Preparation method of nickel-based superalloy component, nickel-based superalloy component and application
By using overlapping three-dimensional models and reasonable laser melting forming parameters in the preparation of nickel-based superalloy components, the cracking problem of nickel-based superalloys during the selective laser melting forming process is solved, and its mechanical properties and applicability are improved, making it suitable for complex Rapid prototyping of structural parts.
Patent Information
- Application Number
- CN202410875368.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-08
AI Technical Summary
Nickel-based superalloys are prone to segregation and cracking during the selective laser melting and forming process, resulting in reduced mechanical properties and service life, making it difficult to meet the rapid prototyping needs of complex and precision structural parts.
Using the preparation method of nickel-based high-temperature alloy components, by establishing a three-dimensional model consisting of two identical models overlapping, setting reasonable laser melting forming parameters and a single laser remelting method, controlling the depth of the melted layer and the depth of remelting, and reducing crack-sensitive crystals limit the total length to avoid the formation of micro cracks.
It significantly inhibits the cracking of nickel-based high-temperature alloy components, improves its uniform deformation ability and load-bearing capacity, increases room temperature tensile strength and elongation, and is suitable for industrial production.
Smart Images

Figure CN118745571A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of additive manufacturing technology, and specifically to a method for preparing a nickel-based high-temperature alloy component, a nickel-based high-temperature alloy component and an application thereof. Background Art
[0002] GH3230 is a Ni-Cr-W based solid solution strengthened high temperature alloy with good high temperature strength, creep resistance and oxidation resistance. It has good high temperature service capability at 700℃-1000℃ and is suitable for long-term use of high temperature components at the hot end of aircraft engines and gas turbines, such as combustion chambers and turbine disks. The traditional casting and forging of GH3230 has a long manufacturing cycle and a simple molding structure, which is difficult to meet the rapid prototyping of special complex structural parts and precision structural parts.
[0003] Selective laser melting (SLM) is an additive manufacturing technology suitable for metal materials. It can form complex structural parts with multiple holes and thin walls by stacking layers according to the three-dimensional model structure, and has good forming density and mechanical properties. However, due to the extremely fast melting rate and large thermal gradient in the selective laser melting process, nickel-based alloys are prone to segregation and cracking during the forming process, especially Ni-Cr-W-based high-temperature alloys with a high degree of alloying, which seriously reduces the mechanical properties and service life of Ni-Cr-W-based high-temperature alloys. Summary of the invention
[0004] In view of the above, it is necessary to propose a preparation method of a nickel-based high-temperature alloy component, a nickel-based high-temperature alloy component and an application thereof, so as to eliminate microcracks in the formed nickel-based high-temperature alloy component and improve the mechanical properties of the nickel-based high-temperature alloy component.
[0005] The present invention provides a method for preparing a nickel-based high-temperature alloy component, comprising the following steps:
[0006] Pretreatment of nickel-based high-temperature alloy powders and stainless steel substrates;
[0007] Establishing a three-dimensional model of a nickel-based high-temperature alloy component, wherein the three-dimensional model is formed by overlapping two identical first models and a second model, slicing the established three-dimensional model along the Z-axis direction to generate a plurality of two-dimensional layers, and after the slicing is completed, setting a forming order of first forming the first model and then forming the second model, so that the second model remelts the first model, wherein the slice thicknesses of the first model and the second model are the same;
[0008] Placing the pretreated nickel-based high-temperature alloy powder in a liftable powder cabin, and placing the pretreated stainless steel substrate in a forming cabin, leveling the stainless steel substrate and the scraper so that the surface of the stainless steel substrate is flush with the surface of the scraper, closing the cabin door of the forming cabin, introducing inert gas into the forming cabin so that the oxygen content in the forming cabin is reduced to a first value, and heating the stainless steel substrate to a second value to complete preheating of the stainless steel substrate;
[0009] Setting laser melting forming parameters, wherein the laser melting forming parameters include that the linear energy density during forming of the second model is 80%-100% of that of the first model, so that the melting layer depth of the second model is 50%-85% of that of the first model;
[0010] Laser layered scanning is performed according to the laser melting forming parameters and the three-dimensional model to achieve laser melting forming and laser remelting. The laser melting and laser remelting processes are repeated to obtain a nickel-based high-temperature alloy component.
[0011] In some embodiments, the nickel-based high-temperature alloy powder is composed of the following by mass fraction: Cr content is 20%-24%, W content is 12.5%-14.5%, Mo content is 1%-3%, Fe content is less than 3%, Co content is less than 1%-5%, C content is 0.1%-0.3%, Si content is 0.2%-0.5%, Mn content is 0.3%-1.0%, Al content is 0.2%-0.5%, B content is 0.001%-0.01%, La content is 0.01%-0.05%, and the balance is Ni element and unavoidable impurities.
[0012] In some embodiments, the step of pretreating the nickel-based high-temperature alloy powder and the stainless steel substrate further comprises:
[0013] The nickel-based high-temperature alloy powder is dried in an inert gas environment for later use, and the stainless steel substrate is polished and wiped with alcohol to remove the surface oxide layer and oil stains, and then dried for later use.
[0014] In some embodiments, the particle size distribution range of the nickel-based high-temperature alloy powder is 20 μm-55 μm.
[0015] In some embodiments, the first value ranges from less than 100 ppm, and the second value ranges from 140° C. to 160° C.
[0016] In some embodiments, the laser melting forming parameters also include laser power, scanning speed, scanning spacing and powder layer thickness. The laser power of the first model ranges from 210W to 250W, the scanning speed ranges from 700mm / s to 1100mm / s, the scanning spacing ranges from 0.08mm to 0.12mm, and the powder layer thickness ranges from 0.03mm to 0.05mm. The laser power of the second model ranges from 200W to 250W, the scanning speed ranges from 700mm / s to 1100mm / s, the scanning spacing ranges from 0.08mm to 0.12mm, and the powder layer thickness ranges from 0.03mm to 0.05mm. The single-layer laser scanning mode is strip bidirectional scanning, and the laser scanning path between adjacent layers rotates 60° to 70° clockwise.
[0017] In some embodiments, an angle between a scanning path of the second model and a scanning path of the first model in the same layer is 0°-67°.
[0018] In some embodiments, the step of performing laser layered scanning according to the laser melting forming parameters and the three-dimensional model to achieve laser melting forming and laser remelting, and the laser melting and laser remelting processes are performed reciprocally to obtain a nickel-based high-temperature alloy component further includes:
[0019] Moving the scraper to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a first layer of nickel-based high-temperature alloy powder;
[0020] Turning on the laser so that the laser performs a first layer scanning along a direction parallel to the bottom edge of the first model to complete the laser forming of the first layer of the first model, thereby completing the laser forming of the first layer of the three-dimensional model;
[0021] Scanning a second time again along a scanning path with an angle of 0°-67° with the scanning direction of the first layer of the first model to complete laser forming of the first layer of the second model;
[0022] Lowering the forming chamber and lifting the powder chamber, moving the scraper to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a second layer of alloy powder;
[0023] Turning on the laser so that the laser scans the second layer along a direction forming an angle of 60°-70° with the scanning direction of the first layer of the first model, thereby completing laser forming of the second layer of the first model;
[0024] Performing a second scan again along a scanning path with an angle of 0°-67° with respect to the scanning direction of the second layer of the first model to complete the laser forming of the second layer of the second model, thereby completing the laser forming of the second layer of the three-dimensional model;
[0025] The forming process of the second layer of the three-dimensional model is repeated cyclically until the forming of all scanned layers is completed, thereby obtaining a nickel-based high-temperature alloy component.
[0026] The embodiment of the present application also provides a nickel-based high-temperature alloy component, which is prepared using the preparation method described above.
[0027] In some embodiments, the nickel-based high-temperature alloy components prepared by the preparation method described above are used in gas turbine combustion chambers, flanges, turbine disks, and petrochemical equipment.
[0028] The preparation method, nickel-based high-temperature alloy component and application of the above-mentioned nickel-based high-temperature alloy component, by setting reasonable laser melting forming parameters and specifically limiting the single laser remelting method and remelting strategy, greatly reduce the total length of crack-sensitive grain boundaries, significantly inhibit the cracking of nickel-based high-temperature alloy components, and avoid the formation of microcracks on the nickel-based high-temperature alloy components. In addition, since the effective inhibition of cracking improves the uniform deformation capacity and bearing capacity of the nickel-based high-temperature alloy components, the room temperature tensile strength and elongation of the nickel-based high-temperature alloy components are significantly improved. In addition, the present application introduces a single remelting method based on the nickel-based high-temperature alloy powder and selective laser melting method, which reduces the heat input effect on the nickel-based high-temperature alloy components, and the three-dimensional model parameter assignment is simple, with strong practicality and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A flow chart of a method for preparing a nickel-based high-temperature alloy component provided in an embodiment of the present application.
[0030] Figure 2 yes Figure 1 Specific step flow chart of step S50 described in .
[0031] Figure 3 Schematic diagram of the scanning paths of Example 1, Example 2 and Comparative Examples 1 and 2 of the present application.
[0032] Figure 4 These are optical micrographs of crack distribution of Example 1, Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3.
[0033] Figure 5 These are micrographs of the molten pool morphologies of Example 1, Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3.
[0034] Figure 6These are the grain morphology images of Example 1, Example 2, Comparative Example 1 and Comparative Example 2.
[0035] Figure 7 It is a statistical distribution diagram of cracking grain boundary angles, and a 30°-40° grain boundary distribution diagram of Example 1, Example 2 and Comparative Example 1.
[0036] Figure 8 The room temperature tensile stress-strain curves of Example 1, Example 2, Comparative Example 1 and Comparative Example 2 are shown. DETAILED DESCRIPTION
[0037] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0038] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the various specific processes and material examples provided by the present application, but those of ordinary skill in the art can appreciate the application of other processes and / or the use of other materials.
[0039] The embodiments of the present application are further described below in conjunction with the accompanying drawings.
[0040] The selective laser melting process has an extremely fast melting rate and a large thermal gradient, which causes segregation and cracking of nickel-based high-temperature alloy components during the forming process, especially nickel-based high-temperature alloy components with a high degree of alloying, which seriously reduces the mechanical properties and service life of nickel-based high-temperature alloy components.
[0041] In an existing embodiment, TiB2 particles are added to the nickel-based high-temperature alloy (GH3230) to achieve crack-free preparation and mechanical property improvement of the nickel-based high-temperature alloy component. However, the addition of TiB2 changes the composition of the nickel-based high-temperature alloy component, and the impact on the inherent performance is difficult to evaluate. In addition, TiB2 has a poor bond with the Ni matrix, and is prone to preferential cracking at the phase interface during high-temperature dynamic load service, thereby reducing service performance.
[0042] In an existing embodiment, Al, Ti, and Ta elements are added to the composition of Haynes 230 (GH3230) to prepare a crack-free nickel-based high-temperature alloy component, which has good room temperature and high temperature tensile properties. However, due to the introduction of a large amount of Al, Ti, and Ta elements in the nickel-based high-temperature alloy component, a large amount of γ' phase appears in the alloy, which changes the inherent properties of the Haynes 230 alloy.
[0043] In an existing implementation, the porosity defects of titanium alloy are eliminated by adopting a low-power dislocation remelting method, and the density of the alloy is improved. The remelting laser scanning path is limited to the middle position between the first scanning paths, the path spacing is d / 2, and the scanning strategy is the same as the first scanning strategy. In addition, using a smaller laser energy, single-scan dense forming cannot be achieved, and the laser scanning line energy density of the remelting process is much smaller than the laser scanning line energy density of the forming process. The remelting depth is not standardized. The main effect is to improve the density of the titanium alloy, and the crack suppression effect is not clear.
[0044] In an existing embodiment, effective suppression of cracks in the K447A alloy is achieved by adopting a method of multiple remelting with a higher energy density, wherein the number of remelting times is 3 to 5 times per layer, the alloy forming efficiency is low, and multiple thermal cycles are prone to severe heat accumulation and residual stress, which is not conducive to the precise forming of thin-walled components and cantilever components.
[0045] Based on the problems existing in the existing implementation methods, the present application proposes a preparation method for effectively inhibiting the SLM process for forming nickel-based high-temperature alloy components without changing the alloy composition and without forming serious heat accumulation.
[0046] See also Figure 1 , the preparation method comprises the following steps:
[0047] S10, pre-treated nickel-based high-temperature alloy powder and stainless steel substrate.
[0048] In some embodiments, the step of pretreating the nickel-based high-temperature alloy powder and the stainless steel substrate further comprises:
[0049] The nickel-based high-temperature alloy powder is dried in an inert gas environment for later use, and the stainless steel substrate is polished and wiped with alcohol to remove the surface oxide layer and oil stains, and then dried for later use.
[0050] The nickel-based high-temperature alloy powder is composed of 20%-24% Cr, 12.5%-14.5% W, 1%-3% Mo, less than 3% Fe, less than 1%-5% Co, 0.1%-0.3% C, 0.2%-0.5% Si, 0.3%-1.0% Mn, 0.2%-0.5% Al, 0.001%-0.01% B, 0.01%-0.05% La, and the remainder is Ni element and unavoidable impurities.
[0051] The particle size distribution range of the nickel-based high-temperature alloy powder is 20 μm-55 μm.
[0052] S20, establishing a three-dimensional model of a nickel-based high-temperature alloy component, wherein the three-dimensional model is formed by overlapping two identical first models and a second model, slicing the established three-dimensional model along the Z-axis direction to generate multiple two-dimensional layers, and after the slicing is completed, setting a forming order of first forming the first model and then forming the second model, so that the second model remelts the first model, wherein the slice thickness of the first model and the second model is the same.
[0053] S30, placing the pretreated nickel-based high-temperature alloy powder in a liftable powder cabin, and placing the pretreated stainless steel substrate in a forming cabin, leveling the stainless steel substrate and the scraper so that the surface of the stainless steel substrate is flush with the surface of the scraper, ensuring that the powder is evenly spread on all parts of the stainless steel substrate, closing the cabin door of the forming cabin, introducing inert gas into the forming cabin to reduce the oxygen content in the forming cabin to a first value, and heating the stainless steel substrate to a second value to complete the preheating of the stainless steel substrate.
[0054] The first value has a range of less than 100 ppm, and the second value has a range of 140°C-160°C.
[0055] S40, setting laser melting forming parameters, wherein the laser melting forming parameters include that the linear energy density during forming of the second model is 80%-100% of that of the first model, so that the melting layer depth of the second model is 50%-85% of that of the first model.
[0056] Among them, the laser melting forming parameters also include laser power, scanning speed, scanning spacing and powder layer thickness. The laser power of the first model ranges from 210W to 250W, the scanning speed ranges from 700mm / s to 1100mm / s, the scanning spacing ranges from 0.08mm to 0.12mm, and the powder layer thickness ranges from 0.03mm to 0.05mm. The laser power of the second model ranges from 200W to 250W, the scanning speed ranges from 700mm / s to 1100mm / s, the scanning spacing ranges from 0.08mm to 0.12mm, and the powder layer thickness ranges from 0.03mm to 0.05mm. The single-layer laser scanning mode is strip bidirectional scanning, and the laser scanning path between adjacent layers rotates 60° to 70° clockwise.
[0057] The powder layer thickness of the first model and the second model is the same, so a larger powder layer thickness is more helpful to avoid columnar growth of grains and control the remelting depth.
[0058] The included angle between the scanning path of the second model and the scanning path of the first model in the same layer is 0°-67°.
[0059] Among them, cracks usually appear in the long dendrite area inside the large molten pool, and the microstructure in the molten pool changes from the cellular crystals at the edge of the molten pool to the large columnar dendrites in the center of the molten pool. In order to eliminate the large columnar dendrites, the melting layer depth of the second model is 50%-85% of the melting layer depth of the first model. The increase in the number of molten pool contours increases the number of cellular crystals, thereby improving the ability of the obtained nickel-based high-temperature alloy components to resist cracking.
[0060] S50, performing laser layered scanning according to the laser melting forming parameters and the three-dimensional model to achieve laser melting forming and laser remelting, and the laser melting and laser remelting processes are repeated to obtain a nickel-based high-temperature alloy component.
[0061] Among them, see Figure 2 The laser layered scanning is performed according to the laser melting forming parameters and the three-dimensional model to realize laser melting forming and laser remelting, and the laser melting and laser remelting processes are repeated to obtain the nickel-based high-temperature alloy component. The step further includes:
[0062] S51, moving the scraper to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a first layer of nickel-based high-temperature alloy powder;
[0063] S52, turning on the laser so that the laser performs a first layer scanning along a direction parallel to the bottom edge of the first model, completing the laser forming of the first layer of the first model, thereby completing the laser forming of the first layer of the three-dimensional model;
[0064] S53, performing a second scan again according to a scanning path with an angle of 0°-67° with the scanning direction of the first layer of the first model, to complete laser forming of the first layer of the second model;
[0065] S54, lowering the forming chamber and raising the powder chamber, moving the scraper to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a second layer of alloy powder;
[0066] S55, turning on the laser so that the laser scans the second layer along a direction that forms an angle of 60°-70° with the scanning direction of the first layer of the first model, thereby completing laser forming of the second layer of the first model;
[0067] S56, performing a second scan again according to a scanning path with an angle of 0°-67° with respect to the scanning direction of the second layer of the first model, completing laser forming of the second layer of the second model, thereby completing laser forming of the second layer of the three-dimensional model;
[0068] S57, the forming process of the second layer of the three-dimensional model is cyclically repeated until the forming of all the scanned layers is completed, thereby obtaining a nickel-based high-temperature alloy component.
[0069] The embodiment of the present application also provides a nickel-based high-temperature alloy component, which is prepared using the above preparation method.
[0070] In some embodiments, the nickel-based high-temperature alloy components prepared by the above preparation method are used in gas turbine combustion chambers, flanges, turbine disks and petrochemical equipment.
[0071] The preparation method, nickel-based high-temperature alloy component and application of the above-mentioned nickel-based high-temperature alloy component, by setting reasonable laser melting forming parameters and specifically limiting the single laser remelting method and remelting strategy, greatly reduce the total length of crack-sensitive grain boundaries, significantly inhibit the cracking of nickel-based high-temperature alloy components, and avoid the formation of microcracks on the nickel-based high-temperature alloy components. In addition, since the effective inhibition of cracking improves the uniform deformation capacity and bearing capacity of the nickel-based high-temperature alloy components, the room temperature tensile strength and elongation of the nickel-based high-temperature alloy components are significantly improved. In addition, the present application introduces a single remelting method based on the nickel-based high-temperature alloy powder and selective laser melting method, which reduces the heat input effect on the nickel-based high-temperature alloy components, and the three-dimensional model parameter assignment is simple, with strong practicality and suitable for industrial production.
[0072] The technical solution of the present application is not limited to the specific implementation modes given below, but also includes any combination of the specific implementation modes.
[0073] Example 1
[0074] This embodiment provides a method for preparing a nickel-based high-temperature alloy component, comprising the following steps:
[0075] Step 1: Powder and substrate pretreatment.
[0076] The nickel-based high-temperature alloy powder is dried in an inert gas environment in advance for use; the stainless steel substrate is polished and wiped with alcohol to remove the surface oxide layer and oil stains, and is dried for use; wherein the particle size of the nickel-based high-temperature alloy powder is 20μm-55μm.
[0077] The nickel-based high-temperature alloy powder has the following composition by mass fraction: 22.2% Cr, 13% W, 2.5% Mo, 1.9% Fe, 2.3% Co, 0.12% C, 0.4% Si, 0.5% Mn, 0.2% Al, 0.002% B, 0.03% La, and the remainder is Ni element and unavoidable impurities.
[0078] Step S2: Building a three-dimensional model.
[0079] A three-dimensional model of a nickel-based high-temperature alloy component to be formed is constructed in the VoxelDance Additive software, wherein the three-dimensional model is formed by overlapping two identical first models and a second model. The constructed three-dimensional model is sliced along the Z-axis direction to generate multiple two-dimensional layers. After the slicing is completed, the forming order of forming the first model first and then the second model is set so that the second model remelts the first model. The slice thickness of the first model and the second model is 0.04 mm.
[0080] Step S3: adjusting the substrate and powder before forming.
[0081] The dried nickel-based high-temperature alloy powder is placed in a liftable powder cabin; the cleaned stainless steel substrate is placed in a forming cabin; the stainless steel substrate and the scraper are leveled so that the surface of the stainless steel substrate is flush with the surface of the scraper to ensure that the powder is evenly spread on the stainless steel substrate; the door of the forming cabin is closed, inert gas is introduced into the forming cabin so that the oxygen content is less than 100 ppm, and the substrate is heated to 150°C at a heating rate of 5°C / min to complete the preheating of the substrate.
[0082] Step S4: Setting forming parameters.
[0083] The parameters of laser melting forming include laser power, scanning speed, scanning spacing and powder layer thickness; the laser power of the first model is 230W, the scanning speed is 900mm / s, the scanning spacing is 0.1mm, and the powder layer thickness is 0.04mm; the laser power of the second model is 230W, the scanning speed is 900mm / s, the scanning spacing is 0.1mm, and the powder layer thickness is 0.04mm; the single-layer laser scanning mode is strip bidirectional scanning, and the laser scanning path between adjacent layers rotates 67° clockwise, where the angle between the second model scanning path and the first model scanning path in the same layer is 0°, and the scanning strategy is as follows: Figure 3 shown.
[0084] The powder layer thickness of the first model and the second model are set to be consistent; the linear energy density during the forming of the second model is 100% of that of the first model, so that the melting layer depth of the second model is 56%-83% of the melting layer depth of the first model.
[0085] Step S5: Laser scanning and melting.
[0086] Laser layered scanning is performed according to the set scanning parameters and model to achieve laser melting forming and laser remelting. The laser melting and laser remelting processes are repeated to obtain nickel-based high-temperature alloy components.
[0087] The specific process of laser scanning melting forming is:
[0088] The scraper is moved to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain the first layer of nickel-based high-temperature alloy powder;
[0089] Turning on the laser to scan the first layer in a direction parallel to the bottom edge of the first model, thereby completing the laser forming of the first layer of the first model;
[0090] Perform a second scan again according to a scanning path with an angle of 0° with the scanning direction of the first layer of the first model to complete the laser forming of the first layer of the second model, thereby completing the laser forming of the first layer of the three-dimensional model;
[0091] The forming chamber is lowered and the powder chamber is raised, and the scraper is moved to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a second layer of nickel-based high-temperature alloy powder;
[0092] Turn on the laser, so that the laser scans the second layer along a direction that forms a 67° angle with the scanning direction of the first layer of the first model, thereby completing the laser forming of the second layer of the first model;
[0093] Perform a second scan again according to a scanning path with an angle of 0° with the scanning direction of the second layer of the first model to complete the laser forming of the second layer of the second model, thereby completing the laser forming of the second layer of the three-dimensional model;
[0094] The forming process of the second layer of the three-dimensional model is repeated cyclically until the forming of all scanned layers is completed, thereby obtaining a nickel-based high-temperature alloy component.
[0095] Among them, the optical micrograph of crack distribution of the formed specimen is as follows: Figure 4 As shown, the crack density is 0.053mm / mm 2 , achieving nearly crack-free selective laser melting preparation of nickel-based high-temperature alloy components.
[0096] Among them, the micrograph of the molten pool morphology of the formed sample is as follows: Figure 5 As shown, the distance between the molten pool contour of the first model and the remelted molten pool contour of the second model of the same powder layer is 16μm-40μm.
[0097] Among them, the grain morphology of the formed sample is as follows Figure 6 As shown, the grains are distributed in a network pattern. The average grain size is 42.47 μm, and the total length of the grain boundary in the field of view is 45.7 mm.
[0098] The cracking grain boundary angle distribution is as follows: Figure 7 As shown, the cracking ratio of grain boundaries in the range of 30°-40° is the largest. The ratio of 30°-40° grain boundaries in the formed specimen is 23.4%, and the total length is calculated to be 10.7 mm.
[0099] Among them, the tensile strength of the prepared nickel-based high-temperature alloy sample is 965MPa and the elongation is 24.3%. Figure 8 shown.
[0100] Example 2
[0101] This embodiment provides a method for preparing a nickel-based high-temperature alloy component, comprising the following steps:
[0102] Step 1: Powder and substrate pretreatment.
[0103] The nickel-based high-temperature alloy powder is dried in an inert gas environment in advance for use; the stainless steel substrate is polished and wiped with alcohol to remove the surface oxide layer and oil stains, and is dried for use; wherein the particle size of the nickel-based high-temperature alloy powder is 20μm-55μm.
[0104] The nickel-based high-temperature alloy powder has the following composition by mass fraction: 22.2% Cr, 13% W, 2.5% Mo, 1.9% Fe, 2.3% Co, 0.12% C, 0.4% Si, 0.5% Mn, 0.2% Al, 0.002% B, 0.03% La, and the remainder is Ni element and unavoidable impurities.
[0105] Step S2: Building a three-dimensional model.
[0106] A three-dimensional model of a nickel-based high-temperature alloy component to be formed is constructed in the VoxelDance Additive software, wherein the three-dimensional model is formed by overlapping two identical first models and a second model. The constructed three-dimensional model is sliced along the Z-axis direction to generate multiple two-dimensional layers. After the slicing is completed, the forming order of forming the first model first and then the second model is set so that the second model remelts the first model. The slice thickness of the first model and the second model is 0.04 mm.
[0107] Step S3: adjusting the substrate and powder before forming.
[0108] The dried nickel-based high-temperature alloy powder is placed in a liftable powder cabin; the cleaned stainless steel substrate is placed in a forming cabin; the stainless steel substrate and the scraper are leveled so that the surface of the stainless steel substrate is flush with the surface of the scraper to ensure that the powder is evenly spread on the stainless steel substrate; the door of the forming cabin is closed, inert gas is introduced into the forming cabin so that the oxygen content is less than 100 ppm, and the substrate is heated to 150°C at a heating rate of 5°C / min to complete the preheating of the substrate.
[0109] Step S4: Setting forming parameters.
[0110] The parameters of laser melting forming include laser power, scanning speed, scanning spacing and powder layer thickness; the laser power of the first model is 230W, the scanning speed is 900mm / s, the scanning spacing is 0.1mm, and the powder layer thickness is 0.04mm; the laser power of the second model is 230W, the scanning speed is 900mm / s, the scanning spacing is 0.1mm, and the powder layer thickness is 0.04mm; the single-layer laser scanning mode is strip bidirectional scanning, and the laser scanning path between adjacent layers rotates 67° clockwise, where the angle between the second model scanning path and the first model scanning path in the same layer is 67°, and the scanning strategy is as follows: Figure 3 shown.
[0111] The powder layer thickness of the first model and the second model is set to be consistent; the linear energy density during the forming of the second model is 100% of that of the first model, so that the melting layer depth of the second model is 54%-81% of the melting layer depth of the first model.
[0112] Step S5: Laser scanning and melting.
[0113] Laser layered scanning is performed according to the set scanning parameters and model to achieve laser melting forming and laser remelting. The laser melting and laser remelting processes are repeated to obtain nickel-based high-temperature alloy components.
[0114] The specific process of laser scanning melting forming is:
[0115] The scraper is moved to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain the first layer of nickel-based high-temperature alloy powder;
[0116] Turning on the laser to scan the first layer in a direction parallel to the bottom edge of the first model, thereby completing the laser forming of the first layer of the first model;
[0117] Perform a second scan again along a scanning path with an angle of 67° with the scanning direction of the first layer of the first model to complete the laser forming of the first layer of the second model, thereby completing the laser forming of the first layer of the three-dimensional model;
[0118] The forming chamber is lowered and the powder chamber is raised, and the scraper is moved to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a second layer of nickel-based high-temperature alloy powder;
[0119] Turn on the laser, so that the laser scans the second layer along a direction that forms a 67° angle with the scanning direction of the first layer of the first model, thereby completing the laser forming of the second layer of the first model;
[0120] Perform a second scan again along a scanning path with an angle of 67° with the scanning direction of the second layer of the first model to complete the laser forming of the second layer of the second model, thereby completing the laser forming of the second layer of the three-dimensional model;
[0121] The forming process of the second layer of the three-dimensional model is repeated cyclically until the forming of all scanned layers is completed, thereby obtaining a nickel-based high-temperature alloy component.
[0122] Among them, the optical micrograph of crack distribution of the formed specimen is as follows: Figure 4 As shown, the crack density is 0.048mm / mm 2 , achieving nearly crack-free selective laser melting preparation of nickel-based high-temperature alloy components.
[0123] Among them, the micrograph of the molten pool morphology of the formed sample is as follows: Figure 5 As shown, the distance between the molten pool contour of the first model and the remelted molten pool contour of the second model of the same powder layer is 18μm-42μm.
[0124] Among them, the grain morphology of the formed sample is as follows Figure 6 As shown, the grains are distributed in a network pattern. The average grain size is 47.69 μm, and the total length of the grain boundaries in the field of view is 41.6 mm.
[0125] The cracking grain boundary angle distribution is as follows: Figure 7As shown, the cracking ratio of grain boundaries in the range of 30°-40° is the largest. The ratio of 30°-40° grain boundaries in the formed specimen is 26.9%, and the total length is calculated to be 11.2 mm.
[0126] Among them, the tensile strength of the prepared nickel-based high-temperature alloy sample is 992MPa and the elongation is 21.4%. Figure 8 shown.
[0127] Comparative Example 1
[0128] This comparative example provides a method for preparing a nickel-based high-temperature alloy component, comprising the following steps:
[0129] Step 1: Powder and substrate pretreatment.
[0130] The nickel-based high-temperature alloy powder is dried in an inert gas environment in advance for use; the stainless steel substrate is polished and wiped with alcohol to remove the surface oxide layer and oil stains, and is dried for use; wherein the particle size of the nickel-based high-temperature alloy powder is 20μm-55μm.
[0131] The nickel-based high-temperature alloy powder has the following composition by mass fraction: 22.2% Cr, 13% W, 2.5% Mo, 1.9% Fe, 2.3% Co, 0.12% C, 0.4% Si, 0.5% Mn, 0.2% Al, 0.002% B, 0.03% La, and the remainder is Ni element and unavoidable impurities.
[0132] Step S2: Building a three-dimensional model.
[0133] A three-dimensional model of the nickel-based high-temperature alloy component to be formed is constructed in the VoxelDance Additive software, wherein the three-dimensional model consists of a model. The constructed three-dimensional model is sliced along the Z-axis direction to generate multiple two-dimensional layers, and the slice thickness is 0.04 mm.
[0134] Step S3: adjusting the substrate and powder before forming.
[0135] The dried nickel-based high-temperature alloy powder is placed in a liftable powder cabin; the cleaned stainless steel substrate is placed in a forming cabin; the stainless steel substrate and the scraper are leveled so that the surface of the stainless steel substrate is flush with the surface of the scraper to ensure that the powder is evenly spread on the stainless steel substrate; the door of the forming cabin is closed, inert gas is introduced into the forming cabin so that the oxygen content is less than 100 ppm, and the substrate is heated to 150°C at a heating rate of 5°C / min to complete the preheating of the substrate.
[0136] Step S4: Setting forming parameters.
[0137] The parameters of laser melting include laser power, scanning speed, scanning spacing and powder layer thickness; the laser power of the 3D model is 230W, the scanning speed is 900mm / s, the scanning spacing is 0.1mm, and the powder layer thickness is 0.04mm; the single-layer laser scanning method is strip bidirectional scanning, and the laser scanning path between adjacent layers rotates 67° clockwise. The scanning strategy is as follows Figure 3 shown.
[0138] Step S5: Laser scanning and melting.
[0139] Laser layered scanning is performed according to the set scanning parameters and model to achieve laser melting forming, thereby obtaining a nickel-based high-temperature alloy component.
[0140] The specific process of laser scanning melting forming is:
[0141] The scraper is moved to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain the first layer of nickel-based high-temperature alloy powder;
[0142] Turn on the laser, so that the laser performs the first layer scanning in a direction parallel to the bottom edge of the three-dimensional model, and completes the laser forming of the first layer of the three-dimensional model;
[0143] The forming chamber is lowered and the powder chamber is raised, and the scraper is moved to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a second layer of nickel-based high-temperature alloy powder;
[0144] Turn on the laser, so that the laser scans the second layer along a direction that forms a 67° angle with the scanning direction of the first layer of the first model, thereby completing the laser forming of the second layer of the three-dimensional model;
[0145] The forming process of the second layer of the three-dimensional model is repeated cyclically until the forming of all scanned layers is completed, thereby obtaining a nickel-based high-temperature alloy component.
[0146] Among them, the optical micrograph of crack distribution of the formed specimen is as follows: Figure 4 As shown, the crack density is 0.283mm / mm 2 .
[0147] Among them, the micrograph of the molten pool morphology of the formed sample is as follows: Figure 5 As shown, the maximum depth of the molten pool is 92 μm.
[0148] Among them, the grain morphology of the formed sample is as follows Figure 6 As shown, the grains are distributed in a network pattern. The average grain size obtained by the scribing method is 38.18 μm, and the total length of the grain boundary in the field of view is 58.1 mm.
[0149] The cracking grain boundary angle distribution is as follows: Figure 7As shown, the cracking ratio of grain boundaries in the range of 30-40° is the largest. The ratio of 30°-40° grain boundaries in the formed specimen is 28.2%, and the total length is calculated to be 16.4 mm.
[0150] Among them, the tensile strength of the prepared nickel-based high-temperature alloy sample is 836±18MPa, and the elongation is 17.3±2.6%. Figure 8 shown.
[0151] Comparative Example 2
[0152] This comparative example provides a method for preparing a nickel-based high-temperature alloy component, comprising the following steps:
[0153] Step 1: Powder and substrate pretreatment.
[0154] The nickel-based high-temperature alloy powder is dried in an inert gas environment in advance for use; the stainless steel substrate is polished and wiped with alcohol to remove the surface oxide layer and oil stains, and is dried for use; wherein the particle size of the nickel-based high-temperature alloy powder is 20μm-55μm.
[0155] The nickel-based high-temperature alloy powder has the following composition by mass fraction: 22.2% Cr, 13% W, 2.5% Mo, 1.9% Fe, 2.3% Co, 0.12% C, 0.4% Si, 0.5% Mn, 0.2% Al, 0.002% B, 0.03% La, and the remainder is Ni element and unavoidable impurities.
[0156] Step S2: Building a three-dimensional model.
[0157] A three-dimensional model of a nickel-based high-temperature alloy component to be formed is constructed in the VoxelDance Additive software, wherein the three-dimensional model is formed by overlapping two identical first models and a second model. The constructed three-dimensional model is sliced along the Z-axis direction to generate multiple two-dimensional layers. After the slicing is completed, the forming order of forming the first model first and then the second model is set so that the second model remelts the first model. The slice thickness of the first model and the second model is 0.04 mm.
[0158] Step S3: adjusting the substrate and powder before forming.
[0159] The dried nickel-based high-temperature alloy powder is placed in a liftable powder cabin; the cleaned stainless steel substrate is placed in a forming cabin; the stainless steel substrate and the scraper are leveled so that the surface of the stainless steel substrate is flush with the surface of the scraper to ensure that the powder is evenly spread on the stainless steel substrate; the door of the forming cabin is closed, inert gas is introduced into the forming cabin so that the oxygen content is less than 100 ppm, and the substrate is heated to 150°C at a heating rate of 5°C / min to complete the preheating of the substrate.
[0160] Step S4: Setting forming parameters.
[0161] The parameters of laser melting forming include laser power, scanning speed, scanning spacing and powder layer thickness; the laser power of the first model is 230W, the scanning speed is 900mm / s, the scanning spacing is 0.1mm, and the powder layer thickness is 0.04mm; the laser power of the second model is 200W, the scanning speed is 900mm / s, the scanning spacing is 0.1mm, and the powder layer thickness is 0.04mm; the single-layer laser scanning mode is strip bidirectional scanning, and the laser scanning path between adjacent layers rotates 67° clockwise, where the angle between the second model scanning path and the first model scanning path in the same layer is 67°, and the scanning strategy is as follows Figure 3 shown.
[0162] The powder layer thickness of the first model and the second model is set to be consistent; the linear energy density during the forming of the second model is 100% of that of the first model, so that the melting layer depth of the second model is 27%-67% of the melting layer depth of the first model.
[0163] Step S5: Laser scanning and melting.
[0164] Laser layered scanning is performed according to the set scanning parameters and model to achieve laser melting forming and laser remelting. The laser melting and laser remelting processes are repeated to obtain nickel-based high-temperature alloy components.
[0165] The specific process of laser scanning melting forming is:
[0166] The scraper is moved to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain the first layer of nickel-based high-temperature alloy powder;
[0167] Turning on the laser to scan the first layer in a direction parallel to the bottom edge of the first model, thereby completing the laser forming of the first layer of the first model;
[0168] Perform a second scan again along a scanning path with an angle of 67° with the scanning direction of the first layer of the first model to complete the laser forming of the first layer of the second model, thereby completing the laser forming of the first layer of the three-dimensional model;
[0169] The forming chamber is lowered and the powder chamber is raised, and the scraper is moved to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a second layer of nickel-based high-temperature alloy powder;
[0170] Turn on the laser, so that the laser scans the second layer along a direction that forms a 67° angle with the scanning direction of the first layer of the first model, thereby completing the laser forming of the second layer of the first model;
[0171] Perform a second scan again along a scanning path with an angle of 67° with the scanning direction of the second layer of the first model to complete the laser forming of the second layer of the second model, thereby completing the laser forming of the second layer of the three-dimensional model;
[0172] The forming process of the second layer of the three-dimensional model is repeated cyclically until the forming of all scanned layers is completed, thereby obtaining a nickel-based high-temperature alloy component.
[0173] Among them, the optical micrograph of crack distribution of the formed specimen is as follows: Figure 4 As shown, the crack density is 0.243mm / mm 2 , achieving nearly crack-free selective laser melting preparation of nickel-based high-temperature alloy components.
[0174] Among them, the micrograph of the molten pool morphology of the formed sample is as follows: Figure 5 As shown, the distance between the molten pool contour of the first model and the remelted molten pool contour of the second model in the same powder layer is 30μm-67μm. Partial remelting can be completely covered by the lower laser scanning molten pool, and the effect of remelting increasing the molten pool fine grain is eliminated.
[0175] Among them, the tensile strength of the prepared nickel-based high-temperature alloy sample is 963MPa and the elongation is 17.6%. Figure 8 shown.
[0176] In summary, comparative example 1 is a sample that has not been remelted. Compared with comparative example 1, the remelting depth of embodiment 1 is 56%-83% of the maximum depth of the molten pool, the crack density is reduced by 81.3%, the grains of the alloy sample are coarsened by 11.2%, the total length of the 30-40° crack-sensitive grain boundary is reduced by 34.7%, the strength is increased by 15.2%, and the elongation is increased by 40.5%;
[0177] Example 2 The remelting depth is 54%-81% of the maximum depth of the molten pool, the crack density is reduced by 83.0%, the grains of the alloy sample are coarsened by 24.9%, the total length of the 30°-40° crack-sensitive grain boundary is reduced by 31.7%, the strength is increased by 18.7%, and the elongation is increased by 23.7%;
[0178] The remelting depth of Comparative Example 2 is 27%-67% of the maximum depth of the molten pool, the crack density is reduced by 14.1%, the strength is increased by 3.2%, and the elongation is increased by 1.7%. Within the test error range of Comparative Example 1, there is almost no improvement in performance.
[0179] The present application controls the elimination of large dendrite areas by designing a laser remelting process to control the remelting depth, thereby reducing the length of crack-sensitive grain boundaries, thereby significantly reducing the crack density in the formed nickel-based high-temperature alloy components, solving the serious cracking problem of nickel-based high-temperature alloy components formed by selective laser melting, and providing a new technical approach for the widespread application of high-performance nickel-based high-temperature alloy components formed by selective laser melting in gas turbine combustion chambers, flanges, turbine disks and petrochemical equipment.
[0180] It is obvious to those skilled in the art that the present application is not limited to the details of the exemplary embodiments described above, and that the present application can be implemented in other specific forms without departing from the spirit or essential features of the present application. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present application is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present application.
[0181] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the preferred embodiments, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.
Claims
1. A method for preparing a nickel-based high-temperature alloy component, characterized in that: The steps include: Pretreatment of nickel-based high-temperature alloy powders and stainless steel substrates; Establishing a three-dimensional model of a nickel-based high-temperature alloy component, wherein the three-dimensional model is formed by overlapping two identical first models and a second model, slicing the established three-dimensional model along the Z-axis direction to generate a plurality of two-dimensional layers, and after the slicing is completed, setting a forming order of first forming the first model and then forming the second model, so that the second model remelts the first model, wherein the slice thicknesses of the first model and the second model are the same; Placing the pretreated nickel-based high-temperature alloy powder in a liftable powder cabin, and placing the pretreated stainless steel substrate in a forming cabin, leveling the stainless steel substrate and the scraper so that the surface of the stainless steel substrate is flush with the surface of the scraper, closing the cabin door of the forming cabin, introducing inert gas into the forming cabin so that the oxygen content in the forming cabin is reduced to a first value, and heating the stainless steel substrate to a second value to complete preheating of the stainless steel substrate; Setting laser melting forming parameters, wherein the laser melting forming parameters include that the linear energy density during forming of the second model is 80%-100% of that of the first model, so that the melting layer depth of the second model is 50%-85% of that of the first model; Laser layered scanning is performed according to the laser melting forming parameters and the three-dimensional model to achieve laser melting forming and laser remelting. The laser melting and laser remelting processes are repeated to obtain a nickel-based high-temperature alloy component.
2. The preparation method according to claim 1, characterized in that The nickel-based high-temperature alloy powder has the following composition by mass fraction: Cr content of 20%-24%, W content of 12.5%-14.5%, Mo content of 1%-3%, Fe content of less than 3%, Co content of less than 1%-5%, C content of 0.1%-0.3%, Si content of 0.2%-0.5%, Mn content of 0.3%-1.0%, Al content of 0.2%-0.5%, B content of 0.001%-0.01%, La content of 0.01%-0.05%, and the balance is Ni element and unavoidable impurities.
3. The preparation method according to claim 1, characterized in that: The step of pretreating the nickel-based high-temperature alloy powder and the stainless steel substrate further comprises: The nickel-based high-temperature alloy powder is dried in an inert gas environment for later use, and the stainless steel substrate is polished and wiped with alcohol to remove the surface oxide layer and oil stains, and then dried for later use.
4. The preparation method according to claim 1, characterized in that: The particle size distribution range of the nickel-based high-temperature alloy powder is 20 μm-55 μm.
5. The preparation method according to claim 1, characterized in that: The first value has a value range of less than 100 ppm, and the second value has a value range of 140°C-160°C.
6. The preparation method according to claim 1, characterized in that: The laser melting forming parameters also include laser power, scanning speed, scanning spacing and powder layer thickness. The laser power of the first model ranges from 210W to 250W, the scanning speed ranges from 700mm / s to 1100mm / s, the scanning spacing ranges from 0.08mm to 0.12mm, and the powder layer thickness ranges from 0.03mm to 0.05mm. The laser power of the second model ranges from 200W to 250W, the scanning speed ranges from 700mm / s to 1100mm / s, the scanning spacing ranges from 0.08mm to 0.12mm, and the powder layer thickness ranges from 0.03mm to 0.05mm. The single-layer laser scanning mode is strip bidirectional scanning, and the laser scanning path between adjacent layers rotates 60° to 70° clockwise.
7. The preparation method according to claim 1, characterized in that: The included angle between the scanning path of the second model and the scanning path of the first model in the same layer is 0°-67°.
8. The preparation method according to claim 7, characterized in that: The step of performing laser layered scanning according to the laser melting forming parameters and the three-dimensional model to achieve laser melting forming and laser remelting, and the laser melting and laser remelting processes are repeated to obtain a nickel-based high-temperature alloy component further includes: Moving the scraper to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a first layer of nickel-based high-temperature alloy powder; Turning on the laser so that the laser performs a first layer scanning along a direction parallel to the bottom edge of the first model to complete the laser forming of the first layer of the first model, thereby completing the laser forming of the first layer of the three-dimensional model; Scanning a second time again along a scanning path with an angle of 0°-67° with the scanning direction of the first layer of the first model to complete laser forming of the first layer of the second model; Lowering the forming chamber and lifting the powder chamber, moving the scraper to evenly spread the nickel-based high-temperature alloy powder in the powder chamber on the stainless steel substrate to obtain a second layer of alloy powder; Turning on the laser so that the laser scans the second layer along a direction forming an angle of 60°-70° with the scanning direction of the first layer of the first model, thereby completing laser forming of the second layer of the first model; Performing a second scan again along a scanning path with an angle of 0°-67° with respect to the scanning direction of the second layer of the first model to complete the laser forming of the second layer of the second model, thereby completing the laser forming of the second layer of the three-dimensional model; The forming process of the second layer of the three-dimensional model is repeated cyclically until the forming of all scanned layers is completed, thereby obtaining a nickel-based high-temperature alloy component.
9. A nickel-based high-temperature alloy component, characterized in that: The method is prepared according to any one of claims 1 to 8.
10. Application of the nickel-based high-temperature alloy component obtained by the preparation method according to any one of claims 1 to 8 in a gas turbine combustion chamber, flange, turbine disk and petrochemical equipment.
Citation Information
Patent Citations
Method for improving mechanical property of 3D printing nickel-based superalloy through in-situ heat treatment
CN112008079A
Method for optimizing nickel-titanium alloy performance based on selective laser melting method
CN115703153A
Uniform forming additive manufacturing method based on SLM
CN117862529A
Cited By
Laser powder bed fusion preparation method suitable for local structure regulation and control of complex parts and application of laser powder bed fusion preparation method
CN119588956A