Method and system for discriminating and inhibiting wood wheel cracks in drying process

By measuring and calculating the dry shrinkage strain and interaction force of wood, the risk of wheel cracking during the drying process is determined, and the drying process is adjusted to solve the problem of wheel cracking suppression in the existing technology and achieve a faster and more efficient wood drying process.

CN118746590APending Publication Date: 2024-10-08NANJING FORESTRY UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410735658.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing technology cannot effectively suppress the occurrence of wheel cracks during the wood drying process, and lacks theoretical guidance in slowing down the moisture discharge rate. It relies more on experience and technology, resulting in increased drying time.

Method used

By measuring the radial shrinkage strain and tensile strength of early wood and late wood, we can calculate the interaction force between early wood and late wood during the drying process to determine whether there is a risk of wheel cracking, and adjust the drying process based on the results, such as reducing the wind speed. , spray steam drying, cooling and humidification to inhibit the occurrence of wheel cracks.

Benefits of technology

Accurately measure the drying shrinkage strain difference and interaction force between early and late wood to determine the risk of wheel cracking, adjust the drying process to avoid wheel cracking, speed up the drying speed, improve drying quality and save costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118746590A_ABST
    Figure CN118746590A_ABST
Patent Text Reader

Abstract

The invention discloses a method and a system for discriminating and inhibiting wood wheel cracks in a drying process, and belongs to the field of wood drying. The method comprises the following steps: in a drying process, measuring respective radial shrinkage strain of an early timber and a late timber in a complete growth wheel of the timber and respective radial shrinkage strain of an independent early timber and an independent late timber of the timber; air shrinkage strain difference values between the early wood and the late wood and between the independent early wood and the independent late wood in the complete growth wheel are calculated; measuring the radial tensile strength F0 of the wood and the elastic modulus of the early wood and the elastic modulus of the late wood; calculating the interaction force F between the morning material and the evening material in the drying process according to the drying shrinkage strain difference between the morning material and the evening material in the complete growth wheel and the independent morning material and the independent evening material in combination with the elastic modulus of the morning material and the elastic modulus of the evening material, and judging whether the wood has wheel cracks or not in the drying process according to the interaction force F between the morning material and the evening material and the radial tensile strength F0 of the wood; and if the wood has the risk of wheel crack in the drying process, the drying process is adjusted to inhibit the wheel crack.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of wood drying, and in particular relates to a method and a system for distinguishing and inhibiting wood ring cracking during the drying process. Background Art

[0002] Wood drying is the process of removing moisture from wood under the action of heat energy, reducing the moisture content of wood, and improving the quality and performance of wood. Drying can reduce deformation, cracking and decay of wood, improve the hardness and stability of wood, and make it more suitable for use in construction, furniture, flooring and other fields. Wood drying technology is an important process in the wood processing and production process.

[0003] During the drying process, wood is prone to cracking, which is related to the diffusion characteristics of water inside the wood. Wood has a multi-level capillary system, and the rate of water diffusion from the inside of the wood to the surface is slower than the rate of water evaporation on the surface, which makes the shrinkage of the surface and inside of the wood inconsistent during the drying process, and there is drying stress. When the drying stress exceeds the ultimate tensile strength that the wood can withstand, the wood will crack.

[0004] According to the direction, wood cracking includes ring cracking and radial cracking. Ring cracking is characterized by cracking along the growth ring, concentrated at the junction of early wood and late wood. Ring cracking is caused by the difference in shrinkage between early wood and late wood. Early wood has a small density and shrinks less when it dries; late wood has a large density and shrinks more when it dries. Therefore, the uneven shrinkage of the two is prone to ring cracking.

[0005] It can be seen that the stress performance and cracking (ring cracking) behavior during the drying process are relatively complex, involving not only the moisture content gradient between the surface and interior of the wood, but also the arrangement of the early and late wood of the wood itself. In order to reduce the cracking phenomenon during the wood drying process, corresponding measures are taken in the prior art: such as changing the drying method, including microwave drying ("A Wood Drying Treatment Method" (CN201710627042.1)), vacuum drying ("A Wood Drying Method" (CN201510800116.8)), intermittent heating drying ("A Basswood Wood Drying Method" (CN201710849406.0)); or pre-treating the wood ("A Wood Drying Method" (CN201610834095.6) and "Improved Wood Drying Process" (CN2018103118)). 13.0)), applying anti-cracking agent (A method for drying wood (CN201710559344.X)), applying coating (A method for reducing degradation in the process of drying wood (CN201810650493.1)); or appropriately adjusting the wood drying process, including steam spraying (A new type of wood drying control system (CN202211184844.7)), reducing wind speed (Method for determining moisture content in wood drying process and wood drying method (CN201710849808.0)), and cooling (A method for drying wood (CN201110370954.8)).

[0006] Based on the above research status, it can be seen that whether changing the drying method, drying process or pre-treating the wood, the essence is to prevent cracking (wheel cracking) by slowing down the rate of water discharge during the drying process. However, as for the degree of slowing down the rate of water discharge, there is no clear theoretical guidance, and it is mostly implemented by experience and technology; in other words, the current method of slowing down the rate of water discharge and preventing cracking comes at the cost of increasing the drying time of the wood. Summary of the invention

[0007] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method and system for distinguishing and inhibiting wood ring cracking during the drying process, thereby solving the problems in the prior art.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] The method for distinguishing and inhibiting wood ring cracking during the drying process comprises the following steps:

[0010] During the drying process, the radial shrinkage strains of the earlywood and latewood in the complete growth ring of the wood, and the radial shrinkage strains of the independent earlywood and independent latewood of the wood are measured;

[0011] Calculate the shrinkage strain difference between the earlywood, latewood and independent earlywood, independent latewood in the complete growth ring;

[0012] Measure the radial tensile strength F0 of wood, as well as the elastic modulus of early wood and late wood;

[0013] According to the difference in shrinkage strain between the earlywood and latewood in the complete growth ring and the independent earlywood and independent latewood, and combined with the elastic modulus of the earlywood and latewood respectively, the interaction force F between the earlywood and latewood during the drying process is calculated.

[0014] Whether the wood will crack during the drying process can be determined based on the interaction force F between the early and late wood and the radial tensile strength F0 of the wood.

[0015] If there is a risk of wood cracking during the drying process, the drying process should be adjusted to suppress the occurrence of cracking.

[0016] Furthermore, the calculation formula for the difference in shrinkage strain between the earlywood, latewood in the complete growth ring and the independent earlywood, independent latewood is:

[0017] Δε 早 =ε 完整-早 -ε 独立-早

[0018] Δε 晚 =ε 独立-晚 -ε 完整-晚

[0019] In the formula, Δε 早 is the shrinkage strain difference between the earlywood in the growth ring and the independent earlywood, Δε 晚 is the difference in shrinkage strain between the latewood in the complete growth ring and the independent latewood; ε 完整-早 , ε 完整-晚 are the radial shrinkage strains of earlywood and latewood in the complete growth ring of wood, respectively; ε 独立-早 , ε 独立-晚 They are the radial shrinkage strains of independent earlywood and independent latewood, respectively.

[0020] Furthermore, the calculation formula for the interaction force F between earlywood and latewood is:

[0021] F=Max(F 早 , F 晚 )

[0022] F 早 =Δε 早 ×E 早

[0023] F 晚 =Δε 晚 ×E 晚

[0024] In the formula, F 早 is the radial tensile stress of the early wood during the drying process, F 晚 is the radial tensile stress of latewood, E 早 、E 晚 are the elastic modulus of earlywood and latewood respectively.

[0025] Furthermore, when judging whether wheel cracking occurs in the wood during the drying process, when F<F0, the wood will not undergo wheel cracking, otherwise there is a risk of wheel cracking.

[0026] Furthermore, the drying process adjustment includes: reducing wind speed, spray drying, cooling and humidifying.

[0027] Furthermore, the radial shrinkage strain of wood is measured by combining digital lens and digital image technology.

[0028] Furthermore, when the digital image correlation technology is used, wood tracheids and wood fibers are selected as natural speckles or artificial speckles are sprayed, and the diameter of the artificial speckles ranges from 10 μm to 100 μm.

[0029] Furthermore, the temperature of the wood is 30-80° C., and the moisture content is 5-25%.

[0030] Furthermore, the wood is: Pinus sylvestris var. mongolica, Pinus massoniana, Cunninghamia lanceolata, Fraxinus mandshurica, Elm or Quercus mongolica.

[0031] The identification and suppression system of wood ring cracking during the drying process includes

[0032] Strain measurement module: During the drying process, the radial shrinkage strain of the earlywood and latewood in the complete growth ring of the wood, and the radial shrinkage strain of the independent earlywood and independent latewood of the wood are measured;

[0033] Difference calculation module: calculate the shrinkage strain difference between earlywood, latewood and independent earlywood and independent latewood in the complete growth ring;

[0034] Tensile strength measurement module: measures the radial tensile strength F0 of wood, as well as the elastic modulus of early wood and late wood;

[0035] Force calculation module: According to the shrinkage strain difference between the earlywood and latewood in the complete growth ring and the independent earlywood and independent latewood, and combined with the elastic modulus of the earlywood and latewood respectively, the interaction force F between the earlywood and latewood during the drying process is calculated.

[0036] Judgment module: judge whether the wood has wheel cracking during the drying process according to the interaction force F between the early and late wood and the radial tensile strength F0 of the wood;

[0037] And, the inhibition module: if there is a risk of wood wheel cracking during the drying process, the drying process is adjusted to inhibit the occurrence of wheel cracking.

[0038] Beneficial effects of the present invention:

[0039] 1. By calculating the difference in shrinkage strain between the earlywood, latewood and independent earlywood, independent latewood in the complete growth ring, the interaction force caused by the inconsistent shrinkage between the earlywood and latewood during the drying process can be accurately determined.

[0040] 2. The shrinkage strain and its difference test temperature and moisture content of the present invention have a wide range of application, and can accurately grasp the dependence of the interaction force between early and late wood and the drying temperature and moisture content.

[0041] 3. By measuring and calculating the interaction force between early and late wood during the drying process, the difference between it and the radial tensile strength of the wood can be accurately compared to determine whether wheel cracking occurs in the wood.

[0042] 4. By judging whether the wood is at risk of wheel cracking, the drying process can be adjusted. Alternatively, the drying speed can be accelerated to improve the drying quality, saving drying time and costs without causing wheel cracking. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0044] Figure 1 It is the radial shrinkage strain distribution diagram of the complete growth ring sample and the independent earlywood and latewood samples of the present invention;

[0045] Figure 2 It is a diagram showing the change in radial shrinkage strain of the complete growth ring sample and the independent early and late wood samples in the growth ring as a function of relative position. DETAILED DESCRIPTION

[0046] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] The method for distinguishing and inhibiting wood ring cracking during the drying process comprises the following steps:

[0049] S1, during the drying process at a temperature of 55°C and a moisture content of 5%, the radial shrinkage strain ε of the complete growth ring of Chinese fir was measured by combining digital camera and digital image correlation technology, including the radial shrinkage strain of earlywood and latewood in the complete growth ring, which were recorded as ε 完整-早 =2.50% and ε 完整-晚 =2.75%. The radial dimension of the complete growth ring is 3 cm. When the digital image correlation technology is used, the artificial speckle is sprayed manually, and the average diameter of the artificial speckle is 50 μm.

[0050] S2, using digital camera and digital image correlation technology, the radial shrinkage strains of independent earlywood and independent latewood of Chinese fir under the same drying conditions as S1 were measured, and recorded as ε 独立-早 =0.50% and ε 独立-晚 =1.75%.

[0051] S3, calculate the shrinkage strain difference between the earlywood, latewood in the complete growth ring and the independent earlywood, independent latewood, respectively, denoted as Δε 早 and Δε 晚 ; The calculation formula is:

[0052] Δε 早 =ε 完整-早 -ε 独立-早 =2.00%

[0053] Δε 晚 =ε 独立-晚 -ε 完整-晚 =1.00%

[0054] S4, measure the radial tensile strength F0 = 3.5 MPa of wood dried under the same conditions as S1, and use a mechanical testing machine to measure the elastic modulus E of early wood and late wood, respectively, denoted as E 早 =180MPa and E 晚 =353MPa.

[0055] S5, based on Δε 早 , Δε 晚 、E 早 and E 晚 , calculate the interaction force F between early and late wood during the drying process:

[0056] F 早 =Δε 早 ×E 早 =3.60MPa;

[0057] F 晚 =Δε 晚 ×E 晚 =3.53MPa;

[0058] F=Max(F 早 , F 晚 )=3.60MPa.

[0059] In the formula, F 早 is the radial tensile stress of the early wood during the drying process, F 晚 is the radial tensile stress of latewood.

[0060] S6, judging whether wheel cracking occurs in the wood during the drying process based on the interaction force F between the early and late wood calculated in S5 and the radial tensile strength F0 of the wood;

[0061] It can be seen that in this embodiment, when F>F0, the fir has the possibility of ring splitting.

[0062] S7, adjusting the drying process by reducing the wind speed to suppress the occurrence of wheel cracking.

[0063] It is worth mentioning that the specific algorithm steps for measuring the radial shrinkage strain of wood by combining digital lens and digital imaging technology are as follows:

[0064] 1) Before the drying process, a digital microscope is used to capture images of independent earlywood and independent latewood samples in a balanced state before drying; after the drying process is completed, a digital microscope is used to capture images of independent earlywood and independent latewood samples in a balanced state after drying.

[0065] 2) Shrinkage strain measurement: the image before drying is set as the reference image, and the image after drying is set as the speckle image. The images before and after shrinkage are analyzed by DIC using VIC-2D software, as shown in Figure 1 shown.

[0066] Observe the shrinkage strain of independent earlywood and independent latewood, and calculate the difference between the shrinkage of independent earlywood and latewood and the complete growth ring, such as Figure 2 As shown. Figure 2 The shrinkage difference between the complete growth ring and the independent earlywood and latewood shows that for the complete growth ring, the latewood will cause the deformation of the adjacent earlywood, making the shrinkage value of the complete growth ring earlywood larger than that of the independent earlywood. This shrinkage difference will change with the drying temperature and moisture content. Generally, the higher the temperature and the more drastic the moisture content change, the greater the shrinkage difference, and the easier it is to cause ring cracking.

[0067] Example 2

[0068] The method for distinguishing and inhibiting wood ring cracking during the drying process comprises the following steps:

[0069] S1, during the drying process at 65℃ and 10% moisture content, the radial shrinkage strain ε of the complete growth ring of Masson pine was measured by combining digital camera and digital image correlation technology, including the radial shrinkage strain of earlywood and latewood in the complete growth ring, which are recorded as ε 完整-早 =2.54% and ε 完整-晚 =2.88%; wherein, the radial dimension of the complete growth ring is 2 cm, and when the digital image correlation technology is used, the tracheids of Masson pine are selected as natural speckles.

[0070] S2, using digital camera and digital image correlation technology, the radial shrinkage strain of Masson pine earlywood and latewood under the same drying conditions as S1 was measured, and recorded as ε 独立-早 =0.95% and ε 独立-晚 =2.06%.

[0071] S3, calculate the shrinkage strain difference between the earlywood, latewood in the complete growth ring and the independent earlywood, independent latewood, respectively, denoted as Δε 早 and Δε 晚 ; The calculation formula is:

[0072] Δε 早 =ε 完整-早 -ε 独立-早 =1.59%

[0073] Δε 晚 =ε 独立-晚 -ε 完整-晚 =0.82%

[0074] S4, measured the radial tensile strength of wood under the same drying conditions as S1, F0 = 19.4 MPa, and measured the elastic modulus of early wood and late wood respectively using a micro-tensile device, recorded as E 早 =418MPa and E 晚 =825MPa.

[0075] S5, based on Δε 早 , Δε 晚 、E 早 and E 晚 , calculate the interaction force F between early and late wood during the drying process:

[0076] F 早 =Δε 早 ×E 早 =6.65MPa;

[0077] F 晚 =Δε 晚 ×E 晚 =6.76MPa;

[0078] F=Max(F早 , F 晚 )=6.76MPa.

[0079] S6, judging whether wheel cracking occurs in the wood during the drying process based on the interaction force F between the early and late wood calculated in S5 and the radial tensile strength F0 of the wood;

[0080] It can be seen that in this embodiment, F<F0, and the Masson pine will not suffer from wheel cracking.

[0081] Example 3

[0082] The method for distinguishing and inhibiting wood ring cracking during the drying process comprises the following steps:

[0083] S1, during the drying process at 60℃ and 15% moisture content, the radial shrinkage strain ε of the complete growth ring of Pinus sylvestris was measured by combining digital camera and digital image correlation technology, including the radial shrinkage strain of earlywood and latewood in the complete growth ring, which are recorded as ε 完整-早 =2.14% and ε 完整-晚 =2.32%; wherein, the radial dimension of the complete growth ring is 5 mm, and when the digital image correlation technology is used, the tracheids of Pinus sylvestris are selected as the natural speckle.

[0084] S2, using digital camera and digital image correlation technology, the radial shrinkage strain of independent earlywood and independent latewood of Pinus sylvestris var. mongolica under the same drying conditions as S1 was measured, and recorded as ε 独立-早 =1.02% and ε 独立-晚 =1.75%.

[0085] S3, calculate the shrinkage strain difference between the earlywood, latewood in the complete growth ring and the independent earlywood, independent latewood, respectively, denoted as Δε 早 and Δε 晚 ; The calculation formula is:

[0086] Δε 早 =ε 完整-早 -ε 独立-早 =1.12%

[0087] Δε 晚 =ε 独立-晚 -ε 完整-晚 =0.57%

[0088] S4, measure the radial tensile strength of wood under the same drying conditions as S1, F0 = 6.7MPa, and use a mechanical testing machine to measure the elastic modulus of early wood and late wood, respectively, recorded as E 早 =231MPa and E 晚 =453MPa;

[0089] S5, based on Δε早 , Δε 晚 、E 早 and E 晚 , calculate the interaction force F between early and late wood during the drying process:

[0090] F 早 =Δε 早 ×E 早 =2.59MPa

[0091] F 晚 =Δε 晚 ×E 晚 =2.58MPa

[0092] F=Max(F 早 , F 晚 )=2.59MPa

[0093] S6, judging whether wheel cracking occurs in the wood during the drying process based on the interaction force F between the early and late wood calculated in S5 and the radial tensile strength F0 of the wood;

[0094] It can be seen that in this embodiment, F<F0, and the Pinus sylvestris var. mongolica will not suffer from wheel cracking.

[0095] Example 4

[0096] The method for distinguishing and inhibiting wood ring cracking during the drying process comprises the following steps:

[0097] S1, during the drying process at 50℃ and 10% moisture content, the radial shrinkage strain ε of the complete growth ring of ash was measured by combining digital camera and digital image correlation technology, including the radial shrinkage strain of earlywood and latewood in the complete growth ring, which were recorded as ε 完整-早 =2.14% and ε 完整-晚 =2.33%. The radial dimension of the complete growth ring is 4 μm. When the digital image correlation technology is used, the artificial speckle is sprayed manually, and the average diameter of the artificial speckle is 100 μm.

[0098] S2, using digital camera and digital image correlation technology, the radial shrinkage strain of independent earlywood and independent latewood of Pinus sylvestris var. mongolica under the same drying conditions as S1 was measured, and recorded as ε 独立-早 =0.69% and ε 独立-晚 =1.57%.

[0099] S3, calculate the shrinkage strain difference between the earlywood, latewood in the complete growth ring and the independent earlywood, independent latewood, respectively, denoted as Δε 早 and Δε 晚 ; The calculation formula is:

[0100] Δε早 =ε 完整-早 -ε 独立-早 =1.45%

[0101] Δε 晚 =ε 独立-晚 -ε 完整-晚 =0.76%

[0102] S4, measured the radial tensile strength F0 = 17.2 MPa of wood dried under the same conditions as S1, and measured the elastic modulus E of early wood and late wood respectively using a micro-tensile device, recorded as E 早 =400MPa and E 晚 =754MPa.

[0103] S5, based on Δε 早 , Δε 晚 、E 早 and E 晚 , calculate the interaction force F between early and late wood during the drying process:

[0104] F 早 =Δε 早 ×E 早 =5.80MPa;

[0105] F 晚 =Δε 晚 ×E 晚 =5.73MPa;

[0106] F=Max(F 早 , F 晚 )=5.80MPa.

[0107] S6, judging whether wheel cracking occurs in the wood during the drying process based on the interaction force F between the early and late wood calculated in S5 and the radial tensile strength F0 of the wood;

[0108] It can be seen that in this embodiment, F<F0, and the ash will not undergo wheel cracking.

[0109] Example 5

[0110] The method for distinguishing and inhibiting wood ring cracking during the drying process comprises the following steps:

[0111] S1, during the drying process at 80℃ and 12% moisture content, the radial shrinkage strain ε of the complete growth ring of elm wood was measured by combining digital camera and digital image correlation technology, including the radial shrinkage strain of earlywood and latewood in the complete growth ring, which are recorded as ε 完整-早 =1.41% and ε 完整-晚=1.56%. The radial size of the complete growth ring is 1000 μm, and the tracheids of elm are selected as natural speckles when using digital image correlation technology.

[0112] S2, using digital camera and digital image correlation technology, the radial shrinkage strain of independent earlywood and independent latewood of elm under the same drying conditions as S1 was measured, and recorded as ε 独立-早 =0.07% and ε 独立-晚 =0.87%.

[0113] S3, calculate the shrinkage strain difference between the earlywood, latewood in the complete growth ring and the independent earlywood, independent latewood, respectively, denoted as Δε 早 and Δε 晚 ; The calculation formula is:

[0114] Δε 早 =ε 完整-早 -ε 独立-早 =1.34%

[0115] Δε 晚 =ε 独立-晚 -ε 完整-晚 =0.69%

[0116] S4, measure the radial tensile strength F0 = 4.25 MPa of wood dried under the same conditions as S1, and use a mechanical testing machine to measure the elastic modulus E of early wood and late wood, respectively, denoted as E 早 =315MPa and E 晚 =619MPa.

[0117] S5, based on Δε 早 , Δε 晚 、E 早 and E 晚 , calculate the interaction force F between early and late wood during the drying process:

[0118] F 早 =Δε 早 ×E 早 =4.22MPa;

[0119] F 晚 =Δε 晚 ×E 晚 =4.27MPa;

[0120] F=Max(F 早 , F 晚 )=4.27MPa.

[0121] S6, judging whether wheel cracking occurs in the wood during the drying process based on the interaction force F between the early and late wood calculated in S5 and the radial tensile strength F0 of the wood;

[0122] It can be seen that in this embodiment, when F>F0, the elm wood has the possibility of ring cracking.

[0123] S7, adjusting the drying process by means of steam injection to suppress the occurrence of wheel cracking.

[0124] Example 6

[0125] The method for distinguishing and inhibiting wood ring cracking during the drying process comprises the following steps:

[0126] S1, during the drying process at 30℃ and 25% moisture content, the radial shrinkage strain ε of the complete growth ring of Chinese fir was measured by combining digital camera and digital image correlation technology, including the radial shrinkage strain of earlywood and latewood in the complete growth ring, which were recorded as ε 完整-早 =2.50% and ε 完整-晚 =2.75%. The radial dimension of the complete growth ring is 3 cm. When the digital image correlation technology is used, the artificial speckle is sprayed manually, and the average diameter of the artificial speckle is 50 μm.

[0127] S2, using digital camera and digital image correlation technology, the radial shrinkage strains of independent earlywood and independent latewood of Chinese fir under the same drying conditions as S1 were measured, and recorded as ε 独立-早 =0.50% and ε 独立-晚 =1.75%.

[0128] S3, calculate the shrinkage strain difference between the earlywood, latewood in the complete growth ring and the independent earlywood, independent latewood, respectively, denoted as Δε 早 and Δε 晚 ; The calculation formula is:

[0129] Δε 早 =ε 完整-早 -ε 独立-早 =1.53%

[0130] Δε 晚 =ε 独立-晚 -ε 完整-晚 =0.78%

[0131] S4, measure the radial tensile strength F0 = 3.5 MPa of wood dried under the same conditions as S1, and use a mechanical testing machine to measure the elastic modulus E of early wood and late wood, respectively, denoted as E 早 =180MPa and E 晚 =353MPa.

[0132] S5, based on Δε 早 , Δε 晚 、E 早 and E 晚, calculate the interaction force F between early and late wood during the drying process:

[0133] F 早 =Δε 早 ×E 早 =2.75MPa;

[0134] F 晚 =Δε 晚 ×E 晚 =2.75MPa;

[0135] F=Max(F 早 , F 晚 )=2.75MPa.

[0136] S6, judging whether wheel cracking occurs in the wood during the drying process based on the interaction force F between the early and late wood calculated in S5 and the radial tensile strength F0 of the wood;

[0137] It can be seen that in this embodiment, when F<F0, the fir will not undergo ring cracking.

[0138] Comparative Example 1

[0139] The conventional wood drying process in Comparative Example 1 comprises the following steps:

[0140] S1, preheating the fir wood for 3 hours at 40°C and relative humidity of 90% to 100%.

[0141] S2, adjust the ambient temperature of the wood drying kiln to 65℃ and keep it warm for 2 days

[0142] S3, when the moisture content of the fir reaches 5%, the water vapor in the kiln is released, and then the relative humidity in the kiln is adjusted to 12%, and a wind speed of 3m / s is introduced into the kiln.

[0143] S4, after drying, the fir wood was found to have ring cracks

[0144] Table 1 Identification and inhibition results of wood wheel cracking in various embodiments and comparative examples

[0145]

[0146] The data in Table 1 reflect the results of wood wheel cracking identification and inhibition in Examples 1-5 and Comparative Example 1. It can be seen from the table that no wheel cracking occurred in the examples, and the drying process can be adjusted in time when the possibility of wheel cracking occurs; the comparative example used a conventional drying process, and wheel cracking occurred in the chord direction.

[0147] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0148] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for distinguishing and inhibiting wood ring cracking during drying, characterized in that: The following steps are involved: During the drying process, the radial shrinkage strains of the earlywood and latewood in the complete growth ring of the wood, and the radial shrinkage strains of the independent earlywood and independent latewood of the wood are measured; Calculate the shrinkage strain difference between the earlywood, latewood and independent earlywood, independent latewood in the complete growth ring; Measure the radial tensile strength F0 of wood, as well as the elastic modulus of early wood and late wood; According to the difference in shrinkage strain between the earlywood and latewood in the complete growth ring and the independent earlywood and independent latewood, and combined with the elastic modulus of the earlywood and latewood respectively, the interaction force F between the earlywood and latewood during the drying process is calculated. Whether the wood will crack during the drying process can be determined based on the interaction force F between the early and late wood and the radial tensile strength F0 of the wood. If there is a risk of wood cracking during the drying process, the drying process should be adjusted to suppress the occurrence of cracking.

2. The method for distinguishing and inhibiting wood ring cracking during the drying process according to claim 1, characterized in that: The calculation formula for the difference in shrinkage strain between the earlywood, latewood and independent earlywood and independent latewood in a complete growth ring is: No 早 =e 完整-早 -e 独立-早 No 晚 =e 独立-晚 -e 完整-晚 In the formula, Δε 早 is the shrinkage strain difference between the earlywood in the growth ring and the independent earlywood, Δε 晚 is the difference in shrinkage strain between the latewood in the complete growth ring and the independent latewood; ε 完整-早 , ε 完整-晚 are the radial shrinkage strains of earlywood and latewood in the complete growth ring of wood, respectively; ε 独立-早 , ε 独立-晚 They are the radial shrinkage strains of independent earlywood and independent latewood, respectively.

3. The method for distinguishing and inhibiting wood ring cracking during the drying process according to claim 2, characterized in that: The calculation formula for the interaction force F between early and late wood is: F=Max(F 早 ,F 晚 ) F 早 =No 早 ×E 早 F 晚 =No 晚 ×E 晚 In the formula, F 早 is the radial tensile stress of the early wood during the drying process, F 晚 is the radial tensile stress of latewood, E 早 、E 晚 are the elastic modulus of earlywood and latewood respectively.

4. The method for distinguishing and inhibiting wood ring cracking during the drying process according to claim 1, characterized in that: When judging whether wheel cracking occurs in the wood during the drying process, when F<F0, the wood will not crack, otherwise there is a risk of wheel cracking.

5. The method for distinguishing and inhibiting wood ring cracking during the drying process according to claim 1, characterized in that: The drying process adjustment includes: reducing wind speed, spray drying, cooling and humidifying.

6. The method for distinguishing and inhibiting wood ring cracking during the drying process according to claim 1, characterized in that: The method for measuring the radial shrinkage strain of wood adopts a combination of digital lens and digital image technology.

7. The method for distinguishing and inhibiting wood ring cracking during the drying process according to claim 6, characterized in that: When using digital image correlation technology, wood tracheids and wood fibers are selected as natural speckles or artificial speckles are sprayed, and the diameter of the artificial speckle spots ranges from 10 μm to 100 μm.

8. The method for distinguishing and inhibiting wood ring cracking during the drying process according to claim 1, characterized in that: The temperature of the wood is 30-80° C., and the moisture content is 5-25%.

9. The method for distinguishing and inhibiting wood wheel cracking during the drying process according to claim 1 or 8, characterized in that: The wood is: larch, masson pine, fir, ash, elm or Mongolian oak.

10. A system for distinguishing and inhibiting wood ring cracking during drying, characterized in that: include Strain measurement module: During the drying process, the radial shrinkage strain of the earlywood and latewood in the complete growth ring of the wood, and the radial shrinkage strain of the independent earlywood and independent latewood of the wood are measured; Difference calculation module: calculate the shrinkage strain difference between earlywood, latewood and independent earlywood and independent latewood in the complete growth ring; Tensile strength measurement module: measures the radial tensile strength F0 of wood, as well as the elastic modulus of early wood and late wood; Force calculation module: According to the shrinkage strain difference between the earlywood and latewood in the complete growth ring and the independent earlywood and independent latewood, and combined with the elastic modulus of the earlywood and latewood respectively, the interaction force F between the earlywood and latewood during the drying process is calculated. Judgment module: judge whether the wood has wheel cracking during the drying process according to the interaction force F between the early and late wood and the radial tensile strength F0 of the wood; And, the inhibition module: if there is a risk of wood wheel cracking during the drying process, the drying process is adjusted to inhibit the occurrence of wheel cracking.