Method for producing steel by alloying vanadium-containing molten iron
By calculating the target dosage of vanadium-containing molten iron and adding scrap steel, the accurate deployment of molten steel in the ladle is achieved, solving the problems of complex and high-cost mixing of molten iron in the existing technology, and improving the efficiency and output of steel production.
Patent Information
- Application Number
- CN202410742655.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-11
AI Technical Summary
In the prior art, the operation steps of adding molten iron to the ladle are complicated and it is difficult to accurately prepare the components of the molten steel, which increases production costs and operational complexity.
By obtaining the end-point composition of the molten steel, calculating the target amount of vanadium-containing molten iron, overloading and then adding scrap steel to form molten iron for the converter, which is mixed into the ladle for alloying through the converter inversion operation, and finally steel is obtained through argon blowing. products to ensure the accurate blending of molten steel components.
The operation steps are simplified, the production cost is reduced, the accurate preparation of molten steel components and the increase of steel production are achieved.
Smart Images

Figure CN118745496A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of steel smelting, and in particular to a method for producing steel by alloying vanadium-containing molten iron. Background Art
[0002] After the converter is finished tapping, since the molten steel in the ladle is in a reducing atmosphere, adding a specific proportion of molten iron into the ladle instead of the carburizer can produce ordinary carbon steel, medium carbon steel and high carbon steel. At the same time, this process has the advantages of stable and uniform carbon absorption rate, and there is no need to consciously increase the tapping temperature. This method can not only effectively increase steel production, but also reduce the consumption of alloys. The method of adding molten iron can also be set before tapping: after adding deoxidizer and alloy to the bottom of the ladle, a small amount of molten iron is added, and the high-temperature steel flow is used to flush, stir and mix during the tapping process to replace the carburizer to produce ordinary carbon steel, medium carbon steel and high carbon steel. If the slag-down process of the converter tapping is well controlled, no violent carbon-oxygen reaction will occur. At this time, adding a specific proportion of molten iron can control the phosphorus content of the molten steel within the specified range. Under the current steel situation, such measures to reduce the production cost of steelmaking have certain feasibility.
[0003] However, according to the actual situation of the steel mill and taking into account the operation rate of the overhead crane, the best ladle iron filling method or combination method can be selected to solve the ladle iron filling problem. At present, there are two ways to achieve the ladle iron filling method:
[0004] (1) At the tapping span of the converter, a certain proportion of molten iron (such as Figure 4 The benefit of this measure is that the electronic scale on the existing overhead crane can be used to accurately measure the weight of the molten iron poured into the ladle, providing accurate data for the furnace front alloy. However, this increases the operation rate of the overhead crane, which will have a greater impact on the normal production organization order, increase production costs, and the overall operation is more complicated;
[0005] (2) On the raw material trough in the converter workshop, a certain amount of molten iron is loaded after or before the converter is tapped, and then poured into the ladle on the ladle car under the converter through the normal converter pouring operation. This process is fed back to the converter operation platform through the electronic scale weighing system on the ladle car, which can display the weight of the poured molten iron, which provides data for the converter carbon matching and alloying operations. The advantage of this process is that it will not significantly increase the operating burden of the converter, only increase the time of one converter pouring, and will not significantly increase the normal operation tasks of the converter. However, this process increases the investment in weighing equipment for the converter ladle car. The ladle scale must meet the use characteristics of high temperature and strong impact, and it is also necessary to use imported high-temperature strain gauges and high-temperature compensation, aging, and testing processes; and in order to achieve the accuracy of the data feedback process, the lead wire also needs to be specially protected, such as setting a flame retardant layer on the outside of the lead wire to prevent the lead wire from being burned by molten steel, which will undoubtedly increase production costs, and will also affect the allocation of molten steel components due to the burning of the flame retardant layer or other equipment. Summary of the invention
[0006] The present application provides a method for producing steel by alloying vanadium-containing molten iron, so as to solve the technical problems in the prior art of adding molten iron to a ladle, which exist in complicated operation steps and difficulty in accurately allocating the composition of molten steel.
[0007] In a first aspect, the present application provides a method for producing steel by alloying vanadium-containing molten iron, the method comprising:
[0008] Obtain the endpoint composition of molten steel;
[0009] Calculate the target amount of vanadium-containing molten iron required for adding molten iron to the ladle according to the endpoint composition of the molten steel, the composition of the vanadium-containing molten iron and the target composition of steel production;
[0010] The vanadium-containing molten iron is overloaded with the target dosage as a reference value, and then scrap steel is added to the vanadium-containing molten iron to obtain molten iron for a converter;
[0011] Performing a converter pouring operation on the converter molten iron so that the converter molten iron is added into a ladle containing the molten steel for alloying to obtain coarse molten steel;
[0012] Blowing argon into the crude molten steel to obtain a steel product;
[0013] Wherein, the chemical composition of the vanadium-containing molten iron includes, by mass fraction:
[0014] C: 4.20% ~ 6.80%, Si: 0.30% ~ 0.70%, Mn: 0.30% ~ 0.70%, P: 0.12% ~ 0.15%, S: 0.02% ~ 0.07%, Ti: 0.10% ~ 0.50%, V: 0.05% ~ 0.20%, Cr: 0.10% ~ 0.20%, and the rest are Fe and unavoidable impurities.
[0015] Optionally, the mass ratio of the overload filling amount to the target amount is 2% to 3%.
[0016] Optionally, the step of obtaining the endpoint composition of the molten steel comprises the following steps:
[0017] Mixing vanadium-containing molten iron and scrap steel to obtain initial smelting molten iron;
[0018] The initial smelting molten iron is subjected to converter blowing to obtain initial dephosphorized molten iron;
[0019] The initial dephosphorized molten iron is subjected to converter tapping and argon blowing treatment to obtain an initial ladle;
[0020] The composition of the initial ladle is detected and calculated to obtain the endpoint composition of the molten steel.
[0021] Optionally, the converter blowing includes a first stage blowing, a second stage blowing and a third stage blowing;
[0022] The oxygen supply intensity of the first stage blowing is 2.9Nm 3 / min / t~3.1Nm 3 / min / t, the blowing time of the first stage is 1min~3min;
[0023] The oxygen supply intensity of the second stage blowing is 3.2Nm 3 / min / t~3.4Nm 3 / min / t, the blowing time of the second stage is 3min~5min;
[0024] The oxygen supply intensity of the third stage blowing is 2.9Nm 3 / min / t~3.1Nm 3 / min / t, and the blowing time of the third stage is 2min~4min.
[0025] Optionally, the temperature of the initial molten steel is 1650° C. to 1670° C., and the carbon content of the initial molten steel is 0.03% to 0.08%.
[0026] Optionally, the converter blowing also includes full iron reduction blowing, the time of the full iron reduction blowing is 2.0 minutes to 2.5 minutes before the end of the converter blowing, and the time of the full iron reduction blowing is ≥120 seconds.
[0027] Optionally, the second stage blowing includes performing the second stage blowing by adding a slag-forming agent, wherein the mass ratio of the slag-forming agent to the total slag amount of the converter blowing is 70% to 80%;
[0028] Wherein, the chemical composition of the slag-forming agent includes, by mass fraction:
[0029] Active lime: 85% to 95% and dolomite: 5% to 15%; and / or,
[0030] The third stage blowing includes adding lime to carry out the third stage blowing, and the amount of lime added is 2.1kg / t to 2.3kg / t.
[0031] Optionally, the mass ratio of the added scrap steel to the molten iron for the converter is 10% to 25%.
[0032] Optionally, the argon pressure of the argon blowing treatment is 0.1 MPa to 0.7 MPa, the gas flow rate of the argon blowing treatment is 1000 NL / min to 1200 NL / min, and the time of the argon blowing treatment is ≥4 min.
[0033] Optionally, the converter steel tapping includes a nitrogen purge stage, and the nitrogen purge time is 2s to 4s.
[0034] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0035] The embodiment of the present application provides a method for producing steel by alloying vanadium-containing molten iron, which comprises first smelting vanadium-containing molten iron and scrap steel to obtain an initial ladle, then calculating the composition of the initial molten steel and the vanadium-containing molten iron in combination with the target composition of steel production to determine the target amount of vanadium-containing molten iron required for subsequent converter refueling, combining the calculated target amount and overloading to ensure that there is enough vanadium-containing molten iron in the converter, at which time the vanadium-containing molten iron will be mixed with the slag and other alloy components in the converter to form molten iron for the converter. Since the vanadium-containing molten iron contains C, V and Ti, which makes the molten iron for the converter contain beneficial elements such as C, V, Ti, Si, Mn and Cr, and then the molten iron in the initial ladle is added by turning the converter, so that the beneficial elements in the molten iron in the converter are introduced into the initial ladle, and the molten iron in the converter is transformed into molten steel; the whole method only needs one more step of overloading and converter turning operation, and the operation rate of the converter charging crane will not be increased, and the operation steps are reduced. At the same time, the target dosage of the method is mainly obtained through calculation, which makes the overall method easy to operate and can achieve accurate allocation of molten steel composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0037] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0038] Figure 1 A schematic flow chart of a method for producing steel by alloying vanadium-containing molten iron provided in an embodiment of the present application;
[0039] Figure 2 A detailed schematic diagram of a method for producing steel by alloying vanadium-containing molten iron provided in an embodiment of the present application;
[0040] Figure 3 A schematic diagram of an industrial process of producing steel by alloying vanadium-containing molten iron provided in an embodiment of the present application;
[0041] Figure 4 This is a schematic diagram of the operation of adding molten iron to the ladle at the current stage provided for this application. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0043] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0044] Figure 1 A schematic flow chart of a method for producing steel by alloying vanadium-containing molten iron provided in an embodiment of the present application is shown as an example;
[0045] like Figure 1 As shown, the embodiment of the present application provides a method for producing steel by alloying vanadium-containing molten iron, the method comprising:
[0046] S1. Obtaining the endpoint composition of molten steel;
[0047] S2 is calculated based on the endpoint composition of the molten steel, the composition of the vanadium-containing molten iron and the target composition of steel production to obtain the target amount of vanadium-containing molten iron required for the ladle with molten iron;
[0048] S3. The target amount is used as a reference value to overload the vanadium-containing molten iron, and then scrap steel is added to the vanadium-containing molten iron to obtain molten iron for the converter;
[0049] S4. The converter is subjected to a converter downdraft operation so that the converter is blended with molten iron into the ladle containing the molten steel for alloying to obtain a coarse grade molten steel;
[0050] S5. The coarse grade molten steel is subjected to argon blowing to obtain a steel product;
[0051] Wherein, the chemical composition of the vanadium-containing molten iron includes, by mass fraction:
[0052] C: 4.20% ~ 6.80%, Si: 0.30% ~ 0.70%, Mn: 0.30% ~ 0.70%, P: 0.12% ~ 0.15%, S: 0.02% ~ 0.07%, Ti: 0.10% ~ 0.50%, V: 0.05% ~ 0.20%, Cr: 0.10% ~ 0.20%, and the rest are Fe and unavoidable impurities.
[0053] In these embodiments, the specific chemical composition of the vanadium-containing molten iron is refined to include: C: 4.20% ~ 6.80%, Si: 0.30% ~ 0.70%, Mn: 0.30% ~ 0.70%, P: 0.12% ~ 0.15%, S: 0.02% ~ 0.07%, Ti: 0.10% ~ 0.50%, V: 0.05% ~ 0.20%, Cr: 0.10% ~ 0.20%, and the rest is Fe and inevitable impurities. This is to clarify the specific contents of C, Mn, Ti, V and Cr in the vanadium-containing molten iron, so as to facilitate the subsequent introduction of beneficial elements in the vanadium-containing molten iron into molten steel by adding molten iron to the ladle, thereby effectively increasing the vanadium and titanium elements in the molten steel and stabilizing the absorption rate of these elements, thereby achieving accurate allocation of the molten steel composition, thereby effectively reducing the steelmaking cost and increasing steel production.
[0054] It should be noted that the amount of molten iron poured out during the converter pouring operation can be counted by the set metering equipment, and in order to facilitate the operation of the overall method, the metering equipment can be combined with the ladle container to control the amount of molten iron added to the ladle in real time.
[0055] It should be noted that the steel tapping from the converter can also include slag pouring and shaking the furnace operation, and the specific steps of the slag pouring and shaking the furnace operation include: tilting the furnace body of the converter from a vertical state to a position at 77° to 82° to the vertical plane and maintaining it for 4s to 6s, and then tilting the furnace body from the position of 77° to 82° to a position at 84° to 85° to the vertical plane. The slag pouring and shaking furnace operation can fully pour out the slag from the converter.
[0056] In some optional embodiments, the mass ratio of the overload filling amount to the target amount is 2% to 3%; in these embodiments, by controlling the specific mass ratio of the overload filling amount to the target amount to 2% to 3%, the vanadium-containing molten iron can be fully mixed with the alloying elements in the converter by overload filling, so as to further increase the content of beneficial elements, thereby facilitating the subsequent introduction of beneficial elements into the molten steel by adding molten iron to the ladle.
[0057] The mass ratio of the overload filling amount to the target amount can be 2.0%, 2.5% or 3.0%.
[0058] Figure 2 A detailed schematic diagram of a method for producing steel by alloying vanadium-containing molten iron provided in an embodiment of the present application is shown as an example;
[0059] like Figure 2 As shown, in some optional embodiments, the method of obtaining the endpoint composition of the molten steel comprises the steps of:
[0060] S101. Mixing vanadium-containing molten iron and scrap steel to obtain an initial smelting molten iron;
[0061] S102. The initial smelting molten iron is subjected to converter blowing to obtain initial dephosphorized molten iron;
[0062] S103. The initial dephosphorized molten iron is subjected to converter tapping and argon blowing to obtain an initial ladle;
[0063] S104. The composition of the initial ladle is detected and calculated to obtain the final composition of the molten steel. In these embodiments, the specific converter smelting process of controlling the initial smelting molten iron includes converter blowing, converter tapping and argon blowing treatment. The vanadium-containing molten iron and scrap steel can be fully mixed by converter blowing, converter tapping and argon blowing treatment to obtain the initial ladle, thereby saving raw materials for steel smelting.
[0064] It should be noted that, during the process of tapping steel from the converter, an iron alloy may be added to the bottom of the ladle for alloying; the iron alloy may be a ferrosilicon alloy, a ferromanganese alloy, or a mixture of a ferrosilicon alloy and a ferromanganese alloy.
[0065] In some optional embodiments, the converter blowing includes a first stage blowing, a second stage blowing and a third stage blowing;
[0066] The oxygen supply intensity of the first stage blowing is 2.9Nm 3 / min / t~3.1Nm 3 / min / t, the blowing time of the first stage is 1min~3min;
[0067] The oxygen supply intensity of the second stage blowing is 3.2Nm 3 / min / t~3.4Nm 3 / min / t, the blowing time of the second stage is 3min~5min;
[0068] The oxygen supply intensity of the third stage blowing is 2.9Nm 3 / min / t~3.1Nm 3 / min / t, and the time of the third stage blowing is 2min~4min; in these embodiments, by refining the specific steps of the converter blowing including the first stage blowing, the second stage blowing and the third stage blowing, and by splitting the converter blowing into three stages, different slag removal measures can be adopted in different stages, so that the smelting molten iron is converted into molten steel with low carbon content after the converter blowing.
[0069] The oxygen supply intensity of the first stage blowing can be 2.9Nm 3 / min / t, 3.0Nm 3 / min / t or 3.1Nm3 / min / t.
[0070] The specific blowing time of the first stage can be 1 min, 2 min or 3 min.
[0071] The oxygen supply intensity of the second stage blowing can be 3.2Nm 3 / min / t, 3.3Nm 3 / min / t or 3.4Nm 3 / min / t.
[0072] The second stage blowing time can be 3 minutes, 4 minutes or 5 minutes.
[0073] The oxygen supply intensity of the third stage blowing can be 2.9Nm 3 / min / t, 3.0Nm 3 / min / t or 3.1Nm 3 / min / t.
[0074] The blowing time of the third stage can be 2 minutes, 3 minutes or 4 minutes.
[0075] It should be noted that during the converter blowing process, the height of the blowing lance used in different stages of blowing from the molten iron will vary. For example, during the first and second stages of blowing, the height of the blowing lance gradually decreases from 1.8m~2.0m to 1.1m~1.3m; and during the third stage of blowing, the height of the blowing lance gradually decreases from 1.1m~1.3m to 0.9m~1.1m.
[0076] In some optional embodiments, the temperature of the initial molten steel is 1650°C ~ 1670°C, and the carbon content of the initial molten steel is 0.03% ~ 0.08%; in this embodiment, the temperature of the initial molten steel is limited to 1650°C ~ 1670°C, and the carbon content of the initial molten steel is limited to 0.03% ~ 0.08%, so that the temperature in the ladle during the molten iron adding stage can be sufficient for the molten iron and molten steel to react, and the carbon content of the initial molten steel in the ladle is adjusted to the target carbon content of the steel product by adding molten iron.
[0077] The temperature of the initial molten steel may be 1650°C, 1655°C, 1660°C, 1665°C or 1670°C.
[0078] The carbon content of the initial molten steel may be 0.03%, 0.04%, 0.05%, 0.06%, 0.07% or 0.08%.
[0079] In some optional embodiments, the converter blowing also includes full iron reduction blowing, and the time of the full iron reduction blowing is 2.0min to 2.5min before the end of the converter blowing, and the time of the full iron reduction blowing is ≥120s; in this embodiment, the specific time of the full iron reduction blowing is controlled to be 2.0min to 2.5min before the end of the converter blowing, and the specific time of the full iron reduction blowing is ≥120s, so that the total iron content of the slag in the final converter is lower than 15%.
[0080] The timing of the full iron blowing is 2.0 min, 2.1 min, 2.2 min, 2.3 min, 2.4 min or 2.5 min before the end of the converter.
[0081] In some optional embodiments, the second stage blowing includes performing the second stage blowing by adding a slag-forming agent, wherein the mass ratio of the slag-forming agent to the total slag amount of the converter blowing is 70% to 80%;
[0082] Wherein, the chemical composition of the slag-forming agent includes, by mass fraction:
[0083] Active lime: 85% to 95% and dolomite: 5% to 15%; and / or,
[0084] The third stage blowing includes adding lime to carry out the third stage blowing, and the amount of lime added is 2.1kg / t to 2.3kg / t; in this embodiment, the mass ratio of the amount of slag-forming agent used and the total slag amount of the converter blowing is controlled to be 70% to 80%, and the chemical composition of the slag-forming agent is limited to include active lime: 85% to 95% and dolomite: 5% to 15%. By adding such slag-forming agent, the impurity elements in the molten iron react completely with the alkaline components of the slag-forming agent to form slag, which is blown out of the molten iron through the second stage blowing and the third stage blowing, so that the carbon content in the molten iron is within the production index of steel products, so as to achieve accurate allocation of the molten steel composition;
[0085] In this embodiment, the specific amount of lime added in the third stage of blowing is limited. The addition of lime can cause the impurity elements in the molten iron to react completely with the lime and form slag, which is then blown out of the molten iron through the third stage of blowing, so that the carbon content in the molten iron is within the production index of steel products, thereby achieving accurate adjustment of the molten steel composition.
[0086] The mass ratio of the amount of the slag-forming agent to the total slag amount of the converter blowing can be 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79% or 80%.
[0087] It should be noted that, measured by mass fraction, the chemical composition of the active lime may include: CaO ≥ 75%, MgO: 8% to 12%, SiO2 ≤ 3.5%, S ≤ 0.20%, P ≤ 0.04%, wherein [CaO] + [MgO] ≥ 85%, [CaO] is the mass fraction of CaO, and [MgO] is the mass fraction of MgO.
[0088] It should be noted that, in terms of mass fraction, the chemical composition of the dolomite may include: CaO≥50%, MgO≥35%, and SiO2≤3%.
[0089] In some optional embodiments, the mass ratio of the added amount of the scrap steel to the molten iron for the converter is 10% to 25%; in these embodiments, the specific mass ratio of the added amount of the scrap steel to the smelting molten iron is limited to 10% to 25%, and the traditional steel smelting raw materials can be replaced by scrap steel, thereby further saving the preparation cost of steel, and the vanadium-containing molten iron can be used as an alloying agent. The V and Ti elements in the vanadium-containing molten iron can partially replace or completely replace the vanadium-nitrogen alloy in steel production, thereby further reducing the cost of steel smelting and achieving accurate adjustment of the molten steel composition.
[0090] The mass ratio of the added amount of the scrap steel to the smelting molten iron can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%.
[0091] In some optional embodiments, the argon pressure of the argon blowing treatment is 0.1MPa~0.7MPa, the gas flow rate of the argon blowing treatment is 1000NL / min~1200NL / min, and the time of the argon blowing treatment is ≥4min; in these embodiments, the specific argon pressure of the argon blowing treatment is limited to 0.1MPa~0.7MPa, and the specific gas flow rate of the argon blowing treatment is limited to 1000NL / min~1200NL / min, so as to clarify the gas intensity of the argon blowing treatment, thereby removing non-metallic inclusions in the molten steel and achieving degassing of the molten steel.
[0092] The argon gas pressure of the argon blowing treatment can be 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa or 0.7 MPa.
[0093] The gas flow rate of the argon blowing treatment may be 1000 NL / min, 1050 NL / min, 1100 NL / min, 1150 NL / min or 1200 NL / min.
[0094] In some optional embodiments, the converter tapping includes a nitrogen purging stage, and the time of the nitrogen purging is 2s to 4s; in these embodiments, the specific time of the nitrogen purging stage in the converter tapping is limited, and the slag on the surface of the molten steel can be removed by nitrogen purging, and the churning of the molten steel surface can also be suppressed, thereby further improving the purity of the molten steel.
[0095] The nitrogen purge time can be 2s, 3s or 4s.
[0096] It should be noted that the distance between the nitrogen purging gun position and the molten steel surface during the nitrogen purging stage is 5m to 7m.
[0097] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0098] Example 1
[0099] Take the production of medium carbon steel (C>0.20%) as an example.
[0100] like Figure 2 and Figure 3 As shown, a method for producing steel by alloying vanadium-containing molten iron comprises:
[0101] Select vanadium-containing molten iron: C: 4.20%, Si: 0.30%, Mn: 0.36%, P: 0.12%, S: 0.02%, Ti: 0.20%, Cr: 0.15%, V: 0.12%, and the rest are Fe and inevitable impurities; the temperature of the vanadium-containing molten iron is 1360°C.
[0102] First, obtain the endpoint composition of molten steel, including the following steps:
[0103] S101. The vanadium-containing molten iron and scrap steel are mixed to obtain an initial smelting molten iron; wherein the vanadium-containing molten iron and scrap steel are added in a ratio of 90t:15t, and the mass ratio of the scrap steel and the initial smelting molten iron is 14%;
[0104] S102. The initial smelting molten iron is subjected to converter blowing to obtain initial dephosphorized molten iron; wherein the specific operation of converter blowing includes:
[0105] First stage blowing: oxygen supply intensity 3.1Nm 3 / min / t for blowing. At the beginning of blowing, the distance between the blowing gun and the initial molten iron surface was 1.8m. During the blowing process, the distance between the blowing gun and the initial molten iron surface fluctuated within the range of 1.6m to 0.9m. The start time of the first stage of blowing was 0min, and the end time was 3min.
[0106] Second stage blowing: After the start of blowing, add 3200kg of active lime (40kg / t steel) and 150kg of light-burned dolomite (2kg / t steel) into the converter within 1 minute. After the addition is completed, control the nitrogen blowing flow rate at the bottom of the nitrogen blowing treatment to 0.1Nm 3 / min / t, the distance between the blowing gun and the initial molten iron surface during the blowing process is 1.6m, the start time of the second stage of blowing is 6min, the end time is 10min, and the next stage is carried out 10min after the start of blowing;
[0107] The third stage of blowing: add 200kg of lime into the converter (according to the addition amount of 2.2kg / t steel); during the blowing process, the distance between the blowing gun and the initial molten iron surface is 1.0m. The start time of the third stage of blowing is 11min and the end time is 13min. Within one minute before the end of blowing, the oxygen supply intensity is increased from 3.1Nm 3 / min / t increased to 3.3Nm 3 / min / t, add 50kg of light-burned dolomite at 12min30s after the start of converter blowing;
[0108] S103. The initial dephosphorized molten iron is subjected to converter tapping and argon blowing to obtain an initial ladle; wherein the converter tapping and argon blowing process comprises the steps of:
[0109] When the converter is poured out at the later stage of steelmaking, the blowing gun is first lifted to a height of 6m from the surface of the initial dephosphorized molten iron, and then purged with nitrogen and oxygen lances. After purging for 3 seconds, the pouring operation is carried out. After the pouring starts, the furnace body is tilted from a vertical state to a position of 77° with the vertical plane and maintained for 4 seconds, and then the furnace is slowly shaken to a position of 84° with the vertical plane to pour out the slag with a high TiO2 content as soon as possible. This slag accounts for 1 / 2 of the total slag volume; in terms of mass fraction, the chemical composition of the slag includes: CaO: 43.23%, MgO: 6.78%, SiO2: 8.8%, TFe: 13.64%, TiO2: 2.02%, V2O5: 1.91%, and the rest is Fe and unavoidable impurities.
[0110] S104. The composition of the initial ladle is detected and calculated to obtain the end-point composition of the molten steel; in terms of mass fraction, the end-point composition of the molten steel includes: C: 0.056%, Mn: 0.091%, P: 0.019%, and the rest is Fe and unavoidable impurities; the temperature of the molten steel is 1660°C.
[0111] S2. Calculate the target amount of vanadium-containing molten iron required for the ladle with molten iron based on the endpoint composition of the molten steel, the composition of the vanadium-containing molten iron, and the target composition of steel production (C> 0.20%): V: 0.025%;
[0112] S3. The target dosage is used as the reference value to overload the vanadium-containing molten iron, and then scrap steel is added to the vanadium-containing molten iron to obtain molten iron for the converter; wherein the vanadium-containing molten iron and scrap steel are added in a ratio of 92t:15t, and the mass ratio of scrap steel to the initial smelting molten iron is 14%;
[0113] S4. The converter is operated with molten iron for the converter downdraft, so that the molten iron for the converter is added to the initial ladle to obtain a coarse grade molten steel; wherein the converter downdraft out of the converter molten iron 1.95t;
[0114] S5. The crude molten steel is subjected to argon blowing treatment for 6 minutes to obtain a steel product; the chemical composition of the steel product includes, by mass fraction, C: 0.24%, Mn: 1.18%, P: 0.026%, V: 0.024%, Ti: 0.03%, and the rest is Fe and unavoidable impurities, and the temperature of the steel is 1635°C.
[0115] Example 2
[0116] Take the production of medium carbon steel (C>0.20%) as an example.
[0117] like Figure 2 and Figure 3 As shown, a method for producing steel by alloying vanadium-containing molten iron comprises:
[0118] Select vanadium-containing molten iron: C: 5.26%, Si: 0.45%, Mn: 0.46%, P: 0.145%, S: 0.012%; Ti: 0.15%, Cr: 0.12%, V: 0.12%, the rest is Fe and inevitable impurities; the temperature of the vanadium-containing molten iron is 1375°C.
[0119] First, obtain the endpoint composition of molten steel, including the following steps:
[0120] S101. The vanadium-containing molten iron and scrap steel are mixed to obtain an initial smelting molten iron; wherein the vanadium-containing molten iron and scrap steel are added in a ratio of 92t:17t, and the mass ratio of the scrap steel and the initial smelting molten iron is 15%;
[0121] S102. The initial smelting molten iron is subjected to converter blowing to obtain initial dephosphorized molten iron; wherein the specific operation of converter blowing includes:
[0122] First stage blowing: oxygen supply intensity 3.1Nm 3 / min / t for blowing. At the beginning of blowing, the distance between the blowing gun and the initial molten iron surface was 1.8m. During the blowing process, the distance between the blowing gun and the initial molten iron surface fluctuated within the range of 1.6m to 0.9m. The start time of the first stage of blowing was 0min, and the end time was 3min.
[0123] Second stage blowing: After the start of blowing, add 2400kg of active lime (40kg / t steel) and 250kg of light-burned dolomite (4kg / t steel) into the converter within 1 minute. The nitrogen blowing flow rate during the nitrogen blowing treatment is 0.1Nm 3 / min / t, during the blowing process, the distance between the blowing gun and the initial molten iron surface is 1.6m, the start time of the adjustment stage is 3min, and the end time is 6min. When the blowing of this stage starts 4min, 500kg of coke is added to the molten iron for blowing. During the blowing process, the distance between the blowing gun and the initial molten iron surface is 1.2m. The start time of the second stage of blowing is 6min, and the end time is 10min. The next stage is carried out 10min after the start of blowing.
[0124] The third stage of blowing: add 200kg of lime into the converter (according to the addition amount of 3.0kg / t steel); during the blowing process, the distance between the blowing gun and the initial molten iron surface is 0.9m. The start time of the third stage of blowing is 11min and the end time is 13min. Within one minute before the end of blowing, the oxygen supply intensity is increased from 3.1Nm 3 / min / t increased to 3.3Nm 3 / min / t, add 50kg of light-burned dolomite at 12min28s of converter blowing;
[0125] S103. The initial dephosphorized molten iron is subjected to converter tapping and argon blowing to obtain an initial ladle; wherein the converter tapping and argon blowing process comprises the steps of:
[0126] When the converter is poured out at the later stage of steelmaking, the blowing gun is first lifted to a height of 6.5m from the surface of the initial dephosphorized molten iron, and then purged with nitrogen and oxygen lances. After purging for 4 seconds, the furnace is poured out. After the start of pouring, the furnace body is tilted from a vertical state to a position of 75° with the vertical plane and maintained for 4 seconds, and then the furnace is slowly shaken to a position of 84° with the vertical plane to pour out the slag with high TiO2 content as soon as possible. This slag accounts for 1 / 2 of the total slag volume; in terms of mass fraction, the chemical composition of the slag includes: CaO: 39.97%, MgO: 8.95%, SiO2: 11.56%, TFe: 13.71%, TiO2: 2.22%, V2O5: 1.82%, and the rest is Fe and unavoidable impurities.
[0127] S104. The composition of the initial ladle is detected and calculated to obtain the end-point composition of the molten steel; in terms of mass fraction, the end-point composition of the molten steel includes: C: 0.045%, Mn: 0.136%, P: 0.022%, and the rest is Fe and unavoidable impurities; the temperature of the molten steel is 1660°C.
[0128] S2. Calculate the target amount of vanadium-containing molten iron required for ladle molten iron based on the endpoint composition of molten steel, the composition of vanadium-containing molten iron and the target composition of steel production (C> 0.20%) to obtain V: 0.025%;
[0129] S3. The target dosage is used as the reference value to overload the vanadium-containing molten iron, and then scrap steel is added to the vanadium-containing molten iron to obtain molten iron for the converter; wherein the vanadium-containing molten iron and scrap steel are added in a ratio of 92t:15t, and the mass ratio of scrap steel to the initial smelting molten iron is 14%;
[0130] S4. The converter is operated to pour the molten iron into the initial ladle to obtain a coarse grade molten steel; wherein the converter is poured out of the converter with molten iron 2.0t;
[0131] S5. The crude molten steel is subjected to argon blowing treatment for 6 minutes to obtain a steel product; the chemical composition of the steel product includes, by mass fraction, C: 0.23%, Mn: 1.25%, P: 0.027%, V: 0.026%, Ti: 0.05%, and the rest is Fe and unavoidable impurities, and the temperature of the steel is 1635°C.
[0132] Example 3
[0133] Take the production of medium carbon steel (C>0.20%) as an example.
[0134] like Figure 2 and Figure 3 As shown, a method for producing steel by alloying vanadium-containing molten iron comprises:
[0135] Select vanadium-containing molten iron: C: 6.20%, Si: 0.57%, Mn: 0.61%, P: 0.14%, S: 0.06%; Ti: 0.12%, Cr: 0.13%, V: 0.06%, and the rest are Fe and inevitable impurities; the temperature of the vanadium-containing molten iron is 1366°C.
[0136] First, obtain the endpoint composition of molten steel, including the following steps:
[0137] S101. The vanadium-containing molten iron and scrap steel are mixed to obtain an initial smelting molten iron; wherein the vanadium-containing molten iron and scrap steel are added in a ratio of 58.5t:16.5t, and the mass ratio of the scrap steel and the initial smelting molten iron is 22%;
[0138] S102. The initial smelting molten iron is subjected to converter blowing to obtain initial dephosphorized molten iron; wherein the specific operation of converter blowing includes:
[0139] First stage blowing: oxygen supply intensity 3.1Nm 3 / min / t for blowing. At the beginning of blowing, the distance between the blowing gun and the initial molten iron surface is 1.6m. During the blowing process, the distance between the blowing gun and the initial molten iron surface fluctuates within the range of 1.6m to 0.9m. The start time of the first stage of blowing is 0min, and the end time is 3min.
[0140] Second stage blowing: After the start of blowing, 3120 kg of active lime (40 kg / t steel) was added to the converter within 1 min. The nitrogen blowing flow rate during the nitrogen blowing treatment was 0.1 Nm 3 / min / t, the distance between the blowing gun and the initial molten iron surface during the blowing process is 1.6m, the start time of the second stage of blowing is 3min, the end time is 6min, and the next stage is carried out 5min after the start of the second stage of blowing;
[0141] The third stage of blowing: add 200kg of lime into the converter (according to the addition amount of 3.0kg / t steel); during the blowing process, the distance between the blowing gun and the initial molten iron surface is 1.0m. The start time of the third stage of blowing is 10min and the end time is 13min. Within one minute before the end of blowing, the oxygen supply intensity is increased from 3.1Nm 3 / min / t increased to 3.3Nm 3 / min / t, add 50kg of light-burned dolomite at 12min35s of converter blowing;
[0142] S103. The initial dephosphorized molten iron is subjected to converter tapping and argon blowing to obtain an initial ladle; wherein the converter tapping and argon blowing process comprises the steps of:
[0143] When the converter is poured out at the later stage of steelmaking, the blowing gun is first lifted to a height of 6.6m from the surface of the initial dephosphorized molten iron, and then purged with nitrogen and oxygen lances. After purging for 7s, the furnace is poured out. After the start of pouring, the furnace body is tilted from a vertical state to a position of 75° with the vertical plane and maintained for 7s, and then the furnace is slowly shaken to a position of 84° with the vertical plane to pour out the slag with a high TiO2 content as soon as possible. This slag accounts for 1 / 2 of the total slag volume; in terms of mass fraction, the chemical composition of the slag includes: CaO: 42.88%, MgO: 7.32%, SiO2: 13.61%, TFe: 14.28%, TiO2: 2.55%, V2O5: 1.62%, and the rest is Fe and unavoidable impurities.
[0144] S104. The composition of the initial ladle is detected and calculated to obtain the end-point composition of the molten steel; in terms of mass fraction, the end-point composition of the molten steel includes: C: 0.055%, Mn: 0.128%, P: 0.028%, and the rest is Fe and unavoidable impurities; the temperature of the molten steel is 1665°C.
[0145] S2 is calculated based on the endpoint composition of molten steel, the composition of vanadium-containing molten iron and the target composition of steel production (C> 0.20%) to obtain the target amount of vanadium-containing molten iron required for the ladle with molten iron;
[0146] S3. The target dosage is used as the reference value to overload the vanadium-containing molten iron, and then scrap steel is added to the vanadium-containing molten iron to obtain molten iron for the converter; wherein the vanadium-containing molten iron and scrap steel are added in a ratio of 92t:15t, and the mass ratio of scrap steel to the initial smelting molten iron is 14%;
[0147] S4. The converter is operated to pour the molten iron into the initial ladle to obtain a coarse grade molten steel; wherein the converter is poured out of the converter with molten iron 2.0t;
[0148] S5. The crude molten steel is subjected to argon blowing treatment for 6 minutes to obtain a steel product; the chemical composition of the steel product includes, by mass fraction, C: 0.23%, Mn: 1.25%, P: 0.027%, V: 0.026%, Ti: 0.05%, and the rest is Fe and unavoidable impurities, and the temperature of the steel is 1639°C.
[0149] Example 4
[0150] Take the production of medium carbon steel (C>0.20%) as an example.
[0151] like Figure 2 and Figure 3 As shown, a method for producing steel by alloying vanadium-containing molten iron comprises:
[0152] Select vanadium-containing molten iron: C: 6.80%, Si: 0.70%, Mn: 0.66%, P: 0.15%, S: 0.07%; Ti: 0.16%, Cr: 0.14%, V: 0.07%, and the rest are Fe and inevitable impurities; the temperature of the vanadium-containing molten iron is 1340°C.
[0153] First, obtain the endpoint composition of molten steel, including the following steps:
[0154] S101. The vanadium-containing molten iron and scrap steel are mixed to obtain an initial smelting molten iron; wherein the vanadium-containing molten iron and scrap steel are added in a ratio of 60.2t:15.9t, and the mass ratio of the scrap steel and the initial smelting molten iron is 21%;
[0155] S102. The initial smelting molten iron is subjected to converter blowing to obtain initial dephosphorized molten iron; wherein the specific operation of converter blowing includes:
[0156] First stage blowing: oxygen supply intensity 3.1Nm 3 / min / t for blowing. At the beginning of blowing, the distance between the blowing gun and the initial molten iron surface is 1.6m. During the blowing process, the distance between the blowing gun and the initial molten iron surface fluctuates within the range of 1.6m to 0.9m. The start time of the first stage of blowing is 0min, and the end time is 3min.
[0157] Second stage blowing: After the start of blowing, 3100 kg of active lime (41 kg / t steel) was added to the converter within 1 min. The nitrogen blowing flow rate during nitrogen blowing was 0.1 Nm 3 / min / t, the distance between the blowing gun and the initial molten iron surface during the blowing process is 1.6m, the start time of the second stage of blowing is 3min, the end time is 6min, and the next stage is carried out 6min after the start of the second stage of blowing;
[0158] The third stage of blowing: add 200kg of lime (according to the addition amount of 1.5kg / t steel) and 600kg of coke into the converter; during the blowing process, the distance between the blowing gun and the initial molten iron surface is 1.0m. The start time of the third stage of blowing is 11min and the end time is 13min. Within one minute before the end of blowing, the oxygen supply intensity is increased from 3.1Nm 3 / min / t increased to 3.3Nm 3 / min / t, add 50kg of light-burned dolomite at 12min30s of converter blowing;
[0159] S103. The initial dephosphorized molten iron is subjected to converter tapping and argon blowing to obtain an initial ladle; wherein the converter tapping and argon blowing process comprises the steps of:
[0160] When the converter is poured out at the later stage of steelmaking, the blowing gun is first lifted to a height of 7.0m from the surface of the initial dephosphorized molten iron, and then purged with nitrogen and oxygen lances. After purging for 8s, the pouring operation is carried out. After the pouring starts, the furnace body is tilted from a vertical state to a position of 75° with the vertical plane and maintained for 3s, and then the furnace is slowly shaken to a position of 84° with the vertical plane to pour out the slag with high TiO2 content as soon as possible. This slag accounts for 2 / 3 of the total slag volume; in terms of mass fraction, the chemical composition of the slag includes: CaO: 39.55%, MgO: 5.49%, SiO2: 13.56%, TFe: 14.12%, TiO2: 1.71%, V2O5: 2.92%, and the rest is Fe and unavoidable impurities.
[0161] S104. The composition of the initial ladle is detected and calculated to obtain the end-point composition of the molten steel; in terms of mass fraction, the end-point composition of the molten steel includes: C: 0.045%, Mn: 0.152%, P: 0.027%, and the rest is Fe and unavoidable impurities; the temperature of the molten steel is 1674°C.
[0162] S2. Calculated based on the endpoint composition of molten steel, the composition of vanadium-containing molten iron and the target composition of steel production (C> 0.20%), the target amount of vanadium-containing molten iron required for the ladle with molten iron V: 0.025%;
[0163] S3. The target dosage is used as the reference value to overload the vanadium-containing molten iron, and then scrap steel is added to the vanadium-containing molten iron to obtain molten iron for the converter; wherein the vanadium-containing molten iron and scrap steel are added in a ratio of 92t:15t, and the mass ratio of scrap steel to the initial smelting molten iron is 14%;
[0164] S4. The converter is operated to pour the molten iron into the initial ladle to obtain a coarse grade molten steel; wherein the converter is poured out of the converter with molten iron 2.0t;
[0165] S5. The crude molten steel is subjected to argon blowing treatment for 6 minutes to obtain a steel product; the chemical composition of the steel product includes, by mass fraction, C: 0.23%, Mn: 1.25%, P: 0.027%, V: 0.026%, Ti: 0.05%, and the rest is Fe and unavoidable impurities, and the temperature of the steel is 1635°C.
[0166] Related experiments and effect data:
[0167] By comparing the steel composition obtained in each embodiment and the comparative example, it can be clearly seen that the embodiment of the present application provides a method for producing steel by alloying vanadium-containing molten iron. Under the premise of adding necessary metering equipment in front of the converter, the vanadium-containing molten iron can be charged in excess of the target amount by 2% to 3% without increasing the operating rate of the converter charging crane. Before the molten steel is blown, it is added to the ladle by pouring the furnace to replace the carburizer in the steel-making process, and the molten steel is formulated with C: 0.10% to 0.20%, Mn: 0.05% to 0.10%, Si: 0.05-0.10%, V: 0.015% to 0.025%, and Ti: 0.02% to 0.03%.
[0168] The method is implemented on medium carbon steel (C>0.20%). Through subsequent calculations, it can be known that the method can comprehensively save 0.10% to 0.20% of the carbon content adjustment demand in the process of molten steel carbon matching, and can also utilize the alloying process of vanadium-containing molten iron with intermediate alloys such as ferrosilicon and ferromanganese, so that 0.02% to 0.05% of beneficial elements can be added to the final molten steel; the method can increase the output of molten steel in the converter by more than 1.5% to 2.0%, and the content of harmful elements is controlled to meet the requirements of the steel grade.
[0169] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0170] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0171] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for producing steel by alloying vanadium-containing molten iron, characterized in that: The method comprises: Obtain the endpoint composition of molten steel; Calculate the target amount of vanadium-containing molten iron required for adding molten iron to the ladle according to the endpoint composition of the molten steel, the composition of the vanadium-containing molten iron and the target composition of steel production; The vanadium-containing molten iron is overloaded with the target dosage as a reference value, and then scrap steel is added to the vanadium-containing molten iron to obtain molten iron for a converter; Performing a converter pouring operation on the converter molten iron so that the converter molten iron is added into a ladle containing the molten steel for alloying to obtain coarse molten steel; Blowing argon into the crude molten steel to obtain a steel product; Wherein, the chemical composition of the vanadium-containing molten iron includes, by mass fraction: C: 4.20% ~ 6.80%, Si: 0.30% ~ 0.70%, Mn: 0.30% ~ 0.70%, P: 0.12% ~ 0.15%, S: 0.02% ~ 0.07%, Ti: 0.10% ~ 0.50%, V: 0.05% ~ 0.20%, Cr: 0.10% ~ 0.20%, and the rest are Fe and unavoidable impurities.
2. The method according to claim 1, characterized in that The mass ratio of the overload filling amount to the target amount is 2% to 3%.
3. The method according to claim 1, characterized in that The method of obtaining the endpoint composition of molten steel comprises the following steps: Mixing vanadium-containing molten iron and scrap steel to obtain initial smelting molten iron; The initial smelting molten iron is subjected to converter blowing to obtain initial dephosphorized molten iron; The initial dephosphorized molten iron is subjected to converter tapping and argon blowing treatment to obtain an initial ladle; The composition of the initial ladle is detected and calculated to obtain the endpoint composition of the molten steel.
4. The method according to claim 3, characterized in that The temperature of the initial molten steel is 1650° C. to 1670° C., and the carbon content of the initial molten steel is 0.03% to 0.08%.
5. The method according to claim 1 or 3, characterized in that: The converter blowing includes first stage blowing, second stage blowing and third stage blowing; The oxygen supply intensity of the first stage blowing is 2.9Nm 3 / min / t~3.1Nm 3 / min / t, the blowing time of the first stage is 1min~3min; The oxygen supply intensity of the second stage blowing is 3.2Nm 3 / min / t~3.4Nm 3 / min / t, the blowing time of the second stage is 3min~5min; The oxygen supply intensity of the third stage blowing is 2.9Nm 3 / min / t~3.1Nm 3 / min / t, and the blowing time of the third stage is 2min~4min.
6. The method according to claim 5, characterized in that The converter blowing also includes full iron reduction blowing, the time of the full iron reduction blowing is 2.0 minutes to 2.5 minutes before the end of the converter blowing, and the time of the full iron reduction blowing is ≥120 seconds.
7. The method according to claim 5, characterized in that The second stage blowing includes adding a slag-forming agent to carry out the second stage blowing, wherein the mass ratio of the slag-forming agent to the total slag amount of the converter blowing is 70% to 80%; Wherein, the chemical composition of the slag-forming agent includes, by mass fraction: Active lime: 85% to 95% and dolomite: 5% to 15%; and / or, The third stage blowing includes adding lime to carry out the third stage blowing, and the amount of lime added is 2.1kg / t to 2.3kg / t.
8. The method according to claim 1, characterized in that The mass ratio of the added amount of the scrap steel to the molten iron for the converter is 10% to 25%.
9. The method according to claim 1, characterized in that: The argon pressure of the argon blowing treatment is 0.1MPa-0.7MPa, the gas flow rate of the argon blowing treatment is 1000NL / min-1200NL / min, and the time of the argon blowing treatment is ≥4min.
10. The method according to claim 1, characterized in that The converter steel tapping includes a nitrogen purge stage, and the nitrogen purge time is 2s to 4s.
Citation Information
Patent Citations
Smelting process for production of grade II hot-rolled reinforced bar
CN102978538A
Method for smelting medium / high-carbon hard-wired steel by vanadium-titanium containing molten iron
CN102994871A
Method for smelting rail steel with vanadium-bearing hot metal as raw materials
CN105018670A
Method for HRB400 steel alloying by using molten iron containing vanadium
CN106480353A
Method for smelting high-corrosion-resistant railway vehicle steel through vanadium-containing high-chromium molten iron
CN109735759A