Edge coating glue as well as preparation method and application thereof

By using a specific composition and structural design in the lithium battery edge coating, the environmental protection issues and performance deficiencies of PVDF in the lithium battery cathode are solved, and efficient mechanical properties and electrolyte resistance are achieved. It is suitable for lithium ion battery cathodes and improves improve overall performance and stability.

CN118745327APending Publication Date: 2024-10-08常州环峰电源科技有限公司 +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410783160.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Currently, PVDF, which is widely used in the field of lithium battery cathodes, has environmental issues, and there are technical bottlenecks in the lithium-ion battery industry. In particular, it is difficult to meet high requirements in terms of performance and stability of edge coating.

Method used

An edge coating glue is used, which consists of polymers, boehmite, additives and solvents. It combines defoaming agents, leveling agents and thickeners in a specific weight ratio and particle size range to form a three-dimensional network structure. Improve peel strength, storage stability and electrolyte resistance, and prepare adhesives by combining soft segments and hard segments to improve solvent resistance and processing performance.

Benefits of technology

Significantly improves the mechanical properties, electrolyte resistance and stability of edge coating, making it suitable for lithium-ion battery positive electrodes, enhancing the ability to support charge transfer, reducing charge transfer resistance, and improving processing performance and adhesion sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004897800780000091
    Figure BDA0004897800780000091
  • Figure HDA0004897800790000011
    Figure HDA0004897800790000011
  • Figure HDA0004897800790000012
    Figure HDA0004897800790000012
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, in particular to the field of IPCC09J7, and more particularly relates to an edge coating adhesive and a preparation method thereof. The high-temperature-resistant coating comprises the following components in parts by weight: 10-15 parts of a polymer, 10-25 parts of boehmite, 0.5-5 parts of an auxiliary agent and 50-70 parts of a solvent. The thickening agent comprises an associated polyurethane thickening agent, so that the peeling strength and the storage stability of the edge coating adhesive can be improved; the auxiliaries comprise a defoaming agent, a flatting agent and a thickening agent, the weight ratio of the defoaming agent to the flatting agent to the thickening agent is (0.5-4): (0.5-3): (0.5-4), and the mechanical property and electrolyte resistance of the edge coating adhesive can be further improved; the particle size of the boehmite D50 is 0.4-4.5 microns, and the weight ratio of the polymer to the boehmite is 1: (1-1.5), so that the strength and electrolyte resistance of the edge coating glue can be improved, and the edge coating glue can be stably applied to the positive electrode of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, in particular to the field of IPCC09J7, and more specifically to an edge coating adhesive and a preparation method thereof. Background Art

[0002] The glue coating on the positive electrode of lithium batteries is used to fix the positive electrode material, isolate the electrolyte from direct contact with the current collector to prevent short circuits, and improve the overall performance and safety of the battery. Driven by national policies and the new energy vehicle market, China's lithium battery industry has risen rapidly, surpassing Japan and South Korea to become the world's largest lithium battery producer. According to relevant statistics, my country's lithium-ion battery production has accounted for more than 70% of the world's total production. Although my country's lithium battery industry has superior overall strength, there are still technical bottlenecks or "stuck necks" in individual links. PVDF (polyvinylidene fluoride), which is widely used in the field of lithium battery positive electrodes, has obvious environmental problems.

[0003] CN114744139A provides a lithium battery pole piece and its preparation process, which relates to the field of lithium battery technology, a coating layer, coated on the center of at least one surface of a current collector; a side coating layer, coated on both sides of at least one surface of the current collector; and the side coating layer covers the positions where the two sides of the coating layer are connected with the current collector by 0.1mm□10mm, and the overlapping area of ​​the side coating layer and the coating layer forms a covering layer; a chemically cross-linked water-insoluble polymer, N-methylpyrrolidone or deionized water, and a coloring material; but the chemically cross-linked water-insoluble polymer is selected from fluoroplastics, polyvinylidene fluoride (PVDF), and polyvinyl chloride (PVF). Summary of the invention

[0004] The first aspect of the present invention provides an edge coating adhesive, which comprises, by weight, 10-15 parts of a polymer, 10-25 parts of boehmite, 0.5-5 parts of an auxiliary agent and 50-70 parts of a solvent.

[0005] The auxiliary agent includes at least one of a defoamer, a leveling agent and a thickener.

[0006] The auxiliary agent comprises a defoamer, a leveling agent and a thickener, and the weight ratio of the defoamer, the leveling agent and the thickener is (0.5-4): (0.5-3): (0.5-4).

[0007] Preferably, the weight ratio of the defoamer, leveling agent and thickener is 1: (0.2-0.8): (0.6-1.2).

[0008] The boehmite D50 particle size is 0.4-4.5 microns.

[0009] Preferably, the boehmite D50 particle size is 0.4-4.5 microns.

[0010] Preferably, the boehmite D50 particle size is 0.5-3 microns.

[0011] Further preferably, the boehmite D50 has a particle size of 1.5-3 μm and is purchased from Anhui Yishitong Materials Technology Co., Ltd., model: BG-613.

[0012] Preferably, the defoaming agent comprises a silicone defoaming agent.

[0013] Preferably, at least one of the following grades is used: at least one of BYK-020, BYK-060N, BYK066N, BYK-077, BYK-085, TSA750S, DC62, DC65 and DC163.

[0014] Further preferably, the defoaming agent includes at least one of BYK066N, BYK-077, and BYK-085.

[0015] Preferably, the leveling agent includes polyester modified polydimethylsiloxane solution, brand: BYK-310.

[0016] Preferably, the thickener comprises an associative polyurethane thickener.

[0017] Further preferably, the thickener comprises a non-ionic associative polyurethane thickener, the active ingredient concentration is ≥40%, and the viscosity is ≤14000cp (25°C).

[0018] The present application has found that the thickener includes an associative polyurethane thickener, which can improve the peel strength and storage stability of the edge coating glue. Its role in the system of the present application is to minimize the volume of the associative network, limit the typical flocculation phenomenon of the non-associative thickening system, reduce the volume-limited flocculation effect, and give the system excellent stability.

[0019] Further research found that the auxiliary agent includes a defoamer, a leveling agent and a thickener, and the weight ratio of the defoamer, the leveling agent and the thickener is 1: (0.2-0.8): (0.6-1.2), which can further improve the mechanical properties and electrolyte resistance of the edge coating glue. It may be an associative polyurethane thickener, whose molecular structure contains hydrophilic and lipophilic groups, which can form multiple micelles, and the lipophilic groups in the molecules can be anchored on the surface of boehmite particles of a specific particle size, and fixed together with the polyether segments in the polymer in the system. At the same time, the polymer interacts with the defoamer and the leveling agent to form a three-dimensional network structure. This state restrains the free movement of latex particles in water and effectively improves the cohesive properties of the edge coating glue.

[0020] Preferably, the thickener includes the following brands: RM12W (Dow Acrysol, USA), RM8W (Dow Acrysol, USA), and 2020NPR (Dow Acrysol, USA).

[0021] Preferably, the weight ratio of the polymer to boehmite is 1:(1-1.5).

[0022] More preferably, the weight ratio of the polymer to boehmite is 1:(1-1.2).

[0023] The research of this application found that the boehmite D50 particle size is 0.4-4.5 microns, and the weight ratio of polymer to boehmite is 1: (1-1.5), which can improve the strength of the edge coating and electrolyte resistance, so that it can be stably applied to the positive electrode of lithium-ion batteries. It may be a specific sub-particle size, which is dispersed on the surface of the polymer and arranged more densely, and some particles enter the pores of the base film, and play a stronger supporting role in the coated diaphragm, and has a stronger ability to resist thermal shrinkage. At the same time, the specific particle size is dispersed in the polymer. Since the liquid electrolyte is the carrier for the migration of lithium ions between the positive and negative electrodes, the high liquid absorption rate of the diaphragm is conducive to the transfer of charge between the lithium ion electrolyte and the surface of the electrode material, thereby reducing the charge transfer resistance and improving the electrolyte resistance.

[0024] Further research found that the binder prepared by combining soft segments and hard segments in the present application can further improve the solvent resistance and processing performance. This may be due to the synergistic effect between the soft segment and the hard segment. The hard segment part improves the dimensional stability (anti-swelling) of the polymer in the electrolyte, and the soft segment part improves the dispersion stability of the polymer on inorganic particles and the adhesion on the electrode, while ensuring the processability of the electrode processing process. At the same time, the soft segment and the hard segment form a soft and hard alternating copolymer of high molecular polymers distributed on the chain segments connected by the same chemical bond, reducing the difficulty of its dispersion in the system.

[0025] The raw materials for preparing the polymer include a first intermediate and a second intermediate, wherein the first intermediate includes an isocyanate-terminated oligomer, and the second intermediate includes one of an amine-terminated oligomer and an anhydride-terminated oligomer.

[0026] The raw material for preparing the first intermediate includes at least one of polyether polyol and polyether amine.

[0027] Preferably, the polyether polyol includes at least one of polypropylene glycol, polytetramethylene glycol and polyethylene glycol.

[0028] Preferably, the molecular weight of the polypropylene glycol is 600-8000.

[0029] At least one of the following models is preferred: PPG-600, PPG-1000, PPG-2000, PPG-3000, PPG-4000, PPG-6000, PPG-8000.

[0030] At least one of the following models is preferred: PPG-600, PPG-1000, PPG-2000.

[0031] Preferably, the molecular weight of the polytetramethylene ether is 650-3000.

[0032] At least one of the following models is preferred: PTMEG-650, PTMEG-1000, PTMEG-1400, PTMEG-1800, PTMEG-2000, PTMEG-3000.

[0033] Preferably, the molecular weight of the polyethylene glycol is 600-8000.

[0034] Preferably, at least one of the following types is selected from the group consisting of polyethylene glycol PEG-600, PEG-800, PEG-1000, PEG-1500, PEG-2000, PEG-3000, PEG-4000, PEG-6000, and PEG-8000.

[0035] Preferably, the molecular weight of the polyetheramine is 400-2000.

[0036] At least one of the following models is preferred: PEA400, PEA1000, PEA2000.

[0037] The raw material for preparing the second intermediate includes at least one of aromatic diamine and aromatic diphthalic anhydride.

[0038] The aromatic diamine includes at least one of diaminodiphenylmethane, diaminodiphenyl ether, p-phenylenediamine, m-phenylenediamine, diaminodiphenyl sulfone, 3,3'-dichloro-4,4'-diaminophenylmethane, and 4,4-diamino-2,2'-bistrifluoromethylbiphenyl.

[0039] The aromatic diphthalic anhydride includes at least one of pyromellitic anhydride, benzophenone tetracarboxylic anhydride, biphenyl tetracarboxylic anhydride, hexafluoroanhydride, 4,4-oxydiphthalic anhydride, trimellitic anhydride, and naphthalene tetracarboxylic anhydride.

[0040] The raw materials for preparing the first intermediate and the second intermediate both further include diisocyanate.

[0041] Preferably, the diisocyanate includes at least one of MDI, TDI, HDI, HMDI, NDI, and IPDI.

[0042] The raw materials for preparing the first intermediate and the second intermediate both further include a solvent, and the solvent is preferably N-methylpyrrolidone (NMP).

[0043] The preparation method of the polymer comprises the following steps:

[0044] Step 1: Dissolve 1-2 mol IPDI in NMP solution and heat to 40-90°C, add 1-1.5 mol PPG-1000, and add an appropriate amount of NMP solution to maintain the overall concentration of the solution at 20-80%, react at 40-90°C for 1-3h to obtain the first intermediate.

[0045] Step 2: Dissolve 1-2 mol of diaminodiphenyl ether in NMP solution (concentration 10-50 wt%), heat to 40-90° C., add 1-1.5 mol of TDI, and add an appropriate amount of NMP solution to maintain the overall concentration of the solution at 10-50 wt%. React at 40-90° C. for 1-3 hours to obtain a second intermediate.

[0046] Step 3: Pour the first intermediate into the second intermediate, and continue the reaction at 80-120°C for 1-2h to obtain the product.

[0047] The second aspect of the present invention provides a method for preparing edge coating adhesive, comprising the following steps: adding a polymer, boehmite and an auxiliary agent to a solvent in sequence, and stirring the mixture evenly to obtain an edge coating adhesive.

[0048] A third aspect of the present invention provides an application of edge coating glue, which is applied to the preparation of lithium battery pole pieces.

[0049] Beneficial effects:

[0050] 1. The thickener includes an associative polyurethane thickener, which can improve the peel strength and storage stability of the edge coating.

[0051] 2. The auxiliary agent includes a defoamer, a leveling agent and a thickener. The weight ratio of the defoamer, the leveling agent and the thickener is 1: (0.2-0.8): (0.6-1.2), which can further improve the mechanical properties and electrolyte resistance of the edge coating.

[0052] 3. The boehmite D50 particle size is 0.4-4.5 microns, and the weight ratio of polymer to boehmite is 1:(1-1.5), which can improve the strength and electrolyte resistance of the edge coating, so that it can be stably applied to the positive electrode of lithium-ion batteries.

[0053] 4. The adhesive prepared by the present application using a combination of soft segments and hard segments can further improve solvent resistance and processing performance.

[0054] 5. The edge coating glue prepared in this application is applied to aluminum foil, and the bonding force between the aluminum foil and the aluminum foil can reach 120N / m. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 This is a photo of Example 1 after the electrolyte resistance test.

[0056] Figure 2 This is a photo of Comparative Example 1 after the electrolyte resistance test. DETAILED DESCRIPTION

[0057] Example 1

[0058] An edge coating adhesive comprises, by weight, 20 parts of a polymer, 20 parts of boehmite, 2.5 parts of an auxiliary agent and 57.5 parts of a solvent.

[0059] The auxiliary agent is 1 part of defoamer, 0.5 part of leveling agent and 1 part of thickener.

[0060] The boehmite D50 has a particle size of 1.5-3 μm and is purchased from Anhui Yishitong Materials Technology Co., Ltd., model: BG-613.

[0061] The defoamer is an organosilicon defoamer with the brand name BYK-085.

[0062] The leveling agent is polyester modified polydimethylsiloxane solution, brand: BYK-310.

[0063] The thickener is: brand RM8W (Dow Acrysol, USA).

[0064] The polymer is homemade, and the preparation method is as follows:

[0065] Step 1: Dissolve 444.64 g IPDI in 900 g NMP solution, heat to 50°C, add 1000 g PPG-1000, and add 544.64 g NMP solution, maintain the overall concentration of the solution at 50 wt%, react at 50°C for 2 h, and obtain the first isocyanate-terminated intermediate.

[0066] Step 2: Dissolve 396.6 g of diaminodiphenylmethane in 856 g of NMP solution, heat to 50° C., add 174.15 g of TDI to obtain a solution with a concentration of 40 wt %, and react at 50° C. for 2 h to obtain an amino-terminated second intermediate.

[0067] Step 3: Add 1444.64 g of the first intermediate to 713.44 g of the second intermediate solution, mix well, and react at 80° C. for 3 h. Add 2880.4 g of solvent to obtain a polymer.

[0068] A method for preparing edge coating glue comprises the following steps: adding a polymer, boehmite and an auxiliary agent into a solvent in sequence, and stirring the mixture evenly to obtain the edge coating glue.

[0069] Comparative Example 1

[0070] An edge coating adhesive comprises, by weight, 20 parts of a polymer, 20 parts of boehmite, 1.5 parts of an auxiliary agent and 58.5 parts of a solvent.

[0071] The auxiliary agent is 1 part of defoamer and 0.5 part of leveling agent.

[0072] The boehmite D50 has a particle size of 1.5-3 μm and is purchased from Anhui Yishitong Materials Technology Co., Ltd., model: BG-613.

[0073] The defoamer is an organosilicon defoamer with the brand name BYK-085.

[0074] The leveling agent is polyester modified polydimethylsiloxane solution, brand: BYK-310.

[0075] The polymer is homemade, and the preparation method is as follows:

[0076] Step 1: Dissolve 444.64 g IPDI in 900 g NMP solution, heat to 50°C, add 1000 g PPG-1000, and add 544.64 g NMP solution, maintain the overall concentration of the solution at 50 wt%, react at 50°C for 2 h, and obtain the first isocyanate-terminated intermediate.

[0077] Step 2: Dissolve 396.6 g of diaminodiphenylmethane in 856 g of NMP solution, heat to 50° C., add 174.15 g of TDI to obtain a solution with a concentration of 40 wt %, and react at 50° C. for 2 h to obtain an amino-terminated second intermediate.

[0078] Step 3: Add 1444.64 g of the first intermediate to 713.44 g of the second intermediate solution, mix well, and react at 80° C. for 3 h. Add 2880.4 g of solvent to obtain a polymer.

[0079] A method for preparing edge coating glue comprises the following steps: adding a polymer, boehmite and an auxiliary agent into a solvent in sequence, and stirring the mixture evenly to obtain the edge coating glue.

[0080] Comparative Example 2

[0081] An edge coating adhesive comprises, by weight, 20 parts of a polymer, 20 parts of boehmite, 1.5 parts of an auxiliary agent and 57.5 parts of a solvent.

[0082] The auxiliary agent is 0.5 part of leveling agent and 1 part of thickener.

[0083] The boehmite D50 has a particle size of 1.5-3 μm and is purchased from Anhui Yishitong Materials Technology Co., Ltd., model: BG-613.

[0084] The leveling agent is polyester modified polydimethylsiloxane solution, brand: BYK-310.

[0085] The thickener is: brand RM8W (Dow Acrysol, USA).

[0086] The polymer is homemade, and the preparation method is as follows:

[0087] Step 1: Dissolve 444.64 g IPDI in 900 g NMP solution, heat to 50°C, add 1000 g PPG-1000, and add 544.64 g NMP solution, maintain the overall concentration of the solution at 50 wt%, react at 50°C for 2 h, and obtain the first isocyanate-terminated intermediate.

[0088] Step 2: Dissolve 396.6 g of diaminodiphenylmethane in 856 g of NMP solution, heat to 50° C., add 174.15 g of TDI to obtain a solution with a concentration of 40 wt %, and react at 50° C. for 2 h to obtain an amino-terminated second intermediate.

[0089] Step 3: Add 1444.64 g of the first intermediate to 713.44 g of the second intermediate solution, mix well, and react at 80° C. for 3 h. Add 2880.4 g of solvent to obtain a polymer.

[0090] A method for preparing edge coating glue comprises the following steps: adding a polymer, boehmite and an auxiliary agent into a solvent in sequence, and stirring the mixture evenly to obtain the edge coating glue.

[0091] Comparative Example 3

[0092] An edge coating adhesive comprises, by weight, 20 parts of a polymer, 20 parts of boehmite, 2.5 parts of an auxiliary agent and 57.5 parts of a solvent.

[0093] The auxiliary agent is 1 part of defoamer, 0.5 part of leveling agent and 1 part of thickener.

[0094] The boehmite D50 has a particle size of 1.5-3 μm and is purchased from Anhui Yishitong Materials Technology Co., Ltd., model: BG-613.

[0095] The defoamer is an organosilicon defoamer with the brand name BYK-085.

[0096] The leveling agent is polyester modified polydimethylsiloxane solution, brand: BYK-310.

[0097] The thickener is: brand THIXATROL (Hemmings, USA).

[0098] The polymer is homemade, and the preparation method is as follows:

[0099] Step 1: Dissolve 444.64 g IPDI in 900 g NMP solution, heat to 50°C, add 1000 g PPG-1000, and add 544.64 g NMP solution, maintain the overall concentration of the solution at 50 wt%, react at 50°C for 2 h, and obtain the first isocyanate-terminated intermediate.

[0100] Step 2: Dissolve 396.6 g of diaminodiphenylmethane in 856 g of NMP solution, heat to 50° C., add 174.15 g of TDI to obtain a solution with a concentration of 40 wt %, and react at 50° C. for 2 h to obtain an amino-terminated second intermediate.

[0101] Step 3: Add 1444.64 g of the first intermediate to 713.44 g of the second intermediate solution, mix well, and react at 80° C. for 3 h. Add 2880.4 g of solvent to obtain a polymer.

[0102] A method for preparing edge coating glue comprises the following steps: adding a polymer, boehmite and an auxiliary agent into a solvent in sequence, and stirring the mixture evenly to obtain the edge coating glue.

[0103] Comparative Example 4

[0104] An edge coating adhesive comprises, by weight, 20 parts of a polymer, 20 parts of boehmite, 2 parts of an auxiliary agent and 57.5 parts of a solvent.

[0105] The auxiliary agent is 1 part of defoamer, 0.5 part of leveling agent and 0.5 part of thickener.

[0106] The boehmite D50 has a particle size of 1.5-3 μm and is purchased from Anhui Yishitong Materials Technology Co., Ltd., model: BG-613.

[0107] The defoamer is an organosilicon defoamer with the brand name BYK-085.

[0108] The leveling agent is polyester modified polydimethylsiloxane solution, brand: BYK-310.

[0109] The thickener is: brand THIXATROL (Hemmings, USA).

[0110] The polymer is homemade, and the preparation method is as follows:

[0111] Step 1: Dissolve 444.64 g IPDI in 900 g NMP solution, heat to 50°C, add 1000 g PPG-1000, and add 544.64 g NMP solution, maintain the overall concentration of the solution at 50 wt%, react at 50°C for 2 h, and obtain the first isocyanate-terminated intermediate.

[0112] Step 2: Dissolve 396.6 g of diaminodiphenylmethane in 856 g of NMP solution, heat to 50° C., add 174.15 g of TDI to obtain a solution with a concentration of 40 wt %, and react at 50° C. for 2 h to obtain an amino-terminated second intermediate.

[0113] Step 3: Add 1444.64 g of the first intermediate to 713.44 g of the second intermediate solution, mix well, and react at 80° C. for 3 h. Add 2880.4 g of solvent to obtain a polymer.

[0114] A method for preparing edge coating glue comprises the following steps: adding a polymer, boehmite and an auxiliary agent into a solvent in sequence, and stirring the mixture evenly to obtain the edge coating glue.

[0115] Performance testing methods and data

[0116] 1. The edge coating glue prepared in the examples and comparative examples was tested for storage stability by placing it in an oven at 70° C. for 2 days to observe whether stratification occurred.

[0117] 2. The edge coating glue prepared in the embodiment and the comparative example was coated on a glass plate and an aluminum foil, dried at 130°C for 1 hour, and the performance tests were performed: the tensile strength and elongation at break were tested according to GB / T13022-1991; the peel strength was tested according to GB / T2790-1995; the bonding substrate was an aluminum foil; electrolyte resistance: the samples of the embodiment and the comparative example were placed in an electrolyte (the electrolyte was Guotai Huarong LB301) for treatment, the treatment condition was immersion at 60°C for 24 hours, and the film was observed to see if it fell off the aluminum foil. Figure 1 As shown, the example did not fall off, while the comparative example 1 fell off.

[0118] 3. Processability

[0119] Take samples of the embodiment and comparative example for testing, and after being evenly dispersed, test the scraper particle size.

[0120] 4. CV curve

[0121] CV curves of the test examples and comparative samples; wherein the battery assembly: the negative electrode is a Li sheet; the positive electrode is a binder + Super (mass ratio 7:3) positive electrode current collector aluminum foil; the electrolyte is 1MLiPF6inEC / DMC=1 / 1vol%. CV test procedure: initial voltage: open circuit voltage; maximum voltage: 5.5V; minimum voltage 2.5V.

[0122] Scanning direction: normal scanning.

[0123] Scan speed: 0.1mV / s for the first circle, 1mV / s for the second circle.

[0124] Sampling interval: Take a data point every 2 seconds for performance test data.

[0125] The test data are listed in Table 1.

[0126] Table 1

[0127]

Claims

1. A side coating, characterized in that: The components include, by weight: 10-15 parts of polymer, 10-25 parts of boehmite, 0.5-5 parts of auxiliary agent and 50-70 parts of solvent.

2. The edge coating glue according to claim 1, characterized in that: The auxiliary agent includes at least one of a defoamer, a leveling agent and a thickener.

3. The edge coating glue according to claim 2, characterized in that: The auxiliary agent comprises a defoamer, a leveling agent and a thickener, and the weight ratio of the defoamer, the leveling agent and the thickener is (0.5-4): (0.5-3): (0.5-4).

4. The edge coating glue according to claim 3, characterized in that: The weight ratio of the polymer to boehmite is 1:(1-1.5).

5. The edge coating glue according to claim 1 or 4, characterized in that: The raw materials for preparing the polymer include a first intermediate and a second intermediate, wherein the first intermediate includes an isocyanate-terminated oligomer, and the second intermediate includes one of an amine-terminated oligomer and an anhydride-terminated oligomer.

6. The edge coating glue according to claim 5, characterized in that: The raw material for preparing the first intermediate includes at least one of polyether polyol and polyether amine.

7. The edge coating glue according to claim 6, characterized in that: The raw material for preparing the second intermediate includes at least one of aromatic diamine and aromatic diphthalic anhydride.

8. The edge coating glue according to claim 7, characterized in that: The raw materials for preparing the first intermediate and the second intermediate both further include diisocyanate.

9. A method for preparing the edge coating glue according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: adding polymer, boehmite and auxiliary agent into solvent in sequence and stirring evenly to obtain the product.

10. An application of the edge coating glue according to any one of claims 1 to 8, characterized in that: Used in the preparation of lithium battery pole pieces.

Citation Information

Cited By

  • Electrolyte-resistant acrylate pressure-sensitive adhesive and preparation method thereof

    CN120843020A