Optimal selection method for high-flux simulated accelerated corrosion test of steel in marine atmospheric environment
By designing orthogonal test tables and multi-factor coupling comprehensive tests, calculating the gray correlation degree, selecting the optimal test plan, and simulating the humidity, heat and irradiation conditions in the marine atmospheric environment, the problem of large differences between the existing simulated accelerated test methods and the actual environment has been solved. problem, improve the efficiency and accuracy of the test, and ensure the validity of the test data.
Patent Information
- Application Number
- CN202410903177.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-08
AI Technical Summary
The existing simulated accelerated test methods are greatly different from the actual marine atmospheric environment, resulting in low correlation and reliability of the corrosion test results of carbon steel and low alloy steel. It is difficult to quickly determine the optimal accelerated corrosion test conditions, and the test efficiency and accuracy are insufficient. .
Design an optimization method for high-throughput simulated accelerated corrosion testing of steel in the marine atmospheric environment. By selecting key environmental factors, designing an orthogonal test table, conducting multi-factor coupling comprehensive tests, calculating gray correlation degrees, selecting the optimal test plan, and simulating heat and humidity , alternating steps of irradiation and dry-wet cycles to reduce test iterations and improve efficiency.
It improves the relevance and accuracy of test data, reduces test complexity and cost, ensures the validity and feasibility of test data, and can quickly determine the optimal accelerated corrosion test conditions.
Smart Images

Figure CN118746536A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of simulation tests, and in particular to an optimization method for a high-throughput simulated accelerated corrosion test of steel in a marine atmospheric environment. Background Art
[0002] Carbon steel and low alloy steel have been widely used in marine engineering structures due to their easy availability and low cost. However, these materials face severe corrosion challenges in the marine atmospheric environment, especially factors such as high chloride ion concentration, high humidity and strong radiation, which make these materials susceptible to severe corrosion, thus affecting the safety and durability of the project.
[0003] At present, the simulated accelerated test methods used to evaluate the marine atmospheric corrosion performance of carbon steel and low alloy steel mainly include salt spray test, wet heat test, high and low temperature alternating test and cyclic immersion test. This simplified simulation method is significantly different from the actual complex marine atmospheric environment, resulting in a low correlation between the accelerated corrosion test results and the corrosion data in the actual environment, and the representativeness and credibility of the test data are questioned.
[0004] In order to simulate the marine atmospheric environment more realistically and improve the relevance of test data, a method for optimizing the high-throughput simulated accelerated corrosion test of steel in the marine atmospheric environment was invented. The method can achieve the coupling of key environmental conditions such as damp heat, irradiation, and immersion, and can quickly determine the optimal accelerated corrosion test conditions for a specific marine atmospheric environment without the need for a large number of test iterations, thereby improving the test efficiency and accuracy. Summary of the invention
[0005] The purpose of the present invention is to provide an optimal method for a high-throughput simulated accelerated corrosion test of steel in a marine atmospheric environment to overcome the deficiencies in the background technology.
[0006] The object of the present invention can be achieved by the following technical scheme: A method for optimizing a high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment, comprising:
[0007] Select key environmental factors in the marine atmospheric environment of the target area;
[0008] Set three levels for each key environmental factor and design an orthogonal test table with four factors and three levels for accelerated corrosion of carbon steel; design nine groups of accelerated corrosion test schemes based on the orthogonal test table;
[0009] According to nine sets of accelerated corrosion test schemes, accelerated corrosion tests were carried out in a multi-factor coupling comprehensive test chamber;
[0010] Obtain weight loss data of accelerated corrosion test, calculate corrosion thickness loss of carbon steel in different cycles, and obtain corrosion thickness loss data; Based on the obtained corrosion thickness loss data, calculate the grey correlation between the accelerated corrosion test designed by orthogonal experiment and the actual marine atmosphere exposure test;
[0011] By comparing the grey correlation of nine groups of accelerated corrosion test schemes designed by orthogonal experiment, the test scheme with the highest grey correlation was selected as the optimal test scheme for accelerated corrosion in marine atmosphere in the target area.
[0012] Furthermore, the target area is the regional marine atmospheric environment simulated in the experiment; key environmental factors include chloride ion concentration, temperature, humidity, and radiation intensity.
[0013] Further, the method to obtain the three levels of each key environmental factor is as follows:
[0014] A single test parameter of the key environmental factor is selected based on the annual average value of the marine atmospheric environment in the target area. The selected single test parameter is taken at one level in the positive direction and one level in the reverse direction respectively, and three different levels are set under each key environmental factor.
[0015] Furthermore, the method for designing nine sets of accelerated corrosion test schemes is as follows:
[0016] Through the orthogonal test table, a four-factor three-level orthogonal test was designed, and nine groups of accelerated corrosion test schemes were screened out after combining four factors at three levels through the least experimental combinations.
[0017] Furthermore, according to the nine sets of accelerated test schemes designed according to the orthogonal test table, accelerated corrosion tests were carried out in a multi-factor coupling comprehensive test chamber, the accelerated corrosion test cycle was defined, and the corrosion conditions of carbon steel were observed and recorded; the accelerated corrosion test was divided into three steps, each step was independent of each other, and one step would automatically enter the next step after completion; the accelerated corrosion test cycles were set to 1d, 2d, 4d, and 8d as days, respectively.
[0018] Furthermore, specific accelerated corrosion tests include:
[0019] The first step is a wet heat step, which lasts for 8 hours. This step controls the temperature and humidity in the equipment to achieve the control of temperature and humidity in the test plan.
[0020] The second step is the illumination step, which lasts for 8 hours. In this step, the irradiation intensity is controlled by a xenon lamp installed in the equipment to achieve the control of the irradiation intensity in the test plan;
[0021] The third step is a dry-wet cycle alternation step, which lasts for 8 hours, with one cycle lasting 1 hour, and a total of 8 cycles. This step controls the chloride ion concentration in the test scheme by preparing soaking solutions with different pollutant concentrations.
[0022] The soaking time in one cycle is 12 minutes, and the drying time is 48 minutes. During the drying period, the temperature and humidity settings are the same as in the first step. At the same time, when preparing soaking solutions with different chloride ion concentrations, 0.01 mol / L NaHSO3 solution is added to simulate a small amount of SO2 gas in the atmosphere.
[0023] Repeat the accelerated corrosion test periodically according to the above steps to simulate long-term environmental exposure.
[0024] Furthermore, after the predetermined accelerated corrosion test cycle is completed, the sample is taken out from the test box and its macroscopic morphology is recorded using a camera; wherein three parallel samples are set under each test condition;
[0025] Immerse the sample in a pickling solution, control the temperature at 20-25°C, and set the initial time to 10 minutes; the pickling solution is prepared by 500ml of distilled water + 500ml of hydrochloric acid + 3.5g of hexamethylenetetramine;
[0026] Among them, if the corrosion products are not cleaned up, the pickling time can be extended until they are cleaned up;
[0027] After pickling, each sample was weighed and the weight of each sample was recorded to obtain the weight loss data of the accelerated corrosion test, including the original weight of the carbon steel and the weight after pickling;
[0028] Calculate the corrosion thickness loss of carbon steel in different cycles and obtain the corrosion thickness loss data of carbon steel in different cycles;
[0029] The calculation formula is:
[0030]
[0031] Wherein, M1 represents the original weight of carbon steel, M2 represents the weight of carbon steel after pickling, ρ represents the density of carbon steel, S represents the surface area of carbon steel exposed to the corrosive environment, and D represents the corrosion thickness loss of carbon steel.
[0032] Furthermore, the method for obtaining the grey correlation coefficient and grey correlation degree of the accelerated corrosion loss of carbon steel in orthogonal test design and the actual marine atmospheric corrosion loss is as follows:
[0033] According to the corrosion loss data obtained, the accelerated corrosion loss of carbon steel in the orthogonal test design was taken as a subsequence, and the test period was 1d, 2d, 4d, and 8d. The corrosion loss of carbon steel in the actual marine atmosphere in the target area for 30d, 60d, 120d, and 240d was taken as the parent sequence.
[0034] The subsequence and the parent sequence are dimensionless respectively;
[0035] The calculation formula is:
[0036]
[0037] In the formula, Y0 represents the dimensionless treatment of corrosion loss in actual marine atmosphere, Y i represents the dimensionless treatment of the accelerated corrosion thickness loss of orthogonal test design, i represents nine groups of accelerated corrosion test schemes, i = 1, 2, ..., 9; k represents four cycles, k = 1, 2, 3, 4; X0(k) represents the corrosion thickness loss in the actual marine atmosphere, X i (k) represents the accelerated corrosion loss of orthogonal test design;
[0038] Calculate the absolute difference series of corrosion loss between the accelerated corrosion of carbon steel in orthogonal test design and the actual marine atmospheric corrosion after dimensionless treatment;
[0039] The calculation formula is:
[0040] Δ 0i =|Y0(k)-Y i (k)|;
[0041] In the formula, Δ 0i is the absolute difference sequence, Y0(k) represents the dimensionless corrosion loss sequence of actual marine atmospheric corrosion, and Y i (k) represents the accelerated corrosion loss sequence after dimensionless processing for the orthogonal design;
[0042] Calculate the grey correlation coefficient and grey correlation degree of the accelerated corrosion loss of carbon steel in orthogonal test design and the actual marine atmospheric corrosion loss;
[0043] The calculation formula is:
[0044]
[0045] In the formula, ζ 0i (k) is the grey correlation coefficient, γ 0i is the grey relational degree, θ is the resolution coefficient, 0<θ<1, It represents the minimum absolute difference of corrosion thickness loss in the accelerated corrosion test of the orthogonal experimental design after dimensionless processing; It represents the maximum absolute difference of corrosion thickness loss in the accelerated corrosion test of the orthogonal experimental design after dimensionless processing.
[0046] Furthermore, the grey correlation degrees of the nine groups of accelerated corrosion test schemes in orthogonal experimental design were compared, and a grey correlation diagram of the nine groups of accelerated corrosion test schemes was drawn; the test scheme with the highest grey correlation degree was selected as the optimal test scheme for accelerated corrosion of marine atmosphere in the target area; wherein the horizontal axis represents nine different test schemes, and the vertical axis represents the value of the grey correlation degree.
[0047] Compared with the existing solutions, the present invention achieves the following beneficial effects:
[0048] The present invention selects key environmental factors in the marine atmospheric environment of the target area, sets three levels for each key environmental factor, designs an orthogonal test table, and designs nine groups of accelerated corrosion test schemes based on the orthogonal test table, which is conducive to the test scheme being closer to the corrosion conditions in the actual marine atmospheric environment and improving the accuracy and efficiency of the test;
[0049] The present invention simulates the corrosion environment in the actual marine atmosphere environment by designing a wet heat step, an illumination step, and a dry-wet cycle alternating step, and determining the test parameters according to actual environmental factors, so as to make the accelerated corrosion mechanism of carbon steel as consistent as possible with the corrosion mechanism in the actual marine atmosphere, effectively reducing the complexity and cost of the test, while ensuring the adequacy and effectiveness of the test data; calculating the grey correlation between the accelerated corrosion test designed by the orthogonal experiment and the actual marine atmosphere exposure test is conducive to evaluating the correlation between the test scheme and the actual situation, and ensuring the effectiveness and feasibility of the test scheme. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] The present invention will be further described below in conjunction with the accompanying drawings.
[0051] Figure 1 The present invention is a flowchart of an optimization method for a high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment.
[0052] Figure 2 The present invention is a flowchart of a multi-factor coupling comprehensive test box in an optimization method for a high-throughput simulated accelerated corrosion test of steel in a marine atmospheric environment.
[0053] Figure 3 It is a grey correlation diagram of nine groups of accelerated corrosion test schemes in a method for optimizing a high-throughput simulated accelerated corrosion test of steel in a marine atmospheric environment according to the present invention. DETAILED DESCRIPTION
[0054] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0055] See also Figure 1-3 The present invention provides an optimal method for a high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment, comprising the following steps:
[0056] Step 1: Select key environmental factors in the marine atmospheric environment of the target area;
[0057] Step 2: Set three levels for each key environmental factor and design an orthogonal test table of four factors and three levels for accelerated corrosion of carbon steel; design nine groups of accelerated corrosion test schemes based on the orthogonal test table;
[0058] Step 3, according to nine groups of accelerated corrosion test schemes, an accelerated corrosion test is performed using a multi-factor coupling comprehensive test chamber;
[0059] Step 4, obtain the weight loss data of the accelerated corrosion test, calculate the corrosion thickness loss of carbon steel in different cycles, and obtain the corrosion thickness loss data; based on the obtained corrosion thickness loss data, calculate the grey correlation between the accelerated corrosion test designed by the orthogonal experiment and the actual marine atmosphere exposure test;
[0060] Step 5: By comparing the grey correlation of the nine groups of accelerated corrosion test schemes designed by orthogonal experiment, the test scheme with the highest grey correlation is selected as the optimal test scheme for accelerated corrosion of marine atmosphere in the target area.
[0061] See also Figure 1-3 , step 1 includes:
[0062] Select key environmental factors in the marine atmospheric environment of the target area; the target area is the marine atmospheric environment of the area simulated by the test;
[0063] Exemplarily, the regional marine atmospheric environment simulated in the test is the marine atmospheric environment of Qinghai; chloride ion concentration, temperature, humidity, and radiation intensity are selected as key environmental factors; the chloride ion concentration, temperature, humidity, and radiation intensity have a significant effect on the corrosion of carbon steel.
[0064] See also Figure 1-3 , the method for obtaining the three levels of each key environmental factor in step 2 is as follows:
[0065] Select a single test parameter of the key environmental factor based on the annual average value of the marine atmospheric environment in the target area, take one level in the positive and negative directions of the selected single test parameter, and set three different levels under each key environmental factor;
[0066] Among them, the level refers to the different thresholds of each key environmental factor, and different thresholds are combined into different levels to ensure the repeatability of the test results, as shown in Table 1;
[0067] Table 1 Factor levels of key environmental factors in the marine atmospheric environment
[0068]
[0069] The method for designing nine sets of accelerated corrosion test plans is as follows:
[0070] Through the orthogonal test table, a four-factor three-level orthogonal test was designed, and nine groups of accelerated corrosion test schemes were screened out after combining four factors at three levels through the minimum test combinations;
[0071] Among them, the conditions of each test are determined by the horizontal numbers in each column, as shown in Table 2;
[0072] Table 2 Orthogonal test table of four factors and three levels for accelerated corrosion of carbon steel
[0073]
[0074] In this step, the orthogonal experimental design allows for simultaneous consideration of multiple key environmental factors and evaluation of their combined effects on carbon steel corrosion. In addition, unlike the traditional full factorial experimental design, the orthogonal experimental design only requires nine experiments, significantly reducing the number of experiments and costs, and facilitating rapid screening of the optimal combination of conditions.
[0075] See also Figure 1-3 , step 3 includes:
[0076] Nine groups of accelerated corrosion test schemes were designed according to the orthogonal test table. Accelerated corrosion tests were carried out in a multi-factor coupling comprehensive test chamber. The accelerated corrosion test cycle was defined and the corrosion conditions of carbon steel were observed and recorded. The accelerated corrosion test was divided into three steps, each of which was independent of each other. After one step was completed, it would automatically enter the next step. The accelerated corrosion test cycles were 1d, 2d, 4d, and 8d, respectively. That is, each test scheme would be evaluated at the above four different time points to monitor the changes in corrosion loss over time.
[0077] Specific accelerated corrosion tests include:
[0078] The first step is a wet heat step, which lasts for 8 hours. This step controls the temperature and humidity in the equipment to achieve the control of temperature and humidity in the test plan.
[0079] It should be noted that this step is also used to simulate the higher temperature and humidity in the actual marine atmospheric environment;
[0080] The second step is the illumination step, which lasts for 8 hours. In this step, the irradiation intensity is controlled by a xenon lamp installed in the equipment to achieve the control of the irradiation intensity in the test plan;
[0081] It should be noted that the light beam produced by the xenon lamp is very similar to sunlight and is very suitable for simulating sunlight exposure. Therefore, it can effectively simulate the strong radiation conditions in the marine atmosphere environment;
[0082] The third step is a dry-wet cycle alternation step, which lasts for 8 hours, with one cycle lasting 1 hour, and a total of 8 cycles. This step controls the chloride ion concentration in the test scheme by preparing soaking solutions with different pollutant concentrations.
[0083] The soaking time in one cycle is 12 minutes, and the drying time is 48 minutes. During the drying period, the temperature and humidity settings are the same as in the first step. At the same time, when preparing soaking solutions with different chloride ion concentrations, 0.01 mol / L NaHSO3 solution is added to simulate a small amount of SO2 gas in the atmosphere.
[0084] Repeat the accelerated corrosion test periodically according to the above steps to simulate long-term environmental exposure.
[0085] In this step, through this structured experimental design, the influence of different environmental factors on the corrosion loss of carbon steel can be systematically evaluated. Each test step is designed to simulate a specific condition in the actual marine atmospheric environment, making the entire test more comprehensive and closer to the actual situation, which is conducive to a better understanding of the corrosion mechanism and provides a scientific basis for the selection and protection of materials.
[0086] See also Figure 1-3 The method for obtaining the weight loss data of the accelerated corrosion test and the corrosion thickness loss data of carbon steel under different cycles in step 4 is as follows:
[0087] After the scheduled accelerated corrosion test cycle, the sample was taken out of the test chamber and its macroscopic morphology was recorded using a camera. In order to ensure the reliability and repeatability of the test results, three parallel samples were set under each test condition.
[0088] Immerse the sample in a pickling solution, control the temperature at 20-25°C, and set the initial time to 10 minutes; the pickling solution is prepared by 500ml of distilled water + 500ml of hydrochloric acid + 3.5g of hexamethylenetetramine;
[0089] Among them, if the corrosion products are not cleaned up, the pickling time can be extended until they are cleaned up;
[0090] After pickling, each sample was weighed and the weight of each sample was recorded to obtain the weight loss data of the accelerated corrosion test, including the original weight of the carbon steel and the weight after pickling;
[0091] Calculate the corrosion thickness loss of carbon steel in different cycles and obtain the corrosion thickness loss data of carbon steel in different cycles;
[0092] The calculation formula is:
[0093]
[0094] Wherein, M1 represents the original weight of carbon steel, M2 represents the weight of carbon steel after pickling, ρ represents the density of carbon steel, S represents the surface area of carbon steel exposed to the corrosive environment, and D represents the corrosion thickness loss of carbon steel.
[0095] The method for obtaining the grey correlation coefficient and grey correlation degree of the accelerated corrosion loss of carbon steel in orthogonal test design and the actual marine atmospheric corrosion loss is as follows:
[0096] According to the corrosion loss data obtained, the accelerated corrosion loss of carbon steel in the orthogonal test design was taken as a subsequence, and the test period was 1d, 2d, 4d, and 8d. The corrosion loss of carbon steel in the actual marine atmosphere in the target area for 30d, 60d, 120d, and 240d was taken as the parent sequence.
[0097] The subsequence and the parent sequence are dimensionless respectively;
[0098] The calculation formula is:
[0099]
[0100]
[0101] In the formula, Y0 represents the dimensionless treatment of corrosion loss in actual marine atmosphere, Y i represents the dimensionless treatment of the accelerated corrosion thickness loss of orthogonal test design, i represents nine groups of accelerated corrosion test schemes, i = 1, 2, ..., 9; k represents four cycles, k = 1, 2, 3, 4; X0(k) represents the corrosion thickness loss in the actual marine atmosphere, X i (k) represents the accelerated corrosion loss of orthogonal test design;
[0102] Calculate the absolute difference series of corrosion loss between the accelerated corrosion of carbon steel in orthogonal test design and the actual marine atmospheric corrosion after dimensionless treatment;
[0103] The calculation formula is:
[0104] Δ 0i =|Y0(k)-Y i (k)|;
[0105] In the formula, Δ 0i is the absolute difference sequence, Y0(k) represents the dimensionless corrosion loss sequence of actual marine atmospheric corrosion, and Y i (k) represents the accelerated corrosion loss sequence after dimensionless processing of orthogonal experimental design;
[0106] Calculate the grey correlation coefficient and grey correlation degree of the accelerated corrosion loss of carbon steel in orthogonal test design and the actual marine atmospheric corrosion loss;
[0107] The calculation formula is:
[0108]
[0109] In the formula, ζ 0i (k) is the grey correlation coefficient, γ 0i is the grey relational degree, θ is the resolution coefficient, 0<θ<1, It represents the minimum absolute difference of corrosion thickness loss in the accelerated corrosion test of the orthogonal experimental design after dimensionless processing; It represents the maximum absolute difference of corrosion thickness loss in the accelerated corrosion test of the orthogonal experimental design after dimensionless processing;
[0110] In this step, by obtaining the corrosion loss data of carbon steel under different cycles, as well as the grey correlation coefficient and grey correlation degree between the accelerated corrosion loss of carbon steel orthogonal test design and the actual marine atmospheric corrosion loss, it is helpful to evaluate the similarity between the accelerated corrosion test results and the actual marine atmospheric corrosion, thereby verifying the effectiveness and reliability of the accelerated corrosion test.
[0111] See also Figure 1-3 , step 5 includes:
[0112] The grey correlation degrees of the nine accelerated corrosion test schemes designed in orthogonal experiment were compared, and the grey correlation diagram of the nine accelerated corrosion test schemes was drawn; the test scheme with the highest grey correlation degree was selected as the optimal test scheme for accelerated corrosion of marine atmosphere in the target area; wherein the horizontal axis represents the nine different test schemes, and the vertical axis represents the value of the grey correlation degree.
[0113] For example, Figure 3 The grey correlation diagram of the nine accelerated corrosion test schemes designed by orthogonal experiment shows that the fourth test scheme has the highest grey correlation and the best correlation. Therefore, the optimal test scheme for accelerated corrosion in the marine atmosphere of the target area is: 2% NaCl + 15 ° C + 75 RH + 800 W / m 2 .
[0114] In this step, the grey correlation coefficient is used to measure the correlation between each set of schemes and the actual marine atmospheric corrosion thickness loss data. By drawing the grey correlation diagram of the nine sets of accelerated corrosion test schemes, the correlation between each set of schemes can be intuitively displayed. This graphical display helps to quickly identify the test scheme with the highest correlation.
[0115] In one or more embodiments provided by the present invention, it should be understood that the disclosed system can be implemented in other ways. For example, the above-described embodiments of the invention are only illustrative, for example, the division of modules is only a logical function division, and there may be other division methods in actual implementation.
[0116] The modules described as separate components may or may not be physically separated, and the components shown as modules may or may not be physical modules, that is, they may be located in one place or distributed on multiple network modules. Some or all of the modules may be selected according to actual needs to achieve the purpose of the solution of this embodiment.
[0117] In addition, each functional module in each embodiment of the present invention may be integrated into one processing module, or each module may exist physically separately, or two or more modules may be integrated into one module. The above-mentioned integrated module may be implemented in the form of hardware or in the form of hardware plus software functional modules.
[0118] It is obvious to a person skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the essential characteristics of the present invention.
[0119] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for optimizing a high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment, characterized in that: include: Select key environmental factors in the marine atmospheric environment of the target area; Set three levels for each key environmental factor and design an orthogonal test table with four factors and three levels for accelerated corrosion of carbon steel; design nine groups of accelerated corrosion test schemes based on the orthogonal test table; According to nine sets of accelerated corrosion test schemes, accelerated corrosion tests were carried out in a multi-factor coupling comprehensive test chamber; Obtain weight loss data of accelerated corrosion test, calculate corrosion thickness loss of carbon steel in different cycles, and obtain corrosion thickness loss data; Based on the obtained corrosion thickness loss data, calculate the grey correlation between the accelerated corrosion test designed by orthogonal experiment and the actual marine atmosphere exposure test; By comparing the grey correlation of nine groups of accelerated corrosion test schemes designed by orthogonal experiment, the test scheme with the highest grey correlation was selected as the optimal test scheme for accelerated corrosion in marine atmosphere in the target area.
2. The method for optimizing the high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment according to claim 1, characterized in that: The target area is the regional marine atmospheric environment simulated in the test; key environmental factors include chloride ion concentration, temperature, humidity, and radiation intensity.
3. The method for optimizing the high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment according to claim 1, characterized in that: The method to obtain the three levels for each key environmental factor is as follows: A single test parameter of the key environmental factor is selected based on the annual average value of the marine atmospheric environment in the target area. The selected single test parameter is taken at one level in the positive and reverse directions respectively, and three different levels are set under each key environmental factor.
4. The method for optimizing the high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment according to claim 3, characterized in that: The method for designing nine sets of accelerated corrosion test plans is as follows: Through the orthogonal test table, a four-factor three-level orthogonal test was designed, and nine groups of accelerated corrosion test schemes were screened out after combining four factors at three levels through the least experimental combinations.
5. The method for optimizing the marine atmospheric environment high-throughput simulated accelerated corrosion test of steel according to claim 4, characterized in that: Nine groups of accelerated test schemes were designed according to the orthogonal test table. Accelerated corrosion tests were carried out in a multi-factor coupling comprehensive test chamber. The accelerated corrosion test cycle was defined and the corrosion conditions of carbon steel were observed and recorded. The accelerated corrosion test was divided into three steps, each of which was independent of each other. After one step was completed, it would automatically enter the next step. The accelerated corrosion test cycles were set to 1d, 2d, 4d, and 8d, respectively.
6. The method for optimizing the high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment according to claim 5, characterized in that: Specific accelerated corrosion tests include: The first step is a wet heat step, which lasts for 8 hours. This step controls the temperature and humidity in the equipment to achieve the control of temperature and humidity in the test plan. The second step is the illumination step, which lasts for 8 hours. In this step, the irradiation intensity is controlled by a xenon lamp installed in the equipment to achieve the control of the irradiation intensity in the test plan; The third step is a dry-wet cycle alternation step, which lasts for 8 hours, with one cycle lasting 1 hour, and a total of 8 cycles. This step controls the chloride ion concentration in the test scheme by preparing soaking solutions with different pollutant concentrations. The soaking time in one cycle is 12 minutes, and the drying time is 48 minutes. During the drying period, the temperature and humidity settings are the same as in the first step. At the same time, when preparing soaking solutions with different chloride ion concentrations, 0.01 mol / L NaHSO3 solution is added to simulate a small amount of SO2 gas in the atmosphere. Repeat the accelerated corrosion test periodically according to the above steps to simulate long-term environmental exposure.
7. The method for optimizing the high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment according to claim 6, characterized in that: After the predetermined accelerated corrosion test cycle is completed, the sample is taken out of the test chamber and its macroscopic morphology is recorded using a camera; three parallel samples are set under each test condition; Immerse the sample in a pickling solution, control the temperature at 20-25°C, and set the initial time to 10 minutes; the pickling solution is prepared by 500ml of distilled water + 500ml of hydrochloric acid + 3.5g of hexamethylenetetramine; Among them, if the corrosion products are not cleaned up, the pickling time can be extended until they are cleaned up; After pickling, each sample was weighed and the weight of each sample was recorded to obtain the weight loss data of the accelerated corrosion test, including the original weight of the carbon steel and the weight after pickling; Calculate the corrosion thickness loss of carbon steel in different cycles and obtain the corrosion thickness loss data of carbon steel in different cycles; The calculation formula is: Wherein, M1 represents the original weight of carbon steel, M2 represents the weight of carbon steel after pickling, ρ represents the density of carbon steel, S represents the surface area of carbon steel exposed to the corrosive environment, and D represents the corrosion thickness loss of carbon steel.
8. The method for optimizing the high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment according to claim 7, characterized in that: The method for obtaining the grey correlation coefficient and grey correlation degree of the accelerated corrosion loss of carbon steel in orthogonal test design and the actual marine atmospheric corrosion loss is as follows: According to the corrosion loss data obtained, the accelerated corrosion loss of carbon steel in the orthogonal test design was taken as a subsequence, and the test period was 1d, 2d, 4d, and 8d. The corrosion loss of carbon steel in the actual marine atmosphere in the target area for 30d, 60d, 120d, and 240d was taken as the parent sequence. The subsequence and the parent sequence are dimensionless respectively; The calculation formula is: In the formula, Y0 represents the dimensionless treatment of corrosion loss in actual marine atmosphere, Y i represents the dimensionless treatment of the accelerated corrosion thickness loss of orthogonal test design, i represents nine groups of accelerated corrosion test schemes, i = 1, 2, ..., 9; k represents four cycles, k = 1, 2, 3, 4; X0(k) represents the corrosion thickness loss in the actual marine atmosphere, X i (k) represents the accelerated corrosion loss of orthogonal test design; Calculate the absolute difference series of corrosion loss between the accelerated corrosion of carbon steel in orthogonal test design and the actual marine atmospheric corrosion after dimensionless treatment; The calculation formula is: Δ 0i =|Y0(k)-Y i (k)|; In the formula, Δ 0i is the absolute difference sequence, Y0(k) represents the dimensionless corrosion loss sequence of actual marine atmospheric corrosion, and Y i (k) represents the accelerated corrosion loss sequence after dimensionless processing of orthogonal experimental design; Calculate the grey correlation coefficient and grey correlation degree of the accelerated corrosion loss of carbon steel in orthogonal test design and the actual marine atmospheric corrosion loss; The calculation formula is: In the formula, ζ 0i (k) is the grey correlation coefficient, γ 0i is the grey relational degree, θ is the resolution coefficient, 0<θ<1, It represents the minimum absolute difference of corrosion thickness loss in the accelerated corrosion test of the orthogonal experimental design after dimensionless processing; It represents the maximum absolute difference of corrosion thickness loss in the accelerated corrosion test of the orthogonal experimental design after dimensionless processing.
9. The method for optimizing the high-throughput simulated accelerated corrosion test of steel in a marine atmosphere environment according to claim 8, characterized in that: The grey correlation degrees of the nine accelerated corrosion test schemes designed in orthogonal experiment were compared, and the grey correlation diagram of the nine accelerated corrosion test schemes was drawn; the test scheme with the highest grey correlation degree was selected as the optimal test scheme for accelerated corrosion of marine atmosphere in the target area; wherein the horizontal axis represents the nine different test schemes, and the vertical axis represents the value of the grey correlation degree.