Method for realizing quantum dot thermally activated delayed fluorescence by using surface defect state and application of ZnSe-ZnS quantum dot
By regulating the particle size of ZnSe core quantum dots and the thickness of the ZnS shell, the surface defect states are used to achieve thermally activated delayed fluorescence of ZnSe@ZnS quantum dots, which solves the problem of insufficient fluorescence lifetime of ZnSe@ZnS quantum dots in the existing technology and achieves Efficient fluorescence lifetime extension and performance optimization.
Patent Information
- Application Number
- CN202410919648.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-08
AI Technical Summary
The fluorescence lifetime of existing ZnSe@ZnS quantum dots is difficult to reach the microsecond level, and the introduction of organic molecules is complex, the fluorescence quantum yield is low, and the carrier dynamics mechanism is complex, which affects the development and utilization of optoelectronic devices.
By controlling the particle size of ZnSe core quantum dots and the thickness of the ZnS shell, thermally activated delayed fluorescence between the quantum dot defect state energy level and its own energy level is achieved, and the surface defect state is used to extend the fluorescence lifetime of ZnSe@ZnS quantum dots from nanoseconds to Hundreds of microseconds, simplifying the material system preparation process.
It achieves a significant extension of the fluorescence lifetime of quantum dots without additional organic molecules, simplifies carrier dynamics, improves the fluorescence emission performance of the material, and is suitable for long-life fluorescence application scenarios.
Smart Images

Figure CN118745342A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermally activated delayed fluorescence, and in particular to a method for realizing thermally activated delayed fluorescence of quantum dots by utilizing surface defect states and the application of ZnSe@ZnS quantum dots. Background Art
[0002] Thermally activated delayed fluorescence is different from traditional fluorescence and phosphorescence emission. Its essence is that when the triplet excited state is close to the singlet excited state in energy, the triplet excited state can be reversed to the singlet excited state through thermal activation. This process takes place at room temperature, which can greatly extend the exciton lifetime and theoretically achieve 100% exciton utilization, which is of great significance for the application of related optoelectronic devices, especially the development of light-emitting diodes.
[0003] In recent years, thermally activated delayed fluorescence material systems with quantum dots as sensitizers and molecules as triplet receptors have begun to attract the attention of researchers. Based on quantum confinement and size effects, the energy levels of quantum dots can be arbitrarily controlled within a large range with their size. This feature makes the design of quantum dot-molecule systems more flexible. For specific quantum dot sensitizers, the selection of receptor molecules is more diversified, which is conducive to the application of thermally activated delayed fluorescence in various scenarios. However, in addition to the thermal activation process based on triplet energy transfer, other carrier processes are usually involved between quantum dots and molecules, such as singlet energy transfer, electron and hole transfer, etc. These carrier processes compete with triplet energy transfer, which not only increases the exciton quenching pathways of quantum dots and significantly reduces their fluorescence quantum yield, but also makes the analysis of carrier dynamics mechanisms more complicated, which is not conducive to the development and utilization of related optoelectronic devices.
[0004] ZnSe@ZnS core-shell quantum dots and similar derivatives are non-toxic blue light quantum dots with great application potential in the fields of environment, biology and display. Prolonging their fluorescence lifetime as much as possible is the key to optimizing the performance of related optoelectronic devices. At present, the means to extend the fluorescence lifetime of ZnSe@ZnS quantum dots mainly include optimizing components, passivating surface defects and introducing organic molecules. Among them, optimizing components or passivating surface defects mainly extend the fluorescence lifetime by regulating the energy level of the quantum dots themselves or inhibiting the non-radiative recombination of the excitons themselves, which cannot reach the microsecond level. The introduction of organic molecules can extend the fluorescence lifetime of quantum dots to microseconds or even milliseconds by realizing thermally activated delayed fluorescence through molecular triplet antisystem crossing (comparative documents: ACS Energy Lett., 2021, 6: 2786, patent: CN115612483A), but as mentioned above, this scheme usually involves complex carrier dynamics mechanisms, and the fluorescence quantum yield is relatively low.
[0005] In view of this, the present invention achieves reasonable energy level matching and surface defect state concentration regulation by controlling the particle size of ZnSe core quantum dots and the thickness of ZnS shell, which can realize thermally activated delayed fluorescence between the energy level of quantum dot defect states and the energy level of quantum dots themselves, and increase the fluorescence lifetime of quantum dots from the original 10ns to 95μs. This scheme does not introduce additional organic molecules, can simplify the preparation process of similar thermally activated delayed fluorescence material systems, reduce the many fluorescence attenuation pathways caused by the introduction of molecules, and thus optimize the fluorescence emission performance of the material. Summary of the invention
[0006] One of the purposes of the present invention is to provide a method for realizing thermally activated delayed fluorescence of quantum dots using surface defect states, and to realize thermally activated delayed fluorescence of ZnSe@ZnS core-shell quantum dots using surface defect states to adapt to the application scenarios of long-lived fluorescence.
[0007] A second object of the present invention is to provide an application of ZnSe@ZnS quantum dots.
[0008] The solution adopted by the present invention to achieve one of the purposes is: a method for realizing thermally activated delayed fluorescence of quantum dots by utilizing surface defect states, wherein ZnSe quantum dots with a first exciton absorption peak at 390nm-410nm are coated in a ZnS shell layer of appropriate thickness to obtain ZnSe@ZnS quantum dots, and in the absence of additional organic molecules, the surface defect states of the quantum dots are utilized to extend the fluorescence lifetime of the ZnSe quantum dots from the nanosecond level to the hundreds of microsecond level.
[0009] Preferably, the particle size of the ZnSe quantum dots is 3.0-4.0 nm; and the thickness of the ZnS shell is 0.3-0.65 nm.
[0010] Preferably, after the ZnSe quantum dots are excited by light, the singlet exciton energy is transferred to the surface defect state energy level through intersystem crossing to form localized triplet excitons. With the help of the smaller energy barrier between the surface defect state energy level and the singlet energy level of the quantum dots, the localized triplet excitons can reversely intersystem cross back to the singlet energy level of the ZnSe quantum dots under the action of thermal activation, thereby realizing thermally activated delayed fluorescence.
[0011] Preferably, the method for preparing ZnSe@ZnS quantum dots comprises the following steps:
[0012] (1) degassing the zinc source, oleic acid, oleylamine and octadecene, mixing them uniformly, injecting a diphenylphosphine solution of selenium powder Se-DPP under an inert atmosphere and at a certain temperature, and reacting for a certain time;
[0013] (2) Injecting zinc stearate octadecene solution ZnSt2-ODE and sulfur powder trioctylphosphine solution ZnSt2-ODE into the reaction system of step (1) in sequence, reacting and encapsulating at a certain temperature, separating the supernatant after the reaction and precipitating multiple times to obtain the ZnSe@ZnS quantum dots.
[0014] Preferably, in step (1), the zinc source is at least one of Zn(Ac)2, ZnSt2, and ZnO, and the mixing temperature is 100-150°C.
[0015] Preferably, in step (1), the reaction temperature is 280-320° C. and the reaction time is 7-15 min.
[0016] Preferably, the concentration range of Se-DPP is 80-110 mg / mL, the concentration of ZnSt2-ODE is 50-75 mg / mL, the concentration of S-TOP is 25-45 mg / mL, and the dosage ratio of the zinc source, oleic acid, oleylamine, octadecene, Se-DPP, ZnSt2-ODE, and S-TOP is 0.4588 g: 3 mL: 1 mL: 15 mL: 0.5 mL: 4-8 mL: 1-4 mL.
[0017] Preferably, in step (2), the reaction temperature is 260-310°C.
[0018] Preferably, in the step (2), the precipitation step is to mix the supernatant, ethanol or acetone, ethyl acetate or methyl acetate in a volume ratio of 0.5-1:1:1 and then centrifuge to obtain a precipitate, and precipitate the supernatant after centrifugation multiple times according to the above method, and combine the obtained precipitates to obtain the ZnSe@ZnS quantum dots.
[0019] The solution adopted by the present invention to achieve the second purpose is: an application of ZnSe@ZnS quantum dots, which can utilize surface defect states to realize quantum dot thermally activated delayed fluorescence and can be applied to light-emitting devices or photocatalytic fields requiring long excited state lifetime.
[0020] The present invention has the following advantages and beneficial effects:
[0021] The present invention utilizes surface defect states to realize thermally activated delayed fluorescence of ZnSe@ZnS core-shell quantum dots to adapt to the application scenarios of long-life fluorescence. The method for realizing thermally activated delayed fluorescence of quantum dots is realized by triplet energy transfer between quantum dots and their defect state energy levels without introducing additional organic molecules.
[0022] Compared with quantum dot-molecule thermally activated delayed fluorescence materials, the present invention does not involve additional ligand molecules, the scheme is simpler to implement, the carrier dynamics involved are simpler, and it is easier to study and apply. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The electron microscope images and absorption spectra of ZnSe@ZnS in Examples 1, 2, and 3;
[0024] Figure 2 The schematic diagram of ZnSe@ZnS thermally activated delayed fluorescence (TADF) is shown in Figure 1. TET is triplet energy transfer (or intersystem crossing); RTET is reverse triplet energy transfer (or reverse intersystem crossing); S0 is the ground state; S1 is the intrinsic singlet excited state of the quantum dot; T1 is the triplet excited state of the defect state of the quantum dot;
[0025] Figure 3 is the fluorescence lifetime of ZnSe@ZnS quantum dots under aerobic and anaerobic conditions in Example 2;
[0026] Figure 4 This is the dependence of the fluorescence intensity of ZnSe@ZnS on temperature in Example 2. DETAILED DESCRIPTION
[0027] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.
[0028] Example 1
[0029] The preparation process of ZnSe@ZnS core-shell structure quantum dots is as follows:
[0030] 0.4588g Zn(Ac)2, 3mL oleic acid, 1mL oleylamine and 15mL octadecene (ODE) were added to a three-necked flask, and the temperature was raised to 120°C and maintained for 60 minutes under vacuum degassing conditions. Nitrogen was introduced into the flask and the solution was heated to 303°C, followed by rapid injection of 0.5mL Se-DPP (0.1888g Se powder and 2mL DPP were added to a 5mL glass bottle with a rotor, and the glass bottle containing the reagents was ultrasonically placed on a hot plate at 100°C until the red solution became clear) and reacted for 7 minutes (the particle size of the obtained ZnSe core quantum dots was measured by transmission electron microscopy to be 3.02±0.23nm), and then 8mL ZnSt2-ODE (0.5176g ZnSt2 and 8mL ODE were added to a 10mL glass bottle and ultrasonicated for 5 minutes to fully mix) and S-TOP (0.077g S powder and 2ml TOP solution was added to a 5 ml glass bottle, and ultrasonicated for 5 minutes to completely dissolve the yellow S powder to present a colorless solution), then the temperature was set to 280 ° C for 60 minutes, and the heater power was turned off after the reaction, the heating jacket was removed, and the temperature was naturally cooled to below 60 ° C, and then the original solution in the flask was poured into a centrifuge tube, and the centrifuge tube was placed in a centrifuge and centrifuged at 3000 rpm for 4 minutes. The supernatant was taken and added to the centrifuge tube in an amount of supernatant: ethanol: ethyl acetate = 1:1:1, and then the supernatant was added to the centrifuge tube and shaken well, and then centrifuged at 10000 rpm for 3 minutes. The obtained precipitate was dissolved with 5 mL of n-hexane, and the obtained supernatant was continued to be added with the same amount of ethanol and ethyl acetate for centrifugation. The obtained precipitate was added Add 5mL of n-hexane solvent, repeat this operation 3 times, and the resulting solution is the ZnSe@ZnS quantum dot solution (the particle size of the ZnSe@ZnS quantum dots measured by transmission electron microscopy is 4.32±0.27nm, and the ZnS shell thickness is about 0.65nm). The ZnSe@ZnS quantum dot solution obtained above is placed in a 1mm quartz cuvette to test the UV-visible absorption spectrum. The concentration of the quantum dots is determined by comparing the UV absorption spectrum. When the quantum dot concentration with the first exciton absorption peak at 390nm is 1umol / L, the absorbance at 380nm is 0.5. According to the Lambert-Beer law, the concentration of the prepared quantum dots can be calculated to be 200uM.
[0031] Take 5 mL of 10 umol / L ZnSe@ZnS quantum dot solution with the first exciton absorption peak at 390 nm, then take 1 mL of the above solution respectively, add 2 mL of n-hexane for dilution to obtain two identical solutions, one of which is placed in an air atmosphere and filled with an ordinary 1 cm cuvette, and the other solution is placed in a glove box and aspirated 20 times with a syringe, then left open for 20 minutes to deoxygenate, and then filled into a 1 cm long head cuvette, and the fluorescence spectra of the two samples are tested separately using Edinburgh FLS980.
[0032] Using 380nm light excitation, the fluorescence lifetime of quantum dots under aerobic and anaerobic conditions was tested respectively, and the result showed that the fluorescence lifetime of quantum dots under aerobic conditions was 5ns, and the fluorescence lifetime of quantum dots under anaerobic conditions was 100ns.
[0033] Figure 1 (a) and (b) show the electron microscope images and absorption spectra of ZnSe@ZnS. It can be seen from the figures that the particle size of ZnSe@ZnS is about 4.3nm, and the corresponding first exciton absorption peak position is 390nm.
[0034] Example 2
[0035] The preparation process of ZnSe@ZnS core-shell structure quantum dots is as follows:
[0036] 0.4588g Zn(Ac)2, 3mL oleic acid, 1mL oleylamine and 15mL octadecene (ODE) were added to a three-necked flask, and the temperature was raised to 120°C and maintained for 60 minutes under vacuum degassing conditions. Nitrogen was introduced into the flask and the solution was heated to 303°C, followed by rapid injection of 0.5mL Se-DPP (0.1888g Se powder and 2mL DPP were added to a 5mL glass bottle with a rotor, and the glass bottle containing the reagents was ultrasonically placed on a hot plate at 100°C until the red solution became clear) and reacted for 10 minutes (the particle size of the obtained ZnSe core quantum dots was measured by transmission electron microscopy to be 3.61±0.18nm), and then 8mL ZnSt2-ODE (0.5176g ZnSt2 and 8mL ODE were added to a 10mL glass bottle and ultrasonically mixed for 5 minutes) and S-TOP (0.077g S powder and 2ml TOP solution was added to a 5 ml glass bottle, and ultrasonicated for 5 minutes to completely dissolve the yellow S powder to present a colorless solution), then the temperature was set to 280 ° C for 60 minutes of reaction, and after the reaction, the heater power was turned off, the heating jacket was removed, and the temperature was naturally cooled to below 60 ° C, and then the original solution in the flask was poured into a centrifuge tube, the centrifuge tube was placed in a centrifuge and centrifuged at 3000 rpm for 4 minutes, the supernatant was taken, and the supernatant: ethanol: ethyl acetate = 1:1:1 was added to the centrifuge tube, shaken and continued to be centrifuged at 10000 rpm for 3 minutes, the obtained precipitate was dissolved with 5 mL of n-hexane, and the same amount of ethanol and ethyl acetate was added to the obtained supernatant for centrifugation, and 5 mL of n-hexane solvent was added to the obtained precipitate, and this operation was repeated 3 times. The obtained solution is a ZnSe@ZnS quantum dot solution (the particle size of the obtained ZnSe@ZnS quantum dots measured by transmission electron microscopy is 4.85±0.17nm, and the ZnS shell thickness is about 0.62nm). The ZnSe@ZnS quantum dot solution obtained above is placed in a 1mm quartz cuvette to test the UV-visible absorption spectrum. The concentration of the quantum dots is determined by comparing the UV absorption spectrum. When the quantum dot concentration with the first exciton absorption peak at 400nm is 1umol / L, the absorbance at 380nm is 0.5. According to the Lambert-Beer law, it can be calculated that the concentration of the prepared quantum dots is 200uM.
[0037] The fluorescence spectrum test process is as in Example 1. Using 380nm light excitation, the quantum dot fluorescence lifetime with the first exciton absorption peak at 400nm under aerobic and anaerobic conditions was tested respectively. Under aerobic conditions, the triplet state was quenched by oxygen, and the quantum dot fluorescence lifetime was 10ns. Under anaerobic conditions, due to thermally activated delayed fluorescence, the quantum dot fluorescence lifetime was 95μs. The variable temperature fluorescence of 203K-303K shows that the fluorescence intensity of ZnSe@ZnS quantum dots gradually increases during the temperature rise from 203K to 233K, which is one of the spectral characteristics of thermally activated delayed fluorescence.
[0038] Figure 1 (c) and (d) show the electron microscope images and absorption spectra of ZnSe@ZnS. It can be seen from the figures that the particle size of ZnSe@ZnS is about 4.8nm, and the corresponding first exciton absorption peak position is 400nm.
[0039] Figure 2 The figure shows the principle diagram of ZnSe@ZnS thermally activated delayed fluorescence (TADF); TET is triplet energy transfer (or intersystem crossing); RTET is reverse triplet energy transfer (or reverse intersystem crossing); S0 is the ground state; S1 is the intrinsic singlet excited state of the quantum dot; T1 is the triplet excited state of the quantum dot defect state
[0040] Figure 3 The figure shows the fluorescence lifetime of ZnSe@ZnS quantum dots under aerobic and anaerobic conditions in this embodiment. It can be seen from the figure that: compared with aerobic conditions, the fluorescence decay of quantum dots under anaerobic conditions is accelerated to a certain extent at short lifetimes (before 100 nanoseconds), which corresponds to the TET process of the intrinsic excitons of ZnSe@ZnS quantum dots to the quantum point defect state; and at a temperature greater than 1 microsecond, there is no fluorescence decay signal under aerobic conditions, and there is a long-lifetime decay signal under anaerobic conditions, which corresponds to the RTET process of the ZnSe@ZnS quantum dot defect state to its singlet state under thermal activation.
[0041] Figure 4 The figure shows the dependence of the fluorescence intensity of ZnSe@ZnS on temperature in this embodiment. It can be seen from the figure that when the temperature is lower than 243K, the fluorescence emission intensity of ZnSe@ZnS quantum dots increases with increasing temperature, which is a typical feature of thermally activated delayed fluorescence.
[0042] Example 3
[0043] The preparation process of ZnSe@ZnS core-shell structure quantum dots is as follows:
[0044] 0.4588g Zn(Ac)2, 3mL oleic acid, 1mL oleylamine and 15mL octadecene (ODE) were added to a three-necked flask, and the temperature was raised to 120°C and maintained for 60 minutes under vacuum degassing conditions. Nitrogen was introduced into the flask and the solution was heated to 303°C, followed by rapid injection of 0.5mL Se-DPP (0.1888g Se powder and 2mL DPP were added to a 5mL glass bottle with a rotor, and the glass bottle containing the reagents was ultrasonically placed on a hot plate at 100°C until the red solution became clear) and reacted for 15 minutes (the particle size of the obtained ZnSe core quantum dots was measured by transmission electron microscopy to be 4.04±0.19nm), and then 8mL ZnSt2-ODE (0.5176g ZnSt2 and 8mL ODE were added to a 10mL glass bottle and ultrasonicated for 5 minutes to fully mix) and S-TOP (0.077g S powder and 2ml TOP solution was added to a 5 ml glass bottle, and ultrasonicated for 5 minutes to completely dissolve the yellow S powder to present a colorless solution), then the temperature was set to 280 ° C for 60 minutes of reaction, and after the reaction, the heater power was turned off, the heating jacket was removed, and the temperature was naturally cooled to below 60 ° C, and then the original solution in the flask was poured into a centrifuge tube, the centrifuge tube was placed in a centrifuge and centrifuged at 3000 rpm for 4 minutes, the supernatant was taken, and the supernatant: ethanol: ethyl acetate = 1:1:1 was added to the centrifuge tube, shaken and continued to be centrifuged at 10000 rpm for 3 minutes, the obtained precipitate was dissolved with 5 mL of n-hexane, and the same amount of ethanol and ethyl acetate was added to the obtained supernatant for centrifugation, and 5 mL of n-hexane solvent was added to the obtained precipitate, and this operation was repeated 3 times. The obtained solution is a ZnSe@ZnS quantum dot solution (the particle size of the obtained ZnSe@ZnS quantum dots measured by transmission electron microscopy is 5.30±0.25nm, and the ZnS shell thickness is about 0.63nm). The ZnSe@ZnS quantum dot solution obtained above is placed in a 1mm quartz cuvette to test the UV-visible absorption spectrum. The concentration of the quantum dots is determined by comparing the UV absorption spectrum. When the quantum dots with the first exciton absorption peak at 410nm have an absorbance of 1umol / L at 380nm, the absorbance is 0.5. According to the Lambert-Beer law, the concentration of the prepared quantum dots can be calculated to be 200uM.
[0045] The fluorescence spectrum test process is the same as in Example 1. Using 380nm light excitation, the quantum dot fluorescence lifetime with the first exciton absorption peak at 410nm under aerobic and anaerobic conditions was tested respectively, and the quantum dot fluorescence lifetime under aerobic conditions was 12ns, and the quantum dot fluorescence lifetime under anaerobic conditions was 7μs.
[0046] Figure 1(e) and (f) show the electron microscope images and absorption spectra of ZnSe@ZnS. It can be seen from the figures that the particle size of ZnSe@ZnS is about 5.3nm, and the corresponding first exciton absorption peak position is 410nm.
[0047] Example 4
[0048] The preparation process of ZnSe@ZnS core-shell structure quantum dots is as follows:
[0049] 0.4588g Zn(Ac)2, 3mL oleic acid, 1mL oleylamine and 15mL octadecene (ODE) were added to a three-necked flask, and the temperature was raised to 120°C and maintained for 60 minutes under vacuum degassing conditions. Nitrogen was introduced into the flask and the solution was heated to 303°C, followed by rapid injection of 0.5mL Se-DPP (0.1888g Se powder and 2mL DPP were added to a 5mL glass bottle with a rotor, and the glass bottle containing the reagents was ultrasonically placed on a hot plate at 100°C until the red solution became clear) and reacted for 10 minutes (the particle size of the obtained ZnSe core quantum dots was measured by transmission electron microscopy to be 3.61±0.18nm), and 4mL ZnSt2-ODE (0.2588g ZnSt2 and 4mL ODE were added to a 5mL glass bottle and ultrasonically mixed for 5 minutes) and S-TOP (0.0385g S powder and 1ml TOP solution was added to a 5 ml glass bottle, and ultrasonicated for 5 minutes to completely dissolve the yellow S powder to present a colorless solution), then the temperature was set to 280 ° C for 60 minutes of reaction, and after the reaction, the heater power was turned off, the heating jacket was removed, and the temperature was naturally cooled to below 60 ° C, and then the original solution in the flask was poured into a centrifuge tube, the centrifuge tube was placed in a centrifuge and centrifuged at 3000 rpm for 4 minutes, the supernatant was taken, and the supernatant: ethanol: ethyl acetate = 1:1:1 was added to the centrifuge tube, shaken and continued to be centrifuged at 10000 rpm for 3 minutes, the obtained precipitate was dissolved with 5 mL of n-hexane, and the same amount of ethanol and ethyl acetate was added to the obtained supernatant for centrifugation, and 5 mL of n-hexane solvent was added to the obtained precipitate, and this operation was repeated 3 times. The obtained solution is a ZnSe@ZnS quantum dot solution (the particle size of the obtained ZnSe@ZnS quantum dots measured by transmission electron microscopy is 4.21±0.22nm, and the ZnS shell thickness is about 0.3nm). The ZnSe@ZnS quantum dot solution obtained above is placed in a 1mm quartz cuvette to test the UV-visible absorption spectrum. The concentration of the quantum dots is determined by comparing the UV absorption spectrum. When the quantum dots with the first exciton absorption peak at 400nm have a concentration of 1umol / L, the absorbance at 380nm is 0.5. According to the Lambert-Beer law, it can be calculated that the concentration of the prepared quantum dots is 200uM.
[0050] The fluorescence spectrum test process is the same as in Example 1. Using 380nm light excitation, the fluorescence lifetime of quantum dots with the first exciton absorption peak at 400nm under aerobic and anaerobic conditions was tested respectively, and the fluorescence lifetime of quantum dots under aerobic conditions was 1ns, and the fluorescence lifetime of quantum dots under anaerobic conditions was 200ns.
[0051] Table 1 shows the spectrum test results of Examples 1-4.
[0052]
[0053] From the data in Table 1, it can be seen that the particle size and shell thickness of ZnSe@ZnS quantum dots are the main factors affecting their thermally activated delayed fluorescence lifetime. Comparing Examples 2 and 4, when the shell thickness of the quantum dots is reduced from 0.62nm to 0.30nm, the longest thermally activated delayed fluorescence lifetime cannot be obtained. This is because the passivation effect of the ZnS shell on the surface of the ZnSe core layer is reduced, and the surface defect state concentration is too high, which causes serious fluorescence quenching of the quantum dots; Comparing Examples 1, 2, and 3, when the ZnS shell thickness is almost the same, when the particle size of the ZnSe core quantum dots is about 3.6nm, the longest thermally activated delayed fluorescence lifetime appears (i.e., Example 2, which is 95μs, which is significantly extended compared to the intrinsic exciton lifetime of the quantum dots of 0.01μs); and the thermally activated delayed fluorescence lifetime obtained in Example 1 is 0.1μs, which is also caused by the excessively high surface defect state concentration of the small-particle ZnSe core quantum dots; for Example 3, when the quantum dot particle size is further increased compared to Example 2, the longest thermally activated delayed fluorescence lifetime cannot be obtained due to the too low surface defect state concentration of the ZnSe core quantum dots. In summary, to achieve the longest thermally activated delayed fluorescence lifetime, it is necessary to simultaneously regulate the quantum dot core particle size and shell thickness to ensure the optimal defect state concentration.
[0054] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.
Claims
1. A method for realizing quantum dot thermally activated delayed fluorescence using surface defect states, characterized in that: ZnSe quantum dots with the first exciton absorption peak at 390nm-410nm are coated in a ZnS shell of appropriate thickness to obtain ZnSe@ZnS quantum dots. In the absence of additional organic molecules, the surface defect states of the quantum dots are used to extend the fluorescence lifetime of the ZnSe quantum dots from nanoseconds to hundreds of microseconds.
2. The method for realizing quantum dot thermally activated delayed fluorescence using surface defect states according to claim 1, characterized in that: The particle size of the ZnSe quantum dots is 3.0-4.0 nm; the thickness of the ZnS shell is 0.3-0.65 nm.
3. The method for realizing quantum dot thermally activated delayed fluorescence using surface defect states according to claim 1, characterized in that: After the ZnSe quantum dots are excited by light, the singlet exciton energy is transferred to the surface defect state energy level through intersystem crossing to form localized triplet excitons. With the help of the smaller energy barrier between the surface defect state energy level and the singlet energy level of the quantum dots, the localized triplet excitons can reversely intersystem cross back to the singlet energy level of the ZnSe quantum dots under the action of thermal activation, thereby realizing thermally activated delayed fluorescence.
4. The method for realizing quantum dot thermally activated delayed fluorescence using surface defect states according to claim 1, characterized in that: The preparation method of ZnSe@ZnS quantum dots comprises the following steps: (1) degassing the zinc source, oleic acid, oleylamine and octadecene, mixing them uniformly, injecting a diphenylphosphine solution of selenium powder Se-DPP under an inert atmosphere and at a certain temperature, and reacting for a certain time; (2) Injecting zinc stearate octadecene solution ZnSt2-ODE and sulfur powder trioctylphosphine solution ZnSt2-ODE into the reaction system of step (1) in sequence, reacting and encapsulating at a certain temperature, separating the supernatant after the reaction and precipitating multiple times to obtain the ZnSe@ZnS quantum dots.
5. The method for realizing quantum dot thermally activated delayed fluorescence using surface defect states according to claim 4, characterized in that: In the step (1), the zinc source is at least one of Zn(Ac)2, ZnSt2, and ZnO, and the mixing temperature is 100-150°C.
6. The method for realizing quantum dot thermally activated delayed fluorescence using surface defect states according to claim 4, characterized in that: In the step (1), the reaction temperature is 280-320° C. and the reaction time is 7-15 min.
7. The method for realizing quantum dot thermally activated delayed fluorescence using surface defect states according to claim 4, characterized in that: The concentration range of Se-DPP is 80-110 mg / mL, the concentration of ZnSt2-ODE is 50-75 mg / mL, the concentration of S-TOP is 25-45 mg / mL, and the dosage ratio of the zinc source, oleic acid, oleylamine, octadecene, Se-DPP, ZnSt2-ODE, and S-TOP is 0.4588 g: 3 mL: 1 mL: 15 mL: 0.5 mL: 4-8 mL: 1-4 mL.
8. The method for realizing quantum dot thermally activated delayed fluorescence using surface defect states according to claim 4, characterized in that: In the step (2), the reaction temperature is 260-310°C.
9. The method for realizing quantum dot thermally activated delayed fluorescence using surface defect states according to claim 4, characterized in that: In the step (2), the precipitation step is to mix the supernatant, ethanol or acetone, ethyl acetate or methyl acetate in a volume ratio of 0.5-1:1:1 and then centrifuge to obtain a precipitate, and precipitate the supernatant after centrifugation multiple times according to the above method, and combine the obtained precipitates to obtain the ZnSe@ZnS quantum dots.
10. An application of ZnSe@ZnS quantum dots, characterized by: The ZnSe@ZnS quantum dots can utilize surface defect states to realize quantum dot thermally activated delayed fluorescence, and can be applied to light-emitting devices or photocatalysis fields that require a long excited state lifetime.