321H medium-thickness plate, method for improving high-temperature yield strength of 321H medium-thickness plate and application of 321H medium-thickness plate
By controlling the content range of C and Ti and using high-temperature and short-time solution treatment, the yield strength and corrosion resistance problems of 321H stainless steel medium-thick plates in high-temperature and high-pressure environments were solved, and the 590°C yield strength was significantly improved. Meet the application requirements of chemical equipment.
Patent Information
- Application Number
- CN202410762500.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult for 321H stainless steel medium-thick plates to meet the high-temperature yield strength and corrosion resistance in high-temperature and high-pressure environments. At the same time, the existing process causes the strength of the steel plates to decrease, and the TiC precipitation phase affects the corrosion resistance.
321H stainless steel continuous casting billet is produced through electric furnace smelting, AOD refining, LF refining, VD denitrification and continuous casting processes, controlling the C content to 0.05~0.06wt%, the Ti content to 0.30~0.35wt%, and N≤0.009wt %, C/Ti is 0.15~0.20, and adopts high temperature and short time solution treatment. The temperature in zones 1-4 of the solution furnace is 950±10℃, the temperature in zones 5-6 is 1130±10℃, and the holding time is 1.0~ 1.5min/mm thickness.
The 590°C yield strength of 321H medium-thick plate is increased to ≥124Mpa, which meets the high-temperature and high-pressure environment requirements of chemical equipment reactors, while optimizing the product structure and performance.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material manufacturing, and specifically relates to a 321H medium and thick plate and a method and application of improving the high temperature yield strength thereof. Background Art
[0002] In some large chemical equipment reactors, high temperature and high pressure reactions are involved, requiring the equipment materials to have high corrosion resistance and high high temperature strength. 321H stainless steel medium and thick plates are common stainless steel materials in chemical equipment. Its Ti and C elements form TiC precipitation phases, which avoids the generation of intergranular chromium depletion when serving in the sensitization temperature range and causes a decrease in corrosion resistance. At the same time, the high C content ensures the yield strength.
[0003] According to the standard, the grain size of 321H medium plate is required to be coarser than level 7. Usually, in order to meet the grain size requirements, high temperature and long time solution treatment is adopted during the solution treatment of steel plate. However, too long solution treatment time will reduce the strength of the steel plate. Therefore, special composition control and solution treatment process are required to make 321H stainless steel medium plate meet the requirements of coarser grain size level 7 and have higher high temperature yield strength. Summary of the invention
[0004] In view of the defects of the prior art, the present invention provides a 321H medium and thick plate and a method and application of improving the high temperature yield strength thereof.
[0005] Specifically, the method for improving the high temperature yield strength of 321H medium and thick plates provided by the present invention comprises:
[0006] (1) 321H stainless steel continuous casting billet is produced by electric furnace smelting, AOD refining, LF refining, VD denitrification and continuous casting process;
[0007] Wherein, the C content in the continuous casting billet is 0.05-0.06wt%, the Ti content is 0.30-0.35wt%, N≤0.009wt%, and C / Ti is 0.15-0.20;
[0008] (2) hot rolling the continuously cast slab to obtain a hot rolled plate;
[0009] (3) A solution furnace is used to perform a solution treatment on the hot-rolled plate.
[0010] In the above method for improving the high temperature yield strength of 321H medium and thick plates, in the VD denitrification process, after the ladle arrives at the workstation, the molten steel temperature is ≥1600°C, and the cycle time is ≥40min under a vacuum degree ≤2mbar.
[0011] In the above method for improving the high temperature yield strength of 321H medium and thick plates, the temperature of zones 1-4 of the solution furnace is 950±10°C, and the temperature of zones 5-6 is 1130±10°C.
[0012] In the above method for improving the high temperature yield strength of 321H medium and thick plates, the holding time of the solution treatment is 1.0 to 1.5 min / mm thickness.
[0013] On the other hand, the present invention provides a 321H medium and thick plate, which is prepared by the above-mentioned method for improving the high temperature yield strength of the 321H medium and thick plate.
[0014] The above-mentioned 321H medium and thick plates have a yield strength of ≥124Mpa at 590°C.
[0015] In yet another aspect, the present invention provides the use of the above-mentioned 321H medium and thick plate in the preparation of chemical equipment.
[0016] In the above application, the chemical equipment is a reactor.
[0017] The technical solution of the present invention has the following beneficial effects:
[0018] According to the method of the present invention, by controlling the C content and the range of C / Ti and optimizing the refining process and the solution treatment process, the product structure and performance are improved, and finally a 321H stainless steel medium and thick plate with a yield strength of ≥124Mpa at 590°C is obtained. DETAILED DESCRIPTION
[0019] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific embodiments. Except for the following contents, the process method of the present invention adopts conventional methods or devices in the art. Unless otherwise specified, the following terms have the meanings commonly understood by those skilled in the art.
[0020] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0021] In order to meet the requirement of 590℃ yield strength ≥124Mpa of 321H stainless steel medium and thick plates for chemical equipment, the present invention improves the yield strength of the medium and thick plates by increasing the lower limit of C content control of 321H stainless steel; in view of the problem of decreased corrosion capacity caused by increased C content, the C / Ti control range is optimized; in order to avoid the influence of TiN inclusions on the surface of the steel plate, a VOD denitrification process is added in the product refining process, and the denitrification rate is 25%; at the same time, the solid solution process of 321H stainless steel medium and thick plates is optimized, and by adopting the idea of higher temperature and shorter time solid solution, the product grain size meets the 7-level coarser while ensuring the high temperature yield strength. After searching, the applicant of the present invention is the only manufacturer in China that meets the requirements of this technical condition.
[0022] Specifically, the present invention provides a method for improving the high temperature yield strength of 321H medium and thick plates, comprising the processes of electric furnace smelting, AOD refining, LF refining, VD denitrification, continuous casting, hot rolling and solution treatment.
[0023] In the smelting, refining and denitrification process, the present invention controls the C content in the molten steel to be 0.05-0.06wt%, the Ti content to be 0.30-0.35wt%, N≤0.009wt%, and C / Ti to be 0.15-0.20.
[0024] The standard stipulates that the lower limit of C content in 321H stainless steel is 0.04%, and the Ti content is required to be greater than or equal to 4 times (C+N). The Ti element reacts with the N element in the molten steel to form TiN inclusions. The TiN inclusions react with the protective slag during the continuous casting process to form "fish" defects on the continuous casting surface, which are difficult to polish clean, resulting in a high probability of scrapping the steel plate. Therefore, in general production, in order to avoid excessive Ti content in the molten steel, the C content is strictly controlled according to the lower limit. The C element is a key element to improve the yield strength of the product. Therefore, the present invention increases the lower limit of the C content by one percentage point (i.e. 0.05%). In order to have enough Ti content in the product to react with C, the product C / Ti range is set to 0.15-0.20, and the lower limit of the Ti content control is also increased accordingly. In addition, the present invention starts from the idea of controlling N, controls the N content of the product to a minimum, and tries to avoid the formation of TiN inclusions.
[0025] The N element is a gas and can be removed by vacuum degassing. The conventional refining process route is AOD→LF→CC. The present invention adds a VD vacuum degassing process after the LF process. After the ladle arrives at the workstation, the molten steel temperature is controlled to be ≥1600°C, and the cycle time is ≥40min under a vacuum degree of ≤2mbar, so that the N content of the product is reduced from 0.012% to 0.009%, and the denitrification rate is 25%.
[0026] The solid solution furnace used in the present invention is a continuous solid solution furnace, wherein zones 1-4 are steel plate preheating zones, and zones 5-6 are steel plate heating zones.
[0027] In the present invention, the steel plate adopts a higher temperature and shorter time concept in the solution process, so that the structure and high temperature performance of 321H medium and thick plates are both improved. Preferably, the temperature of zones 1-4 of the solution furnace is 950±10°C, the temperature of zones 5-6 is 1130±10°C, and the insulation time of the steel plate in the solution furnace is controlled at 1.0-1.5min / mm thickness.
[0028] The steel plate is preheated to 950℃±10℃ in zones 1-4, which allows the steel plate to quickly heat up to 1130℃ in zones 5-6. Moreover, the grains of the steel plate will not grow at this temperature, effectively avoiding the risk of reducing the strength of the steel plate. High-temperature heat treatment is used in zones 5-6, and the temperature is controlled at 1130±10℃, so that the grain size of the steel plate can quickly reach the requirements of grade 7 or coarser.
[0029] According to the effects of solution temperature and time on the grain size and 590°C high temperature yield strength of 321H hot rolled plate shown in Table 1, it can be seen that solution treatment according to the method of the present invention can make the product meet the effect of coarser grain size of grade 7 and higher 590°C high temperature yield strength than 124 MPa.
[0030] Through practice, the 321H medium and thick plate prepared according to the method of the present invention has a yield strength of ≥124 MPa at 590°C, which meets the application requirements in the preparation of chemical equipment (especially large reactors).
[0031] Example
[0032] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods without specific conditions in the following examples are based on conventional methods and conditions.
[0033] Embodiment 1:
[0034] (1) 321H stainless steel continuous casting billet was produced by electric furnace + AOD + LF + VD + continuous casting process. During the VD process, the molten steel temperature was 1620°C, the vacuum degree was 1.8 mbar, the cycle time was 45 min, and the composition of the continuous casting billet was as follows: C 0.052, Si 0.58, Mn 0.88, P0.0031, S 0.001, Cr 17.21, Ni 9.17, N 0.008, Ti 0.31, C / Ti=17;
[0035] (2) 321H continuous casting billet is hot rolled into medium plate product, product specifications thickness × width × length (mm): 30 × 1800 × 6000;
[0036] (3) Solution treatment of 321 hot-rolled plate: the temperature of zone 1-4 is 950℃, the temperature of zone 5-6 is 1130℃, the thickness of the steel plate is 30mm, the insulation time of the steel plate in the furnace is 30min, the furnace is 30m, and the wire speed of the steel plate in the furnace is 1m / min.
[0037] The 30mm thick 321H stainless steel medium plate produced through the above steps has a grain size of grade 6 and an Rp0.2 of 130Mpa at 590℃.
[0038] Embodiment 2:
[0039] (1) 321H stainless steel continuous casting billet was produced by electric furnace + AOD + LF + VD + continuous casting process. During the VD process, the molten steel temperature was 1625°C, the vacuum degree was 1.7 mbar, the cycle time was 40 min, and the composition of the continuous casting billet was as follows: C 0.055, Si 0.61, Mn 0.85, P0.0029, S 0.001, Cr 17.18, Ni 9.05, N 0.007, Ti 0.33, C / Ti=16.8;
[0040] (2) 321H continuous casting billet is hot rolled into medium plate product, product specifications thickness × width × length (mm): 40 × 2300 × 7200;
[0041] (3) Solution treatment of 321 hot-rolled plate: the temperature of zone 1-4 is 950℃, the temperature of zone 5-6 is 1130℃, the thickness of the steel plate is 40mm, the insulation time of the steel plate in the furnace is 40min, the furnace is 30m, and the wire speed of the steel plate in the furnace is 0.75m / min.
[0042] The 40mm thick 321H stainless steel medium plate produced through the above steps has a grain size of 6-5 and an Rp0.2 of 134Mpa at 590℃.
[0043] Example 3
[0044] According to the method of Example 1, 321H hot-rolled plate was prepared and subjected to heat treatment tests at different temperatures and holding times. The results are shown in Table 1.
[0045] Table 1: Effect of solution temperature and time on grain size and 590℃ high temperature yield strength of 321H hot rolled plate
[0046] Temperature(℃) Time (min) Grain size grade <![CDATA[R p0.2 (N / mm 2 )]]> Result determination 1090 30 8 130 Failure 1090 40 8 135 Failure 1090 50 8 128 Failure 1100 30 8 125 Failure 1100 40 8 120 Failure 1100 50 8 119 Failure 1130 30 7 134 qualified 1130 40 7 125 qualified 1130 50 6 115 Failure 1150 30 6 120 Failure 1150 40 4-5 112 Failure 1150 50 3-4 111 Failure
[0047] The present invention has been disclosed above with preferred embodiments, but those skilled in the art should understand that these embodiments are only used to describe the present invention and should not be understood as limiting the scope of the present invention. It should be noted that all changes and substitutions equivalent to these embodiments should be deemed to be included in the scope of the claims of the present invention. Therefore, the scope of protection of the present invention should be based on the scope defined in the claims.
Claims
1. A method for improving the high temperature yield strength of 321H medium and thick plates, characterized in that: include: (1) 321H stainless steel continuous casting billet is produced by electric furnace smelting, AOD refining, LF refining, VD denitrification and continuous casting process; Wherein, the C content in the continuous casting billet is 0.05-0.06wt%, the Ti content is 0.30-0.35wt%, N≤0.009wt%, and C / Ti is 0.15-0.20; (2) hot rolling the continuously cast slab to obtain a hot rolled plate; (3) A solution furnace is used to perform a solution treatment on the hot-rolled plate.
2. The method for improving the high temperature yield strength of 321H medium and thick plate according to claim 1, characterized in that: In the VD denitrification process, after the ladle arrives at the workstation, the temperature of the molten steel is ≥1600℃, and the cycle time is ≥40min at a vacuum degree ≤2mbar.
3. The method for improving the high temperature yield strength of 321H medium and thick plate according to claim 1, characterized in that: The temperature of zones 1-4 of the solid solution furnace is 950±10°C, and the temperature of zones 5-6 is 1130±10°C.
4. The method for improving the high temperature yield strength of 321H medium and thick plate according to claim 1, characterized in that: The holding time of the solution treatment is 1.0 to 1.5 min / mm thickness.
5. A 321H medium and thick plate, characterized in that: The steel plate is prepared by the method for improving the high temperature yield strength of 321H medium and thick plates as described in any one of claims 1 to 4.
6. The 321H medium and thick plate according to claim 5, characterized in that: 590℃ yield strength ≥124Mpa.
7. Use of the 321H medium and thick plate according to claim 5 or 6 in the preparation of chemical equipment.
8. The use according to claim 7, characterized in that: The chemical equipment is a reactor.
Citation Information
Patent Citations
High-strength atmospheric corrosion-resistant medium plate and manufacturing method thereof
CN101736204A
High-temperature solution treatment method of 347H medium plate
CN111893259A
Control method for narrowing grain size of high-carbon heat-resistant stainless steel
CN111944969A
Production method for improving yield strength of ultra-low N Ti-containing austenitic stainless steel medium plate product
CN111996438A
High-strength high-corrosion-resistance austenitic stainless steel cold-rolled coil plate and preparation method thereof
CN116005062A