Preparation and observation method for interface structure of zirconium-titanium-stainless steel explosive cladding plate

Through the methods of step-by-step grinding, chemical polishing and corrosive solution etching, the interface structure of the zirconium-titanium-stainless steel explosive composite plate is clearly displayed, which solves the problem of unclear interface observation in the existing technology and realizes the zirconium-titanium-stainless steel interface. The clear display and obvious boundaries are suitable for promotion and application.

CN118746474APending Publication Date: 2024-10-08西安汉唐分析检测有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410802907.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing technology cannot clearly display the zirconium-titanium interface and titanium-stainless steel interface structure in the zirconium-titanium-stainless steel explosive composite plate, resulting in unclear observation and easy misjudgment.

Method used

Different types of polishing methods and appropriate polishing sequences are used to polish zirconium, titanium and stainless steel, combined with corrosive solution etching. Through step-by-step grinding, chemical polishing, mechanical polishing and corrosive solution etching, the interface structure is clearly revealed and the boundaries are obvious. , to avoid corrosion pits and embossments.

Benefits of technology

Achieved clear observation of the interface structure of the zirconium-titanium-stainless steel explosive composite plate, with clear boundaries and no obvious corrosion pits and embossments, which solved the difficulty of observation caused by the corrosion resistance of different metals. The method is easy to operate, non-toxic, and suitable for popularization and application. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118746474A_ABST
    Figure CN118746474A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation and observation method for an interface structure of a zirconium-titanium-stainless steel explosive cladding plate. The method comprises the following steps: 1, machining the zirconium-titanium-stainless steel explosive cladding plate to form an interface structure observation plane, and then grinding and washing; 2, immersing in an etchant solution for chemical polishing; 3, mechanical rough polishing and mechanical fine polishing; 4, immersing into an etchant solution for etching; and 5, observing the interface structure. According to the method, different types of polishing methods are adopted, a proper polishing sequence is selected to polish zirconium, titanium and stainless steel in the zirconium-titanium-stainless steel explosive composite plate in sequence, etching is carried out by adopting an etchant solution, so that a zirconium-titanium interface structure and a titanium-stainless steel interface structure are clearly shown, the boundary is obvious, and the performance of the explosive composite plate is improved. The method has no obvious corrosion pits and embossments in the interface structure, solves the problem that the interface microstructure of the composite board is difficult to clearly display due to different corrosion resistance of zirconium, titanium and stainless steel, is simple and non-toxic, does not need special equipment, and is suitable for popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallographic microstructure observation of metal materials, and in particular relates to a method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosion composite plate. Background Art

[0002] Because zirconium has better corrosion resistance than stainless steel, titanium, and nickel alloys (corrosion resistance to some highly corrosive media), and also has good mechanical properties, many highly corrosive equipment have begun to use zirconium. In some highly corrosive occasions, using pure zirconium to manufacture pressure vessels is costly and wastes resources. The zirconium plate and steel plate are made into a composite plate by the method of explosive composite, which combines their advantages and reduces the manufacturing cost. Referring to the ASME specification, the zirconium grades commonly used to manufacture pressure vessels are R60700 and R60702.

[0003] At present, R60702 is generally used to manufacture chemical corrosion-resistant equipment. When R60702 is used to manufacture zirconium-steel composite steel plates, good composite quality can be obtained when the bottom steel plate is medium-strength container steel. However, when the strength of the steel plate is increased, or the thickness is increased to more than 10mm, the composite difficulty increases accordingly. At this time, a titanium layer with a thickness of 2mm to 6mm should be added between zirconium and steel as a transition layer to ensure the quality of the composite plate. This composite method is called three-layer composite. Titanium transition is used because titanium and zirconium are elements of the same family, and the metallurgical properties of the materials are similar. The explosive composite of the two will not produce intermetallic compounds, and the composite process of pure titanium and steel is relatively mature, which can fully guarantee the composite quality. Therefore, high-quality zirconium-steel composite plates all adopt a layer of pure titanium plate as a transition layer between the two.

[0004] At present, there is no corresponding preparation method and fixed corrosive agent for zirconium-titanium-stainless steel explosive composite plate to show the microstructure of zirconium-titanium interface and titanium-stainless steel interface. Due to the different hardness and corrosion resistance of zirconium, titanium and stainless steel, it is easy to cause corrosion pits and embossing of interface microstructure, which affects the observation of interface structure and leads to wrong conclusions. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosion composite plate in view of the deficiencies of the above-mentioned prior art. The method adopts different types of polishing methods, and selects a suitable polishing sequence to polish the zirconium, titanium and stainless steel in the zirconium-titanium-stainless steel explosion composite plate in turn, and combines the use of corrosive solution etching to make the zirconium-titanium interface structure and the titanium-stainless steel interface structure clearly visible, with obvious boundaries, and no obvious corrosion pits and convexities in the interface structure, which solves the problem that the interface microstructure of the composite plate is difficult to clearly show due to the different corrosion resistance of zirconium, titanium and stainless steel.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosive composite plate, characterized in that the method comprises the following steps:

[0007] Step 1: Mechanically process the zirconium-titanium-stainless steel explosion composite plate to obtain an interface structure observation plane, and then grind the machined interface structure observation plane on a metallographic pre-grinder, and wash away the sand on the observation plane after grinding;

[0008] Step 2: immerse the interface structure observation plane after washing away the sand in step 1 into a corrosion solution for chemical polishing for 2s to 5s;

[0009] Step 3, placing the interface structure observation plane after chemical polishing in step 2 on a polishing machine for mechanical rough polishing and mechanical fine polishing respectively, until the surface of the interface structure observation plane is smooth and bright, without scratches and drag;

[0010] Step 4: immerse the interface structure observation plane after mechanical fine polishing in step 3 into the corrosion solution for etching for 2s to 5s;

[0011] Step 5: Place the interface structure observation plane after etching in step 4 under a metallographic microscope, and observe the interface structure by open field observation.

[0012] Since the zirconium-titanium-stainless steel explosion composite plate contains three different types of metals, namely zirconium, titanium and stainless steel, and zirconium, titanium and stainless steel have different wear resistance characteristics and different corrosion resistance to fixed corrosive agents, it is impossible to polish and sample the three metals in the composite plate at the same time in the prior art. In view of this problem, the present invention mechanically processes the zirconium-titanium-stainless steel explosion composite plate to obtain an interface structure observation plane, then removes the excess and damage layer on the surface of the composite plate by grinding, washes away the particles attached to the surface of the composite plate by washing, and then chemically polishes the zirconium metal surface in the composite plate to present a mirror gloss, mechanically rough polishes the stainless steel surface in the composite plate to present a mirror gloss, and mechanically fine polishes the titanium surface in the composite plate to present a mirror gloss, and then corrodes the metallographic structure by corrosive solution erosion, which is used for metallographic microscope observation, so that the zirconium-titanium interface structure and the titanium-stainless steel interface structure in the zirconium-titanium-stainless steel explosion composite plate are clearly displayed, and the boundaries are obvious, and there are no obvious corrosion pits and convexities in the interface structure.

[0013] The above-mentioned method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosive composite plate is characterized in that the specific process of grinding in step 1 is: using a particle size of 120 # , 400 # , 800# and 1200 #The metallographic water sandpaper is used for grinding step by step. Each time the metallographic water sandpaper is changed for grinding, the grinding direction is turned 90° to ensure that the previous grinding marks are completely eliminated.

[0014] The above-mentioned method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosion composite plate is characterized in that the corrosion solution in step 2 is composed of the following components in volume percentage: HF 10% to 15%, HNO3 20% to 30%, and the balance is H2O. The present invention immerses the interface structure observation plane washed away with sand particles into the corrosion solution to chemically polish the zirconium material in the composite plate. By controlling the composition ratio of HF and HNO3 in the corrosion solution, it is ensured that the corrosion solution will not only play a chemical polishing role on the zirconium material, but also will not easily over-corrode the zirconium interface and cause pitting and convexity, which is conducive to the clear appearance of the zirconium-titanium interface structure.

[0015] The above-mentioned method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosion composite plate is characterized in that the polishing cloth for mechanical rough polishing in step three is a canvas polishing cloth, the polishing agent is a diamond spray with a particle size of 5 μm, and the polishing cloth for mechanical fine polishing is a damping polishing cloth, and the polishing agent is a SiO2 suspension with a particle size of 0.5 μm.

[0016] The above-mentioned method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosive composite plate is characterized in that the corrosive solution in step 4 is composed of the following components in volume percentage: HF 2% to 5%, HNO3 5% to 10%, and the balance is H2O. The present invention immerses the interface structure observation plane after mechanical fine polishing into the corrosive solution for etching to corrode the titanium material in the composite plate. By controlling the composition ratio of the corrosive solution, it is ensured that the corrosive solution has a corrosive effect on the titanium material. At the same time, for the zirconium material in the composite plate that is extremely sensitive to hydrofluoric acid, the corrosive solution of this composition can not only cause the titanium material to corrode the structure under the corresponding etching time, but also prevent the zirconium material from being over-corroded, thereby facilitating the clear appearance of the zirconium-titanium interface structure and the titanium-stainless steel interface structure.

[0017] The above-mentioned method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosion composite plate is characterized in that the HF and HNO3 are both analytically pure reagents.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] 1. The present invention adopts different types of polishing methods and selects a suitable polishing order to polish the zirconium, titanium and stainless steel in the zirconium-titanium-stainless steel explosion composite plate in turn, and combines the use of corrosive solution etching to make the zirconium-titanium interface structure and titanium-stainless steel interface structure in the zirconium-titanium-stainless steel explosion composite plate clearly visible, and the boundary is obvious, and there are no obvious corrosion pits and convexities in the interface structure, thereby avoiding the shortcomings of unclear observed interface microstructure of the zirconium-titanium-stainless steel explosion composite plate, over-corrosion and easy misjudgment due to improper polishing and corrosion.

[0020] 2. The present invention controls the composition ratio of the corrosive solution used in chemical polishing and etching and the corresponding processing time, so that different metals in the zirconium-titanium-stainless steel explosion composite plate are corroded to a good degree, and the adverse effects on other metal structures are avoided, which is conducive to the clear appearance of each interface structure and solves the problem that the same corrosive agent cannot be used to achieve good corrosion of different metals in the composite plate.

[0021] 3. The preparation and observation method of the present invention is easy to operate and non-toxic, can clearly observe the interface structure of the zirconium-titanium-stainless steel explosion composite plate, and does not require any special equipment, so it is suitable for promotion and application.

[0022] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a microstructure diagram (100×) of the zirconium-titanium interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in Example 1 of the present invention.

[0024] Figure 2 This is a microstructure diagram (100×) of the titanium-stainless steel interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in Example 1 of the present invention.

[0025] Figure 3 This is a microstructure diagram (100×) of the zirconium-titanium interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in Example 2 of the present invention.

[0026] Figure 4 This is a microstructure diagram (100×) of the titanium-stainless steel interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in Example 2 of the present invention.

[0027] Figure 5 This is a microstructure diagram (100×) of the zirconium-titanium interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in Example 3 of the present invention.

[0028] Figure 6This is a microstructure diagram (100×) of the titanium-stainless steel interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in Example 3 of the present invention. DETAILED DESCRIPTION

[0029] Example 1

[0030] This embodiment includes the following steps:

[0031] Step 1: Mechanically process the zirconium-titanium-stainless steel explosion composite plate to obtain an interface structure observation plane, and then grind the machined interface structure observation plane on a metallographic pre-grinder, and wash away the sand on the observation plane after grinding; the specific process of the grinding is: using a particle size of 120 # , 400 # , 800# and 1200 # Grind step by step with metallographic water sandpaper. Each time you change the metallographic water sandpaper for grinding, turn the grinding direction 90° to ensure that the last grinding marks are completely eliminated.

[0032] Step 2: Immerse the interface structure observation plane after washing away the sand in step 1 in a corrosion solution for chemical polishing for 5 seconds; the corrosion solution is composed of the following components in volume percentage: HF 10%, HNO3 20%, H2O 70%, and HF and HNO3 are analytical grade reagents;

[0033] Step 3, placing the interface structure observation plane after chemical polishing in step 2 on a polishing machine for mechanical rough polishing and mechanical fine polishing respectively, until the surface of the interface structure observation plane is smooth and bright, without scratches and drag; the polishing cloth for mechanical rough polishing is a canvas polishing cloth, the polishing agent is a diamond spray with a particle size of 5 μm, and the polishing cloth for mechanical fine polishing is a damping polishing cloth, and the polishing agent is a SiO2 suspension with a particle size of 0.5 μm;

[0034] Step 4: Immerse the interface structure observation plane after mechanical fine polishing in step 3 in a corrosion solution for etching for 5 seconds; the corrosion solution is composed of the following components in volume percentage: HF 2%, HNO3 5%, H2O 93%, and HF and HNO3 are analytically pure reagents;

[0035] Step 5: Place the interface structure observation plane after etching in step 4 under a metallographic microscope, and observe the interface structure by open field observation.

[0036] Figure 1 The microstructure of the zirconium-titanium interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in this embodiment (100×) is shown in FIG. Figure 1 It can be seen that the titanium-zirconium interface is well corroded, the interface structure is clearly visible without protrusions, and there are no interfering pits or over-corrosion black spots.

[0037] Figure 2 The microstructure of the titanium-stainless steel interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in this embodiment (100×) is shown in FIG. Figure 2 It can be seen that the titanium-stainless steel interface has no embossing or scratches, and the details are clear.

[0038] Example 2

[0039] This embodiment includes the following steps:

[0040] Step 1: Mechanically process the zirconium-titanium-stainless steel explosion composite plate to obtain an interface structure observation plane, and then grind the machined interface structure observation plane on a metallographic pre-grinder, and wash away the sand on the observation plane after grinding; the specific process of the grinding is: using a particle size of 120 # , 400 # , 800# and 1200 # Grind step by step with metallographic water sandpaper. Each time you change the metallographic water sandpaper for grinding, turn the grinding direction 90° to ensure that the last grinding marks are completely eliminated.

[0041] Step 2: Immerse the interface structure observation plane after washing away the sand in step 1 in a corrosion solution for chemical polishing for 3 seconds; the corrosion solution is composed of the following components in volume percentage: HF 10%, HNO3 20%, H2O 70%, and HF and HNO3 are analytical grade reagents;

[0042] Step 3, placing the interface structure observation plane after chemical polishing in step 2 on a polishing machine for mechanical rough polishing and mechanical fine polishing respectively, until the surface of the interface structure observation plane is smooth and bright, without scratches and drag; the polishing cloth for mechanical rough polishing is a canvas polishing cloth, the polishing agent is a diamond spray with a particle size of 5 μm, and the polishing cloth for mechanical fine polishing is a damping polishing cloth, and the polishing agent is a SiO2 suspension with a particle size of 0.5 μm;

[0043] Step 4: immerse the interface structure observation plane after mechanical fine polishing in step 3 into a corrosion solution for etching for 3 seconds; the corrosion solution is composed of the following components in volume percentage: HF 5%, HNO3 10%, H2O 85%, and HF and HNO3 are analytical grade reagents;

[0044] Step 5: Place the interface structure observation plane after etching in step 4 under a metallographic microscope, and observe the interface structure by open field observation.

[0045] Figure 3 The microstructure of the zirconium-titanium interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in this embodiment (100×) is shown in FIG. Figure 3It can be seen that the titanium-zirconium interface is well corroded, the interface structure is clearly visible without protrusions, and there are no interfering pits or over-corrosion black spots.

[0046] Figure 4 The microstructure of the titanium-stainless steel interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in this embodiment (100×) is shown in FIG. Figure 4 It can be seen that the titanium-stainless steel interface has obvious no embossing or scratches, and the details are clear.

[0047] Example 3

[0048] This embodiment includes the following steps:

[0049] Step 1: Mechanically process the zirconium-titanium-stainless steel explosion composite plate to obtain an interface structure observation plane, and then grind the machined interface structure observation plane on a metallographic pre-grinder, and wash away the sand on the observation plane after grinding; the specific process of the grinding is: using a particle size of 120 # , 400 # , 800# and 1200 # Grind step by step with metallographic water sandpaper. Each time you change the metallographic water sandpaper for grinding, turn the grinding direction 90° to ensure that the last grinding marks are completely eliminated.

[0050] Step 2: Immerse the interface structure observation plane after washing away the sand in step 1 in a corrosion solution for chemical polishing for 2 seconds; the corrosion solution is composed of the following components in volume percentage: HF 15%, HNO3 30%, H2O 55%, and HF and HNO3 are analytical grade reagents;

[0051] Step 3, placing the interface structure observation plane after chemical polishing in step 2 on a polishing machine for mechanical rough polishing and mechanical fine polishing respectively, until the surface of the interface structure observation plane is smooth and bright, without scratches and drag; the polishing cloth for mechanical rough polishing is a canvas polishing cloth, the polishing agent is a diamond spray with a particle size of 5 μm, and the polishing cloth for mechanical fine polishing is a damping polishing cloth, and the polishing agent is a SiO2 suspension with a particle size of 0.5 μm;

[0052] Step 4: The interface structure observation plane after mechanical fine polishing in step 3 is immersed in a corrosion solution for etching for 2 seconds; the corrosion solution is composed of the following components in volume percentage: HF 2%, HNO3 10%, H2O 88%, and HF and HNO3 are both analytically pure reagents;

[0053] Step 5: Place the interface structure observation plane after etching in step 4 under a metallographic microscope, and observe the interface structure by open field observation.

[0054] Figure 5The microstructure of the zirconium-titanium interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in this embodiment (100×) is shown in FIG. Figure 5 It can be seen that the titanium-zirconium interface is well corroded, the interface structure is clearly visible without protrusions, and there are no interfering pits or over-corrosion black spots.

[0055] Figure 6 The microstructure of the titanium-stainless steel interface in the interface structure of the zirconium-titanium-stainless steel explosive composite plate in this embodiment (100×) is shown in FIG. Figure 6 It can be seen that the titanium-stainless steel interface has obvious no embossing or scratches, and the details are clear.

[0056] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosive composite plate, characterized in that: The method comprises the following steps: Step 1: Mechanically process the zirconium-titanium-stainless steel explosion composite plate to obtain an interface structure observation plane, and then grind the machined interface structure observation plane on a metallographic pre-grinder, and wash away the sand on the observation plane after grinding; Step 2: immerse the interface structure observation plane after washing away the sand in step 1 into a corrosion solution for chemical polishing for 2s to 5s; Step 3, placing the interface structure observation plane after chemical polishing in step 2 on a polishing machine for mechanical rough polishing and mechanical fine polishing respectively, until the surface of the interface structure observation plane is smooth and bright, without scratches and drag; Step 4: immerse the interface structure observation plane after mechanical fine polishing in step 3 into the corrosion solution for etching for 2s to 5s; Step 5: Place the interface structure observation plane after etching in step 4 under a metallographic microscope, and observe the interface structure by open field observation.

2. The method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosive composite plate according to claim 1, characterized in that: The specific process of grinding in step 1 is: using a particle size of 120 # , 400 # , 800# and 1200 # The metallographic water sandpaper is used for grinding step by step. Each time the metallographic water sandpaper is changed for grinding, the grinding direction is turned 90° to ensure that the previous grinding marks are completely eliminated.

3. The method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosive composite plate according to claim 1 is characterized in that: The etching solution in step 2 is composed of the following components in volume percentage: HF 10% to 15%, HNO3 20% to 30%, and the balance H2O.

4. The method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosive composite plate according to claim 1, characterized in that: The polishing cloth for mechanical rough polishing in step 3 is a canvas polishing cloth, the polishing agent is a diamond spray with a particle size of 5 μm, and the polishing cloth for mechanical fine polishing is a damping polishing cloth, and the polishing agent is a SiO2 suspension with a particle size of 0.5 μm.

5. The method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosive composite plate according to claim 1, characterized in that: The etching solution in step 4 is composed of the following components in volume percentage: HF 2% to 5%, HNO3 5% to 10%, and the balance is H2O.

6. The method for preparing and observing the interface structure of a zirconium-titanium-stainless steel explosive composite plate according to claim 3 or 5, characterized in that: The HF and HNO3 are analytically pure reagents.

Citation Information

Cited By

  • Corrosion display method of TA22 titanium alloy grain structure

    CN119804246A