Method for recovering copper from waste PCBs (printed circuit boards) through electro-deposition

By using methylsulfonic acid for oxidative leaching and electrodeposition technology in waste PCB boards, the problem of environmental pollution in the existing technology is solved, efficient and environmentally friendly copper recovery and precious metal enrichment are achieved, and the efficiency and efficiency of resource recovery are improved. Environmental protection effect.

CN118745518APending Publication Date: 2024-10-08CENT SOUTH UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410994075.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

In the existing technology, when recovering copper from waste PCB boards, incineration or solvents such as acids and alkalis are often used, which leads to environmental pollution and lacks green and environmentally friendly alternatives.

Method used

Methanesulfonic acid is used as the leaching liquid to perform oxidative leaching in the crushed and ground metal powder, and then copper is precipitated from the liquid phase through electrodeposition technology to achieve efficient copper extraction and enrichment of precious metals such as gold, silver, and platinum in the process. And the leachate is recycled to reduce resource waste.

Benefits of technology

It achieves efficient and environmentally friendly extraction of copper from waste PCB boards, reduces the generation of waste gas and waste water, improves the recovery rate, and improves the efficiency of resource recovery and environmental protection effects through the enrichment and electrodeposition recycling of precious metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a method for recovering copper from a waste PCB (printed circuit board) through electro-deposition. The method comprises the following steps: crushing the waste PCB of the computer, and separating copper-containing metal powder from plastic powder by adopting density and electromagnetic separation equipment; the copper-containing metal powder is subjected to oxidation leaching in a methanesulfonic acid solution, the copper element enters a leaching solution along with the proceeding of the reaction, and precious metals such as gold, silver and platinum are enriched in leaching residues; and carrying out electro-deposition at a certain temperature by taking the leachate as an electro-deposition solution and an inert cathode and anode plate as a polar plate, and depositing and separating out copper ions in the solution at a cathode to obtain high-quality cathode copper. According to the method, 99% of cathode copper products are obtained through electro-deposition while the waste PCBs are efficiently leached, the whole reaction system has the advantages of being clean and efficient in selectivity, and the method has important significance in promoting recycling of valuable metal of the waste PCBs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for recovering copper from waste PCB boards by electro-deposition, belonging to the field of waste recycling. Background Art

[0003] Electronic waste contains several metals, including some precious metals such as Au, Ag and Pd. The extraction of these metals not only escalates environmental issues, but also can improve resource recycling and promote economic development to a certain extent. Waste electrical and electronic products collected from the industry and domestic consumers are pre-processed before being used for metal extraction. The pre-processing process includes manual screening, disassembly, crushing and shredding. The stripped process parts can be separated according to the metal to be recycled. The discarded PCB boards or components are ground into specific sizes through the crushing and shredding process.

[0004] In the past and recent studies, several methods have been applied to extract metals from electronic waste. The methods used for metal extraction include electrochemical, pyrometallurgical, hydrometallurgical and biological leaching, and a number of studies have been conducted on the extraction of metals from metal powders. At present, the recovery of copper resources in waste PCB boards mostly adopts incineration or solvents such as acids, alkalis, and strong oxidants, which has a high recovery rate, but produces a large amount of waste water, waste gas and solid residues, causing great secondary pollution to the environment, which is contrary to the concept of resource recovery and sustainable development. Therefore, it is urgent to find a green solvent to replace the traditional environmentally unfriendly recovery method. In the present invention, a green and environmentally friendly solvent is used as a leaching solution, and electrodeposition work is carried out to achieve efficient copper extraction. In addition, when leaching metal-containing powders, precious metals such as gold, silver, and platinum are enriched in the slag, which can be further recovered. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for recovering copper from waste PCB boards by electrodeposition. The method provided by the present invention can realize the efficient and environmentally friendly extraction of valuable metal copper from waste PCB boards. When copper is separated from the solid phase to the liquid phase, no waste gas is generated. At the same time, the leached residue can realize the enrichment of precious metals such as gold, silver, and platinum. The leaching liquid is used as the electrolytic liquid of the back-end process for electrodeposition to obtain a cathode copper product. The electrolytic liquid can be returned to the leaching process for reuse, thereby realizing the closed-loop circulation of methanesulfonic acid.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A method for recovering copper from waste PCBs by electrodeposition, comprising the steps of crushing and grinding the waste PCBs to obtain metal-containing powder; sequentially passing the metal-containing powder through density separation and electromagnetic separation equipment to obtain metal powder free of plastic and magnetic substances; oxidizing and leaching the metal powder in a methanesulfonic acid system, wherein copper elements in the metal powder are dissolved into a solution as the reaction proceeds; connecting the leaching solution and inert anode and cathode plates to a direct current power supply via a wire as an electrolytic system for electrodeposition, wherein metallic copper is precipitated on a cathode to obtain high-quality cathode copper.

[0008] The method described above obtains metal-containing powder through crushing and grinding, wherein more than 80% of the powder particles are smaller than 200 meshes.

[0009] The method comprises the following steps: performing density separation on the metal-containing powder to obtain plastic powder and metal-containing powder; and then performing electromagnetic separation on the metal powder to obtain magnetic metal powder and copper-containing metal powder.

[0010] In the method, the concentration of methanesulfonic acid is 1-5 mol / L, the mechanical stirring speed is 50-300 rpm, the temperature is 30-70°C, the liquid-solid ratio is 3:1-10:1, and the leaching time is 0.5h-3.5h. Preferably, the concentration of methanesulfonic acid is 1-3 mol / L, the mechanical stirring speed is 100-200 rpm, the temperature is 30-50°C, the liquid-solid ratio is 3:1-5:1, and the leaching time is 1-2h.

[0011] In the method, the oxidizing substance introduced is one of oxygen, ozone and hydrogen peroxide, the gas flow rate is 0.1-1L / min, the amount of hydrogen peroxide added is calculated to completely oxidize copper to divalent copper, expressed as an excess coefficient, and the hydrogen peroxide excess coefficient is 0.8-1.5. Preferably, the oxidizing substance introduced is hydrogen peroxide, and the hydrogen peroxide excess coefficient is 1-1.2.

[0012] In the method, the cathode and anode plates are made of titanium, stainless steel and graphite, and the wire is made of copper. Preferably, the cathode and anode plates are made of high-purity titanium.

[0013] The method described herein has a current density of 50-300 A / m during electrodeposition. 2 , inter-electrode distance 2-5 cm, temperature 25-40°C, electrodeposition time 4-12 h. Preferably, the current density during electrodeposition is 50-150 A / m 2 , inter-electrode distance 2-3cm, temperature 25-35℃, electrodeposition time 6-8h.

[0014] Principles and advantages

[0015] The method of the present invention specifically recycles and utilizes valuable metals such as copper in PCB boards, separates plastic powder and magnetic material from copper-containing metal powder by density and electromagnetic separation, and the copper element in the copper-containing metal powder is efficiently leached in a methanesulfonic acid solution. The leaching rate of methanesulfonic acid to gold, silver and platinum is low, and enrichment in slag can be achieved. The leaching solution containing high-concentration copper is used as an electrodeposition solution for electrodeposition, and electrodeposition is performed at a fixed current density to obtain a high-quality cathode copper product.

[0016] The present invention uses green solvent methanesulfonic acid when extracting copper elements from waste PCBs, which has little harm to the environment and can achieve efficient leaching of copper. In the leaching process, the requirements for the acidity and liquid-to-solid ratio of methanesulfonic acid are relatively small, and the acid and water consumption are relatively small compared with other wet systems. In the electrodeposition process, high-quality cathode copper is obtained while having the advantages of low power consumption and high current efficiency. The present invention is of great significance for promoting the recovery of valuable metals in waste PCBs, energy saving and consumption reduction, and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] none Specific implementation plan

[0018] The following examples are intended to further illustrate the present invention but are not intended to limit the present invention.

[0019] Example 1

[0020] The raw materials are waste PCB boards provided by a company. The main metal components and contents are as follows:

[0021]

[0022] The waste PCB was crushed and ground to obtain 200g of metal-containing powder, of which more than 80% of the powder particles were less than 200 mesh. The metal-containing powder was placed in a density separation device to obtain plastic powder and metal powder. The metal powder was further screened by an electromagnetic separation device to obtain magnetically separated metal powder and copper-containing metal powder. The pretreatment process enriched the copper content to a certain extent. In the leaching process, 100g of copper-containing metal powder was weighed, and the concentration of methanesulfonic acid was 2mol / L, the liquid-solid ratio was 5:1, the leaching time was 1.5h, the excess coefficient of hydrogen peroxide was 1.2, the temperature was 50℃, and the mechanical stirring speed was 200rpm. Under these conditions, the copper-containing metal powder was leached. After the reaction, the leachate and the leach residue were obtained. The leachate and the leach residue were analyzed for components. The leachate contained 48g / L copper, and the contents of Au, Ag and Pd in ​​the leach residue were 0.42%, 0.38% and 0.09% respectively. Prepare two high-purity titanium plates as anode and cathode respectively. The cathode and cathode plates are polished with 500, 1000 and 2000 mesh sandpaper respectively before use, and then rinsed with deionized water and alcohol. The cathode plate is exposed in the electrolyte for 6*6cm2 The area of ​​the cathode current efficiency is convenient for calculating. The electrolytic cell uses a special cubic cell. The power supply is a DC power supply. The power supply and the two anode and cathode plates are connected by copper wires. The distance between the plates is 3 cm. In order to prevent the influence of rust on the cell voltage, the wires are rusted by 400 mesh and 800 grit sandpaper before use. The leachate from the previous process is used as the electrolytic solution. At a current density of 150A / m 2 After 8 hours of electrodeposition, cathode copper product was obtained on the cathode. The calculated current efficiency was 96.6%, and the purity of cathode copper product was 99.67%.

[0023] Example 2

[0024] The waste PCB board shown in Example 1 is used as a raw material, and the waste PCB is crushed and ground to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are less than 200 meshes. The metal-containing powder is placed in a density separation device to obtain plastic powder and metal powder, and the metal powder is further screened by an electromagnetic separation device to obtain magnetically separated metal powder and copper-containing metal powder. The pretreatment process enriches the copper content to a certain extent. In the leaching process, 100g of copper-containing metal powder is weighed, and a methanesulfonic acid concentration of 3mol / L, a liquid-solid ratio of 5:1, a leaching time of 2h, a hydrogen peroxide excess coefficient of 1.2, a temperature of 50°C, and a mechanical stirring speed of 200rpm are used. Under these conditions, the copper-containing metal powder is leached. After the reaction is completed, a leachate and a leach residue are obtained. The leachate and the leach residue are analyzed for components. The leachate contains 54g / L copper, and the contents of Au, Ag and Pd in ​​the leach residue are 0.41%, 0.36% and 0.09% respectively. Prepare two high-purity titanium plates as anode and cathode respectively. The cathode and cathode plates are polished with 500, 1000 and 2000 mesh sandpaper respectively before use, and then rinsed with deionized water and alcohol. The cathode plate is exposed in the electrolyte for 6*6cm 2 The area of ​​the cathode current efficiency is convenient for calculating. The electrolytic cell uses a special cubic cell. The power supply is a DC power supply. The power supply and the two anode and cathode plates are connected by copper wires. The plate distance is 3 cm. In order to prevent the influence of rust on the cell voltage, the wires are rusted by 400 mesh and 800 grit sandpaper before use. The leachate from the previous process is used as the electrolytic solution. At a current density of 100A / m 2 After 8 hours of electrodeposition, cathode copper product was obtained on the cathode. The calculated current efficiency was 97%, and the purity of cathode copper product was 99.47%.

[0025] Example 3

[0026] The waste PCB board shown in Example 1 is used as a raw material, and the waste PCB is crushed and ground to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are less than 200 meshes. The metal-containing powder is placed in a density separation device to obtain plastic powder and metal powder, and the metal powder is further screened by an electromagnetic separation device to obtain magnetically separated metal powder and copper-containing metal powder. The pretreatment process enriches the copper content to a certain extent. In the leaching process, 100g of copper-containing metal powder is weighed, and a methanesulfonic acid concentration of 1mol / L, a liquid-solid ratio of 4:1, a leaching time of 2h, a hydrogen peroxide excess coefficient of 1.2, a temperature of 50°C, and a mechanical stirring speed of 200rpm are used. Under these conditions, the copper-containing metal powder is leached. After the reaction is completed, a leachate and a leach residue are obtained. The leachate and the leach residue are analyzed for components. The leachate contains 56g / L copper, and the contents of Au, Ag and Pd in ​​the leach residue are 0.45%, 0.376% and 0.1% respectively. Prepare two high-purity titanium plates as anode and cathode respectively. The cathode and cathode plates are polished with 500, 1000 and 2000 mesh sandpaper respectively before use, and then rinsed with deionized water and alcohol. The cathode plate is exposed in the electrolyte for 6*6cm 2 The area of ​​the cathode current efficiency is convenient for calculating. The electrolytic cell uses a special cubic cell. The power supply is a DC power supply. The power supply and the two anode and cathode plates are connected by copper wires. The plate distance is 3 cm. In order to prevent the influence of rust on the cell voltage, the wires are rusted by 400 mesh and 800 grit sandpaper before use. The leachate from the previous process is used as the electrolytic solution. At a current density of 100A / m 2 After 8 hours of electrodeposition, cathode copper product was obtained on the cathode. The calculated current efficiency was 96.7%, and the purity of cathode copper product was 99.64%.

[0027] Comparative Example 1 (Leachate under the parameters not provided by the present invention)

[0028] The waste PCB board shown in Example 1 is used as a raw material, and the waste PCB is crushed and ground to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are less than 200 meshes. The metal-containing powder is placed in a density separation device to obtain plastic powder and metal powder, and the metal powder is further screened by an electromagnetic separation device to obtain magnetically separated metal powder and copper-containing metal powder. The pretreatment process enriches the copper content to a certain extent. In the leaching process, 100g of copper-containing metal powder is weighed, and a methanesulfonic acid concentration of 2mol / L, a liquid-solid ratio of 5:1, a leaching time of 0.5h, a hydrogen peroxide excess coefficient of 1.2, a temperature of 70°C, and a mechanical stirring speed of 200rpm are used. Under these conditions, the copper-containing metal powder is leached. After the reaction is completed, a leachate and a leach residue are obtained. The leachate and the leach residue are analyzed for components. The leachate contains 38g / L copper, and the contents of Au, Ag and Pd in ​​the leach residue are 0.37%, 0.25 and 0.05% respectively. Prepare two high-purity titanium plates as anode and cathode respectively. The cathode and cathode plates are polished with 500, 1000 and 2000 mesh sandpaper respectively before use, and then rinsed with deionized water and alcohol. The cathode plate is exposed in the electrolyte for 6*6cm 2 The area of ​​the cathode current efficiency is convenient for calculating. The electrolytic cell uses a special cubic cell. The power supply is a DC power supply. The power supply and the two anode and cathode plates are connected by copper wires. The distance between the plates is 3 cm. In order to prevent the influence of rust on the cell voltage, the wires are rusted by 400 mesh and 800 grit sandpaper before use. The leachate from the previous process is used as the electrolytic solution. At a current density of 150A / m 2 After 8 hours of electrodeposition, cathode copper product was obtained on the cathode. The calculated current efficiency was 95.6%, and the purity of cathode copper product was 94.67%.

[0029] Comparative Example 2 (without addition of oxidizing substance)

[0030] The waste PCB board shown in Example 1 is used as a raw material, and the waste PCB is crushed and ground to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are less than 200 meshes. The metal-containing powder is placed in a density separation device to obtain plastic powder and metal powder, and the metal powder is further screened by an electromagnetic separation device to obtain magnetically separated metal powder and copper-containing metal powder. The pretreatment process enriches the copper content to a certain extent. In the leaching process, 100g of copper-containing metal powder is weighed, and a methanesulfonic acid concentration of 2mol / L, a liquid-solid ratio of 5:1, a leaching time of 1.5h, a hydrogen peroxide excess coefficient of 1.2, a temperature of 50°C, and a mechanical stirring speed of 200rpm are used. Under these conditions, the copper-containing metal powder is leached. After the reaction is completed, a leachate and a leach residue are obtained. The leachate and the leach residue are analyzed for components. The leachate contains 22g / L copper, and the contents of Au, Ag and Pd in ​​the leach residue are 0.03%, 0.04 and 0.02% respectively. Prepare two high-purity titanium plates as anode and cathode respectively. The cathode and cathode plates are polished with 500, 1000 and 2000 mesh sandpaper respectively before use, and then rinsed with deionized water and alcohol. The cathode plate is exposed in the electrolyte for 6*6cm 2 The area of ​​the cathode current efficiency is convenient for calculating. The electrolytic cell uses a special cubic cell. The power supply is a DC power supply. The power supply and the two anode and cathode plates are connected by copper wires. The distance between the plates is 3 cm. In order to prevent the influence of rust on the cell voltage, the wires are rusted by 400 mesh and 800 grit sandpaper before use. The leachate from the previous process is used as the electrolytic solution. At a current density of 150A / m 2 After 8 hours of electrodeposition, cathode copper product was obtained on the cathode. The calculated current efficiency was 86.6%, and the purity of cathode copper product was 87.67%.

[0031] Comparative Example 3 (without mechanical stirring)

[0032] The waste PCB board shown in Example 1 is used as a raw material, and the waste PCB is crushed and ground to obtain 200g of metal-containing powder, wherein more than 80% of the powder particles are less than 200 meshes. The metal-containing powder is placed in a density separation device to obtain plastic powder and metal powder, and the metal powder is further screened by an electromagnetic separation device to obtain magnetically separated metal powder and copper-containing metal powder. The pretreatment process enriches the copper content to a certain extent. In the leaching process, 100g of copper-containing metal powder is weighed, and a methanesulfonic acid concentration of 2mol / L, a liquid-solid ratio of 5:1, a leaching time of 1.5h, a hydrogen peroxide excess coefficient of 1.2, and a temperature of 50°C are prepared. Under these conditions, the copper-containing metal powder is leached. After the reaction is completed, a leachate and a leach residue are obtained. The leachate and the leach residue are analyzed for components. The leachate contains 30g / L copper, and the contents of Au, Ag and Pd in ​​the leach residue are 0.27%, 0.19 and 0.04% respectively. Prepare two high-purity titanium plates as anode and cathode respectively. The cathode and cathode plates are polished with 500, 1000 and 2000 mesh sandpaper respectively before use, and then rinsed with deionized water and alcohol. The cathode plate is exposed in the electrolyte for 6*6cm 2 The area of ​​the cathode current efficiency is convenient for calculating. The electrolytic cell uses a special cubic cell. The power supply is a DC power supply. The power supply and the two anode and cathode plates are connected by copper wires. The distance between the plates is 3 cm. In order to prevent the influence of rust on the cell voltage, the wires are rusted by 400 mesh and 800 grit sandpaper before use. The leachate from the previous process is used as the electrolytic solution. At a current density of 150A / m 2 After 8 hours of electrodeposition, cathode copper product was obtained on the cathode. The calculated current efficiency was 89.6%, and the purity of cathode copper product was 93.67%.

Claims

1. A method for recovering copper from waste PCBs by electroplating. Features: The waste PCB boards are crushed and ground to obtain metal-containing powders; the metal-containing powders are sequentially passed through density and electromagnetic separation equipment to obtain metal powders free of plastic and magnetic substances; the metal powders are oxidized and leached in a methanesulfonic acid system, and as the reaction proceeds, the copper element in the metal powders dissolves into the solution, and precious metals such as gold, silver, and platinum are enriched in the leached residue; the leachate and the inert anode and cathode plates are connected to a DC power supply through wires as an electrolytic deposition system, and metallic copper is precipitated on the cathode to obtain high-quality cathode copper.

2. The method according to claim 1, Features: The metal-containing powder is obtained by crushing and grinding, wherein more than 80% of the powder particles are smaller than 200 meshes.

3. The method according to claim 1, Features: The metal-containing powder is subjected to density separation equipment to obtain plastic powder and metal powder; secondly, the metal powder is subjected to electromagnetic separation to obtain magnetic metal powder and copper-containing metal powder.

4. The method according to claims 1 and 3, Features: The copper-containing metal powder is oxidized and leached in a methanesulfonic acid system, wherein the methanesulfonic acid concentration is 1-5 mol / L, the mechanical stirring speed is 50-300 rpm, the temperature is 30-70°C, the liquid-solid ratio is 3:1-10:1, and the leaching time is 0.5h-3.5h.

5. The method according to claims 1 and 4, Features: The oxidizing substance introduced is one of oxygen, ozone and hydrogen peroxide, the gas flow rate is 0.1-1L / min, the amount of hydrogen peroxide added is calculated based on the complete oxidation of copper to divalent copper, expressed as an excess coefficient, and the hydrogen peroxide excess coefficient is 0.8-1.

5.

6. The method according to claim 1, Features: The selected material of the anode and cathode plates is one of titanium plate, stainless steel plate and graphite, and the wire is a copper wire.

7. The method according to claim 1, Features: The current density during electrodeposition is 50-300A / m 2 , inter-electrode distance 2-5cm, temperature 25-40℃, electrodeposition time 4-12h.

Citation Information

Cited By

  • Selective leaching method for copper in waste circuit board

    CN120400548A

  • A selective leaching method of copper in waste circuit board

    CN120400548B