Compression performance test system and test method
By using a single camera in the compression performance testing system to collect images of the front and back of the composite laminate, the problem in the existing technology of being unable to simultaneously measure the deformation of the front and back of the sample is solved, the accuracy and fault tolerance of the test are improved, and the test is realized. Accurate acquisition of multi-parameter compression performance data for composite materials.
Patent Information
- Application Number
- CN202410777410.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-17
AI Technical Summary
The existing compression performance testing system cannot simultaneously measure the deformation of the front and back sides of the composite laminate sample, resulting in low test accuracy and fault tolerance, and the inability to obtain compression modulus and failure strain data.
A compression performance testing system is designed, which uses a single camera to collect images of the front and back of the sample through the reflection path of the first reflection mechanism and the second reflection mechanism, and combines the clamp unit and compression unit to measure the compression performance parameters of composite materials.
The accuracy and fault tolerance rate of the test system are improved, and the front and back data of the sample can be obtained at the same time, including parameters such as compressive strength, compressive strain, compressive modulus, compressive Poisson's ratio, and failure strain, to meet the compression performance testing needs of composite materials. .
Smart Images

Figure CN118746488A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of mechanical performance testing, and in particular to a compression performance testing system and a testing method. Background Art
[0002] Composite materials are widely used in aerospace, marine engineering, transportation and other fields because of their advantages such as high specific strength and specific stiffness, strong designability, good fatigue fracture resistance, corrosion resistance, as well as composite effects, multi-functional compatibility, and manufacturing synchronization.
[0003] Compression performance is a basic mechanical property and an important design parameter of composite materials. The 11 basic engineering constants of composite laminates include 0° and 90° compression strength and modulus. As a composite material used in main load-bearing structures, compression failure is one of the main failure mechanisms when it is loaded with external forces such as bending compression in actual complex force fields. Unlike the tensile failure of composite materials, the formation of compression failure is instantaneous and the damage to the material is very large. Compression performance has become a key factor restricting the overall performance of composite materials and the utilization rate of structural materials. Therefore, the compression performance of composite materials and its related experimental research have been a hot topic of widespread concern among scholars at home and abroad for many years.
[0004] Due to the limitation of fixture space, the compression performance of existing testing systems can usually only obtain the deformation of a certain surface of the composite laminate specimen, and cannot achieve simultaneous measurement of the back-to-back surfaces of the specimen, which greatly reduces the accuracy. In addition, there is only data from one surface. If there is a problem in the test, the compression modulus and failure strain data cannot be obtained, and the fault tolerance rate is low. Summary of the invention
[0005] In view of this, the present invention provides a compression performance testing system, which can capture images of the front and back sides of a sample using a single camera, thereby improving the accuracy and fault tolerance of the testing system.
[0006] The present invention also provides a testing method including the compression performance testing system.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A compression performance testing system comprises: a fixture unit, a compression unit, a collection unit and an analysis unit;
[0009] The clamp unit comprises: a first reflection mechanism, a second reflection mechanism and a clamp assembly;
[0010] The clamp assembly is used to support the sample, the first reflection mechanism is arranged on the front side of the sample, and is used to reflect the image of the front side of the sample, and the second reflection mechanism is arranged on the back side of the sample, and is used to reflect the image of the back side of the sample;
[0011] The compression unit comprises: an upper pressing plate and a lower pressing plate arranged opposite to each other, wherein the upper pressing plate and the lower pressing plate form a compression space to compress the sample;
[0012] The acquisition unit comprises: a camera, which is located on the reflection path of the first reflection mechanism and the reflection path of the second reflection mechanism, and is used to acquire images of the front and back sides of the sample, and the camera is connected to the analysis unit.
[0013] In some embodiments, the first reflecting mechanism is provided with a first prism for reflecting the image of the front side;
[0014] The second reflecting mechanism is provided with a second prism for reflecting the image of the reverse surface.
[0015] In some embodiments, the first reflection mechanism is further provided with a first lower apex for supporting the first prism, and the first prism is capable of rotating relative to the first lower apex;
[0016] The second reflection mechanism is further provided with a second lower apex for supporting the second prism, and the second prism is capable of rotating relative to the second lower apex.
[0017] In some embodiments, the first reflection mechanism is further provided with a first upper apex for fixing the first prism, and the first upper apex and the first lower apex are symmetrically arranged;
[0018] The second reflection mechanism is also provided with a second upper apex for fixing the second prism, and the second upper apex and the second lower apex are symmetrically arranged.
[0019] In some embodiments, the clamp assembly includes: a first clamping plate and a second clamping plate, wherein the first clamping plate and the second clamping plate form a supporting space to support the sample;
[0020] The ends of the sample located in the supporting space extend toward the upper pressing plate and the lower pressing plate respectively.
[0021] In some embodiments, a V-shaped groove is disposed on one side of the first clamping plate and the second clamping plate forming the supporting space.
[0022] In some embodiments, the clamp assembly further includes: a base, the second clamping plate being vertically disposed on the base;
[0023] The first clamping plate is provided with a first mounting hole, the second clamping plate is provided with a second mounting hole, and the first mounting hole and the second mounting hole are arranged in a corresponding position so that the mounting member passes through the first mounting hole and the second mounting hole in sequence.
[0024] In some embodiments, the first clamping plate is provided with a first opening for capturing the image of the front side, and the second clamping plate is provided with a second opening for capturing the image of the back side;
[0025] The first opening faces the first reflecting mechanism, and the second opening faces the second reflecting mechanism.
[0026] In some embodiments, the analysis unit includes: a controller and a computer;
[0027] The controller is used to control the upper pressing plate and the lower pressing plate to compress the sample and transmit the collected load information to the computer; the image information of the camera is transmitted to the computer.
[0028] In some embodiments, it also includes: a high and low temperature environment box;
[0029] The clamp unit and the compression unit can both be placed in the high and low temperature environment box.
[0030] A method for testing a compression performance test system, using the above-mentioned compression performance test system, comprises the following steps:
[0031] S1. placing the sample to be tested in an atmospheric environment for state pretreatment to obtain a pretreated sample;
[0032] S2, measuring the value of the width w and the value of the thickness h of the section to be tested in the pretreated sample;
[0033] S3, spraying speckles on the front and back surfaces of the section to be tested;
[0034] S4, placing the pretreated sample in the compression performance testing system to perform a compression performance testing operation;
[0035] The operation of placing the pretreated sample in the compression performance testing system for compression performance testing includes:
[0036] S41: clamping the pretreated sample on the clamp assembly so that the section to be tested of the clamped pretreated sample and the first reflection mechanism and the second reflection mechanism of the compression performance testing system are at the same level;
[0037] S42, placing the fixture unit and the compression unit in a high and low temperature environment box, and adjusting the high and low temperature environment box according to different compression performance test temperature conditions, so that the test environment temperature of the pretreated sample reaches the corresponding compression performance test temperature condition;
[0038] S43. Under the compression performance test temperature conditions, the compression performance parameters of the test section of the pretreated sample are obtained through the compression performance test system; the compression performance parameters include at least any one of compression strength, compression strain, compression modulus, compression Poisson's ratio, offset compression strength, bending percentage and failure strain.
[0039] In some embodiments, the S43 includes:
[0040] Under the compression performance test temperature conditions, the axial displacement values v of the first test point of the test section of the sample before and after the compression deformation are respectively measured by the analysis unit. A , the axial displacement value v of the second test point of the test section of the sample before and after compression deformation B Under the compression performance test temperature conditions, the lateral displacement value v of the third test point of the test section of the sample before and after the compression deformation is measured by the analysis unit. C , the lateral displacement value v of the fourth test point of the test section of the sample before and after compression deformation D ;
[0041] Measure the value of l0; the value of l0 is the axial distance between the first test point and the second test point before compression deformation; use Calculate the axial compressive strain ε 01 ;
[0042] Measurement CD The value of l CD The value of is the lateral distance between the third test point and the fourth test point before compression deformation; using Calculate the transverse compressive strain ε 02 .
[0043] In some embodiments, it also includes:
[0044] Measure the axial strain value ε at the lowest point of the strain range of the measured section respectively x1 and the axial strain value ε at the highest point of the strain range of the measured section x2 ;
[0045] Calculate the transverse strain value ε at the lowest point of the strain range of the measured section y1 and the transverse strain value ε at the highest point of the strain range of the measured section y2 ;
[0046] use Calculate Said is the compression Poisson's ratio.
[0047] In some embodiments, the S43 includes:
[0048] Under the compression performance test temperature conditions, measuring the value of the front strain ε1 and the value of the back strain ε2;
[0049] use Calculate the bending percentage By.
[0050] In some embodiments, the S43 includes:
[0051] Under the compression performance test temperature conditions, the maximum breaking load P of the tested section is detected by the analysis unit. m ;
[0052] use Calculate F c , the F c is the compressive strength.
[0053] In some embodiments, the S43 includes:
[0054] Under the compression performance test temperature conditions, the axial strain value ε at the lowest point of the strain range of the section to be tested is measured respectively. x1 and the axial strain value ε at the highest point of the strain range of the measured segment x2 ;
[0055] The load value P1 corresponding to the lowest point of the strain range of the section to be measured and the load value P2 corresponding to the highest point of the strain range of the section to be measured are respectively measured by the analysis unit;
[0056] use Calculate E c , the E c is the compression modulus.
[0057] In some embodiments, the S43 includes:
[0058] Under the compression performance test temperature condition, a compression stress-compression strain curve of the section to be tested is obtained, and based on the compression stress-compression strain curve, the compression elastic modulus line of the section to be tested is translated from the origin to a fixed strain value, and the compression elastic modulus line is extended to intersect with the compression stress-compression strain curve, and the intersection point is the offset compression strength value of the section to be tested; and / or
[0059] Under the compression performance test temperature condition, the section to be tested is brought into an instantaneous failure state, and the failure strain value of the section to be tested is measured.
[0060] It can be seen from the above technical scheme that the compression performance testing system provided by the present invention, compared with the existing technology, is a technical scheme in which the camera is arranged on the reflection path of the first reflection mechanism and the second reflection mechanism, thereby realizing the use of a single camera to simultaneously capture images of the front and back sides of the sample, thereby improving the accuracy of the testing system and avoiding the problem of being unable to obtain values such as the compression modulus and failure strain due to collecting data from only one side (front or back), thereby improving the fault tolerance of the compression performance testing system.
[0061] The present invention also provides a testing method for a compression performance testing system. Since the compression performance testing system mentioned above is adopted, it also has corresponding beneficial effects. For details, please refer to the above description, which will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0063] Figure 1 This is a schematic diagram of the overall structure of the compression performance test system;
[0064] Figure 2 This is an axonometric view of the fixture unit of the compression performance testing system;
[0065] Figure 3 This is a front view of the fixture unit of the compression performance testing system;
[0066] Figure 4 is a schematic structural diagram of a first clamping plate of a clamp unit;
[0067] Figure 5 A first isometric view of a second clamping plate and other structures of the clamp unit;
[0068] Figure 6 A second isometric view of a second clamping plate and other structures of the clamp unit;
[0069] Figure 7 is a structural schematic diagram of a prism stage of a fixture unit;
[0070] Figure 8 It is a structural schematic diagram of the top tip of the fixture unit;
[0071] Fig. 9 It is a schematic diagram of the structure of the sample;
[0072] Fig.10 The schematic diagram of the sample decomposition;
[0073] Fig.11 This is a flow chart of the test method of the compression performance test system.
[0074] Among them, 1 is a high and low temperature environment box 1; 2a is an upper pressure plate, 2b is a lower pressure plate; 3a is a first light source, 3b is a second light source; 4 is a fixture unit; 5 is a controller; 6 is a computer; 7 is a camera; 8 is a first clamping plate; 9 is an upper top, 9a is a first upper top, 9b is a second upper top; 10a is a first prism, 10b is a second prism; 11a is a first lower top, 11b is a second lower top; 12 is a prism stand, 12a is a first prism stand, 12b is a second prism stand; 13 is a pad; 14 is a base; 15 is a sample, 15a is the front side, 15b is the back side; 16 is a second clamping plate. DETAILED DESCRIPTION
[0075] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0076] The compression performance testing system provided by the embodiment of the present invention is as follows: Figure 1-Figure 10 As shown, it includes: a clamp unit 4, a compression unit, a collection unit and an analysis unit;
[0077] The fixture unit 4 includes: a first reflection mechanism, a second reflection mechanism and a fixture assembly;
[0078] The fixture assembly is used to support the sample 15, the first reflection mechanism is arranged on the side of the front surface 15a of the sample 15, and is used to reflect the image of the front surface 15a of the sample 15, and the second reflection mechanism is arranged on the side of the back surface 15b of the sample 15, and is used to reflect the image of the back surface 15b of the sample 15;
[0079] The compression unit includes: an upper pressing plate 2a and a lower pressing plate 2b which are arranged opposite to each other, and the upper pressing plate 2a and the lower pressing plate 2b form a compression space to compress the sample 15;
[0080] The acquisition unit includes: a camera 7, which is located on the reflection path of the first reflection mechanism and the reflection path of the second reflection mechanism, and is used to acquire images of the front side 15a and the back side 15b of the sample 15, and the camera 7 is connected to the analysis unit.
[0081] In the above technical solution, when the sample 15 is compressed, both the front surface 15a and the back surface 15b of the sample 15 are deformed, the first reflection mechanism reflects the deformed image (speckle pattern) of the front surface 15a to the camera 7 for collection, and the second reflection mechanism reflects the deformed image (speckle pattern) of the back surface 15b to the camera 7 for collection. A single camera can be used to collect images of the front and back surfaces of the sample 15. The image information collected by the camera 7 is transmitted to the analysis unit, and the analysis unit calculates the compressive strength, compressive strain, compression modulus, compressive Poisson's ratio, offset compressive strength and failure strain of the sample 15 through analysis.
[0082] Compared with the existing technology, the present technical solution sets the camera 7 on the reflection path of the first reflection mechanism and the second reflection mechanism, thereby realizing the use of a single camera to simultaneously capture images of the front and back sides of the sample 15, thereby improving the accuracy of the test system and avoiding the problem of being unable to obtain values such as compression modulus and failure strain due to collecting data from only one side (front or back), thereby improving the fault tolerance of the present compression performance test system.
[0083] Further, such as Figure 2 As shown, the first reflecting mechanism is provided with a first prism 10a for reflecting the image of the front side 15a;
[0084] The second reflecting mechanism is provided with a second prism 10b for reflecting the image of the reverse surface 15b.
[0085] In the above scheme, the image of the front side 15a of the sample 15 reflected by the first prism 10a is collected by the camera 7, and the image of the back side 15b of the sample 15 reflected by the second prism 10b is collected by the camera 7; preferably, the first prism 10a and the second prism 10b are both rectangular total reflection prisms, which are formed by gluing two isosceles right-angle prisms, and the 45° inclined surface of the isosceles right-angle prism is coated with a reflective film.
[0086] Further, if Figure 2 As shown, the first reflection mechanism is further provided with a first lower apex 11a for supporting the first prism 10a, and the first prism 10a can rotate relative to the first lower apex 11a;
[0087] The second reflection mechanism is further provided with a second lower apex 11 b for supporting the second prism 10 b, and the second prism 10 b is rotatable relative to the second lower apex 11 b.
[0088] In the above technical solution, the prism is rotated by manually rotating the prism, thereby completing the adjustment of the prism angle, so that the camera 7 can better capture images.
[0089] Furthermore, Figure 2 , Figure 3 and Figure 8As shown, the first reflection mechanism is further provided with a first upper apex 9a for fixing the first prism 10a, and the first upper apex 9a and the first lower apex 11a are symmetrically arranged;
[0090] The second reflection mechanism is further provided with a second upper apex 9b for fixing the second prism 10b, and the second upper apex 9b and the second lower apex 11b are symmetrically arranged.
[0091] In the above technical solution, after the prism is manually rotated, the angle of the prism is fixed by using the upper apex; at the same time, the upper apex and the lower apex are symmetrically arranged, which is beneficial to the stability of the structure.
[0092] In this technical solution, if Figure 2-Figure 6 As shown, the clamp assembly includes: a first clamping plate 8 and a second clamping plate 16, the first clamping plate 8 and the second clamping plate 16 form a supporting space to support the sample 15;
[0093] The ends (front and rear ends) of the sample 15 located in the supporting space extend toward the upper platen 2a and the lower platen 2b, respectively.
[0094] In the above technical solution, the first clamping plate 8 and the second clamping plate 16 form a supporting space, which plays a role of lateral support and protection during the loading process of the upper pressure plate 2a and the lower pressure plate 2b; the ends of the sample 15 located in the supporting space extend in the direction of the upper pressure plate 2a and the direction of the lower pressure plate 2b respectively, that is, the head and tail ends of the sample 15 are both protruded relative to the supporting space, and the action force of the upper pressure plate 2a and the lower pressure plate 2b directly acts on the head and tail ends of the sample 15.
[0095] Further, such as Figure 4 and Figure 5 As shown, a V-shaped groove is provided on one side of the first clamping plate 8 and the second clamping plate 16 forming the supporting space.
[0096] In the above technical solution, V-shaped grooves are provided to prevent the sample 15 from contacting the first clamping plate 8 and the second clamping plate 16 in the supporting space when the sample 15 is compressed, thereby reducing the relative friction load between the sample 15 and the first clamping plate 8 and the second clamping plate 16.
[0097] Further, such as Figure 2 and Figure 3 As shown, the clamp assembly further includes: a base 14, a second clamping plate 16 vertically disposed on the base 14;
[0098] The first clamping plate 8 is provided with a first mounting hole, and the second clamping plate 16 is provided with a second mounting hole. The first mounting hole and the second mounting hole are arranged in a corresponding position so that the mounting member passes through the first mounting hole and the second mounting hole in sequence.
[0099] In the above technical solution, the first clamping plate 8 and the second clamping plate 16 are both in the shape of an "I", and the middle part of the first clamping plate 8 and the second clamping plate 16 forms a supporting space for placing the sample 15; preferably, circular threaded through holes (i.e., mounting holes) are provided at the four corners of the first clamping plate 8 and the second clamping plate 16, and the corresponding mounting parts pass through the corresponding threaded through holes in sequence to relatively fix the first clamping plate 8 and the second clamping plate 16; at the same time, the base 14 extends along the length direction, the upper pressure plate 2a acts on the upper end of the sample 15, the lower end of the sample 15 extends to the base 14, and the lower pressure plate 2b acts on the base 14. Preferably, a pad 13 can be provided between the base 14 and the lower end of the sample 15.
[0100] Further, such as Figure 2 and Figure 3 As shown, the first clamping plate 8 is provided with a first opening for collecting an image of the front side 15a, and the second clamping plate 16 is provided with a second opening for collecting an image of the back side 15b;
[0101] The first opening faces the first reflecting mechanism, and the second opening faces the second reflecting mechanism.
[0102] In the above technical solution, by setting the first opening and the second opening, the first reflecting mechanism and the second reflecting mechanism can reflect the image on the front side 15a and the image on the back side 15b. Preferably, the first reflecting mechanism and the second reflecting mechanism are both vertically arranged on the base 14, and the first opening, the second opening, the prism of the first reflecting mechanism and the prism of the second reflecting mechanism are all located on the same horizontal plane.
[0103] In this technical solution, if Figure 1 As shown, the analysis unit includes: a controller 5 and a computer 6;
[0104] The controller 5 is used to control the upper pressing plate 2 a and the lower pressing plate 2 b to compress the sample 15 , and transmit the collected load information to the computer 6 ; the image information of the camera 7 is transmitted to the computer 6 .
[0105] In the above technical solution, the compressive strength, compressive strain, compression modulus, compressive Poisson's ratio, offset compressive strength and failure strain of the sample 15 are obtained through the controller 5 and computer settings.
[0106] In this technical solution, if Figure 1 As shown, it also includes: a high and low temperature environment box 1;
[0107] The fixture unit 4 and the compression unit can both be placed in the high and low temperature environment box 1 , and the temperature during the test can be adjusted through the high and low temperature environment box 1 .
[0108] A method for testing a compression performance test system, such as Fig.11 As shown, the steps include:
[0109] In step S1, the sample 15 to be tested is placed in an atmospheric environment for state pretreatment to obtain a pretreated sample 15, wherein the atmospheric environment is (23±2)° C. and the relative humidity is (50±10)%.
[0110] In step S2, the value of the width w and the value of the thickness h of the section to be tested in the pre-treated sample 15 are measured;
[0111] In step S3, speckles are sprayed on the front surface 15a and the back surface 15b of the section to be measured. In the subsequent calculation and analysis, the compressive strain can be calculated using the virtual points of the first test point A, the second test point B, the third test point C and the fourth test point D; in addition, the first test point A and the second test point B are located on the same surface, and the third test point C and the fourth test point D are located on the same surface.
[0112] In step S4, the pretreated sample 15 is placed in a compression performance testing system to perform a compression performance testing operation;
[0113] The pretreated sample 15 is placed in a compression performance test system to perform a compression performance test. The operation includes:
[0114] In step S41, the pretreated sample 15 is clamped on the clamp assembly so that the section to be tested of the clamped pretreated sample 15 is at the same level as the first reflection mechanism and the second reflection mechanism of the compression performance test system;
[0115] In step S42, the fixture unit 4 and the compression unit are placed in the high and low temperature environment box 1, and the high and low temperature environment box 1 is adjusted according to different compression performance test temperature conditions so that the test environment temperature of the pretreated sample 15 reaches the corresponding compression performance test temperature condition;
[0116] In step S43, under the compression performance test temperature conditions, the compression performance parameters of the test section of the pretreated sample 15 are obtained through the compression performance test system; the compression performance parameters include at least any one of compression strain, compression Poisson's ratio, bending percentage, compression strength, compression modulus, offset compression strength and failure strain.
[0117] Preferably, S43 includes:
[0118] Under the compression performance test temperature conditions, the axial displacement values v of the first test point A of the test section of the sample 15 before and after the compression deformation are measured by the analysis unit. A , the axial displacement value v of the second test point B of the test section of sample 15 before and after compression deformation BUnder the compression performance test temperature conditions, the lateral displacement value v of the third test point C of the test section of the sample 15 before and after the compression deformation is measured by the analysis unit. C , the lateral displacement value v of the fourth test point D of the test section of sample 15 before and after compression deformation D ;
[0119] Measure the value of l0; the value of l0 is the axial distance between the first test point A and the second test point B before compression deformation; use Calculate the axial compressive strain ε 01 ;
[0120] Measurement CD The value of l CD The value of is the lateral distance between the third test point C and the fourth test point D before compression deformation; Calculate the transverse compressive strain ε 02 .
[0121] Furthermore, it also includes: measuring the axial strain value ε at the lowest point of the strain range of the measured segment x1 and the axial strain value ε at the highest point of the strain range of the measured section x2 ; The above mentioned values can be measured by the analysis unit;
[0122] Calculate the transverse strain value ε at the lowest point of the strain range of the measured section y1 and the transverse strain value ε at the highest point of the strain range of the measured section y2 ;
[0123] use Calculate is the compression Poisson's ratio.
[0124] In the above technical solution, the lowest point and the highest point are the values under ideal conditions. In some cases, the lowest point and the highest point can take the closest values, and ε x1 is 1000με, ε x2 It is 3000με.
[0125] Furthermore, S43 includes:
[0126] Under the compression performance test temperature conditions, measure the value of the front strain ε1 and the value of the back strain ε2; the above values can be measured by the analysis unit;
[0127] use Calculate the bending percentage By.
[0128] Furthermore, S43 includes:
[0129] Under the compression performance test temperature conditions, the maximum breaking load P of the tested section is detected by the analysis unit. m ;
[0130] use Calculate F c , F c is the compressive strength.
[0131] Furthermore, S43 includes:
[0132] Under the compression performance test temperature conditions, measure the axial strain value ε at the lowest point of the strain range of the tested section x1 and the axial strain value ε at the highest point of the strain range of the measured section x2 ; The above mentioned values can be measured by the analysis unit;
[0133] The load value P1 corresponding to the lowest point of the strain range of the section to be measured and the load value P2 corresponding to the highest point of the strain range of the section to be measured are measured by the analysis unit respectively;
[0134] use Calculate E c , E c is the compression modulus.
[0135] Furthermore, S43 includes:
[0136] Under the compressive performance test temperature condition, a compressive stress-compressive strain curve of the section to be tested is obtained, and based on the compressive stress-compressive strain curve, the compressive elastic modulus line of the section to be tested is translated from the origin to a fixed strain value, and the extended compressive elastic modulus line intersects with the compressive stress-compressive strain curve, and the intersection point is the offset compressive strength value of the section to be tested; and / or
[0137] Under the compression performance test temperature conditions, the section to be tested is brought into an instantaneous failure state, and the failure strain value of the section to be tested is measured.
[0138] The technical features mentioned above, the technical features to be mentioned below, and the technical features shown separately in the drawings can be combined with each other arbitrarily, as long as the combined technical features are not contradictory. All feasible feature combinations are technical contents clearly recorded in this article. Any of the multiple sub-features contained in the same sentence can be applied independently, and does not have to be applied together with other sub-features.
[0139] The present invention is further described below in conjunction with specific embodiments:
[0140] like Figure 1-Figure 9As shown, a compression performance testing system and testing method include a fixture unit 4, a compression unit, a collection unit and an analysis unit; wherein the electronic universal testing machine includes the compression unit.
[0141] The compression unit comprises: an upper pressing plate 2a and a lower pressing plate 2b; used to provide a compressive load to the sample 15 compressed by the composite laminate;
[0142] Clamp unit 4: The clamp unit 4 is used to provide lateral support and protection to the specimen 15 during the loading process; Figure 2 and Figure 3 The fixture as a whole is a "mountain" shaped structure, the overall structure is basically a mirror symmetrical structure, including a first splint 8 ( Figure 4 ), top 9( Figure 8 ), a first prism 10a and a second prism 10b, a first lower apex 11a and a second lower apex 11b, as Figure 7 The prism stand 12 (including the first prism stand 12a and the second prism stand 12b), the backing plate 13, the base 14 ( Figure 5 and Figure 6 ), composite compression specimen 15 ( Fig. 9 ) is installed in the fixture unit 4; the first clamping plate 8 is in an I-shaped shape as a whole, with a height of 73mm, a thickness of 15.8mm, a maximum width of 38.1mm, a width of 12.7mm in the middle, and circular through holes are set at the four corners of the "I" shape, with a hole diameter of 4.76mm, which can be fixed to the base 14 by bolts; a 10mm×10mm rectangular through hole (i.e., the first opening) is set in the center of the first clamping plate 8; the prism stand 12 is in a Z-shaped shape as a whole, with a through hole set at the top for installing the upper apex, and a rectangular groove above for installing the total reflection prism; a lower apex is set on the lower surface of the rectangular groove. A top cap with vertical stripes is set at the top of the upper apex, which can increase the friction when rotating. The total reflection prism is installed in the rectangular groove of the prism stand through the upper and lower apex pressing. The bottom of the prism stand is provided with a T-shaped nose with a hole for connecting with the base 14; the base 14 is a T-shaped structure as a whole, with a protruding second clamping plate 16 at the center of the base crossbeam, and the second clamping plate 16 has a protruding I-shaped structure to support the back plate, and circular threaded through holes are provided at the four corners of the "I" shape. The inner surface of the second clamping plate 16 is provided with a V-shaped groove, and a 10mm×10mm rectangular through hole (i.e., the second opening) is provided at the center. The first clamping plate 8 can be fixed to the second clamping plate 16 of the base 14 by bolts passing through the threaded holes at the four corners. Two threaded countersunk holes are provided at the center of the base 14 near the second clamping plate 16, and the pad 13 is fixed to the base by countersunk bolts. The width of the pad 13 is the same as the width of the base crossbeam, and the length is about 50mm. The pad 13 can be replaced after being worn. T-shaped grooves are arranged on both sides of the base crossbeam, and the T-shaped nose with a hole at the bottom of the prism stand can be embedded in the T-shaped grooves to adjust the relative position by sliding, and can be fixed by bolts.
[0143] The acquisition unit includes: a camera 7 (the camera 7 also includes a lens) and an electronic universal testing machine, a first light source 3a, a second light source 3b and other optical accessories;
[0144] The analysis unit includes: a controller 5 and a computer 6. The controller 5 is connected to the electronic universal testing machine and the computer 6. The controller 5 controls the electronic universal testing machine, collects load information and transmits it to the computer 6. At the same time, the image information collected by the image acquisition unit is transmitted to the computer, and the deformation information is obtained by analysis and calculation. The stress-strain curve is obtained by the analysis software, and the material strength, modulus, Poisson's ratio, failure strain and other data are calculated.
[0145] In this scheme, the sample 15 is 80 mm long, 12-15 mm wide, with a target thickness of about 1 mm. The actual thickness depends on the number of composite material layers and the thickness of a single layer. Reinforcement sheets are attached to both ends, and the working section length is 4.75 mm. Before the test, speckles are prepared on the front and back sides of the working section of the sample.
[0146] Embodiment 1:
[0147] Use Figure 1 The system shown is used to test the room temperature compression properties of composite laminates.
[0148] 1. Sample pretreatment: Before testing, place the sample to be tested 15 in an atmosphere of (23±2)℃ and relative humidity of (50±10)% for 24 hours for state conditioning. At least 5 samples should be tested for each test condition, unless valid results can be obtained using fewer samples;
[0149] 2. Dimension measurement: measure the width w and thickness h of each sample 15 to be tested and record the dimension information;
[0150] 3. Speckle preparation: First, the reinforcement area of sample 15 was protected with paper tape, and then the front and back of the working section of the sample were wiped with anhydrous ethanol. Then, a thin layer of primer was evenly sprayed on the front and back surfaces of the sample using white spray paint. After about 5 minutes, black spray paint was used to spray randomly distributed speckle marking points on the front and back surfaces of the sample.
[0151] 4. Clamping of sample 15 and adjustment of fixture: Adjust the composite material fixture unit 4 according to Figure 2Assemble as shown, install the sample 15 to be tested between the first clamping plate 8 and the second clamping plate 16, and place the bottom of the sample 15 flatly on the pad 13, in contact with the upper surface of the pad 13. The center of the working section of the sample 15, the center of the first opening, the center of the second opening, and the center of the total reflection prism are all on a horizontal line at the same height, so that the sample 15 is in the center of the fixture unit 4. Tighten the bolts on each end of the fixture unit 4 in a diagonal manner, tighten the bolts on the clamping plate to 0.7~1.0J, or tighten the bolts with a tightening torque of 1N·m, so that the first clamping plate 8 and the second clamping plate 16 are close to the surface of the sample 15. Adjust the relative position of the total reflection prism and the prism stand so that the speckle pattern on the front and back sides of the working section of the sample 15 is reflected to the same image plane through the reflection of the two total reflection prisms.
[0152] 5. Adjustment of the acquisition unit and analysis unit: Preheat the camera, and quickly fine-tune the position, aperture size, and light source intensity of the camera 7 so that the working section of the tested sample 15 can be clearly and completely presented in the center of the collected image. Arrange the video extensometer marking points based on the Digital Image Correlation (DIC) method in the working section of the sample 15. Adjust the controller 5 to set the data acquisition frequency and data transmission method.
[0153] 6. Loading and data recording: Manually preload a certain load and then unload it to minimize the gap between the electronic universal testing machine and the fixture. Then apply a compressive load to the sample 15 at a fixed rate of 1mm / min to 1.3mm / min, and synchronously trigger the image and data acquisition system through control 5 to collect images. At the same time, the load information recorded by the electronic universal testing machine is synchronously input into the digital image correlation algorithm analysis software installed in the computer, and combined with the strain information measured by the video extensometer to draw the stress-strain curve in real time; continue to load until the specimen is destroyed, and record the time, load, deformation and other information.
[0154] 7. Test validity judgment: observe and record the failure mode of each specimen 15, and judge the validity of the test based on the failure mode: if the specimen 15 fails within the working section and there is no obvious defect at the failure site, it is a valid test; if the failure occurs at an obvious defect, or the end of the specimen 15 is crushed, it is considered an invalid test. Combined with the picture and stress-strain curve, if the above abnormal phenomenon occurs after the elastic deformation of the specimen 15, the elastic modulus test result is valid.
[0155] The bending percentage can be calculated by the following formula. For valid test results, the bending percentage should not be greater than 10%. Otherwise, it is invalid data.
[0156] Where ε1 is the positive strain of sample 15; ε2 is the negative strain of sample 15.
[0157] 8. Calculation of results:
[0158] The compressive strength of composite laminates is calculated by the following formula:
[0159] Where F c is the compressive strength of the laminate, MPa; P m is the maximum destructive load, N, measured by an electronic universal testing machine; w is the width of the working section of sample 15, mm; h is the thickness of the working section of sample 15, mm.
[0160] The axial or transverse compressive strain measured by an optical extensometer is:
[0161] Where v A and v B is the image displacement of points A and B in the axial or lateral direction in the compression direction in the collected working section speckle pattern of sample 15, and the unit of measurement is mm; l0 is the image distance between points A and B before compression deformation, and the unit of measurement is mm, that is, the original gauge length of the optical extensometer.
[0162] Calculate the compression modulus using the formula: Where E c is the compression modulus, measured in MPa; P1 is ε x1 The load at P2 is ε x2 The load at the point is measured in N; ε x1 is the actual strain value closest to the lowest point in the strain range, usually 1000με; x2 The actual strain value closest to the highest point of the strain range is usually 3000με.
[0163] Calculate the compression Poisson's ratio using the formula, In the formula The compression Poisson’s ratio is calculated by measuring the two ε x (Right now x1 and x2 ) Transverse strain ε at the end of the strain range y .
[0164] The offset compressive strength is determined from the compressive stress-compressive strain curve. The compressive elastic modulus line is translated from the origin to a fixed strain value, and the line is extended to intersect the stress-strain curve. The compressive stress at the intersection is taken as the offset compressive strength. The offset strain value is usually 0.2%.
[0165] The strain of the sample 15 at the moment of failure or as close to the moment of failure as possible is obtained by measurement, which is the failure strain.
[0166] Finally, the mean value, standard deviation and coefficient of dispersion of the test results are calculated. The above results are all retained to 3 significant figures.
[0167] Embodiment 2:
[0168] Use Figure 1 The system shown is used to test the high temperature compression properties of composite laminates.
[0169] The surface speckle of the sample 15 needs to be prepared by high temperature resistant spray paint. A high and low temperature environment box 1 is added, and an observation window is provided on the front of the high and low temperature environment box 1. The observation window glass is usually made of high temperature resistant quartz glass. The high and low temperature environment box 1 is connected to the test machine. During the test, the upper and lower pressure plates and the fixture unit 4 are placed in the high and low temperature environment box 1. The light source in the acquisition unit uses a blue light or a purple light source, and a narrow bandpass filter is configured in front of the lens.
[0170] The specific steps are as follows:
[0171] 1. Pretreatment of sample 15: Before testing, place the sample 15 to be tested in an atmosphere of (23±2)℃ and relative humidity of (50±10)% for 24 hours for state conditioning. At least 5 samples 15 should be tested for each test condition, unless valid results can be obtained using fewer samples 15. If the sample 15 needs moisture absorption or water immersion treatment, relevant treatment needs to be performed before the test.
[0172] 2. Dimension measurement: Measure the width and thickness of each test sample 15 and record them.
[0173] 3. Speckle preparation: First, the reinforcement area of the sample 15 was protected with paper tape, and then the front and back of the working section area of the sample 15 were wiped with anhydrous ethanol. Then, a thin layer of primer was evenly sprayed on the front and back surfaces of the sample 15 using white high-temperature resistant spray paint. After about 5 minutes, high-temperature resistant black spray paint was used to spray randomly distributed speckle marking points on the front and back surfaces of the sample 15.
[0174] 4. Clamping of sample 15 and adjustment of fixture: High temperature test requires the use of high and low temperature environment box 1 for testing. High and low temperature environment box 1 is connected to the electronic universal testing machine. The upper and lower pressure plates and fixture unit 4 are placed in the high and low temperature environment box 1. The front of the environment box is equipped with an observation window. The observation window glass is usually made of high temperature resistant quartz glass. Before the test, preheat the environment box and fixture unit 4 to the required test temperature and keep it warm for 30 minutes. Fix the fixture unit 4 according to Figure 2Assemble as shown, after the sample 15 to be tested is installed, the center of the working section of the sample 15, the center of the first opening, the center of the second opening and the center of the total reflection prism are all on a horizontal line at the same height, so that the sample 15 is in the center of the fixture unit. Tighten the bolts on each end of the fixture in a diagonal manner, tighten the bolts on the clamp to 0.7-1.0J, or tighten the bolts with a tightening torque of 1N·m, so that the first clamp 8 and the second clamp 16 are close to the surface of the sample 15. Adjust the relative position of the total reflection prism and the prism stand so that the speckle pattern on the front and back sides of the working section of the sample 15 is reflected to the same image plane through the reflection of the two total reflection prisms.
[0175] 5. Adjustment of the acquisition unit and analysis unit: For high temperature tests, the light source in the acquisition unit is selected to be a blue light or a purple light source, and a narrow bandpass filter is configured in front of the lens. Preheat the camera, and quickly fine-tune the camera position, aperture size, and light source intensity, so that the working section area of the tested sample 15 can be collected by the acquisition unit through the observation window glass, and presented clearly and completely in the center of the collected image. Arrange the video extensometer marking points based on the Digital Image Correlation (DIC) method in the working section of the sample 15; adjust the controller 5 to set the data acquisition frequency and data transmission method.
[0176] 6. Loading and data recording: Before loading, the temperature of the sample 15 is raised to the temperature to be tested, and the test is started after the high temperature dry state is kept for 5 minutes. The test is started after the high temperature wet state is kept for 2 minutes. It should be noted that during the preheating stage of the sample 15, the fan power in the high and low temperature environment box 1 is increased to make the temperature in the high and low temperature environment box 1 quickly reach uniformity. When the test is started, the fan power is reduced to ensure uniform temperature, reduce the disturbance effect of hot air, and reduce the vibration of the high and low temperature environment box 1. First, manually preload a certain load and then unload it to minimize the gap between the electronic universal testing machine and the fixture. Then, a compressive load is applied to the sample 15 at a fixed rate of 1mm / min to 1.3mm / min, and the image and data acquisition system is synchronously triggered by the controller 5 to collect images. At the same time, the load information recorded by the electronic universal testing machine is synchronously input into the digital image correlation algorithm analysis software installed in the computer, and the stress-strain curve is drawn in real time in combination with the strain information measured by the video extensometer. Continuous loading until the specimen is destroyed. Record time, load, deformation and other information.
[0177] Among them, the test validity judgment and result calculation are the same as those of the room temperature test.
[0178] Embodiment three:
[0179] Use Figure 1 The system shown is used to test the low temperature compression properties of composite laminates.
[0180] The surface speckle of the sample 15 needs to be prepared with a low-temperature resistant coating. A high and low temperature environment box 1 is added, which is cooled by liquid nitrogen or a compressor, and a desiccant is placed for drying. The front of the high and low temperature environment box 1 is equipped with an observation window. The observation window glass is usually made of quartz glass and is equipped with a heating and defrosting device. The high and low temperature environment box 1 is connected to the test machine. During the test, the upper and lower pressure plates and the fixture unit 4 are placed in the high and low temperature environment box 1. The light source in the acquisition unit uses a blue light or a purple light source, and a narrow bandpass filter is configured in front of the lens.
[0181] The specific steps are as follows:
[0182] 1. Pretreatment of sample 15: Before testing, place the sample 15 to be tested in an atmosphere of (23±2)℃ and relative humidity of (50±10)% for 24 hours for state conditioning. At least 5 samples 15 should be tested for each test condition, unless valid results can be obtained using fewer samples 15.
[0183] 2. Dimension measurement: Measure the width and thickness of each test sample 15 and record them.
[0184] 3. Speckle preparation: First, the reinforcement area of the sample 15 is protected with paper tape, and then the front and back of the working section area of the sample 15 are wiped with anhydrous ethanol. Then, a thin layer of primer is evenly sprayed on the front and back surfaces of the sample 15 using white low-temperature resistant paint. After about 5 minutes, use black low-temperature resistant paint to spray randomly distributed speckle marking points on the front and back surfaces of the sample 15.
[0185] 4. Clamping of sample 15 and adjustment of fixture: High temperature test needs to be carried out in high and low temperature environment box 1. High and low temperature environment box 1 is connected to the electronic universal testing machine. The upper and lower pressure plates and fixture unit are placed in the high and low temperature environment box 1. The front of the environment box is equipped with an observation window. The observation window glass is usually made of quartz glass. Before the test, precool the environment box and fixture unit to the required test temperature and keep it warm for 30 minutes. Fix the fixture unit 4 according to Figure 2 Assemble as shown, the bottom of sample 15 is placed flat on the pad 13 and contacts the upper surface of pad 13. The center of the working section of sample 15, the center of the first opening, the center of the second opening and the center of the total reflection prism are all on a horizontal line at the same height, so that sample 15 is in the center of the fixture unit. Tighten the bolts on each end of the fixture in a diagonal manner, tighten the bolts on the clamp to 0.7~1.0J, or tighten the bolts with a tightening torque of 1N·m, so that the clamp of sample 15 and the base support back plate are against sample 15. Adjust the relative position of the total reflection prism and the prism stand so that the speckle pattern on the front and back sides of the working section of sample 15 is reflected to the same image plane through the reflection of the two total reflection prisms.
[0186] 5. Adjustment of the acquisition unit and analysis unit: Preheat the camera and quickly fine-tune the camera position, aperture size, and light source intensity so that the working section area of the tested sample 15 can be collected by the acquisition unit through the observation window glass and presented clearly and completely in the center of the collected image. Arrange the video extensometer marking points based on the Digital Image Correlation (DIC) method in the working section of the sample 15. Adjust the control unit to set the data acquisition frequency and data transmission method.
[0187] 6. Loading and data recording: Before loading, the temperature of sample 15 is lowered to the temperature to be tested, and the test is started after keeping warm for 5 minutes. It should be noted that during the pre-cooling stage of sample 15, the fan power in the high and low temperature environment box 1 is increased to make the temperature in the high and low temperature environment box 1 quickly reach uniformity. When the test starts, the fan power is reduced to ensure uniform temperature, reduce the air disturbance effect, and reduce the vibration of the high and low temperature environment box 1. First, manually preload a certain load and then unload it to minimize the gap between the electronic universal testing machine and the fixture. Then, a compressive load is applied to sample 15 at a fixed rate of 1mm / min to 1.3mm / min. The image and data acquisition system is synchronously triggered by the controller to collect images. At the same time, the load information recorded by the electronic universal testing machine is synchronously input into the digital image correlation algorithm analysis software installed in the computer, and the stress-strain curve is drawn in real time in combination with the strain information measured by the video extensometer. Continuous loading until the specimen is destroyed. Record time, load, deformation and other information.
[0188] Among them, the test validity judgment and result calculation are the same as those of the room temperature test.
[0189] Technical effects of the present invention:
[0190] The system of the present invention has a compact structure, high space utilization, convenient use, easy operation, low cost, reliability and durability. Aiming at the shortcomings of the existing non-contact composite material compression performance test system, a special compression fixture (i.e., fixture unit 4) is designed for matching use. The fixture is cleverly designed and highly applicable. It can be used in different test environments, and different parts can be flexibly adjusted according to different materials, sample sizes and working conditions. The parameters are controllable and the operation is simple and easy. The entire system and method are also sufficient to meet the requirements of the corresponding test standard method for composite laminates.
[0191] Compared with the existing traditional test systems and test methods, the composite laminate compression performance test system and method of use based on a single camera and end loading method can obtain multiple parameters such as compression strength, compression elastic modulus, compression Poisson's ratio and compression failure strain through the same sample. The strain information on both sides of the sample can be accurately obtained only through a single camera, which lays the foundation for the accurate processing of compression performance data, test process monitoring and test result validity judgment, saving manpower and material costs. Furthermore, the problem of compression performance testing under high temperature and high humidity environment is solved through non-contact methods, which can provide data and technical support for material research and development and composite material structure design.
[0192] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0193] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A compression performance testing system, It is characterized in that include: A clamp unit (4), a compression unit, a collection unit and an analysis unit; The clamp unit (4) comprises: a first reflection mechanism, a second reflection mechanism and a clamp assembly; The clamp assembly is used to support the sample (15); the first reflection mechanism is arranged on the front side (15a) of the sample (15) and is used to reflect the image of the front side (15a) of the sample (15); the second reflection mechanism is arranged on the back side (15b) of the sample (15) and is used to reflect the image of the back side (15b) of the sample (15); The compression unit comprises: an upper pressing plate (2a) and a lower pressing plate (2b) arranged opposite to each other, wherein the upper pressing plate (2a) and the lower pressing plate (2b) form a compression space to compress the sample (15); The acquisition unit comprises: a camera (7), the camera (7) being located on a reflection path of the first reflection mechanism and a reflection path of the second reflection mechanism, and being used for acquiring images of the front side (15a) and the back side (15b) of the sample (15), and the camera (7) being connected to the analysis unit.
2. The compression performance testing system according to claim 1, It is characterized in that The first reflecting mechanism is provided with a first prism (10a) for reflecting the image of the front side (15a); The second reflecting mechanism is provided with a second prism (10b) for reflecting the image of the reverse surface (15b).
3. The compression performance testing system according to claim 2, It is characterized in that The first reflection mechanism is also provided with a first lower apex (11a) for supporting the first prism (10a), and the first prism (10a) is capable of rotating relative to the first lower apex (11a); The second reflection mechanism is also provided with a second lower apex (11b) for supporting the second prism (10b), and the second prism (10b) is capable of rotating relative to the second lower apex (11b).
4. The compression performance testing system according to claim 3, It is characterized in that The first reflection mechanism is also provided with a first upper top (9a) for fixing the first prism (10a), and the first upper top (9a) and the first lower top (11a) are symmetrically arranged; The second reflection mechanism is also provided with a second upper top (9b) for fixing the second prism (10b), and the second upper top (9b) and the second lower top (11b) are symmetrically arranged.
5. The compression performance testing system according to claim 1, It is characterized in that The clamp assembly comprises: a first clamping plate (8) and a second clamping plate (16), wherein the first clamping plate (8) and the second clamping plate (16) form a supporting space to support the sample (15); The ends of the sample (15) located in the supporting space extend toward the upper pressing plate (2a) and the lower pressing plate (2b) respectively.
6. The compression performance testing system according to claim 5, It is characterized in that A V-shaped groove is provided on one side of the first clamping plate (8) and the second clamping plate (16) forming the supporting space.
7. The compression performance testing system according to claim 5, It is characterized in that The clamp assembly further comprises: a base (14), wherein the second clamping plate (16) is vertically arranged on the base (14); The first clamping plate (8) is provided with a first mounting hole, and the second clamping plate (16) is provided with a second mounting hole. The first mounting hole and the second mounting hole are arranged in a corresponding position so that the mounting member passes through the first mounting hole and the second mounting hole in sequence.
8. The compression performance testing system according to claim 5, It is characterized in that The first clamping plate (8) is provided with a first opening for collecting the image of the front side (15a), and the second clamping plate (16) is provided with a second opening for collecting the image of the back side (15b); The first opening faces the first reflecting mechanism, and the second opening faces the second reflecting mechanism.
9. The compression performance testing system according to claim 1, It is characterized in that The analysis unit comprises: a controller (5) and a computer (6); The controller (5) is used to control the upper pressing plate (2a) and the lower pressing plate (2b) to compress the sample (15) and transmit the collected load information to the computer; the image information of the camera (7) is transmitted to the computer (6).
10. The compression performance testing system according to claim 1, It is characterized in that Also includes: High and low temperature environment chamber (1); The clamp unit (4) and the compression unit can both be placed in the high and low temperature environment box (1).
11. A method for testing a compression performance testing system, It is characterized in that The compression performance testing system according to any one of claims 1 to 10 comprises the following steps: S1, placing the sample (15) to be tested in an atmospheric environment for state pretreatment to obtain a pretreated sample (15); S2, measuring the value of the width w and the value of the thickness h of the section to be tested in the pretreated sample (15); S3, spraying speckles on the front side (15a) and the back side (15b) of the section to be tested; S4, placing the pretreated sample (15) in the compression performance testing system to perform a compression performance testing operation; The operation of placing the pretreated sample (15) in the compression performance testing system for compression performance testing comprises: S41: clamping the pretreated sample (15) on the clamp assembly so that the section to be tested of the clamped pretreated sample (15) and the first reflection mechanism and the second reflection mechanism of the compression performance testing system are at the same level; S42, placing the fixture unit (4) and the compression unit in a high and low temperature environment box (1), and adjusting the high and low temperature environment box (1) according to different compression performance test temperature conditions, so that the test environment temperature of the pretreated sample (15) reaches the corresponding compression performance test temperature condition; S43. Under the compression performance test temperature conditions, the compression performance parameters of the test section of the pretreated sample (15) are obtained through the compression performance test system; the compression performance parameters include at least any one of compression strength, compression strain, compression modulus, compression Poisson's ratio, offset compression strength, bending percentage and failure strain.
12. The test method according to claim 11, It is characterized in that The S43 includes: Under the compression performance test temperature conditions, the axial displacement values v of the first test point (A) of the test section of the sample (15) before and after the compression deformation are respectively measured by the analysis unit. A , the axial displacement value v of the second test point (B) of the test section of the sample (15) before and after compression deformation B Under the compression performance test temperature conditions, the lateral displacement value v of the third test point (C) of the test section of the sample (15) before and after the compression deformation is measured by the analysis unit. C , the lateral displacement value v of the fourth test point (D) of the test section of the sample (15) before and after compression deformation D ; Measurement 0 The value of l 0 The value of is the axial distance between the first test point (A) and the second test point (B) before compression deformation; using Calculate the axial compressive strain ε 01 ; Measurement CD The value of l CD The value of is the lateral distance between the third test point (C) and the fourth test point (D) before compression deformation; using Calculate the transverse compressive strain ε 02 .
13. The test method according to claim 12, It is characterized in that Also includes: Measure the axial strain value ε at the lowest point of the strain range of the measured section respectively x1 and the axial strain value ε at the highest point of the strain range of the measured section x2 ; Calculate the transverse strain value ε at the lowest point of the strain range of the measured segment y1 and the transverse strain value ε at the highest point of the strain range of the measured section y2 ; use Calculate Said is the compression Poisson's ratio.
14. The testing method according to claim 11, It is characterized in that The S43 includes: Under the compression test temperature conditions, the front strain ε is measured. 1 The value of the reverse strain ε 2 The value of use Calculate the bending percentage B y .
15. The testing method according to claim 11, It is characterized in that The S43 includes: Under the compression performance test temperature conditions, the maximum breaking load P of the tested section is detected by the analysis unit. m ; use Calculate F c , the F c For the compressive strength.
16. The testing method according to claim 11, It is characterized in that The S43 includes: Under the compression performance test temperature conditions, the axial strain value ε at the lowest point of the strain range of the section to be tested is measured respectively. x1 and the axial strain value ε at the highest point of the strain range of the measured segment x2 ; The load value P corresponding to the lowest point of the strain range of the measured segment is measured by the analysis unit. 1 The load value P corresponding to the highest point of the strain range of the measured segment 2 ; use Calculate E c , the E c is the compression modulus.
17. The testing method according to claim 11, It is characterized in that The S43 includes: Under the compression performance test temperature condition, a compression stress-compression strain curve of the section to be tested is obtained, and based on the compression stress-compression strain curve, the compression elastic modulus line of the section to be tested is translated from the origin to a fixed strain value, and the compression elastic modulus line is extended to intersect with the compression stress-compression strain curve, and the intersection point is the offset compression strength value of the section to be tested; and / or Under the compression performance test temperature condition, the section to be tested is brought into an instantaneous failure state, and the failure strain value of the section to be tested is measured.
Citation Information
Patent Citations
Non-contact crack opening displacement measuring device and method for bending fracture test
CN110174315A
High-low temperature hydraulic large-load compression test system for composite material
CN112378778A
Columnar rhizome Poisson's ratio measurement system and method based on image processing
CN117740527A