Functional film heterogeneous substrate structure, preparation method thereof and electronic component
By introducing auxiliary substrates and multi-temperature processing in the preparation of heterogeneous thin film structures, the problem of bubble defects caused by traditional high-temperature annealing is solved, a high-quality functional thin film heterogeneous substrate structure is achieved, and device performance and stability are improved.
Patent Information
- Application Number
- CN202410847326.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-08
AI Technical Summary
In the preparation process of traditional heterogeneous thin film structures, high-temperature annealing leads to the formation of bubble defects at the bonding interface, which affects device performance. Increasing the vacuum to reduce bubble defects will lead to a decrease in bonding strength and affect device stability.
By introducing an auxiliary substrate, the functional thin film layer is transferred to the target substrate, and a multi-temperature treatment method is used, including first surface ion implantation, first temperature treatment, second temperature treatment and third temperature treatment, to form a functional thin film heterogeneous The substrate structure avoids high-temperature annealing, reduces the impact of ion beam stripping, and introduces an intermediate layer at the bonding interface to improve bubble defects.
It significantly reduces bubble defects at the bonding interface, improves bonding strength and device performance, avoids the adverse effects of high-temperature annealing on performance, and achieves the preparation of high-quality functional thin film heterogeneous substrate structures.
Smart Images

Figure CN118748146A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a functional thin film heterogeneous substrate structure and a preparation method thereof, and an electronic component. Background Art
[0002] Functional thin film technology is currently widely used in core electronic components such as photonics devices, power devices, acoustic resonators and filters.
[0003] In the traditional process of preparing heterogeneous thin film structures, the target wafer is bonded to the supporting substrate wafer, and then high-temperature annealing is performed to enhance the bonding strength. However, during the high-temperature annealing process, bubble defects will form at the bonding interface, resulting in a significant impact on the performance of acoustic, optical, and electrical devices prepared using the heterogeneous thin film structure, limiting the scope of use of the heterogeneous thin film structure.
[0004] In the related art, in order to reduce the bubble defects at the bonding interface, the main method is to improve the vacuum degree of the bonding step. However, this method will cause a decrease in the bonding strength and may cause debonding in subsequent steps, affecting the stability and performance of the device. Summary of the invention
[0005] In view of at least one technical problem in the prior art, the purpose of the present application is to provide a functional thin film heterogeneous substrate structure and a preparation method thereof, and an electronic component.
[0006] In order to solve the above technical problems, on the one hand, the present application provides a method for preparing a functional thin film heterogeneous substrate structure, the preparation method comprising:
[0007] Providing an auxiliary substrate and a functional substrate, and performing ion implantation on a first surface of the functional substrate to obtain a defect layer; the first surface is away from the defect layer;
[0008] Performing a first bonding process on the auxiliary substrate and the functional substrate to obtain a first intermediate substrate structure; the bonding interface between the functional substrate and the auxiliary substrate is the first surface;
[0009] Performing a first temperature treatment on the first surface, and performing a peeling treatment on the first intermediate substrate structure along the defective layer to form a second intermediate substrate structure; the second intermediate substrate structure comprises an intermediate film layer, and an exposed surface of the intermediate film layer away from the auxiliary substrate is a second surface;
[0010] performing a second temperature treatment on the second surface to form a functional thin film layer based on the intermediate thin film layer;
[0011] Providing a target substrate, performing a second bonding process on the functional thin film layer and the target substrate, and performing a third temperature process on the second surface to form a composite substrate structure;
[0012] The auxiliary substrate in the composite substrate structure is separated from the first surface to form a functional thin film heterogeneous substrate structure; the functional thin film heterogeneous substrate structure includes the functional thin film layer and the target substrate from top to bottom.
[0013] In some embodiments, a first temperature of performing the first temperature treatment on the first surface and a third temperature of performing the third temperature treatment on the second surface are lower than a second temperature of performing the second temperature treatment on the second surface.
[0014] In some embodiments, the first temperature treatment, the second temperature treatment, and the third temperature treatment satisfy at least one of the following process conditions:
[0015] The first temperature treatment time is 3h to 30h, the heating rate ranges from 1°C / min to 2.5°C / min, and the first temperature ranges from 100°C to 600°C;
[0016] The second temperature treatment time is 3h to 30h, the heating rate is 1°C / min to 5°C / min, and the second temperature range is 200°C to 1100°C;
[0017] The third temperature treatment time is 3h to 30h, the heating rate ranges from 0.5°C / min to 2°C / min, and the third temperature ranges from 100°C to 500°C;
[0018] The gas atmosphere of the first temperature treatment, the second temperature treatment and the third temperature treatment is at least one of air, oxygen, nitrogen, an inert gas and a vacuum environment.
[0019] In some embodiments, the crystal orientation / polarization of the first surface of the functional thin film layer is the same as that of the functional substrate, and the crystal orientation / polarization of the second surface of the functional thin film layer is opposite to that of the functional substrate.
[0020] In some embodiments, the target substrate undergoes a second bonding process through the intermediate layer and the functional thin film layer;
[0021] The functional thin film heterogeneous substrate structure includes the intermediate layer, and the intermediate layer is located between the target substrate and the functional thin film layer;
[0022] Wherein, the bonding method of the second bonding treatment includes at least one of plasma activation bonding and surface activation bonding.
[0023] In some embodiments, the intermediate layer is prepared on at least one bonding surface of the functional film layer or the target substrate;
[0024] The material of the intermediate layer includes at least one of silicon oxide, amorphous silicon or silicon nitride, and when the second bonding process uses a surface activated bonding process, the intermediate layer cannot be silicon oxide.
[0025] In some embodiments, before separating the auxiliary substrate in the composite substrate structure from the first surface, the method further includes:
[0026] forming a barrier layer on a surface of the target substrate away from the second surface;
[0027] Wherein, the ratio of the thickness of the barrier layer to that of the auxiliary substrate is greater than or equal to a preset ratio.
[0028] In some embodiments, the separating the auxiliary substrate in the composite substrate structure from the first surface comprises at least one of a wafer grinding and a wet etching process, and the wet etching method comprises one or more of the following steps:
[0029] At room temperature, using a hydrofluoric acid solution or a buffered oxide etching solution with a mass fraction between 30% and 40% and an etching time ranging from 10s to 10000s, the oxide layer on the surface of the auxiliary substrate is removed by etching;
[0030] In an environment of 30° C. to 60° C., using a potassium hydroxide solution or a tetramethylammonium hydroxide solution with a mass fraction of 35% to 65% and an etching time ranging from 1 hour to 60 hours, the auxiliary substrate is etched away;
[0031] In an environment of 30° C. to 60° C., a mixed solution of an ammonia solution with a mass fraction of 10%-20% and a hydrogen peroxide solution with a mass fraction of 10%-20% is used, and the etching time ranges from 100s to 1000s to remove the residual particle layer on the surface.
[0032] On the other hand, the present application also provides a functional thin film heterogeneous substrate structure, which is prepared by any of the methods described above.
[0033] On the other hand, the present application also provides an electronic component, which includes a functional thin film heterogeneous substrate structure prepared by any of the above methods, or the functional thin film heterogeneous substrate structure described above.
[0034] The functional thin film heterogeneous substrate structure and its preparation method, and electronic components of the present application have at least the following beneficial effects:
[0035] In the embodiment of the present application, an auxiliary substrate is introduced to transfer the functional film layer to the target substrate, thereby forming a functional film heterogeneous substrate structure including a first surface and a second surface. Since the second surface in the intermediate film layer is subjected to a second temperature treatment, a high-quality functional film layer can be obtained, and the influence of ion beam stripping on the crystal quality can be significantly reduced; in addition, the first surface is far away from the ion implantation damage area in the functional substrate, which can not only significantly reduce the influence of ion beam stripping on the crystal quality, but also the third temperature treatment is performed after the functional film layer is bonded to the target substrate, without the need for high-temperature annealing treatment, which improves the bonding strength while avoiding the adverse effects on the performance caused by the conversion of water molecules at the bonding interface into interface bubbles, thus significantly improving the problem of bubble defects at the bonding interface.
[0036] In addition, unlike the conventional method which can only prepare a functional film surface whose exposed surface has a crystal orientation opposite to that of the functional substrate, the present application can more conveniently obtain a functional film whose first surface has the same crystal orientation as the functional substrate surface, which is beneficial to the efficient selection of raw materials. The preparation method of the present application can prepare a large number of functional film heterogeneous substrate structures with required structures at low cost and high reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions and advantages in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0038] Figure 1 is a schematic diagram of a method for preparing a functional thin film heterogeneous substrate structure provided in an embodiment of the present application;
[0039] Figure 2 It is a schematic diagram of a preparation process of a functional thin film heterogeneous substrate structure provided in an embodiment of the present application;
[0040] Figure 3A It is an electron microscope image of the interface and film edge of a functional thin film heterogeneous substrate structure provided in the related art;
[0041] Figure 3B It is an electron microscope image of the interface and film edge of another functional thin film heterogeneous substrate structure provided in the related art;
[0042] Figure 4 This is an electron microscope image of the interface and film edge of a functional thin film heterogeneous substrate structure provided in an embodiment of the present application. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0044] The "one embodiment" or "embodiment" referred to below refers to a specific feature, structure or characteristic that may be included in at least one implementation of the present invention. In the description of the present invention, unless otherwise clearly specified and limited, the orientation or position relationship indicated by the terms "upper", "lower", "left", "right", "top", "bottom", etc. is based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Moreover, the terms "first", "second", etc. are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein.
[0045] It should be understood that when describing the structure of a component, when a layer or a region is referred to as being located "on" or "above" another layer or another region, it may mean that it is directly located on the other layer or another region, or that other layers or regions are included between it and the other layer or another region. Moreover, if the component is turned over, the layer or a region will be located "below" or "beneath" another layer or another region.
[0046] In the traditional process of preparing heterogeneous thin film structures, the target wafer is bonded to the supporting substrate wafer, and then high-temperature annealing is performed to enhance the bonding strength. However, during the high-temperature annealing process, bubble defects will form at the bonding interface, resulting in a significant impact on the performance of acoustic, optical, and electrical devices prepared using the heterogeneous thin film structure, limiting the scope of use of the heterogeneous thin film structure.
[0047] In the related art, in order to reduce the bubble defects at the bonding interface, the main method is to improve the vacuum degree of the bonding step. However, this method will cause a decrease in the bonding strength and may cause debonding in subsequent steps, affecting the stability and performance of the device.
[0048] The present invention proposes a functional thin film heterogeneous substrate structure and a preparation method thereof, and an electronic component. The method comprises: providing an auxiliary substrate and a functional substrate, performing ion implantation on a first surface of the functional substrate to obtain a defect layer; the first surface is away from the defect layer; performing a first bonding treatment on the auxiliary substrate and the functional substrate to obtain a first intermediate substrate structure; the bonding interface between the functional substrate and the auxiliary substrate is the first surface; performing a first temperature treatment on the first surface, performing a stripping treatment on the first intermediate substrate structure along the defect layer to form a second intermediate substrate structure; the second intermediate substrate structure comprises an intermediate thin film layer, and the exposed surface of the intermediate thin film layer away from the auxiliary substrate is the second surface; performing a second temperature treatment on the second surface, and forming a functional thin film layer based on the intermediate thin film layer; providing a target substrate, performing a second bonding treatment on the functional thin film layer and the target substrate, and performing a third temperature treatment on the second surface to form a composite substrate structure; separating the auxiliary substrate in the composite substrate structure from the first surface to form a functional thin film heterogeneous substrate structure; the functional thin film heterogeneous substrate structure comprises a functional thin film layer and a target substrate from top to bottom.
[0049] In this way, the functional thin film layer is transferred to the target substrate by introducing an auxiliary substrate, forming a functional thin film heterogeneous substrate structure including a first surface and a second surface. Since the second surface in the intermediate thin film layer is subjected to the second temperature treatment, a high-quality functional thin film layer can be obtained, and the influence of ion beam stripping on the crystal quality can be significantly reduced; in addition, the first surface is far away from the ion implantation damage area in the functional substrate, which can not only significantly reduce the influence of ion beam stripping on the crystal quality, but also the third temperature treatment is performed after the functional thin film layer is bonded to the target substrate, without the need for high-temperature annealing treatment, which improves the bonding strength while avoiding the adverse effects on the performance caused by the conversion of water molecules at the bonding interface into interface bubbles, and significantly improves the problem of bubble defects at the bonding interface.
[0050] like Figure 1 to Figure 2 As shown, the embodiment of the present application provides a method for preparing a functional thin film heterogeneous substrate structure, comprising:
[0051] S101, providing an auxiliary substrate and a functional substrate, and performing ion implantation on a first surface of the functional substrate to obtain a defect layer; the first surface is away from the defect layer.
[0052] In this embodiment, the auxiliary substrate is made of silicon oxide. Of course, in other embodiments, the auxiliary substrate may be made of other suitable materials, such as silicon, silicon carbide, silicon on insulator, etc.
[0053] Exemplarily, the thickness and diameter of the auxiliary substrate may be any values that meet the requirements, for example, the thickness is 200 um to 1000 um, and the diameter of the wafer is 50 mm to 200 mm, which are not specifically limited here.
[0054] The functional substrate is a substrate for forming a functional thin film layer. Exemplarily, the material of the functional substrate may include, but is not limited to, one or more of lithium niobate, lithium tantalate, gallium nitride, calcium fluoride, silicon carbide, silicon, silicon oxide, sapphire, diamond, quartz, aluminum nitride, silicon on insulator, lithium niobate on insulator, and lithium tantalate on insulator. The thickness of the functional substrate may be any value that meets the requirements and is not specifically limited here.
[0055] In an embodiment, Figure 2 As shown, the functional substrate 20 includes a first surface a1 for ion implantation. The first surface a1 in the functional substrate 20 is subjected to ion implantation of first ions to form a defect layer (not shown) in the functional substrate 20. In the functional substrate 20, the region located in the defect layer and the vicinity thereof is an implantation damage region. The first surface a1 in the functional substrate 20 is away from the defect layer and also away from the implantation damage region.
[0056] Optionally, the type of the first ion may include one or more of hydrogen ions, helium ions and argon ions, the implantation energy may be 40 KeV to 400 KeV, and the implantation dose may be 1E14 / cm 2 to 1E17 / cm 2 The implanted first ions are distributed near the defect layer and away from the first surface.
[0057] S103, performing a first bonding process on the auxiliary substrate and the functional substrate to obtain a first intermediate substrate structure; the bonding interface between the functional substrate and the auxiliary substrate is a first surface.
[0058] In an embodiment, continue as Figure 2 As shown, the auxiliary substrate 10 and the first surface a1 of the functional substrate 20 can be subjected to a first bonding process by a wafer bonding process to obtain a first intermediate substrate structure 31. At this time, the bonding interface between the functional substrate 20 and the auxiliary substrate 10 is the first surface a1.
[0059] Optionally, the wafer bonding process may be, but is not limited to, direct bonding, hydrophilic bonding, or one or more of the above. As an example, taking direct bonding as an example, the surfaces to be bonded are subjected to plasma activation treatment, and the two surfaces are directly bonded, and the type of plasma activation includes, but is not limited to, nitrogen, oxygen, or argon, and the bonding temperature may be 20° C. to 800° C.
[0060] S105, performing a first temperature treatment on the first surface, and performing a stripping treatment on the first intermediate substrate structure along the defective layer to form a second intermediate substrate structure; the second intermediate substrate structure includes an intermediate film layer, and an exposed surface of the intermediate film layer away from the auxiliary substrate is a second surface.
[0061] In an embodiment, continue as Figure 2As shown, after performing the first bonding process, the first surface a1 may be subjected to a first temperature treatment to enhance the bonding strength of the bonding interface in the first intermediate substrate structure. At the same time, the first intermediate substrate structure 31 is subjected to a stripping process along the defect layer to strip off part of the functional substrate to form a second intermediate substrate structure 32. The stripping process may include but is not limited to mechanical stripping or thermal stripping.
[0062] The second intermediate substrate structure 32 includes an auxiliary substrate 10 and an intermediate film layer 21, which is the remaining functional substrate thin layer. The exposed surface of the intermediate film layer 21 away from the auxiliary substrate 10 is the second surface a2. Similar to the material of the functional substrate, the material of the intermediate film layer is at least one of lithium niobate, lithium tantalate, aluminum nitride, gallium nitride, calcium fluoride, silicon, silicon oxide, sapphire, silicon carbide, and diamond.
[0063] S107, performing a second temperature treatment on the second surface to form a functional thin film layer based on the intermediate thin film layer.
[0064] In an embodiment, continue as Figure 2 As shown, after forming the second intermediate substrate structure, the second surface of the intermediate film layer in the second intermediate substrate structure can be subjected to a second temperature treatment to convert the intermediate film layer 21 into a functional film layer 22. Since the intermediate film layer is obtained based on ion implantation and stripping of the functional substrate, the second surface of the intermediate film layer is subjected to a second temperature treatment to help the intermediate film layer recover its crystal quality after ion implantation, reduce the adverse effects of ion implantation, and form a functional film layer with high crystal quality. The second temperature treatment here refers to a high temperature annealing treatment.
[0065] Optionally, the thickness of the functional film layer is 0.02 um to 20 um, and the diameter of the film layer is 50 mm to 200 mm.
[0066] In some embodiments, the crystal orientation / polarization of the first surface of the functional thin film layer is the same as that of the functional substrate, and the crystal orientation / polarization of the second surface of the functional thin film layer is opposite to that of the functional substrate. In this way, the functional thin film layer is transferred to the target substrate by introducing an auxiliary substrate, so that the crystal orientation / polarization of the exposed first surface of the functional thin film layer is the same as that of the functional substrate, which is conducive to the efficient selection of raw materials, and is convenient for preparing a functional thin film heterogeneous substrate structure of a specific cut according to demand, thereby reducing the preparation cost and reliability.
[0067] S109, providing a target substrate, performing a second bonding process on the functional thin film layer and the target substrate, and performing a third temperature process on the second surface to form a composite substrate structure.
[0068] Optionally, the material of the target substrate may include, but is not limited to, one or more of silicon, silicon oxide, sapphire, silicon carbide, quartz, aluminum nitride, gallium nitride, diamond, lithium niobate, lithium tantalate, silicon on insulator, lithium niobate on insulator, lithium tantalate on insulator, etc. The thickness of the target substrate may be 200um to 1000um, and the diameter of the wafer may be 50mm to 200mm.
[0069] In an embodiment, continue as Figure 2 As shown, after forming the functional film layer 22, the provided target substrate 40 and the functional film layer 22 can be subjected to a second bonding treatment, where the bonding interface of the second bonding treatment is the second surface a2. Afterwards, the second surface of the second bonding treatment is subjected to a third temperature treatment to form a composite substrate structure 33, which includes an auxiliary substrate 10, a functional film layer 22 and a target substrate 40. Here, by performing a third temperature treatment on the second surface, the bonding strength of the bonding interface in the composite substrate structure can be enhanced. In addition, the third temperature treatment here can be a low-temperature heat treatment, without the need for a high-temperature heat treatment, which can avoid the appearance of bubbles at the bonding interface and reduce bubble defects.
[0070] In some embodiments, the bonding method of the second bonding process includes at least one of plasma activated bonding (PAB) and surface activated bonding (SAB). Optionally, the bonding temperature of the second bonding process is in the range of 20°C-30°C. The gas used in plasma activated bonding is Ar, O2 or N2, the activation time is not less than 10s, and the activation gas pressure is not higher than 10mbar; the gas used in surface activated bonding is Ar, and the activation vacuum is not higher than 1e-7mbar.
[0071] S111, separating the auxiliary substrate in the composite substrate structure from the first surface to form a functional thin film heterogeneous substrate structure; the functional thin film heterogeneous substrate structure includes a functional thin film layer and a target substrate from top to bottom.
[0072] In an embodiment, continue as Figure 2 As shown, after forming the functional thin film layer, the auxiliary substrate 10 in the composite substrate structure 33 can be separated from the first surface a1 to form a functional thin film heterogeneous substrate structure 50. The functional thin film heterogeneous substrate structure 50 includes a functional thin film layer 22 and a target substrate 40 from top to bottom. The functional thin film layer 22 has a first surface a1 and a second surface a2. The first surface is the surface of the functional thin film layer away from the bonding interface, and the second surface is the bonding interface between the functional thin film layer and the target substrate. In the process of forming the functional thin film heterogeneous substrate structure, the first surface or the second surface is sequentially subjected to a first temperature treatment, a second temperature treatment, and a third temperature treatment.
[0073] In some embodiments, a first temperature at which the first surface is subjected to the first temperature treatment and a third temperature at which the second surface is subjected to the third temperature treatment are less than or equal to a second temperature at which the second surface is subjected to the second temperature treatment.
[0074] In some embodiments, the absolute value of the difference between the first temperature of the first surface subjected to the first temperature treatment and the third temperature of the second surface subjected to the third temperature treatment is 0-300° C. Generally, the value of the first temperature is greater than the value of the third temperature, and the temperature difference between the two is 0-300° C.
[0075] In some embodiments, the first temperature treatment, the second temperature treatment, and the third temperature treatment satisfy at least one of the following process conditions:
[0076] 1) The first temperature treatment time is 3h to 30h, the heating rate ranges from 1°C / min to 2.5°C / min, and the first temperature ranges from 100°C to 600°C;
[0077] 2) The second temperature treatment time is 3h to 30h, the heating rate is 1°C / min to 5°C / min, and the second temperature range is 200°C to 1100°C;
[0078] 3) The time of the third temperature treatment is 3h to 30h, the heating rate ranges from 0.5°C / min to 2°C / min, and the third temperature ranges from 100°C to 500°C;
[0079] 4) The gas atmosphere of the first temperature treatment, the second temperature treatment and the third temperature treatment is at least one of air, oxygen, nitrogen, an inert gas and a vacuum environment.
[0080] The first temperature, the second temperature and the third temperature can be any suitable value in the above-mentioned processing time, temperature range and heating rate range, which are not given examples one by one here. The first temperature treatment, the second temperature treatment and the third temperature treatment are configured by the above-mentioned process conditions, and the mutual cooperation of multiple temperature treatments can further reduce the probability of bubble defects while ensuring the quality of the prepared substrate structure.
[0081] Optionally, the process of separating the auxiliary substrate from the first surface includes at least one of a grinding process and an etching process. In addition, after separating the auxiliary substrate from the first surface, the first surface is planarized, and the planarized removal thickness can be 0 to 100 nm.
[0082] In some embodiments, the grinding process includes: performing wafer thinning on a surface of the bonding structure away from the target substrate so that the remaining thickness of the auxiliary substrate is no greater than 50 um.
[0083] In some other embodiments, the etching process includes a wet etching process, wherein the wet etching method includes one or more of the following steps:
[0084] At room temperature, using a hydrofluoric acid solution or a buffered oxide etching solution with a mass fraction of 30% to 40% and an etching time ranging from 10s to 10000s, the oxide layer on the surface of the auxiliary substrate is etched away;
[0085] In an environment of 30° C. to 60° C., using a potassium hydroxide solution or a tetramethylammonium hydroxide solution with a mass fraction of 35% to 65% and an etching time ranging from 1 h to 60 h, the auxiliary substrate is etched away;
[0086] In an environment of 30° C. to 60° C., a mixed solution of an ammonia solution with a mass fraction of 10%-20% and a hydrogen peroxide solution with a mass fraction of 10%-20% is used, and the etching time ranges from 100s to 1000s to remove the residual particle layer on the surface.
[0087] In some embodiments, the target substrate undergoes a second bonding process through the intermediate layer and the functional film layer. At this time, the functional film heterogeneous substrate structure further includes an intermediate layer, and the intermediate layer is located between the target substrate and the functional film layer. In this way, by introducing the intermediate layer at the bonding interface position, the bubble defects at the bonding interface are further improved, thereby improving the device performance.
[0088] In some embodiments, the intermediate layer is prepared on at least one bonding surface of the functional film layer or the target substrate. Alternatively, the intermediate layer can be prepared on the second surface of the functional film layer, or the intermediate layer can be prepared on the target substrate, or the intermediate layer can be prepared on the second surface of the functional film layer and the target substrate. The intermediate layer assists the second bonding process between the functional film layer and the target substrate.
[0089] Optionally, the material of the intermediate layer includes at least one of silicon oxide, amorphous silicon or silicon nitride, and when the second bonding process uses a surface activated bonding process, the intermediate layer cannot be silicon oxide. Exemplarily, the thickness of the intermediate layer can range from 0 to 10000 nm.
[0090] In some embodiments, before separating the auxiliary substrate in the composite substrate structure from the first surface, the method further includes: forming a barrier layer on the surface of the target substrate away from the second surface. Wherein, the ratio of the thickness of the barrier layer to the auxiliary substrate is greater than or equal to a preset ratio. Exemplarily, the preset ratio may include any value in the range of 0.002-0.005, such as 0.003. The material of the barrier layer may be silicon oxide. In this way, by providing a barrier layer on the target substrate, the target substrate is protected from damage and adverse effects in subsequent processes, thereby improving the quality of the device.
[0091] In the above embodiment, the functional film layer is transferred to the target substrate by introducing an auxiliary substrate, so as to form a functional film heterogeneous substrate structure including a first surface and a second surface. Since the second surface in the intermediate film layer is subjected to the second temperature treatment, a high-quality functional film layer can be obtained, and the influence of ion beam stripping on the crystal quality can be significantly reduced; in addition, the first surface is far away from the ion implantation damage area in the functional substrate, which can not only significantly reduce the influence of ion beam stripping on the crystal quality, but also the third temperature treatment is performed after the functional film layer is bonded to the target substrate, without the need for high-temperature annealing treatment, which improves the bonding strength while avoiding the adverse effects on the performance caused by the conversion of water molecules at the bonding interface into interface bubbles, and significantly improves the problem of bubble defects at the bonding interface.
[0092] In addition, unlike the conventional method which can only prepare a functional film surface whose exposed surface has a crystal orientation opposite to that of the functional substrate, the present application can more conveniently obtain a functional film whose first surface has the same crystal orientation as the functional substrate surface, which is beneficial to the efficient selection of raw materials. The preparation method of the present application can prepare a large number of functional film heterogeneous substrate structures with required structures at low cost and high reliability.
[0093] On the other hand, the present application also provides a functional thin film heterogeneous substrate structure, wherein the functional thin film heterogeneous substrate structure comprises a functional thin film layer and a target substrate, the functional thin film layer has a first surface and a second surface, the first surface is a surface of the functional thin film layer away from a bonding interface, and the second surface is a bonding interface between the functional thin film layer and the target substrate. In the process of forming the functional thin film heterogeneous substrate structure, the first surface or the second surface is sequentially subjected to a first temperature treatment, a second temperature treatment, and a third temperature treatment.
[0094] In some embodiments, a first temperature at which the first surface is subjected to the first temperature treatment and a third temperature at which the second surface is subjected to the third temperature treatment are less than or equal to a second temperature at which the second surface is subjected to the second temperature treatment.
[0095] In some embodiments, an absolute value of a difference between a first temperature at which the first surface is subjected to the first temperature treatment and a third temperature at which the second surface is subjected to the third temperature treatment is in a range of 0 to 300°C.
[0096] In some embodiments, the first temperature treatment, the second temperature treatment, and the third temperature treatment satisfy at least one of the following process conditions:
[0097] 1) The first temperature treatment time is 3h to 30h, the heating rate ranges from 1°C / min to 2.5°C / min, and the first temperature ranges from 100°C to 600°C;
[0098] 2) The second temperature treatment time is 3h to 30h, the heating rate is 1°C / min to 5°C / min, and the second temperature range is 200°C to 1100°C;
[0099] 3) The time of the third temperature treatment is 3h to 30h, the heating rate ranges from 0.5°C / min to 2°C / min, and the third temperature ranges from 100°C to 500°C;
[0100] 4) The gas atmosphere of the first temperature treatment, the second temperature treatment and the third temperature treatment is at least one of air, oxygen, nitrogen, an inert gas and a vacuum environment.
[0101] The first temperature, the second temperature and the third temperature may be any suitable value in the above-mentioned processing time, temperature range and heating rate range, which are not given examples one by one here.
[0102] In some embodiments, the crystal orientation of the first surface of the functional thin film layer is the same as that of the functional substrate, and the crystal orientation of the second surface of the functional thin film layer is opposite to that of the functional substrate.
[0103] In some embodiments, the functional thin film heterogeneous substrate structure further includes an intermediate layer, and the intermediate layer is located between the target substrate and the functional thin film layer.
[0104] In some embodiments, the intermediate layer is prepared on at least one bonding surface of the functional film layer or the target substrate. Alternatively, the intermediate layer can be prepared on the second surface of the functional film layer, or the intermediate layer can be prepared on the target substrate, or the intermediate layer can be prepared on the second surface of the functional film layer and the target substrate. The intermediate layer assists the second bonding process between the functional film layer and the target substrate.
[0105] It should be noted that the above-mentioned functional thin film heterogeneous substrate structure is prepared by the above-mentioned method. The specific details and beneficial effects in the embodiment of the functional thin film heterogeneous substrate structure here can be referred to the embodiment of the preparation method of the above-mentioned functional thin film heterogeneous substrate structure, and the details and beneficial effects not expanded in the above-mentioned structure embodiment can be referred to the above-mentioned method embodiment, which will not be repeated here.
[0106] In order to verify the improvement effect of the functional thin film heterogeneous substrate structure prepared by the method embodiment of the present application, the effect is compared by collecting electron microscope images of the functional thin film heterogeneous substrate structure before and after the improvement. Figure 3A It is an electron microscope image of the interface and film edge of a functional thin film heterogeneous substrate structure prepared by a PAB bonding process in the related art. Figure 3B It is an electron microscope image of the interface and film edge of a functional thin film heterogeneous substrate structure prepared by the SAB bonding process in the related art. Figure 4: is an electron microscope image of the interface and film edge of the improved functional thin film heterogeneous substrate structure prepared by the method embodiment of the present application. After comparative analysis, it can be seen that before the improvement, Figure 3A and Figure 3B As shown in FIG. 1 , there are a large number of bubble defects in the functional thin film heterogeneous substrate structure prepared in the related art; and after improvement, as shown in FIG. Figure 4 As shown, the improved functional thin film heterogeneous substrate structure prepared by the method embodiment of the present application has almost no bubble defects.
[0107] On the other hand, the present application also provides an electronic component, which includes a functional thin film heterogeneous substrate structure prepared by any of the above methods, or the aforementioned functional thin film heterogeneous substrate structure.
[0108] Exemplarily, the electronic components may be acoustic, optical or electrical devices, for example, the electronic components may include but are not limited to photonic devices, power devices, acoustic resonators and filters, etc. The electronic components also include an electrode layer, which may be directly or indirectly disposed on the surface of the functional thin film heterogeneous substrate structure to realize the device function of the electronic components.
[0109] It should be noted that the specific details and beneficial effects of the above electronic component embodiments can be found in the above structural embodiments or method embodiments, which will not be repeated here.
[0110] The above description has fully disclosed the specific implementation methods of the present application. It should be pointed out that any changes made by technicians familiar with the field to the specific implementation methods of the present application do not deviate from the scope of the claims of the present application. Accordingly, the scope of the claims of the present application is not limited to the above specific implementation methods.
Claims
1. A method for preparing a functional thin film heterogeneous substrate structure, characterized in that: The preparation method comprises: Providing an auxiliary substrate and a functional substrate, and performing ion implantation on a first surface of the functional substrate to obtain a defect layer; the first surface is away from the defect layer; Performing a first bonding process on the auxiliary substrate and the functional substrate to obtain a first intermediate substrate structure; the bonding interface between the functional substrate and the auxiliary substrate is the first surface; Performing a first temperature treatment on the first surface, and performing a peeling treatment on the first intermediate substrate structure along the defective layer to form a second intermediate substrate structure; the second intermediate substrate structure comprises an intermediate film layer, and an exposed surface of the intermediate film layer away from the auxiliary substrate is a second surface; performing a second temperature treatment on the second surface to form a functional thin film layer based on the intermediate thin film layer; Providing a target substrate, performing a second bonding process on the functional thin film layer and the target substrate, and performing a third temperature process on the second surface to form a composite substrate structure; The auxiliary substrate in the composite substrate structure is separated from the first surface to form a functional thin film heterogeneous substrate structure; the functional thin film heterogeneous substrate structure includes the functional thin film layer and the target substrate from top to bottom.
2. The method according to claim 1, characterized in that: A first temperature of the first temperature treatment performed on the first surface and a third temperature of the third temperature treatment performed on the second surface are lower than a second temperature of the second temperature treatment performed on the second surface.
3. The method according to claim 2, characterized in that The first temperature treatment, the second temperature treatment and the third temperature treatment meet at least one of the following process conditions: The first temperature treatment time is 3h to 30h, the heating rate ranges from 1°C / min to 2.5°C / min, and the first temperature ranges from 100°C to 600°C; The second temperature treatment time is 3h to 30h, the heating rate is 1°C / min to 5°C / min, and the second temperature range is 200°C to 1100°C; The third temperature treatment time is 3h to 30h, the heating rate ranges from 0.5°C / min to 2°C / min, and the third temperature ranges from 100°C to 500°C; The gas atmosphere of the first temperature treatment, the second temperature treatment and the third temperature treatment is at least one of air, oxygen, nitrogen, an inert gas and a vacuum environment.
4. The method according to claim 1, characterized in that The crystal orientation / polarization of the first surface of the functional thin film layer is the same as that of the functional substrate, and the crystal orientation / polarization of the second surface of the functional thin film layer is opposite to that of the functional substrate.
5. The method according to any one of claims 1 to 4, characterized in that: The target substrate is subjected to a second bonding process via the intermediate layer and the functional thin film layer; The functional thin film heterogeneous substrate structure includes the intermediate layer, and the intermediate layer is located between the target substrate and the functional thin film layer; Wherein, the bonding method of the second bonding treatment includes at least one of plasma activation bonding and surface activation bonding.
6. The method according to claim 5, characterized in that The intermediate layer is prepared on the bonding surface of at least one layer of the functional film layer or the target substrate; The material of the intermediate layer includes at least one of silicon oxide, amorphous silicon or silicon nitride, and when the second bonding process uses a surface activated bonding process, the intermediate layer cannot be silicon oxide.
7. The method according to claim 1, characterized in that Before separating the auxiliary substrate in the composite substrate structure from the first surface, the method further comprises: forming a barrier layer on a surface of the target substrate away from the second surface; Wherein, the ratio of the thickness of the barrier layer to that of the auxiliary substrate is greater than or equal to a preset ratio.
8. The method according to claim 1, characterized in that The step of separating the auxiliary substrate in the composite substrate structure from the first surface comprises at least one of wafer grinding and wet etching processes, and the wet etching method comprises one or more of the following steps: At room temperature, a hydrofluoric acid solution or a buffered oxide etchant with a mass fraction between 30% and 40% is used, and the etching time ranges from 10s to 10000s; Etching and removing the oxide layer on the surface of the auxiliary substrate; In an environment of 30° C. to 60° C., using a potassium hydroxide solution or a tetramethylammonium hydroxide solution with a mass fraction of 35% to 65% for an etching time ranging from 1 hour to 60 hours to remove the auxiliary substrate; In an environment of 30° C. to 60° C., a mixed solution of an ammonia solution with a mass fraction of 10%-20% and a hydrogen peroxide solution with a mass fraction of 10%-20% is used, and the etching time ranges from 100s to 1000s to remove the residual particle layer on the surface.
9. A functional thin film heterogeneous substrate structure, characterized in that: The functional thin film heterogeneous substrate structure is prepared by the method according to any one of claims 1-8.
10. An electronic component, characterized in that: The electronic component comprises a functional thin film heterogeneous substrate structure prepared by the method according to any one of claims 1 to 8, or the electronic component comprises the functional thin film heterogeneous substrate structure according to claim 9.