Efficient heat treatment thick steel plate for high-performance hydrogen storage equipment and manufacturing method thereof

Through new chemical composition design and efficient heat treatment process, the problem that existing technology cannot effectively produce high-performance thickness steel plates has been solved, and the 65-110mm thickness steel plates have excellent strength, low-temperature toughness and formability, meeting the needs of high-performance hydrogen storage equipment manufacturing needs and improve heat treatment efficiency.

CN118745554AActive Publication Date: 2024-10-08ANGANG STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410861852.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-08
Estimated Expiration
2044-06-28

Smart Images

  • Figure BDA0004919315220000071
    Figure BDA0004919315220000071
  • Figure BDA0004919315220000072
    Figure BDA0004919315220000072
  • Figure BDA0004919315220000081
    Figure BDA0004919315220000081
Patent Text Reader

Abstract

The invention provides a thick steel plate for efficient heat treatment high-performance hydrogen storage equipment and a manufacturing method of the thick steel plate. The steel plate comprises the following components in percentage by weight: 0.06%-0.09% of C, 0.37%-0.49% of Si, 1.45%-1.57% of Mn, less than or equal to 0.010% of P, less than or equal to 0.005% of S, 1.2%-1.4% of Ni, 0.03%-0.05% of V, 0.005%-0.01% of Ti, 0.020%-0.045% of Alt, 3%-10% of V / Ti and the balance of Fe and inevitable impurities. The production method of the steel plate comprises the steps of smelting, continuous casting, slab heating, rolling, hot straightening, slow cooling and heat treatment. Under the room temperature condition of the steel plate, at the T / 4 position of the steel plate, Rm is larger than or equal to 885 MPa and smaller than or equal to 970 MPa, Rel is larger than or equal to 755 MPa and smaller than or equal to 780 MPa, at the T / 2 position of the steel plate, Rm is larger than or equal to 890 MPa and smaller than or equal to 970 MPa, and Rel is larger than or equal to 750 MPa and smaller than or equal to 770 MPa; under the condition of-60 DEG C, KV2 is greater than or equal to 130J. The microscopic structure of the steel plate is a ferrite and sorbite structure, and the volume ratio of ferrite to sorbite is 3.5-4.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal materials, and in particular relates to a thick steel plate for efficient heat treatment and high-performance hydrogen storage equipment and a manufacturing method thereof. Background Art

[0002] Hydrogen energy has the characteristics of wide sources, convenient storage and transportation, efficient use, clean and environmentally friendly, etc. It is not only a clean energy, but also an important means to support the cleanness of fossil energy and the scale of renewable energy. From the perspective of hydrogen energy development trends, hydrogen energy technology has become a new generation of disruptive energy technology leading industrial transformation.

[0003] The development of steel plates for hydrogen energy storage and transportation equipment focuses on a good match of strength and toughness to ensure the low-temperature service performance of the steel plates. With the upgrading of domestic pressure-bearing manufacturing equipment, domestic petrochemical projects are developing in the direction of large-scale and high-performance. The demand for thick steel plates is increasing, and it is particularly important to solve the uniformity of grains in the thickness direction of thick steel plates. The performance of some traditional steel for pressure equipment and the corresponding manufacturing methods can no longer meet the requirements of the development trend of hydrogen energy storage and transportation. In addition, although some grades can meet the project design requirements at this stage, there is still a need for upgrading in the long run. Therefore, it is urgent to develop an efficient production method to produce high-performance steel plates for hydrogen storage equipment.

[0004] The public invention patent "A low temper brittle Cr-Mo series high temperature resistant pressure equipment steel plate" (CN104805380A) describes a steel plate composed of the following components in weight percentage: C: 0.05%~0.17%, Si: 0.30%, Mn: 0.40%~0.65%, S: 0.035%, P: 0.015%, Cr: 0.80%~1.15%, Mo: 0.45%~0.60%, Sn: 0.005%, Sb: 00025‰, As: 0.005‰; under the above composition, the normalizing + tempering heat treatment method is adopted to produce steel plates with a thickness specification of 20-40mm. No research has been conducted on steel plates with a thickness of less than 20mm and more than 40mm, and the research content needs to be improved urgently for full thickness steel plates.

[0005] The disclosed invention patent "A steel plate for pressure vessels with a thickness of more than 200-250 mm and resistance to hydrogen-induced cracking" (CN113278878A) describes a steel plate composed of the following components in weight percentage: C: 0.10-0.20%, Si: 0.15-0.40%, Mn: 0.95-1.35%, P: ≤0.005%, S: ≤0.0008%, Cr: 0.10-0.30%, Ni: 0.25-0.40%, Mo: 0.08-0.12%, Alt: 0.02-0.05%, Nb: 0.01-0.02%, V: 0.01-0.03%, Ti: 0.01-0.02%, B: ≤0.0005%, and the remainder is Fe and unavoidable impurity elements. The above ingredients combined with normalizing + water accelerated cooling + tempering heat treatment process are only for the production of steel plates with a thickness specification of 200-250mm. The total heat treatment time is more than 12 hours, which seriously occupies heat treatment resources and does not conform to the idea of ​​efficient production.

[0006] The invention patent "A method for producing thin high-toughness 12Cr1MoVR pressure vessel steel plate" (CN114855057A) states that the steel plate is composed of the following weight percentages: C: 0.12-0.14%, Si: 0.25-0.35%, Mn: 0.50-0.65%, P: ≤0.015%, S: ≤0.005%, Nb: 0.025-0.035%, V: 0.15-0.30%, Cr: 0.90-1.20%, Mo: 0.25-0.35%, Als: 0.15-0.32%, H≤1.7ppm; O: ≤0.0036%; N: ≤0.0044%; the rest is iron and unavoidable impurities. The thickness of the steel plate is 10-40mm, and no research has been done on the steel plate with a thickness of more than 40mm, and only the room temperature impact value is given. The lack of a series of impact studies does not meet the design requirements for steel plates used in hydrogen storage equipment. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to prepare a thick steel plate for high-performance hydrogen storage equipment with efficient heat treatment, and through a new chemical composition design, an efficient heat treatment method and a special production and manufacturing process, the steel plate T / 4: 885MPa≤Rm≤970MPa, 755MPa≤Rel≤780MPa, the steel plate T / 2: 890MPa≤Rm≤970MPa, 750MPa≤Rel≤770MPa; at -60°C, KV2≥130J. That is, a steel plate with a thickness of (65-110) mm with excellent strength, low-temperature toughness, formability and plate shape is obtained, which meets the manufacturing and application requirements of high-performance hydrogen storage equipment.

[0008] The object of the invention is achieved in this way:

[0009] A thick steel plate for high-performance hydrogen storage equipment with efficient heat treatment, whose chemical composition range is: C: 0.06% to 0.09%, Si: 0.37% to 0.49%, Mn: 1.45% to 1.57%, P: ≤0.010%, S: ≤0.005%, Ni: 1.2% to 1.4%, V: 0.03% to 0.05%, Ti: 0.005 to 0.01%, Alt: 0.020% to 0.045%, and the balance is Fe and unavoidable inclusions.

[0010] Furthermore, the V / Ti=3-10.

[0011] Furthermore, at room temperature, the steel plate T / 4: 885MPa≤R m ≤970MPa、755MPa≤R el ≤780MPa, Steel plate T / 2: 890MPa≤R m ≤970MPa、750MPa≤R el ≤770MPa; KV2≥130J under -60℃ condition.

[0012] Furthermore, the steel plate has a ferrite+sorbite structure, and the volume ratio of ferrite to sorbite is 3.5-4.

[0013] Furthermore, the thickness of the steel plate is 65 to 110 mm.

[0014] The reasons for the composition design of the present invention are as follows:

[0015] C: 0.06%~0.09%

[0016] C is the main element in steel, and the combination of C and strong carbide alloy elements in steel plays a precipitation strengthening role. However, too high a carbon content will affect the machining performance of the steel, and oversaturated carbides will also affect the low-temperature toughness of the steel plate. Therefore, the present invention sets the C content range to 0.06% to 0.09%.

[0017] Si: 0.37%~0.49%

[0018] Si is used as a reducing agent and deoxidizer in the steelmaking process. Si is a cheap alloying element. Adding an appropriate amount of Si to steel can improve the hardness and strength of ferrite in the steel. When the silicon content is higher than 0.49%, it is easy to form hard phase compounds, which affects the plasticity and toughness of the steel plate and is prone to cracks during later processing. Therefore, the present invention sets the Si content range to 0.37% to 0.49%.

[0019] Mn: 1.45%~1.57%

[0020] Mn is an element that strongly stabilizes austenite, reduces the lower critical point of steel, increases the degree of supercooling when austenite is cooled, and refines the pearlite structure to improve the mechanical properties of the steel plate. However, too high a Mn content will increase the tendency of grain coarsening in steel, so the present invention sets the Mn content range to 1.45% to 1.57%.

[0021] P:≤0.010%, S:≤0.005%

[0022] S and P are harmful elements in steel and must be strictly controlled to ensure the purity and plasticity of the steel. Therefore, the present invention limits P to 0.010% and S to 0.005%.

[0023] Ni: 1.2%~1.4%

[0024] The lattice constant of Ni element is similar to that of γ iron, so it can form a continuous solid solution, which can lower the critical point and increase the stability of austenite. It is an alloy element that strengthens the austenite zone and has the effect of refining ferrite grains. At the same time, it can reduce the quenching temperature, increase the hardenability of the steel plate, and ensure the comprehensive improvement of the strength, plasticity and toughness of the steel, especially the low-temperature toughness. The steel plate for hydrogen storage equipment needs to have good corrosion resistance due to the use requirements. Ni can form a dense oxide film on the surface of the steel plate, thereby improving the corrosion resistance of the steel plate. However, considering the comprehensive cost, the present invention sets the Ni content range at 1.2% to 1.4%.

[0025] V: 0.03%~0.05%

[0026] V is a strong carbide-forming element, which exists in the form of carbides in steel, plays a role in precipitation strengthening, refines the structure of steel, reduces the grain size, and thus improves the strength and yield ratio of the steel plate after normalizing and the low-temperature toughness. However, when the content is too high, it will have a negative impact on the hardenability of the steel plate, so the present invention sets the V content range to 0.03% to 0.05%.

[0027] Ti: 0.005~0.01%

[0028] Ti has a strong affinity with nitrogen, oxygen and carbon, and its affinity with sulfur is stronger than that of iron. It is a good deoxidizing and degassing agent and an effective element for fixing nitrogen and carbon. It is easy to combine with C in steel to play a precipitation strengthening role. At the same time, it is finely dispersed in the steel plate matrix with appropriate production technology, so that the toughness of the steel plate is not reduced while the strength is improved. However, when the Ti content is too high, the carbide size is too large, which will affect the toughness and hardenability of the steel plate. Therefore, the present invention adds Ti: 0.005-0.01%. When Ti and V are added to the steel plate at the same time, the two work together to form a multi-component composite precipitation phase (Ti, V) X (X = C, N), forming fine and dispersed carbon and nitrogen precipitates, pinning the grain boundaries and playing a precipitation strengthening role. In addition, the TiC particles that can still stably exist when heated in the high temperature section can effectively improve the low-temperature toughness, so the V / Ti ratio is controlled in the range of 3-10.

[0029] Alt: 0.020%~0.045%

[0030] Alt is a commonly used deoxidizer in steel. Adding a small amount of aluminum can refine the grains and improve the strength and impact toughness of steel. Too high an amount will affect the hot working properties, welding properties and cutting properties of steel. The present invention limits the Alt content to 0.020% to 0.045%.

[0031] The second technical solution of the present invention is to provide a method for manufacturing thick steel plates for high-performance hydrogen storage equipment with efficient heat treatment, including smelting, continuous casting, slab heating, rolling, hot straightening, slow cooling, and heat treatment. A short-time normalizing heat treatment combined with a two-stage controlled rolling method is used to produce container steel plates with a thickness of 65-110 mm. The structure of the entire thickness section of the produced steel plate is uniform, and the steel plate has good strength and toughness matching at 1 / 4 and 1 / 2 thickness, and excellent low-temperature performance.

[0032] 1. Smelting process: The smelting of molten steel is carried out in a converter, using high-quality scrap steel and molten iron as raw materials, and the molten iron content is controlled at more than 78% to ensure the purity of the steel and reduce the difficulty of subsequent processes. Strictly control the setting of converter dephosphorization and decarburization smelting parameters. In order to effectively reduce the content of harmful elements P, the oxygen blowing for dephosphorization is controlled at 8 to 12 minutes, and the oxygen blowing for decarburization is controlled at 7 to 9 minutes, and the mass fraction of phosphorus in the molten steel is controlled to be less than 0.005%; further use the LF refining furnace for deep desulfurization treatment, and the sulfur content is controlled below 0.003%; degassing is completed in the VD furnace, the net cycle time is 7 to 12 minutes, and the calming time before pouring is 5 to 7 minutes.

[0033] 2. Casting process: After breaking the vacuum, the slab continuous casting machine is used for casting, and the casting temperature is controlled. The casting temperature of the tundish molten steel is 1495-1506℃, the superheat is set to 10-20℃, and the billet drawing rate during casting is 1.0-1.2m / min. Low-temperature casting is better to refine the original cast structure. In order to control the central segregation and looseness of the continuous casting billet, electromagnetic stirring or continuous casting billet light reduction process is adopted, in which the light reduction rate is controlled at 8-10%, and the billet is stacked and slowly cooled after it comes off the line. The stacking slow cooling time is 24-36h.

[0034] 3. Heating process: The continuous casting slab is sent to the heating furnace for heating. The slab is heated through the preheating section, heating section and soaking section before being taken out of the furnace. The temperature range of the preheating section is 790-835°C, the temperature range of the heating section is 1185-1210°C, and the temperature range of the soaking section is 1235-1265°C. The soaking time of the slab is controlled at 4.6-5.4h. When the heating temperature is lower than 1235°C, the coarse precipitates in the continuous casting slab cannot be dissolved, the austenitization of the steel plate is incomplete, and the final rolling temperature of the first stage cannot be guaranteed; when the heating temperature is higher than 1250°C, it is easy to cause the fine precipitates in the continuous casting slab to dissolve again and cause excessive grain growth.

[0035] 4. Rolling process:

[0036] The rolling adopts a three-stage controlled rolling method. The first stage recrystallization zone starts at a rolling temperature of 1150-1160°C, and the recrystallization zone ends at a rolling temperature of ≥1115°C. The original austenite structure is fully refined, and the total deformation rate is controlled at more than 50%. Large deformation rapid rolling is adopted, and the rolling speed is 3.7-4.2 m / s; the non-recrystallization zone starts at a rolling temperature of 900-950°C, and the final rolling temperature is 830-860°C, but the reduction is controlled at 3-5% at this point. Small deformation and multiple rapid rolling, with a rolling speed of 3.5-3.8 m / s. At this time, the austenite grains are further flattened and elongated. With the increase of grain boundary area, the ferrite nucleation rate increases in the subsequent phase transformation process, and the grains are fully refined; three-stage homogeneous rolling, the starting rolling temperature is 760-790°C, the ending rolling temperature is 672-680°C, and the reduction is controlled at 1-3%. At this stage, the surface quality of the steel plate is further adjusted to improve the service performance of the steel plate.

[0037] 5. Heat treatment process: Since elements such as C, Mn, Ni, V, and Ti are added to the steel, the steel plate can obtain a ferrite + troostite structure with excellent strength and toughness after rolling. However, the grain size distribution of the steel plate is uneven, there is concentration of structural stress and thermal stress, and delayed cracks are easily generated during flame cutting. Therefore, heat treatment should be used in time to soften and eliminate stress. Heating for too long will cause secondary growth as much as possible and increase production costs. Therefore, the present invention adopts a short-time normalizing heat treatment to ensure that the strength of the hydrogen storage steel plate is not lost, and the steel plate has suitable plastic toughness and good processing performance. Therefore, the normalizing heat treatment temperature of the steel is 870-890°C, and a short-time insulation system of 10-15 minutes is adopted, the heating rate is controlled at 0.9-1.1min / mm, and the cooling rate is 23-26°C / s.

[0038] The beneficial effects of the present invention are:

[0039] (1) On the basis of strengthening elements C, Si, and Mn, by adding appropriate amounts of Ni, V, and Ti alloying elements, while strictly controlling the content of harmful elements P and S, combined with production process optimization, a refined ferrite + troostite structure is obtained, and the volume ratio of ferrite to troostite is 3.5 to 4. The second phase carbide particles with a size of less than 10nm are evenly dispersed, ensuring the strong plasticity and low-temperature toughness of the steel plate.

[0040] (2) The mechanical properties of the steel plate for hydrogen storage equipment obtained through a unique production process are as follows: at room temperature, at T / 4 of the steel plate: 885MPa≤Rm≤970MPa, 755MPa≤Rel≤780MPa; at T / 2 of the steel plate: 890MPa≤Rm≤970MPa, 750MPa≤Rel≤770MPa; at -60°C, KV2≥130J.

[0041] (3) The present invention obtains a high-performance steel plate for hydrogen storage equipment with excellent plate shape and a thickness specification of (65 to 110) mm. DETAILED DESCRIPTION

[0042] The present invention will be further described below by way of examples.

[0043] The embodiment of the present invention performs smelting, continuous casting, slab heating, rolling, hot straightening, slow cooling and heat treatment according to the component ratio of the technical solution, and is characterized in that:

[0044] Slab heating

[0045] The temperature range of the preheating section is 790-835°C, the temperature range of the heating section is 1185-1210°C, the temperature range of the soaking section is 1235-1265°C, and the soaking time of the slab is controlled at 4.6-5.4h;

[0046] Rolling process

[0047] The rolling adopts a three-stage controlled rolling method. The first-stage recrystallization zone has a start rolling temperature of 1150-1160°C, a recrystallization zone rolling end temperature of ≥1115°C, a total deformation rate of more than 50%, and a large deformation rapid rolling method with a rolling speed of 3.7-4.2 m / s. The second-stage non-recrystallization zone has a start rolling temperature of 900-950°C, a final rolling temperature of 830-860°C, but the reduction is controlled at 3-5%, and a small deformation multi-pass rapid rolling method is adopted with a rolling speed of 3.5-3.8 m / s. The three-stage homogenous rolling method has a start rolling temperature of 760-790°C, a final rolling temperature of 672-680°C, and a controlled reduction of 1-3%.

[0048] Heat Treatment

[0049] The normalizing heat treatment temperature is 870-890°C, and a short-time insulation system of 10-15 minutes is adopted, the heating rate is controlled at 0.9-1.1 min / mm, and the cooling rate is 23-26°C / s.

[0050] Furthermore, in the smelting process, the dephosphorization oxygen blowing is controlled within 8 to 12 minutes, and the decarburization oxygen blowing is controlled within 7 to 9 minutes, so that the mass fraction of phosphorus in the molten steel is controlled to be less than 0.005%; the LF refining furnace is further used for deep desulfurization treatment, and the sulfur content is controlled below 0.003%; the degassing is completed in the VD furnace, the net cycle time is 7 to 12 minutes, and the calming time before pouring is 5 to 7 minutes.

[0051] Furthermore, the continuous casting process adopts a slab continuous casting machine for casting, focusing on controlling the casting temperature, the tundish molten steel casting temperature is 1495-1506°C, the superheat is set to 10-20°C, and the billet drawing rate during casting is 1.0-1.2m / min. Low temperature casting is better to refine the original cast structure. In order to control the central segregation and looseness of the continuous casting billet, electromagnetic stirring or continuous casting billet light reduction process is adopted, wherein the light reduction rate is controlled at 8-10%, the billet is stacked and slowly cooled after it comes off the line, and the enclosure stacking is adopted, the number of enclosure faces is controlled at 2-3, and the stacking slow cooling time is 24-36h, so as to improve the internal quality of the steel plate and reduce the occurrence of defects such as cracks.

[0052] The embodiments specifically illustrate the content of the present invention. These embodiments are only general descriptions of the content of the present invention and do not limit the content of the present invention. Table 1 shows the chemical composition of the embodiment of the present invention, Table 2 shows the smelting and continuous casting process parameters of the embodiment steel, Table 3 shows the rolling parameters of the embodiment steel, Table 4 shows the heat treatment parameters of the embodiment steel, and Table 5 shows the final effect of the mechanical properties of the embodiment.

[0053] Table 1 Chemical composition of the examples (wt, %)

[0054]

[0055] Table 2 Smelting and continuous casting process parameters of the embodiment

[0056]

[0057] Table 3 shows the rolling parameters of the example steel

[0058]

[0059] Table 4 Heat treatment process parameters of example steel

[0060]

[0061] Table 5 Final results of organization and mechanical properties of the examples

[0062]

[0063] As can be seen from the above, the mechanical properties of the steel plate for high-performance hydrogen storage equipment with excellent plate shape and thickness of (65-110) mm provided by the present invention are as follows: at room temperature (0-25°C), the steel plate T / 4: 885MPa≤R m ≤970MPa、755MPa≤R el ≤780MPa, Steel plate T / 2: 890MPa≤R m ≤970MPa、750MPa≤R el ≤770MPa; KV2≥130J under -60℃ condition.

[0064] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.

Claims

1. A thick steel plate for high-performance hydrogen storage equipment with high-efficiency heat treatment, characterized in that: Calculated by weight percentage, it includes the following components: C: 0.06%-0.09%, Si: 0.37%-0.49%, Mn: 1.45%-1.57%, P: ≤0.010%, S: ≤0.005%, Ni: 1.2%-1.4%, V: 0.03%-0.05%, Ti: 0.005-0.01%, Alt: 0.020%-0.045%, and the balance is Fe and unavoidable inclusions.

2. The thick steel plate for high-performance hydrogen storage equipment with high-efficiency heat treatment according to claim 1, characterized in that: The V / Ti=3-10.

3. The thick steel plate for high-performance hydrogen storage equipment with high-efficiency heat treatment according to claim 1, characterized in that: The steel plate is at room temperature, at T / 4 of the steel plate: 885MPa≤R m ≤970MPa、755MPa≤R el ≤780MPa, steel plate T / 2: 890MPa≤R m ≤970MPa、750MPa≤R el ≤770MPa; KV2≥130J under -60℃ condition.

4. The thick steel plate for high-performance hydrogen storage equipment with high-efficiency heat treatment according to claim 1, characterized in that: The steel plate has a microstructure of ferrite + troostite, with a volume ratio of ferrite to troostite of 3.5 to 4; and also includes second phase particles TiC and VC, with sizes of 4 to 6 nm and 7 to 9 nm respectively.

5. The thick steel plate for high-performance hydrogen storage equipment with high-efficiency heat treatment according to claim 1, characterized in that: The thickness of the steel plate is 65 to 110 mm.

6. A method for manufacturing a thick steel plate for high-performance hydrogen storage equipment with high-efficiency heat treatment according to any one of claims 1 to 5, comprising smelting, continuous casting, slab heating, rolling, hot straightening, slow cooling, and heat treatment, characterized in that: Slab heating The temperature range of the preheating section is 790-835°C, the temperature range of the heating section is 1185-1210°C, the temperature range of the soaking section is 1235-1265°C, and the soaking time of the slab is controlled at 4.6-5.4h; Rolling process The rolling adopts a three-stage controlled rolling method. The first-stage recrystallization zone has a start rolling temperature of 1150-1160°C, a recrystallization zone rolling end temperature of ≥1115°C, a total deformation rate of more than 50%, and a large deformation rapid rolling method with a rolling speed of 3.7-4.2 m / s. The second-stage non-recrystallization zone has a start rolling temperature of 900-950°C, a final rolling temperature of 830-860°C, but the reduction is controlled at 3-5%, and a small deformation multi-pass rapid rolling method is adopted with a rolling speed of 3.5-3.8 m / s. The three-stage homogenous rolling method has a start rolling temperature of 760-790°C, a final rolling temperature of 672-680°C, and a controlled reduction of 1-3%. Heat Treatment The normalizing heat treatment temperature is 870-890°C, and a short-time insulation system of 10-15 minutes is adopted, the heating rate is controlled at 0.9-1.1 min / mm, and the cooling rate is 23-26°C / s.

7. The method for manufacturing a thick steel plate for high-performance hydrogen storage equipment with high-efficiency heat treatment according to claim 6, characterized in that: In the smelting process, the oxygen blowing for dephosphorization is controlled within 8 to 12 minutes, and the oxygen blowing for decarburization is controlled within 7 to 9 minutes; the LF refining furnace is further used for deep desulfurization treatment; the degassing is completed in the VD furnace, the net cycle time is 7 to 12 minutes, and the calming time before pouring is 5 to 7 minutes.

8. The method for manufacturing a thick steel plate for high-performance hydrogen storage equipment with high-efficiency heat treatment according to claim 6, characterized in that: The continuous casting process adopts a slab continuous casting machine for casting, focusing on controlling the casting temperature, the tundish molten steel casting temperature is 1495-1506°C, the superheat is set to 10-20°C, and the billet drawing rate during casting is 1.0-1.2m / min. Low temperature casting is better to refine the original cast structure. In order to control the central segregation and looseness of the continuous casting billet, electromagnetic stirring or continuous casting billet light reduction process is adopted, wherein the light reduction rate is controlled at 8-10%, the billet is stacked and slowly cooled down after it comes off the line, and the enclosure stacking is adopted, the number of enclosure faces is controlled at 2-3, and the stacking slow cooling time is 24-36h.

Citation Information

Patent Citations

  • Low-compression-ratio 690 MPa-grade super-thick steel plate and manufacturing method thereof

    CN110791713A

  • Extra-thick container steel plate with excellent low-temperature impact toughness at center

    CN111363973A

  • Steel sheet having excellent low-temperature toughness and method for producing same

    CN112011725A

  • 36kg-grade extra-thick low-temperature high-toughness ship plate steel and production method thereof

    CN114438415A

  • SA537CL1 steel plate with thickness of 60-100mm and excellent die welding performance and manufacturing method of SA537CL1 steel plate

    CN117418159A