Film stripping liquid capable of improving film stripping efficiency and preparation method thereof
By using composite alkali, penetrants and corrosion inhibitors in the stripping liquid, the problem of limited diffusion rate of the traditional stripping liquid is solved, the metal surface film layer is effectively removed, residues are reduced, and production efficiency and product quality are improved. .
Patent Information
- Application Number
- CN202410898382.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-05
AI Technical Summary
The diffusion rate of traditional peeling liquid is limited during the peeling process, resulting in low peeling efficiency, long time and possible residues, which affects product quality.
The stripping liquid is composed of compound alkali, penetrant, organic solvent and corrosion inhibitor. Through specific mass ratio and preparation method, the permeability and activity of the stripping liquid are improved, and the film removal ability and protection of the metal surface are enhanced.
It significantly improves the peeling efficiency, shortens the peeling time, reduces residues, and improves product quality and production efficiency.
Smart Images

Figure BDA0004929743330000121 
Figure BDA0004929743330000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of film stripping technology, and in particular to a film stripping liquid capable of improving film stripping efficiency and a preparation method thereof. Background Art
[0002] In the electronics manufacturing and metal surface treatment industries, the film stripping process is a key step for removing coatings or films from metal or circuit board surfaces. Traditional film stripping fluids often face diffusion rate limitations, which directly affects the efficiency and effectiveness of the film stripping process.
[0003] The main components of the stripper, such as surfactants, solvents and other active components, need to diffuse into the interior of the dry film to achieve effective stripping. The rate of this step is a key factor in the stripping speed. However, the poor hydrophilicity of the dry film will limit the penetration speed of the stripper, thereby slowing down the entire stripping process.
[0004] Many dry film materials are designed with low hydrophilicity to provide specific protective properties, but this also limits the diffusion of water and active ingredients in the stripper. Due to the limited diffusion rate, the stripping process may take a long time, which reduces production efficiency and increases costs. During the stripping process, if the stripper cannot fully penetrate the dry film, it may result in incomplete film peeling, leaving residues and affecting the quality of the final product.
[0005] China's invention patent CN108008606B discloses a film stripping solution for photosensitive dry film and its production method and application. The film stripping solution includes inorganic base, organic base, solvent, additive and water; wherein the alkali equivalent is 0.4-1.25mol / L, and the content of inorganic base is 0.5-2g / L, and the volume of organic base added accounts for 2-5% of the film stripping solution. The invention uses organic base as the main film stripping component to react with the dry film polymer, and at the same time, a certain amount of inorganic base components are added to supplement the concentration of OH- during the film stripping process; the use of high-boiling alcohol ether solvents can better penetrate and swell the dry film. The additive aromatic azole chelate is a film-forming substance with a specific affinity to metals, thereby ensuring that the surface of the conductive film layer will not be oxidized and corroded during the film stripping process. Its configuration is simple and safe, and it has a strong ability to strip dry film under normal spraying and stamping conditions, and has high production efficiency and yield. However, the film stripping time of the film stripping solution of the invention is still long, and there is still a certain amount of residue. Summary of the invention
[0006] In view of the limitations of the prior art, the present invention provides a novel stripping solution and a preparation method thereof, aiming to improve the stripping efficiency, reduce the stripping time and residues, and improve the quality of the final product.
[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0008] The invention discloses a film stripping liquid capable of improving film stripping efficiency, which is composed of the following components: a composite alkali, a penetrant, an organic solvent, a corrosion inhibitor and water.
[0009] The stripping solution capable of improving stripping efficiency is composed of the following components in parts by weight: 25 to 35 parts of composite alkali, 10 to 20 parts of penetrant, 5 to 10 parts of organic solvent, 1 to 4 parts of corrosion inhibitor, and 40 to 50 parts of water.
[0010] The composite alkali is composed of an inorganic alkali and an organic alkali in a mass ratio of 10-15:1-3, the inorganic alkali is composed of sodium hydroxide, potassium hydroxide and sodium carbonate in a mass ratio of 8-10:2-4:1; the organic alkali is composed of ethanolamine and propylenediamine in a mass ratio of 0.7-0.9:1-1.5.
[0011] The organic solvent is one or more of ethylene glycol dimethyl ether, cyclohexanone and ethyl acetate.
[0012] The corrosion inhibitor is composed of octadecyl phosphate, oleic acid, sodium molybdate, sodium nitrate, benzotriazole and zinc sulfate in a mass ratio of 9-11:9-11:2-4:40-60:6-8:18-22.
[0013] The preparation method of the penetrant is as follows, in parts by weight:
[0014] S1, add 400-600 parts of water to the reaction kettle and preheat it to 40-60°C, gradually add 10-15 parts of 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy, 13-16 parts of estriol trisulfate trisodium salt and 20-30 parts of sulfated castor oil to the water, stir each raw material until it is completely dissolved after adding, maintain 40-60°C and continue stirring for 20-40 minutes to obtain a uniform solution;
[0015] S2. While stirring, add 4 to 6 parts of emulsifier and 7 to 9 parts of bis(1-methyl-2-hydroxyethyl) ether, and continue stirring for 5 to 15 minutes; add 1 to 3 parts of composite defoamer; continue stirring until the defoamer is completely dispersed, and filter with a microporous filter to remove possible solid particles or insoluble matter to obtain a penetrant.
[0016] The emulsifier is sucrose fatty acid ester.
[0017] The composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester and isopropanol in a mass ratio of 0.8-1.2:1-3:0.8-1.2.
[0018] The pore size of the microporous filter is 0.4-0.5 μm.
[0019] A method for preparing a stripping solution that can improve stripping efficiency is as follows:
[0020] Step 1, weighing each raw material according to weight, mixing the composite base, penetrant, organic solvent and water, adding them into a stirring kettle, heating and stirring, the heating temperature is controlled at 50-60° C., the stirring rate is controlled at 100-200 rpm, the stirring time is 20-40 minutes, and then cooling to room temperature to obtain a mixed solution;
[0021] Step 2: Add water and corrosion inhibitor to the mixed solution prepared in step 1, and then stir at room temperature at a stirring rate of 400 to 600 rpm for 100 to 150 minutes to obtain a stripping solution.
[0022] The effects of various substances mentioned in the present invention are as follows:
[0023] The composite alkali is composed of inorganic alkali and organic alkali. It is the main active ingredient in the stripping solution and is responsible for removing the film layer on the metal surface.
[0024] Inorganic alkalis are composed of sodium hydroxide, potassium hydroxide, and sodium carbonate. These substances are strongly alkaline and can react chemically with the film layer on the metal surface to promote the dissolution and peeling of the film layer.
[0025] The organic base is composed of ethanolamine and propylenediamine. These organic bases usually have better permeability and help to improve the penetration of the stripping solution, so that the stripping solution can act more deeply on the metal surface.
[0026] Penetrants enhance the penetration ability of the stripping solution, allowing it to more effectively penetrate the film layer on the metal surface.
[0027] 10-Hydroxy-18-[2-[2-(sulfonyloxy)ethoxy]] is a surfactant that helps improve the wettability of the solution, thereby enhancing penetration.
[0028] Estriol trisulfate trisodium salt has the effect of increasing the wettability and permeability of the solution.
[0029] Sulfated castor oil may help reduce friction during the peeling process.
[0030] Sucrose fatty acid esters may act as emulsifiers, helping to maintain the stability of the solution.
[0031] Bis(1-methyl-2-hydroxyethyl) ether may act as a solvent or co-solvent to help dissolve the other ingredients.
[0032] As an organic solvent, ethylene glycol dimethyl ether helps to dissolve the complex base and other ingredients, and may also provide some penetration and cleaning effects.
[0033] Corrosion inhibitors protect the metal surface during the stripping process and prevent excessive corrosion.
[0034] Octadecyl phosphate is used as a component of corrosion inhibitor to reduce corrosion on metal surfaces.
[0035] Oleic acid acts as a corrosion inhibitor, helping to protect the metal from being attacked by the active ingredients in the stripping solution.
[0036] Sodium molybdate is used as a component of corrosion inhibitor to improve the corrosion resistance of metals.
[0037] Sodium nitrate, as a component of corrosion inhibitor, may be used to adjust the pH value of the solution.
[0038] Benzotriazole is a commonly used metal corrosion inhibitor.
[0039] Zinc sulfate is used as part of the corrosion inhibitor.
[0040] The composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester and isopropyl alcohol, and is used to control the foam generated in the solution during the preparation process to ensure the stability and performance of the solution.
[0041] Through the synergistic effect of these substances, the film stripping solution of the present invention can effectively remove the film layer on the metal surface while protecting the metal from corrosion, thereby improving the film stripping efficiency and the quality of metal surface treatment.
[0042] Compared with the prior art, it has the following beneficial effects:
[0043] 1) The film stripping solution of the present invention can strip the film layer on the metal surface more quickly through the synergistic effect of a specific composite alkali and a penetrant, thereby improving the film stripping efficiency.
[0044] 2) The film stripping solution of the present invention leaves the surface of the substrate clean after film stripping, without any residue or fine residue, which helps to improve the quality of subsequent processes and reduce cleaning work.
[0045] 3) The specific mass ratio of the composite alkali and the corrosion inhibitor in the stripping solution of the present invention and the special formula of the penetrant improve the activity and selectivity of the stripping solution and reduce the corrosion to the substrate.
[0046] 4) Due to the high efficiency of the film stripping liquid, the film stripping time can be shortened, thereby improving the overall production efficiency. DETAILED DESCRIPTION
[0047] Main sources of substances:
[0048] 10-Hydroxy-18-[2-[2-(sulfonyloxy)ethoxy]: CAS: 85153-73-7.
[0049] Sodium laureth sulfate: CAS: 3088-31-1.
[0050] Estriol trisulfate trisodium salt: CAS: 100940-55-4.
[0051] Sulfated castor oil: CAS: 8002-33-3.
[0052] Bis(1-methyl-2-hydroxyethyl) ether: CAS: 108-61-2.
[0053] Sucrose fatty acid esters: CAS number: 37318-31-3.
[0054] Sorbitan fatty acid ester: Jinan Flanders Chemical Co., Ltd., model: S-80.
[0055] Polyethylene glycol: Guangzhou Nacheng Chemical Co., Ltd., model: 400#.
[0056] Commercially available penetrant: Jiangsu Hai'an Petrochemical Plant, product number: JFC-E.
[0057] The invention discloses a method for preparing a film stripping liquid, which aims to improve the film stripping efficiency. The film stripping liquid is usually used in industrial production, especially in the process of metal surface treatment, to remove the coating or film layer on the metal surface.
[0058] A film stripping liquid capable of improving film stripping efficiency is composed of the following components by weight: 25 to 35 parts of composite alkali, 10 to 20 parts of penetrant, 5 to 10 parts of organic solvent, 1 to 4 parts of corrosion inhibitor and 40 to 50 parts of water.
[0059] The composite alkali is composed of an inorganic alkali and an organic alkali in a mass ratio of 10-15:1-3, the inorganic alkali is composed of sodium hydroxide, potassium hydroxide and sodium carbonate in a mass ratio of 8-10:2-4:1; the organic alkali is composed of ethanolamine and propylenediamine in a mass ratio of 0.7-0.9:1-1.5.
[0060] The present invention firstly mixes a composite alkali (composed of an inorganic alkali and an organic alkali) with a penetrant and ethylene glycol dimethyl ether. The composition of the composite alkali is key because it determines the chemical properties and stripping ability of the film stripping solution.
[0061] Inorganic alkali: sodium hydroxide, potassium hydroxide, sodium carbonate, these strong alkalis provide the basic chemical activity of the stripping solution.
[0062] Organic bases: ethanolamine, propylenediamine, these organic bases enhance the permeability and film stripping ability of the composite base.
[0063] The organic solvent is one or more of ethylene glycol dimethyl ether, cyclohexanone and ethyl acetate.
[0064] The corrosion inhibitor is composed of octadecyl phosphate, oleic acid, sodium molybdate, sodium nitrate, benzotriazole and zinc sulfate in a mass ratio of 9-11:9-11:2-4:40-60:6-8:18-22.
[0065] Corrosion inhibitors are added to the mixed solution. These substances can slow down or prevent corrosion on the metal surface and protect the metal from excessive erosion by the active ingredients in the stripping solution.
[0066] A method for preparing a stripping solution that can improve stripping efficiency is as follows:
[0067] Step 1, weighing each raw material according to weight, mixing the composite base, penetrant, organic solvent and water, adding them into a stirring kettle, heating and stirring, the heating temperature is controlled at 50-60° C., the stirring rate is controlled at 100-200 rpm, the stirring time is 20-40 minutes, and then cooling to room temperature to obtain a mixed solution;
[0068] Step 2: Add water and corrosion inhibitor to the mixed solution prepared in step 1, and then stir at room temperature at a stirring rate of 400 to 600 rpm for 100 to 150 minutes to obtain a stripping solution.
[0069] During the heating and stirring process, the various components are fully mixed to form a uniform solution, which helps to improve the uniformity and stability of the stripping solution.
[0070] The preparation method of the penetrant is as follows, in parts by weight:
[0071] S1, add 400-600 parts of water to the reaction kettle and preheat it to 40-60°C, gradually add 10-15 parts of 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy, 13-16 parts of estriol trisulfate trisodium salt and 20-30 parts of sulfated castor oil to the water, stir each raw material until it is completely dissolved after adding, maintain 40-60°C and continue stirring for 20-40 minutes to obtain a uniform solution;
[0072] S2. While stirring, add 4 to 6 parts of emulsifier and 7 to 9 parts of bis(1-methyl-2-hydroxyethyl) ether, and continue stirring for 5 to 15 minutes; add 1 to 3 parts of composite defoamer; continue stirring until the defoamer is completely dispersed, and filter with a microporous filter to remove possible solid particles or insoluble matter to obtain a penetrant.
[0073] The emulsifier is sucrose fatty acid ester.
[0074] The composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester and isopropanol in a mass ratio of 0.8-1.2:1-3:0.8-1.2.
[0075] The pore size of the microporous filter is 0.4-0.5 μm.
[0076] The preparation of the penetrant includes multiple components, such as 10-hydroxy-18-[2-[2-(sulfonic acid oxy)ethoxy], estriol trisulfate trisodium salt, sulfated castor oil, etc. These components help to improve the permeability of the stripping solution so that it can better penetrate and remove the film layer on the metal surface.
[0077] Through the synergistic effect of compound alkali and penetrant, the stripping solution can more effectively penetrate and remove the film layer on the metal surface.
[0078] Example 1
[0079] A method for preparing a stripping solution that can improve stripping efficiency is as follows:
[0080] Step 1, 30g of composite alkali, 15g of penetrant, 8g of ethylene glycol dimethyl ether and 29g of water were mixed and added into a stirred tank, and the mixture was heated and stirred at 55°C, the stirring rate was controlled at 150 rpm, the stirring time was 30 minutes, and then cooled to room temperature to obtain a mixed solution;
[0081] Step 2: Add 15 g of water and 3 g of corrosion inhibitor to the mixed solution prepared in step 1, and then stir at room temperature at a stirring rate of 500 rpm for 120 minutes to obtain a stripping solution.
[0082] The composite base is composed of an inorganic base and an organic base in a mass ratio of 13:2, the inorganic base is composed of sodium hydroxide, potassium hydroxide, and sodium carbonate in a mass ratio of 9:3:1; the organic base is composed of ethanolamine and propylenediamine in a mass ratio of 0.8:1.2;
[0083] The corrosion inhibitor is composed of octadecyl phosphate, oleic acid, sodium molybdate, sodium nitrate, benzotriazole and zinc sulfate in a mass ratio of 10:10:3:50:7:20.
[0084] The preparation method of the penetrant is as follows:
[0085] S1, add 500g water to the reactor and preheat to 50°C, gradually add 12g 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy, 15g estriol trisulfate trisodium salt and 25g sulfated castor oil to the water, stir each raw material until it is completely dissolved, maintain 50°C and continue stirring for 30 minutes to obtain a uniform solution;
[0086] S2. While stirring, add 5 g of sucrose fatty acid ester and 8 g of bis(1-methyl-2-hydroxyethyl) ether, and continue stirring for 10 minutes; add 2 g of a composite defoamer, wherein the composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester, and isopropanol in a mass ratio of 1:2:1; continue stirring until the defoamer is completely dispersed, and filter using a microporous filter with a pore size of 0.45 μm to remove possible solid particles or insoluble matter to obtain a penetrant.
[0087] Example 2
[0088] A method for preparing a film stripping solution that can improve film stripping efficiency is basically the same as that in Example 1, except that the preparation method of the penetrant is different:
[0089] The preparation method of the penetrant is as follows:
[0090] S1, add 500g water to the reactor and preheat to 50°C, gradually add 12g sodium laureth sulfate, 15g estriol trisulfate trisodium salt and 25g sulfated castor oil to the water, stir each raw material until completely dissolved, maintain 50°C and continue stirring for 30 minutes to obtain a uniform solution;
[0091] S2. While stirring, add 5 g of sucrose fatty acid ester and 8 g of bis(1-methyl-2-hydroxyethyl) ether, and continue stirring for 10 minutes; add 2 g of a composite defoamer, wherein the composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester, and isopropanol in a mass ratio of 1:2:1; continue stirring until the defoamer is completely dispersed, and filter using a microporous filter with a pore size of 0.45 μm to remove possible solid particles or insoluble matter to obtain a penetrant.
[0092] Example 3
[0093] A method for preparing a film stripping solution that can improve film stripping efficiency is basically the same as that in Example 1, except that the preparation method of the penetrant is different:
[0094] The preparation method of the penetrant is as follows:
[0095] S1, add 500g water to the reactor and preheat to 50 ℃, gradually add 12g10-hydroxy-18-[2-[2-(sulfonic acid group oxygen base) ethoxy, 15g 2-ethyl-3-hydroxyhexyl sodium sulfate and 25g sulfated castor oil to the water, stir until each raw material is completely dissolved after adding, maintain 50 ℃ and continue stirring for 30 minutes to obtain a uniform solution;
[0096] S2. While stirring, add 5 g of sucrose fatty acid ester and 8 g of bis(1-methyl-2-hydroxyethyl) ether, and continue stirring for 10 minutes; add 2 g of a composite defoamer, wherein the composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester, and isopropanol in a mass ratio of 1:2:1; continue stirring until the defoamer is completely dispersed, and filter using a microporous filter with a pore size of 0.45 μm to remove possible solid particles or insoluble matter to obtain a penetrant.
[0097] Example 4
[0098] A method for preparing a film stripping solution that can improve film stripping efficiency is basically the same as that in Example 1, except that the preparation method of the penetrant is different:
[0099] The preparation method of the penetrant is as follows:
[0100] S1, add 500g water to the reactor and preheat to 50 ℃, gradually add 12g10-hydroxy-18-[2-[2-(sulfonic acid group oxygen base) ethoxy, 15g 2-ethylhexyl sulfate sodium salt and 25g sulfated castor oil to the water, stir until each raw material is completely dissolved after adding, maintain 50 ℃ and continue stirring for 30 minutes to obtain a uniform solution;
[0101] S2. While stirring, add 5 g of sucrose fatty acid ester and 8 g of bis(1-methyl-2-hydroxyethyl) ether, and continue stirring for 10 minutes; add 2 g of a composite defoamer, wherein the composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester, and isopropanol in a mass ratio of 1:2:1; continue stirring until the defoamer is completely dispersed, and filter using a microporous filter with a pore size of 0.45 μm to remove possible solid particles or insoluble matter to obtain a penetrant.
[0102] Example 5
[0103] A method for preparing a film stripping solution that can improve film stripping efficiency is basically the same as that in Example 1, except that the preparation method of the penetrant is different:
[0104] The preparation method of the penetrant is as follows:
[0105] S1, add 500g water to the reactor and preheat to 50°C, gradually add 12g 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy, 15g estriol trisulfate trisodium salt and 25g sulfated castor oil to the water, stir each raw material until it is completely dissolved, maintain 50°C and continue stirring for 30 minutes to obtain a uniform solution;
[0106] S2. While stirring, add 5 g of cetearyl glucoside and 8 g of bis(1-methyl-2-hydroxyethyl) ether, and continue stirring for 10 minutes; add 2 g of a composite defoamer, wherein the composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester, and isopropanol in a mass ratio of 1:2:1; continue stirring until the defoamer is completely dispersed, and filter using a microporous filter with a pore size of 0.45 μm to remove possible solid particles or insoluble matter to obtain a penetrant.
[0107] Example 6
[0108] A method for preparing a film stripping solution that can improve film stripping efficiency is basically the same as that in Example 1, except that the preparation method of the penetrant is different:
[0109] The preparation method of the penetrant is as follows:
[0110] S1, add 500g water to the reactor and preheat to 50°C, gradually add 12g 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy, 15g estriol trisulfate trisodium salt and 25g sulfated castor oil to the water, stir each raw material until it is completely dissolved, maintain 50°C and continue stirring for 30 minutes to obtain a uniform solution;
[0111] S2. While stirring, add 5 g of sucrose fatty acid ester and 8 g of triethylene glycol monoisopropyl ether, and continue stirring for 10 minutes; add 2 g of a composite defoamer, wherein the composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester, and isopropanol in a mass ratio of 1:2:1; continue stirring until the defoamer is completely dispersed, and filter using a microporous filter with a pore size of 0.45 μm to remove possible solid particles or insoluble matter to obtain a penetrant.
[0112] Example 7
[0113] A method for preparing a film stripping solution that can improve film stripping efficiency is basically the same as that in Example 1, except that the preparation method of the penetrant is different:
[0114] The preparation method of the penetrant is as follows:
[0115] S1, add 500g water to the reactor and preheat to 50°C, gradually add 12g 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy, 15g estriol trisulfate trisodium salt and 25g sulfated castor oil to the water, stir each raw material until it is completely dissolved, maintain 50°C and continue stirring for 30 minutes to obtain a uniform solution;
[0116] S2. While stirring, add 5 g of sucrose fatty acid ester and 8 g of diethylene glycol tert-butyl ether, and continue stirring for 10 minutes; add 2 g of a composite defoamer, wherein the composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester, and isopropanol in a mass ratio of 1:2:1; continue stirring until the defoamer is completely dispersed, and filter using a microporous filter with a pore size of 0.45 μm to remove possible solid particles or insoluble matter to obtain a penetrant.
[0117] Comparative Example 1
[0118] A method for preparing a film stripping solution that can improve film stripping efficiency is basically the same as that in Example 1, except that the preparation method of the penetrant is different:
[0119] The preparation method of the penetrant is as follows:
[0120] S1, add 500g water to the reactor and preheat to 50°C, gradually add 12g 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy, 15g estriol trisulfate trisodium salt and 25g sulfated castor oil to the water, stir each raw material until it is completely dissolved, maintain 50°C and continue stirring for 30 minutes to obtain a uniform solution;
[0121] S2. While stirring, add 5 g of sucrose fatty acid ester and 8 g of bis(1-methyl-2-hydroxyethyl) ether, and continue stirring for 10 minutes; filter using a microporous filter with a pore size of 0.45 μm to remove possible solid particles or insoluble matter to obtain a permeate.
[0122] Comparative Example 2
[0123] A method for preparing a stripping solution that can improve stripping efficiency is as follows:
[0124] Step 1, 30g of composite alkali, 15g of commercially available penetrant, 8g of ethylene glycol dimethyl ether and 29g of water were mixed and added into a stirred tank, and heated and stirred at 55°C, with a stirring rate of 150 rpm and a stirring time of 30 minutes, and then cooled to room temperature to obtain a mixed solution;
[0125] Step 2: Add 15 g of water and 3 g of corrosion inhibitor to the mixed solution prepared in step 1, and then stir at room temperature at a stirring rate of 500 rpm for 120 minutes to obtain a stripping solution.
[0126] The composite base is composed of an inorganic base and an organic base in a mass ratio of 13:2, the inorganic base is composed of sodium hydroxide, potassium hydroxide and sodium carbonate in a mass ratio of 9:3:1; the organic base is composed of ethanolamine and propylenediamine in a mass ratio of 0.8:1.2.
[0127] The corrosion inhibitor is composed of octadecyl phosphate, oleic acid, sodium molybdate, sodium nitrate, benzotriazole and zinc sulfate in a mass ratio of 10:10:3:50:7:20.
[0128] Comparative Example 3
[0129] A method for preparing a stripping solution that can improve stripping efficiency is as follows:
[0130] Step 1, 30g of composite base, 8g of ethylene glycol dimethyl ether and 29g of water were mixed and added into a stirred tank, and the mixture was heated and stirred at 55°C, the stirring rate was controlled at 150 rpm, the stirring time was 30 minutes, and then cooled to room temperature to obtain a mixed solution;
[0131] Step 2: Add 15 g of water and 3 g of corrosion inhibitor to the mixed solution prepared in step 1, and then stir at room temperature at a stirring rate of 500 rpm for 120 minutes to obtain a stripping solution.
[0132] The composite base is composed of an inorganic base and an organic base in a mass ratio of 13:2, the inorganic base is composed of sodium hydroxide, potassium hydroxide and sodium carbonate in a mass ratio of 9:3:1; the organic base is composed of ethanolamine and propylenediamine in a mass ratio of 0.8:1.2.
[0133] The corrosion inhibitor is composed of octadecyl phosphate, oleic acid, sodium molybdate, sodium nitrate, benzotriazole and zinc sulfate in a mass ratio of 10:10:3:50:7:20.
[0134] Test Example 1
[0135] Stripping ability test
[0136] The stripping liquid prepared in the embodiment and the comparative example was used to strip the ultra-fine circuits of the printed circuit board. The treatment conditions were: the stripping liquid spraying pressure was 1.8 kg / cm 2 , the stripping liquid temperature is 50℃, the line width / dry film width = 30 / 30um, and the dry film thickness is 50um. Record the time required for stripping. Take the average value of the stripping time, and the test results are shown in Table 1.
[0137] Table 1
[0138]
[0139]
[0140] Test Example 2
[0141] Residue inspection
[0142] For Test Example 1, after stripping the film, use a microscope or a high-power magnifying glass to check the surface of the substrate to confirm whether there is any dry film or other material residue. The test results are shown in Table 2.
[0143] Table 2
[0144] Experimental protocol Residue inspection Example 1 Clean, no residue Example 2 Clean, with small residues Example 3 Clean, with small residues Example 4 Clean, with small residues Example 5 Clean, with small residues Example 6 Clean, with small residues Example 7 Clean, with small residues Comparative Example 1 Not clean, some residue Comparative Example 2 Not clean, some residue Comparative Example 3 Not clean, with large residues
[0145] It can be seen from test examples 1 to 2 that the stripping solution obtained in Example 1 of the present invention has a shorter stripping time and less residue after stripping.
[0146] In Example 1 of the present invention, the penetrant component 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy used has a specific chemical structure, which is why it shows better stripping efficiency and less residue than the sodium lauryl polyether sulfate used in Example 2. 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy may have a longer carbon chain and a sulfonate group, which increases its wetting and penetration ability in the dry film. The long chain structure helps to better interact with the polymer chain of the dry film and promote stripping. The sulfonate group may form a stronger interaction with the polar group in the dry film material through ionic action, which helps to improve the stripping efficiency. Since the molecular structure of 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy may have better intermolecular forces, such as hydrogen bonding, this may enhance its interaction with the dry film, thereby improving the stripping efficiency, and the stronger the interaction, the easier it may be to remove from the surface of the substrate after stripping, thereby reducing residues.
[0147] In Example 1 of the present invention, estriol trisulfate trisodium salt was used, which showed better stripping efficiency and less residues compared with 2-ethyl-3-hydroxyhexyl sodium sulfate used in Example 3 and 2-ethylhexyl sulfate sodium salt used in Example 4. Estriol trisulfate trisodium salt has three sulfate groups, which increases its solubility and wettability in water, thereby possibly improving its spreadability and permeability on the dry film surface. Due to the hydrophilicity of the sulfate group, estriol trisulfate trisodium salt may form a thinner liquid film on the dry film surface, which helps to improve wettability and spreadability, which is a key factor in stripping efficiency. The sulfate group may form a stronger interaction with the polar groups in the dry film material through ionic action, which helps to improve the stripping efficiency.
[0148] 10-Hydroxy-18-[2-[2-(sulfonyloxy)ethoxy] is an anionic surfactant with one sulfate group and one sulfonate group. Similarly, estriol trisulfate trisodium salt is also an anionic surfactant with multiple sulfate groups. In aqueous solution, these charged groups can be attracted together through charge interactions to form a micellar structure. This structure helps improve the stability and foam performance of the solution. Hydrogen bonding may occur between the hydroxyl groups in 10-hydroxy-18-[2-[2-(sulfonyloxy)ethoxy] and estriol trisulfate trisodium salt. Hydrogen bonding is a strong non-covalent interaction that can enhance the binding force between molecules and thus affect the physical and chemical properties of the solution. The structures of 10-hydroxy-18-[2-[2-(sulfonyloxy)ethoxy and estriol trisulfate trisodium salt complement each other in aqueous solution to form a more stable and effective surfactant system involving charge interactions, hydrogen bonding, and possible synergistic effects. These interactions jointly determine the properties of the mixed solution, including surface tension and foam stability, which in turn affect its application in stripping solutions.
[0149] Example 1 of the present invention uses sucrose fatty acid esters, while cetearyl glucoside is used in Example 5. Sucrose fatty acid esters may have a more suitable hydrophilic-lipophilic balance, which makes it more effective as a surfactant in the stripping solution and can better reduce the surface tension between water and the dry film, thereby improving wettability and permeability. The molecular structure of sucrose fatty acid esters may help it better penetrate into the microstructure of the dry film, which may be due to its molecular size and shape being more suitable for the pores of the dry film.
[0150] Compared with Examples 6 and 7, from the perspective of molecular structure, the shorter alkyl chain of bis(1-methyl-2-hydroxyethyl) ether may make it easier to penetrate and disperse, thereby improving the stripping efficiency. In addition, the hydrophilic part of bis(1-methyl-2-hydroxyethyl) ether may contribute to its stability and emulsification ability in aqueous solution.
[0151] Example 1 Compared with Comparative Example 1, the composite defoamer plays an important role in the preparation process of the stripping solution. The function of the defoamer is to reduce or eliminate the foam in the solution and improve the clarity and use efficiency of the stripping solution. During the stripping process, the foam may affect the permeability of the stripping solution and the cleaning effect on the film layer, so the addition of a defoamer helps to maintain the stability of the solution and improve the stripping efficiency. The composite defoamer is usually composed of a variety of surfactants and additives to provide a synergistic effect, thereby more effectively reducing the foam. The present invention uses a composite defoamer composed of polyethylene glycol, sorbitan fatty acid ester and isopropanol in a mass ratio of 1:2:1, which can provide excellent defoaming performance. Polyethylene glycol may reduce the formation of foam by reducing surface tension. Sorbitan fatty acid ester may inhibit the growth of foam by adsorbing on the foam surface. Isopropanol may accelerate the rupture of foam by reducing surface tension. By adding a composite defoamer, the stability of the stripping solution is improved, which helps to improve the stripping efficiency and the cleanliness of the film layer. The selection and dosage of defoamer need to be optimized according to the specific application conditions and the performance requirements of the stripping fluid.
Claims
1. A film stripping solution capable of improving film stripping efficiency, characterized in that: It is composed of the following components: composite alkali, penetrant, organic solvent, corrosion inhibitor and water.
2. The film stripping solution capable of improving film stripping efficiency as claimed in claim 1, characterized in that: The invention is composed of the following components in parts by weight: 25 to 35 parts of composite alkali, 10 to 20 parts of penetrant, 5 to 10 parts of organic solvent, 1 to 4 parts of corrosion inhibitor and 40 to 50 parts of water.
3. The stripping solution capable of improving stripping efficiency according to claim 1 or 2, characterized in that: The composite alkali is composed of an inorganic alkali and an organic alkali in a mass ratio of 10-15:1-3, the inorganic alkali is composed of sodium hydroxide, potassium hydroxide and sodium carbonate in a mass ratio of 8-10:2-4:1; the organic alkali is composed of ethanolamine and propylenediamine in a mass ratio of 0.7-0.9:1-1.
5.
4. The stripping solution capable of improving stripping efficiency according to claim 1 or 2, characterized in that: The organic solvent is one or more of ethylene glycol dimethyl ether, cyclohexanone and ethyl acetate.
5. The film stripping solution capable of improving film stripping efficiency according to claim 1 or 2, characterized in that: The corrosion inhibitor is composed of octadecyl phosphate, oleic acid, sodium molybdate, sodium nitrate, benzotriazole and zinc sulfate in a mass ratio of 9-11:9-11:2-4:40-60:6-8:18-22.
6. The film stripping solution capable of improving film stripping efficiency according to claim 1 or 2, characterized in that: The preparation method of the penetrant is as follows, in parts by weight: S1, add 400-600 parts of water to the reaction kettle and preheat it to 40-60°C, gradually add 10-15 parts of 10-hydroxy-18-[2-[2-(sulfonic acid group oxy) ethoxy, 13-16 parts of estriol trisulfate trisodium salt and 20-30 parts of sulfated castor oil to the water, stir each raw material until it is completely dissolved after adding, maintain 40-60°C and continue stirring for 20-40 minutes to obtain a uniform solution; S2. While stirring, add 4 to 6 parts of emulsifier and 7 to 9 parts of bis(1-methyl-2-hydroxyethyl) ether, and continue stirring for 5 to 15 minutes; add 1 to 3 parts of composite defoamer; continue stirring until the defoamer is completely dispersed, and filter with a microporous filter to remove possible solid particles or insoluble matter to obtain a penetrant.
7. The film stripping solution capable of improving film stripping efficiency according to claim 6, characterized in that: The emulsifier is sucrose fatty acid ester.
8. The film stripping solution capable of improving film stripping efficiency as claimed in claim 6, characterized in that: The composite defoamer is composed of polyethylene glycol, sorbitan fatty acid ester and isopropanol in a mass ratio of 0.8-1.2:1-3:0.8-1.
2.
9. The film stripping solution capable of improving film stripping efficiency according to claim 6, characterized in that: The pore size of the microporous filter is 0.4-0.5 μm.
10. A method for preparing a film stripping solution capable of improving film stripping efficiency as claimed in claims 1 to 9, characterized in that: Here’s how: Step 1, weighing each raw material according to weight, mixing the composite base, penetrant, organic solvent and water, adding them into a stirring kettle, heating and stirring, the heating temperature is controlled at 50-60° C., the stirring rate is controlled at 100-200 rpm, the stirring time is 20-40 minutes, and then cooling to room temperature to obtain a mixed solution; Step 2: Add water and corrosion inhibitor to the mixed solution prepared in step 1, and then stir at room temperature at a stirring rate of 400 to 600 rpm for 100 to 150 minutes to obtain a stripping solution.
Citation Information
Patent Citations
Film stripping liquid for light sensing dry film and production method and application of film stripping liquid
CN108008606A
Organic film stripping solution
CN108319118A
Film stripping liquid and preparation method thereof
CN113563888A
High-pressure spraying cleaning agent for automatic line spraying and preparation method of high-pressure spraying cleaning agent
CN115852381A
Detergent composition comprising lipase
CN116670261A
Cited By
Hyperfine circuit film stripping liquid and preparation method thereof
CN120844092A
An ultra-fine circuit stripping solution and its preparation method
CN120844092B