, and then ball-mill them with an alkaline solution; Step 03: The turbid liquid obtained by ball milling in step 02 is sieved, and the solid part is the semi-finished fiber; Step 04: Wash the semi-finished fiber and mix and cook it with a 10-15% KOH solution, with a material-to-liquid ratio of 10-15; Step 05: After steaming, wash and dry to obtain betel nut fiber.

6. The filling material for cloakroom wooden door according to claim 5, characterized in that: In step 04, the cooking time is 3-4 hours and the cooking temperature is 120-135°C.

7. A method for preparing a cloakroom wooden door filling material according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: preparing the coating material, comprising the following steps: Step 1a: Stir water, pH adjuster, dispersant and calcium carbonate until uniform to obtain slurry; Step 1b: mixing the acrylic emulsion, the film-forming aid, the film-forming aid, the betel nut fiber, the mullite and the slurry until uniform, and then adding the defoaming agent and mixing until uniform to obtain a coating material; Step 2: Brush the coating material evenly onto the surface of the wood core, and after drying, obtain the cloakroom wooden door filling material.

8. A wooden door using the cloakroom wooden door filling material according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Coating for wood windows and doors, and production method of coating

    CN107815238A

  • High-hardness and quick-drying water-based two-component filling clear primer and preparation method thereof

    CN111961398A

  • Wooden door surface treatment process

    CN116475044A

  • Foaming material capable of being quickly degraded for shoe soles and preparation method of foaming material

    CN117362774A