Semiconductor device and method for manufacturing semiconductor device
By introducing oxygen and nitrogen into the metal oxide layer of the semiconductor device to form an oxygen concentration gradient, the problem of carrier density and defect energy levels in miniaturized transistors is solved, and electrical characteristics, reliability and power consumption are improved. promote.
Patent Information
- Application Number
- CN202410756119.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-03-13
- Filing Date
- 2018-03-02
- Publication Date
- 2024-10-08
AI Technical Summary
In miniaturized transistors, the carrier density and defect energy level in the channel region have a significant impact on the electrical characteristics and reliability. It is difficult to achieve semiconductor devices with good electrical characteristics, reliability and low power consumption at the same time using existing technology.
A metal oxide layer containing indium and zinc is used to form an oxygen concentration gradient in the film thickness direction and introduce excess oxygen and nitrogen into the insulating layer to suppress the formation of oxygen vacancies and hydrogen, thereby reducing carrier density and defects. density of states.
A semiconductor device with good electrical characteristics is realized, which improves reliability and productivity while reducing power consumption.
Smart Images

Figure CN118748210A_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese invention patent application with the application date of March 2, 2018, application number 201810172995.8, and invention name “Semiconductor device and method for manufacturing semiconductor device”. Technical Field
[0002] One embodiment of the present invention relates to a semiconductor device and a method for manufacturing the semiconductor device. One embodiment of the present invention relates to a transistor and a method for manufacturing the transistor. One embodiment of the present invention relates to a display device and a method for manufacturing the display device.
[0003] Note that in this specification, etc., a semiconductor device refers to any device that can operate by utilizing semiconductor characteristics. A display device, a light-emitting device, a lighting device, an electro-optical device, a semiconductor circuit, and an electronic device may include a semiconductor device.
[0004] One embodiment of the present invention is not limited to the above-mentioned technical field. As an example of the technical field of one embodiment of the present invention disclosed in this specification, etc., there can be cited semiconductor devices, display devices, light-emitting devices, lighting devices, power storage devices, storage devices, and their driving methods or their manufacturing methods. Background Art
[0005] Oxide semiconductors have attracted attention as semiconductor materials that can be used for transistors. For example, Patent Document 1 discloses a semiconductor device in which a plurality of oxide semiconductor layers are stacked, in which an oxide semiconductor layer used as a channel contains indium and gallium, and the ratio of indium is higher than that of gallium, thereby improving field effect mobility (sometimes simply referred to as mobility or μFE).
[0006] Since oxide semiconductors that can be used for semiconductor layers can be formed by sputtering or the like, they can be used for semiconductor layers of transistors that constitute large display devices. In addition, since part of the production equipment for transistors using amorphous silicon can be improved and used, equipment investment can also be suppressed. In addition, transistors using oxide semiconductors have high field effect mobility, so a high-function display device with an integrated drive circuit can be realized.
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2014-7399 Summary of the invention
[0008] With the high definition of display devices or the high integration of semiconductor devices, transistors are required to be miniaturized. As a specific example of miniaturization of transistors, shortening the channel length can be cited. However, in transistors with short channel lengths, the carrier density and defect energy levels in the channel region significantly affect electrical characteristics and reliability.
[0009] In view of the above problems, one of the purposes of one embodiment of the present invention is to provide a semiconductor device with good electrical characteristics. One of the purposes of one embodiment of the present invention is to provide a semiconductor device with high reliability. One of the purposes of one embodiment of the present invention is to provide a semiconductor device with low power consumption. One of the purposes of one embodiment of the present invention is to provide a novel semiconductor device. One of the purposes of one embodiment of the present invention is to provide a method for manufacturing a semiconductor device with high productivity. One of the purposes of one embodiment of the present invention is to provide a method for manufacturing a semiconductor device with high yield. One of the purposes of one embodiment of the present invention is to provide a novel method for manufacturing a semiconductor device.
[0010] Note that the description of these purposes does not prevent the existence of other purposes. One embodiment of the present invention does not necessarily achieve all of the above purposes. In addition, purposes other than the above can be extracted from the description of the specification, drawings, claims, etc.
[0011] One embodiment of the present invention is a semiconductor device, comprising: a gate electrode; a first insulating layer on the gate electrode; a metal oxide layer on the first insulating layer; a pair of electrodes on the metal oxide layer; and a second insulating layer on the pair of electrodes, wherein the metal oxide layer contains indium, element M (M is one or more of gallium, aluminum, silicon, boron, yttrium, tin, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten and magnesium) and zinc, the first insulating layer includes a first region and a second region, the first region is in contact with the metal oxide layer and includes a region whose oxygen content is higher than that of the second region, the second region includes a region whose nitrogen content is higher than that of the first region, the metal oxide layer has at least an oxygen concentration gradient in the film thickness direction, and the concentration gradient is higher on the first region side and the second insulating layer side.
[0012] In the above semiconductor device, it is preferable that the first region includes a region greater than or equal to 1 nm and less than or equal to 10 nm in a film thickness direction.
[0013] In the semiconductor device, preferably, when the atomic number ratio of In is 1, the atomic number ratio of M in the metal oxide layer is 0.5 to 1.5, and the atomic number ratio of Zn is 0.1 to 2.
[0014] In the semiconductor device, preferably, when the atomic ratio of In is 4, the atomic ratio of M is 1.5 to 2.5, and the atomic ratio of Zn is 2 to 4 in the metal oxide layer.
[0015] In the semiconductor device, preferably, when the atomic ratio of In is 5, the atomic ratio in the metal oxide layer is 0.5 to 1.5, and the atomic ratio of Zn is 5 to 7.
[0016] In the above semiconductor device, it is preferred that the metal oxide layer includes a first metal oxide layer and a second metal oxide layer on the first metal oxide layer, and the first metal oxide layer includes a region having lower crystallinity than the second metal oxide layer.
[0017] In the above-mentioned semiconductor device, it is preferred that the metal oxide layer includes a first metal oxide layer, a second metal oxide layer on the first metal oxide layer, and a third metal oxide layer in contact with the lower side of the first metal oxide layer, and the first metal oxide layer includes a region whose crystallinity is lower than that of one or both of the second metal oxide layer and the third metal oxide layer.
[0018] In the above semiconductor device, preferably, a third insulating layer is further included on the second insulating layer, and the third insulating layer contains silicon and nitrogen.
[0019] In the above semiconductor device, preferably, a third insulating layer is further included on the second insulating layer, and the third insulating layer contains element X (X is one or more of aluminum, indium, gallium, and zinc) and oxygen.
[0020] One embodiment of the present invention is a method for manufacturing a semiconductor device, comprising: a process of forming a gate electrode; a process of forming a first insulating layer on the gate electrode; a process of adding oxygen near the surface of the first insulating layer; a process of forming a metal oxide layer on the first insulating layer; a process of forming a pair of electrodes on the metal oxide layer; and a process of forming a second insulating layer on the pair of electrodes, wherein in the process of forming the metal oxide layer, the process is divided into a first process and a second process, film formation is continuously performed in a vacuum, the first process is performed before the second process, and in the second process, the oxygen flow ratio in the entire film forming gas is higher than that in the first process.
[0021] One embodiment of the present invention is a method for manufacturing a semiconductor device, comprising: a process of forming a gate electrode; a process of forming a first insulating layer on the gate electrode; a process of adding oxygen near the surface of the first insulating layer; a process of forming a metal oxide layer on the first insulating layer; a process of forming a pair of electrodes on the metal oxide layer; and a process of forming a second insulating layer on the pair of electrodes, wherein in the process of forming the metal oxide layer, the process is divided into a first process to a third process, and film formation is continuously performed in a vacuum, the first process is performed before the second process, and in the second process, the oxygen flow rate ratio in the entire film forming gas is higher than that in the first process, and the third process is performed before the first process, and the oxygen flow rate ratio in the entire film forming gas is higher than that in the first process.
[0022] According to one embodiment of the present invention, a semiconductor device with good electrical characteristics can be provided. According to one embodiment of the present invention, a semiconductor device with high reliability can be provided. According to one embodiment of the present invention, a semiconductor device with low power consumption can be provided. According to one embodiment of the present invention, a novel semiconductor device can be provided. According to one embodiment of the present invention, a method for manufacturing a semiconductor device with high productivity can be provided. According to one embodiment of the present invention, a method for manufacturing a semiconductor device with high yield can be provided. According to one embodiment of the present invention, a novel method for manufacturing a semiconductor device can be provided.
[0023] Note that the description of these effects does not prevent the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of the above effects. In addition, effects other than the above can be extracted from the description of the specification, drawings, claims, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figures 1A to 1C It is an example of the structure of a semiconductor device;
[0025] FIG. 2A to FIG. 2C is a schematic diagram showing the path of oxygen diffusing in a semiconductor layer;
[0026] Figure 3A and Figure 3B is a cross-sectional view showing an example of a gap portion;
[0027] FIG. 4A to FIG. 4C It is an example of the structure of a semiconductor device;
[0028] FIG. 5A to FIG. 5C It is an example of the structure of a semiconductor device;
[0029] FIG. 6A to FIG. 6C It is an example of the structure of a semiconductor device;
[0030] FIG. 7A to FIG. 7C It is an example of the structure of a semiconductor device;
[0031] FIG. 8A to FIG. 8C It is an example of the structure of a semiconductor device;
[0032] 9A to 9C It is an example of the structure of a semiconductor device;
[0033] FIG. 10A to FIG. 10C is a diagram illustrating a method for manufacturing a semiconductor device;
[0034] FIG. 11A to FIG. 11C is a diagram illustrating a method for manufacturing a semiconductor device;
[0035] Fig. 12A and Fig. 12Bis a diagram illustrating a method for manufacturing a semiconductor device;
[0036] Fig.13A and Fig. 13B is a diagram illustrating a method for manufacturing a semiconductor device;
[0037] FIG. 14A to FIG. 14C is a diagram illustrating a method for manufacturing a semiconductor device;
[0038] Fig.15A and Fig. 15B It is a structural example of a display device;
[0039] Fig.16 It is a structural example of a display device;
[0040] Fig.17 It is a structural example of a display device;
[0041] Fig.18 It is a structural example of a display device;
[0042] Fig.19 It is a structural example of a display device;
[0043] Fig. 20 It is a structural example of a display device;
[0044] FIG. 21A to FIG. 21C is a block diagram and circuit diagram of the display device;
[0045] Fig. 22 is a block diagram of a display device;
[0046] FIG. 23A to FIG. 23D It is a structural example of an electronic device;
[0047] Fig.24A and Fig. 24B It is a structural example of a television device;
[0048] Fig.25 is the XPS spectrum according to Example 1;
[0049] FIG. 26A to FIG. 26C is a cross-sectional TEM image according to Example 1;
[0050] Fig.27A and Fig.27B is a cross-sectional TEM image according to Example 1;
[0051] Fig.28 is a diagram illustrating measurement coordinates of a sample according to Example 2;
[0052] Fig.29 is the XPS spectrum according to Example 2;
[0053] Fig.30is the XPS spectrum according to Example 2;
[0054] Fig.31 is the XPS spectrum according to Example 2;
[0055] Fig.32 is the XPS spectrum according to Example 2;
[0056] Fig.33A and Fig.33B is the Id-Vg characteristic of the transistor according to Example 3;
[0057] Fig.34A and Fig.34B is the Id-Vg characteristic of the transistor according to Example 3;
[0058] Fig.35A and Fig.35B is the Id-Vg characteristic of the transistor according to Example 3;
[0059] Fig.36A and Fig.36B is the Id-Vg characteristic of the transistor according to Example 3;
[0060] Fig.37 It is the GBT test result of the transistor according to Example 3. DETAILED DESCRIPTION
[0061] The following describes the embodiments with reference to the accompanying drawings. However, a person skilled in the art can easily understand that the embodiments can be implemented in a plurality of different forms, and the methods and details can be transformed into various forms without departing from the purpose and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the contents described in the embodiments shown below.
[0062] In the accompanying drawings, for the sake of clarity, the size, thickness of the layer or the region are sometimes exaggerated. Therefore, the present invention is not necessarily limited to the above-mentioned dimensions. In addition, in the accompanying drawings, ideal examples are schematically shown, so the present invention is not limited to the shapes or numerical values shown in the accompanying drawings.
[0063] The ordinal numbers such as “first”, “second” and “third” used in the present specification are added to avoid confusion among constituent elements, and are not intended to limit the number.
[0064] In this specification, for convenience, words and phrases such as "upper" and "lower" indicating configuration are used to explain the positional relationship of the components with reference to the drawings. In addition, the positional relationship of the components is appropriately changed according to the direction in which each component is described. Therefore, the words and phrases described in this specification are not limited and can be appropriately replaced according to the situation.
[0065] In this specification, etc., a transistor refers to an element including at least three terminals: a gate, a drain, and a source. The transistor has a channel region between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode), and current can flow between the source and the drain through the channel region. Note that in this specification, etc., the channel region refers to a region where current mainly flows.
[0066] In addition, when transistors with different polarities are used or when the direction of current changes during circuit operation, the functions of the source and the drain may be interchanged. Therefore, in this specification, etc., the source and the drain may be interchanged.
[0067] In this specification, "electrical connection" includes connection through "an element having some kind of electrical function". Here, "an element having some kind of electrical function" is not particularly limited as long as it can transmit and receive electrical signals between the connected objects. For example, "an element having some kind of electrical function" includes not only electrodes and wiring, but also switching elements such as transistors, resistors, inductors, capacitors, and other elements having various functions.
[0068] In this specification, "parallel" means a state where the angle formed by two straight lines is greater than -10° and less than 10°. Therefore, a state where the angle is greater than -5° and less than 5° is also included. In addition, "perpendicular" means a state where the angle formed by two straight lines is greater than 80° and less than 100°. Therefore, a state where the angle is greater than 85° and less than 95° is also included.
[0069] In addition, in this specification, "film" and "layer" may be interchanged. For example, "conductive layer" may be replaced with "conductive film". Also, for example, "insulating film" may be replaced with "insulating layer".
[0070] In this specification, etc., unless otherwise specified, the off-state current refers to the drain current when the transistor is in the off state (also referred to as the non-conducting state or the blocking state). Unless otherwise specified, in an n-channel transistor, the off state refers to the state in which the voltage Vgs between the gate and the source is lower than the threshold voltage Vth, and in a p-channel transistor, the off state refers to the state in which the voltage Vgs between the gate and the source is higher than the threshold voltage Vth. For example, the off-state current of an n-channel transistor sometimes refers to the drain current when the voltage Vgs between the gate and the source is lower than the threshold voltage Vth.
[0071] The off-state current of a transistor sometimes depends on Vgs. Therefore, "the off-state current of the transistor is less than 1" sometimes means that there is a value of Vgs that makes the off-state current of the transistor less than 1. The off-state current of a transistor sometimes refers to: an off-state when Vgs is a predetermined value; an off-state when Vgs is a value within a predetermined range; or an off-state when Vgs is a value that can obtain a sufficiently low off-state current, etc.
[0072] As an example, consider an n-channel transistor with a threshold voltage Vth of 0.5 V and a drain current of 1×10 -9 A, the drain current when Vgs is 0.1V is 1×10 -13 A, the drain current when Vgs is -0.5V is 1×10 -19 A, the drain current when Vgs is -0.8V is 1×10 -22 A. At Vgs of -0.5V or in the range of -0.5V to -0.8V, the drain current of this transistor is 1×10 -19 A or less, so the off-state current of the transistor is sometimes called 1×10 -19 A or less. Due to the existence of the drain current of the transistor being 1×10 -22 A below Vgs, so the off-state current of the transistor is sometimes called 1×10 -22 A or below.
[0073] In this specification and the like, the off-state current of a transistor having a channel width W is sometimes expressed as a current value per channel width W. In addition, the off-state current of a transistor having a channel width W is sometimes expressed as a current value per a predetermined channel width (e.g., 1 μm). In the latter case, the unit of the off-state current is sometimes expressed as a unit having the dimension of current / length (e.g., A / μm).
[0074] The off-state current of a transistor sometimes depends on the temperature. In this specification, unless otherwise specified, the off-state current sometimes refers to the off-state current at room temperature, 60°C, 85°C, 95°C or 125°C. Alternatively, it sometimes refers to the off-state current at a temperature that ensures the reliability of a semiconductor device including the transistor or at a temperature at which a semiconductor device including the transistor is used (for example, any temperature between 5°C and 35°C). "The off-state current of the transistor is less than I" sometimes means that there is a value of Vgs that makes the off-state current of the transistor less than I at room temperature, 60°C, 85°C, 95°C, 125°C, a temperature that ensures the reliability of a semiconductor device including the transistor or at a temperature at which a semiconductor device including the transistor is used (for example, any temperature between 5°C and 35°C).
[0075] The off-state current of a transistor sometimes depends on the voltage Vds between the drain and the source. In this specification, unless otherwise specified, the off-state current sometimes refers to the off-state current when Vds is 0.1V, 0.8V, 1V, 1.2V, 1.8V, 2.5V, 3V, 3.3V, 10V, 12V, 16V or 20V. Alternatively, it sometimes refers to the off-state current when the Vds that ensures the reliability of the semiconductor device including the transistor or the Vds used by the semiconductor device including the transistor. "The off-state current of the transistor is less than 1" sometimes means: when Vds is 0.1V, 0.8V, 1V, 1.2V, 1.8V, 2.5V, 3V, 3.3V, 10V, 12V, 16V, 20V, the Vds that ensures the reliability of the semiconductor device including the transistor or the Vds used by the semiconductor device including the transistor, there is a value of Vgs that makes the off-state current of the transistor less than 1.
[0076] In the above description of off-state current, the drain can be referred to as the source. That is, the off-state current sometimes refers to the current flowing through the source when the transistor is in the off state.
[0077] In this specification, the off-state current may be referred to as leakage current. In this specification, the off-state current may refer to, for example, current flowing between a source and a drain when a transistor is in an off state.
[0078] In this specification, etc., the threshold voltage of a transistor refers to the gate voltage (Vg) when a channel is formed in the transistor. Specifically, the threshold voltage of a transistor sometimes refers to the gate voltage (Vg) at the intersection of the straight line with the maximum slope and the drain current (Id) at the point where the square root is 0 (Id is 0A) in a curve (Vg-√Id characteristic) plotted with the gate voltage (Vg) on the horizontal axis and the drain current (Id) on the vertical axis. Alternatively, the threshold voltage of a transistor sometimes refers to the value of Id[A]×L[μm] / W[μm] when L is the channel length and W is the channel width, and the value is 1×10 -9 Gate voltage (Vg) at [A].
[0079] Note that in this specification, for example, when the conductivity is sufficiently low, it may have the characteristics of an "insulator" even when it is expressed as a "semiconductor". In addition, the boundary between "semiconductors" and "insulators" is unclear, so it is sometimes not possible to accurately distinguish them. Therefore, the "semiconductors" described in this specification may be replaced with "insulators".
[0080] In addition, in this specification, for example, when the conductivity is sufficiently high, it may have the characteristics of a "conductor" even when it is expressed as a "semiconductor". In addition, the boundary between "semiconductor" and "conductor" is unclear, so it is sometimes impossible to accurately distinguish them. Therefore, the "semiconductor" recorded in this specification may be replaced by "conductor".
[0081] In this specification, etc., metal oxide refers to the oxide of metal in a broad sense. Metal oxides are classified into oxide insulators, oxide conductors (including transparent oxide conductors) and oxide semiconductors (Oxide Semiconductor, also referred to as OS), etc. For example, when a metal oxide is used in the active layer of a transistor, the metal oxide is sometimes referred to as an oxide semiconductor. In other words, when a metal oxide has at least one of an amplification effect, a rectification effect, and a switching effect, the metal oxide is called a metal oxide semiconductor (metal oxide semiconductor), referred to as OS. In addition, OS FET can be replaced by a transistor containing a metal oxide or an oxide semiconductor.
[0082] In addition, in this specification and the like, a metal oxide containing nitrogen may also be referred to as a metal oxide (metal oxide). In addition, a metal oxide containing nitrogen may also be referred to as a metal oxynitride (metal oxynitride).
[0083] In this specification, CAAC (c-axis aligned crystal) or CAC (Cloud-Aligned Composite) may be described. Note that CAAC is an example of a crystal structure, and CAC is an example of a function or a material configuration.
[0084] In addition, in this specification, etc., CAC-OS or CAC-metal oxide has a conductive function in a part of the material, an insulating function in another part of the material, and a semiconductor function as a whole. In addition, when CAC-OS or CAC-metal oxide is used in the active layer of a transistor, the conductive function is a function of allowing electrons (or holes) used as carriers to flow through, and the insulating function is a function of not allowing electrons used as carriers to flow through. Through the complementary effects of the conductive function and the insulating function, CAC-OS or CAC-metal oxide can have a switching function (open / close function). By separating each function in CAC-OS or CAC-metal oxide, each function can be maximized.
[0085] In addition, in this specification, CAC-OS or CAC-metal oxide includes a conductive region and an insulating region. The conductive region has the function of the above-mentioned conductivity, and the insulating region has the function of the above-mentioned insulation. In addition, in the material, the conductive region and the insulating region are sometimes separated at a nanoparticle level. In addition, the conductive region and the insulating region are sometimes unevenly distributed in the material. In addition, sometimes the conductive region is observed to be fuzzy at its edge and connected in a cloud shape.
[0086] In CAC-OS or CAC-metal oxide, the conductive region and the insulating region may be dispersed in the material with a size of 0.5 nm to 10 nm, preferably 0.5 nm to 3 nm.
[0087] In addition, CAC-OS or CAC-metal oxide is composed of components with different band gaps. For example, CAC-OS or CAC-metal oxide is composed of a component with a wide gap caused by an insulating region and a component with a narrow gap caused by a conductive region. In this structure, when carriers are allowed to flow through, the carriers mainly flow through the component with the narrow gap. In addition, the component with a narrow gap complements the component with a wide gap, and the carriers flow through the component with the wide gap in conjunction with the component with the narrow gap. Therefore, when the above-mentioned CAC-OS or CAC-metal oxide is used in the channel region of a transistor, a high current driving force, that is, a large on-state current and a high field effect mobility can be obtained in the on-state of the transistor.
[0088] That is, CAC-OS or CAC-metal oxide may also be referred to as a matrix composite material (matrix composite) or a metal matrix composite material (metal matrix composite).
[0089] Below, an example of the crystal structure of a metal oxide is described. Note that a metal oxide formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic number ratio]) is used as an example for description. A metal oxide formed by sputtering using the above target at a substrate temperature of more than 100°C and less than 130°C is called sIGZO, and a metal oxide formed by sputtering using the above target at a substrate temperature of room temperature (RT) is called tIGZO. For example, sIGZO has a crystal structure of one or both of nc (nano crystal) and CAAC. In addition, tIGZO has a crystal structure of nc. Note that the room temperature (RT) referred to here includes the temperature when the substrate is not intentionally heated. The CAAC structure is a crystal structure in which multiple IGZO nanocrystals have c-axis orientation and are connected in a non-oriented manner on the ab plane.
[0090] In this specification, etc., a display panel which is one form of a display device refers to a panel which can display (output) an image etc. on a display surface. Therefore, a display panel is one form of an output device.
[0091] In addition, in this specification, etc., a structure in which a connector such as an FPC (Flexible Printed Circuit) or TCP (Tape Carrier Package) is installed on a display panel substrate, or a structure in which an IC (integrated circuit) is directly mounted on a substrate by a COG (Chip On Glass) method, etc. is sometimes referred to as a display panel module or display module, or simply as a display panel, etc.
[0092] In addition, in this specification, etc., a touch sensor refers to a sensor that can detect contact, pressure, or proximity of a detected object such as a finger or a stylus. In addition, it can also have a function of detecting its position information. Therefore, a touch sensor is a form of an input device. For example, a touch sensor can have a structure having more than one sensor element.
[0093] In addition, in this specification, etc., a substrate including a touch sensor is sometimes referred to as a touch sensor panel, or simply as a touch sensor, etc. In addition, in this specification, etc., a structure in which a connector such as an FPC or TCP is mounted on a substrate of a touch sensor panel, or a structure in which an IC is mounted on a substrate in a COG manner, etc. is sometimes referred to as a touch sensor panel module, a touch sensor module, a sensor module, or simply as a touch sensor, etc.
[0094] Note that in this specification, a touch screen, which is one form of a display device, has the following functions: a function of displaying (outputting) an image on a display surface; and a function of acting as a touch sensor that detects when a detected object such as a finger or a stylus pen touches, is pressed, or approaches the display surface. Therefore, a touch screen is one form of an input / output device.
[0095] A touch screen may also be referred to as a display panel (or display device) having a touch sensor or a display panel (or display device) having a touch sensor function, for example.
[0096] The touch screen may include a display panel and a touch sensor panel, or may have a structure in which a touch sensor function is provided inside or on the surface of the display panel.
[0097] In addition, in this specification, etc., a structure in which a connector such as an FPC or TCP is installed on a substrate of a touch screen, or a structure in which an IC is installed on a substrate using a COG method, etc. is sometimes referred to as a touch screen module, a display module, or simply a touch screen.
[0098] Implementation Method 1
[0099] In this embodiment, a semiconductor device and a method for manufacturing the same, which are one embodiment of the present invention, are described. Here, a transistor, which is one embodiment of the semiconductor device, is described.
[0100] A transistor of one embodiment of the present invention includes a first conductive layer used as a gate electrode, a first insulating layer used as a gate insulating layer, a semiconductor layer, a second conductive layer and a third conductive layer used as a source electrode or a drain electrode, and a second insulating layer and a third insulating layer used as a protective layer.
[0101] A metal oxide film is preferably used as the semiconductor layer. In particular, it is preferably composed of indium, element M (M is one or more of gallium, aluminum, silicon, boron, yttrium, tin, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten and magnesium), and zinc. In particular, element M is preferably aluminum, gallium, yttrium or tin.
[0102] By using a metal oxide film with a low impurity concentration and a low defect state density as a semiconductor layer, a transistor with good electrical characteristics can be manufactured, so it is preferred. Here, the state with low impurity concentration and low defect state density is referred to as "high-purity intrinsic" or "substantially high-purity intrinsic". Because there are few carrier generation sources in the high-purity intrinsic or substantially high-purity intrinsic semiconductor layer, the carrier density can sometimes be reduced. Therefore, the transistor having a channel region formed in the semiconductor layer can be suppressed from having an electrical characteristic of a negative threshold voltage (also called a normally-on characteristic). Because the high-purity intrinsic or substantially high-purity intrinsic semiconductor layer has a lower defect state density, it is possible to have a lower trap state density. In addition, the off-state current of the high-purity intrinsic or substantially high-purity intrinsic semiconductor layer is significantly small.
[0103] The carrier density and defect energy level in the channel region of a transistor affect the electrical characteristics and reliability of the transistor. In particular, in a transistor with a short channel length, the carrier density and defect energy level in the channel region significantly affect the electrical characteristics and reliability. Therefore, by reducing the carrier density and defect energy level in the channel region, even a transistor with a short channel length can obtain good electrical characteristics and reliability.
[0104] Sometimes oxygen is separated from the metal oxide film included in the semiconductor layer, thereby forming oxygen vacancies (hereinafter sometimes referred to as Vo). If there are many oxygen vacancies in the semiconductor layer, the defect state density in the semiconductor layer increases, thereby having a negative impact on the electrical properties and reliability of the transistor. Therefore, in the transistor manufacturing process, a sufficient amount of oxygen is introduced into the semiconductor layer to reduce oxygen vacancies, thereby manufacturing transistors with good electrical properties and high reliability. In addition, in addition to reducing oxygen vacancies, it is also important to suppress the occurrence of oxygen vacancies in the transistor manufacturing process.
[0105] When there are oxygen vacancies and hydrogen in the semiconductor layer, hydrogen (hereinafter sometimes referred to as VoH) is sometimes introduced into the oxygen vacancies. VoH becomes a carrier generation source, sometimes having a negative impact on the electrical characteristics and reliability of the transistor. Therefore, by reducing the hydrogen and VoH in the semiconductor layer, the carrier density can be reduced, thereby manufacturing a transistor with good electrical characteristics and high reliability. In addition to the reduction of hydrogen and VoH, it is also important to suppress the diffusion of impurities containing hydrogen from the outside into the semiconductor layer. As impurities containing hydrogen, for example, there are hydrogen, water, etc.
[0106] As one method of reducing oxygen vacancies in the semiconductor layer, a method of disposing a layer that can release oxygen by heating near the semiconductor layer and performing a heat treatment to supply oxygen from the layer to the semiconductor layer can be used.
[0107] The second insulating layer used as a protective layer is in contact with the top surface of the semiconductor layer. The second insulating layer preferably contains oxygen. The second insulating layer is more preferably an insulating film whose oxygen content exceeds the stoichiometric composition. For example, an insulating film containing silicon and oxygen or an insulating film containing silicon, oxygen, and nitrogen is preferably used.
[0108] In this specification, etc., oxygen contained in excess of the stoichiometric composition is sometimes referred to as excess oxygen (exO). Alternatively, excess oxygen refers to oxygen released from a film or layer containing oxygen, for example, by heating. Excess oxygen, for example, moves inside the film or layer. The movement of excess oxygen includes a case where it moves between atoms in the film or layer and a case where it moves one by one in a manner that replaces oxygen constituting the film or layer. In addition, in this specification, etc., excess oxygen (exO) is sometimes referred to simply as oxygen.
[0109] By providing a second insulating film on the semiconductor layer and then performing a heat treatment, oxygen diffuses from the second insulating layer to the semiconductor layer, and oxygen is supplied to the semiconductor layer. The oxygen supplied to the semiconductor layer approaches the oxygen vacancies in the semiconductor layer, and the oxygen is captured by the oxygen vacancies to fill the oxygen vacancies. In addition, the oxygen approaches the hydrogen contained in the semiconductor layer, and the oxygen reacts with the hydrogen to become water (H2O), and is separated from the semiconductor layer as a water molecule. In addition, the oxygen approaches the VoH contained in the semiconductor layer, and the oxygen fills the oxygen vacancies of the VoH. In addition, the hydrogen contained in the VoH reacts with other oxygen to become water, and is separated from the semiconductor layer as water. In this way, the oxygen contained in the second insulating layer can reduce the oxygen vacancies, hydrogen and VoH in the semiconductor layer.
[0110] The third insulating layer used as a protective layer is in contact with the top surface of the second insulating layer. The third insulating layer preferably uses a material with a higher nitrogen concentration than the second insulating layer. For example, it is preferred to include an insulating film with silicon and nitrogen as main components. The insulating film with silicon and nitrogen as main components has the characteristic that water, hydrogen and oxygen are not easy to diffuse. Therefore, by providing the third insulating layer on the second insulating layer, it is possible to suppress the diffusion (detachment) of oxygen from the semiconductor layer and the second insulating layer to the outside. Therefore, the increase of oxygen vacancies in the semiconductor layer can be suppressed.
[0111] As the third insulating layer, for example, an oxide containing element X (X is one or more of aluminum, indium, gallium, and zinc) can be used. In particular, it is preferable to use an insulating film containing metal and oxygen as main components. For example, aluminum oxide or In-Ga-Zn oxide can be used as the third insulating layer.
[0112] Sometimes, voids are generated in the second insulating layer. If there are voids, impurities such as water and hydrogen may diffuse from the outside to the semiconductor layer through the voids, and the amount of hydrogen in the semiconductor layer may increase. By providing a third insulating layer on the second insulating layer to cover the voids, it is possible to suppress the diffusion of impurities from the outside to the semiconductor layer through the voids, thereby suppressing the increase of hydrogen in the semiconductor layer.
[0113] By providing the third insulating layer on the second insulating layer, oxygen vacancies, hydrogen, and VoH in the semiconductor layer can be reduced. Therefore, a transistor having good electrical characteristics and high reliability can be manufactured.
[0114] A more specific example of one embodiment of the present invention will be described below with reference to the drawings. A transistor will be described below as an example of a semiconductor device.
[0115] <Structural Example 1>
[0116] Figure 1A A top view of a transistor 100A of a semiconductor device according to one embodiment of the present invention is shown. Figure 1B and Figure 1C A cross-sectional view thereof is shown. Figure 1B Equivalent to following Figure 1A The cross-sectional view cut along the dot-dash line X1-X2 shown in FIG. Figure 1C Equivalent to following Figure 1A The cross-sectional view cut along the dotted line Y1-Y2 shown in FIG. Figure 1A For the sake of convenience, some components of transistor 100A (gate insulating layer, etc.) are omitted. In addition, the dot-dash line X1-X2 direction is sometimes referred to as the channel length direction, and the dot-dash line Y1-Y2 direction is sometimes referred to as the channel width direction. In addition, in the top view of the transistor below, Figure 1A Similarly, some of the components are omitted.
[0117] The transistor 100A includes a conductive layer 104 on a substrate 102, an insulating layer 106 on the substrate 102 and the conductive layer 104, a metal oxide layer 108 on the insulating layer 106, and conductive layers 112a and 112b that are in contact with the top surface of the metal oxide layer 108 and are spaced apart from each other on the metal oxide layer 108. In addition, the transistor 100A includes an insulating layer 114 on the conductive layer 112a, the conductive layer 112b and the metal oxide layer 108, and an insulating layer 116 on the insulating layer 114.
[0118] Part of the conductive layer 104 functions as a gate electrode. Part of the insulating layer 106 functions as a gate insulating layer. The conductive layer 112a functions as one of a source electrode and a drain electrode, and the conductive layer 112b functions as the other of the source electrode and the drain electrode. The insulating layer 114 and the insulating layer 116 function as protective layers.
[0119] The transistor 100A is a so-called channel-etched single-gate structure transistor.
[0120] like Figure 1A , Figure 1B and Figure 1CAs shown, the metal oxide layer 108 preferably has a stacked structure of a first metal oxide layer 108a and a second metal oxide layer 108b on the first metal oxide layer 108a.
[0121] Both the first metal oxide layer 108a and the second metal oxide layer 108b preferably include a metal oxide. The above-mentioned materials can be used for both the first metal oxide layer 108a and the second metal oxide layer 108b.
[0122] When the first metal oxide layer 108a and the second metal oxide layer 108b respectively include a region where the atomic number ratio of In is greater than the atomic number ratio of M, the field effect mobility of the transistor can be improved, so it is preferred. As an example, the atomic number ratios of In, M and Zn in the first metal oxide layer 108a and the second metal oxide layer 108b are preferably In:M:Zn=4:2:3 or in the vicinity thereof, or In:M:Zn=5:1:7 or in the vicinity thereof. Here, "nearby" includes the following cases: when In is 4, M is greater than 1.5 and less than 2.5, and Zn is greater than 2 and less than 4; and when In is 5, M is greater than 0.5 and less than 1.5, and Zn is greater than 5 and less than 7. By making the first metal oxide layer 108a and the second metal oxide layer 108b have substantially the same composition, the same sputtering target can be used, so the manufacturing cost can be suppressed.
[0123] The first metal oxide layer 108a and the second metal oxide layer 108b can respectively adopt In:M:Zn=1:1:1 or its vicinity as the atomic number ratio of In, M and Zn. Here, "nearby" includes the following cases: when In is 1, M is greater than 0.5 and less than 1.5, and Zn is greater than 0.1 and less than 2. By making the atomic number ratio of In and M approximately the same, the generation of oxygen vacancies in the first metal oxide layer 108a and the second metal oxide layer 108b can be suppressed, so it is preferred. Since the generation of oxygen vacancies can be suppressed, transistors with good electrical characteristics and high reliability can be manufactured.
[0124] The first metal oxide layer 108a and the second metal oxide layer 108b may also be formed using targets of different compositions, but it is particularly preferred to use a laminated film formed continuously using targets of the same composition without being exposed to the atmosphere. By forming the film continuously, in addition to being able to be processed in one film forming apparatus, it is also possible to suppress impurities from remaining between the first metal oxide layer 108a and the second metal oxide layer 108b. Since the impurities in the metal oxide layer may become a carrier source, by suppressing the increase of impurities, a transistor with good electrical characteristics and high reliability can be manufactured.
[0125] The second metal oxide layer 108b preferably includes a region having higher crystallinity than the first metal oxide layer 108a. When the second metal oxide layer 108b includes a region having high crystallinity, the second metal oxide layer 108b can be made into a film having higher etching resistance than the first metal oxide layer 108a. Therefore, it is possible to prevent the second metal oxide layer 108b from disappearing due to etching when the conductive layer 112a and the conductive layer 112b are formed. Therefore, the following can be achieved: Figure 1A , Figure 1B and Figure 1C Furthermore, by using a highly crystalline film as the second metal oxide layer 108b on the back channel side of the transistor, impurities that may diffuse into the first metal oxide layer 108a on the conductive layer 104 side can be reduced, so that a transistor with good electrical characteristics and high reliability can be manufactured.
[0126] By using a film including a region having lower crystallinity than the second metal oxide layer 108b as the first metal oxide layer 108a, oxygen can be easily diffused in the first metal oxide layer 108a, so that the ratio of oxygen vacancies in the first metal oxide layer 108a can be reduced. In particular, the first metal oxide layer 108a is close to the conductive layer 104 side and is a layer where a channel is mainly easily formed. Therefore, by using a film with less oxygen vacancies as the first metal oxide layer 108a, a transistor with good electrical characteristics and high reliability can be manufactured.
[0127] The first metal oxide layer 108a and the second metal oxide layer 108b can be formed separately by, for example, making the film formation conditions different. For example, the first metal oxide layer 108a and the second metal oxide layer 108b can be formed separately by making the flow rate of oxygen gas in the film formation gas different.
[0128] At this time, as the film forming condition of the first metal oxide layer 108a, the ratio of the oxygen gas flow rate in the total gas flow rate (also referred to as the oxygen flow rate ratio or the oxygen partial pressure) is set to be greater than 0% and less than 30%, preferably greater than 5% and less than 15%. By adopting the oxygen flow rate ratio within the above range, the crystallinity of the first metal oxide layer 108a can be reduced.
[0129] On the other hand, as the film forming condition of the second metal oxide layer 108b, the oxygen flow rate ratio is set to be greater than 30% and less than 100%, preferably greater than 50% and less than 100%, and more preferably greater than 70% and less than 100%. By adopting the oxygen flow rate ratio within the above range, the crystallinity of the second metal oxide layer 108b can be improved.
[0130] When the oxygen flow rate is relatively high, a region having a spinel-type crystal structure is sometimes generated in the metal oxide layer. When a region having a spinel-type crystal structure is included, the oxygen vacancy density in the region and / or the interface between the region and other regions is sometimes increased. Therefore, an oxygen flow rate ratio that does not generate a region having a spinel-type crystal structure can be used, for example, an oxygen flow rate ratio greater than 30% and less than 50%.
[0131] The substrate temperature when forming the first metal oxide layer 108a and the second metal oxide layer 108b is preferably above room temperature (25°C) and below 200°C, and more preferably above room temperature and below 130°C. By adopting the substrate temperature in the above range, when a large-area glass substrate is used, the bending or distortion of the substrate can be suppressed. Here, by making the substrate temperatures of the first metal oxide layer 108a and the second metal oxide layer 108b the same, productivity can be improved. In addition, for example, when the substrate temperatures of the first metal oxide layer 108a and the second metal oxide layer 108b are different, the crystallinity of the second metal oxide layer 108b can be further improved by increasing the substrate temperature when forming the second metal oxide layer 108b.
[0132] For example, it is preferable to use a CAC-OS (Cloud-Aligned Composite oxide semiconductor) film as the first metal oxide layer 108 a and a CAAC-OS (c-axis-aligned crystalline oxide semiconductor) film as the second metal oxide layer 108 b .
[0133] The crystallinity of the first metal oxide layer 108 a and the second metal oxide layer 108 b can be analyzed by, for example, X-ray diffraction (XRD), transmission electron microscope (TEM), electron diffraction, or the like.
[0134] The thickness of the first metal oxide layer 108a is greater than 1 nm and less than 50 nm, preferably greater than 5 nm and less than 30 nm. In addition, the thickness of the second metal oxide layer 108b is greater than 10 nm and less than 100 nm, preferably greater than 20 nm and less than 50 nm.
[0135] The boundary (interface) between the first metal oxide layer 108a and the second metal oxide layer 108b may not be clearly confirmed. Therefore, in the drawings for explaining one embodiment of the present invention, these boundaries are indicated by dotted lines.
[0136] In the metal oxide layer 108, when oxygen vacancies in the metal oxide layer 108 react with hydrogen to form VoH, the carrier density may increase. Therefore, it is preferable that the metal oxide layer 108 has fewer oxygen vacancies. In addition, it is preferable that the metal oxide layer 108 has fewer impurities. In particular, it is preferable that the metal oxide layer 108 has fewer impurities including hydrogen. By having fewer oxygen vacancies and impurities, the formation of VoH in the metal oxide layer 108 can be suppressed. Therefore, the carrier density can be reduced, and a transistor with good electrical characteristics and high reliability can be obtained.
[0137] The metal oxide layer 108 may also have a single-layer structure. When the metal oxide layer 108 has the same structure as the metal oxide layer 108a, the on-state current of the transistor can be increased. In addition, when the metal oxide layer 108 has the same structure as the metal oxide layer 108b, the reliability of the transistor can be improved.
[0138] An insulating film containing oxygen formed in an atmosphere containing oxygen can be used as the insulating layer 114. The insulating film formed in an atmosphere containing oxygen can be a film that easily releases a large amount of oxygen by heating. In addition, the insulating layer 114 is preferably made of a material having a lower nitrogen concentration than that of the insulating layer 116. For example, an insulating film containing silicon and oxygen, an insulating film containing silicon, oxygen, and nitrogen, or the like is preferably used. In particular, a silicon oxide film or a silicon oxynitride film is more preferably used.
[0139] In this specification, silicon oxynitride refers to a film containing silicon, oxygen and nitrogen, and having a higher oxygen content than nitrogen content in its composition. Silicon nitride oxide refers to a film containing silicon, oxygen and nitrogen, and having a higher nitrogen content than oxygen content in its composition. The composition can be measured using Rutherford Backscattering Spectrometry (RBS) or the like.
[0140] When a silicon oxide film, a silicon oxynitride film or the like is used as the insulating layer 114, it is preferably formed using a plasma enhanced chemical vapor deposition (PECVD) apparatus. The PECVD apparatus is preferred because it can form an insulating film with high step coverage of the formed surface and a small number of defects.
[0141] The insulating layer 114 may have a stacked structure of an insulating layer 114a and an insulating layer 114b on the insulating layer 114a. The insulating layer 114a and the insulating layer 114b preferably include an excess oxygen region, respectively. When the insulating layer 114a and the insulating layer 114b include the excess oxygen region, oxygen can be supplied to the metal oxide layer 108. Since oxygen vacancies that may be formed in the metal oxide layer 108 can be filled with oxygen, a transistor with good electrical characteristics and high reliability can be provided.
[0142] The insulating layer 114a in contact with the back channel side of the metal oxide layer 108 can use an oxide film having a nitrogen content lower than that of the insulating layer 114b. By using an oxide film having a low nitrogen content as the insulating layer 114a, nitrogen oxides (NO2) that may form energy levels can be less likely to form in the insulating layer 114a in contact with the metal oxide layer 108. x , x is greater than 0 and less than 2, preferably greater than 1 and less than 2. Typically, it is NO2 or NO). The insulating layer 114a can be formed using a PECVD device. The insulating layer 114a can be formed under film forming conditions where the power and chamber pressure are lower than the power and chamber pressure when the insulating layer 114b is formed.
[0143] The insulating layer 114a is an insulating film that allows oxygen to permeate, and also serves as a film for alleviating damage to the metal oxide layer 108 when forming an insulating layer 114b to be formed later.
[0144] The insulating layer 114b provided on the insulating layer 114a may have a structure using an oxide film containing excess oxygen (exO) more than the insulating layer 114a. The insulating layer 114b may be formed using a PECVD device. The insulating layer 114b may be formed under film forming conditions in which the power and the chamber pressure thereof are higher than the power and the chamber pressure when the insulating layer 114a is formed. In addition, the substrate temperature when forming the insulating layer 114b is preferably not less than 180°C and not more than 280°C. Since the film formed at the above substrate temperature has a weak bonding force between silicon and oxygen, a portion of the oxygen in the film is released by heat treatment in a subsequent process. As a result, an insulating film having an oxygen content exceeding the stoichiometric composition and a portion of the oxygen released due to heating can be formed, which is preferred.
[0145] When the insulating layer 114a and the insulating layer 114b are made of the same material, the interface between the insulating layer 114a and the insulating layer 114b may not be clearly confirmed. Therefore, in this embodiment, the interface between the insulating layer 114a and the insulating layer 114b is shown by a dotted line. In addition, in this embodiment, a two-layer structure of the insulating layer 114a and the insulating layer 114b is described, but one embodiment of the present invention is not limited to this. For example, a single-layer structure of the insulating layer 114a or the insulating layer 114b or a stacked structure of three or more layers may also be used.
[0146] Will refer to Figure 2A and Figure 2B The path of oxygen diffusing from the insulating layer 114 into the metal oxide layer 108 will be described. Figure 2A and Figure 2B is a schematic diagram showing the path of oxygen diffusing into the metal oxide layer 108, Figure 2A is a schematic diagram of the channel length direction. Figure 2BIt is a schematic diagram of the channel width direction.
[0147] Oxygen contained in the insulating layer 114a and the insulating layer 114b diffuses from the upper side, that is, through the second metal oxide layer 108b to the first metal oxide layer 108a ( Figure 2A and Figure 2B Route 1 shown).
[0148] Alternatively, oxygen contained in the insulating layer 114a and the insulating layer 114b diffuses from each side of the first metal oxide layer 108a and the second metal oxide layer 108b into the metal oxide layer 108 ( Figure 2B Route 2 shown).
[0149] For example, in Figure 2A and Figure 2B In Route 1 shown in FIG. 1 , when the crystallinity of the second metal oxide layer 108 b is high, the diffusion of oxygen may be hindered. Figure 2B In Route 2 shown, oxygen may be diffused from each side of the first metal oxide layer 108 a and the second metal oxide layer 108 b to the first metal oxide layer 108 a and the second metal oxide layer 108 b.
[0150] exist Figure 2B In Route 2 shown in FIG. 1 , when the first metal oxide layer 108a includes a region whose crystallinity is lower than that of the second metal oxide layer 108b, the region becomes a diffusion path for oxygen, and oxygen can be diffused to the second metal oxide layer 108b whose crystallinity is higher than that of the first metal oxide layer 108a. Figure 2A and Figure 2B Although not shown in the figure, when the insulating layer 106 and the region 106 a contain oxygen, the oxygen diffuses from the insulating layer 106 and the region 106 a into the metal oxide layer 108 .
[0151] As described above, by making the metal oxide layer 108 have a stacked structure of films having different crystal structures and making the region with low crystallinity a diffusion path for oxygen, a transistor with excellent electrical characteristics and high reliability can be provided.
[0152] By adopting a structure in which the insulating layer 114 is provided on the metal oxide layer 108, the metal oxide layer 108 has an oxygen concentration gradient in the film thickness direction, and the oxygen concentration is sometimes higher on the side of the insulating layer 114. Examples of elemental analysis methods include energy dispersive X-ray spectroscopy (EDX), secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), and Auger electron spectroscopy (AES).
[0153] Will refer to Figure 2C Oxygen diffused from the insulating layer 114a and the insulating layer 114b to the first metal oxide layer 108a and the second metal oxide layer 108b will be described. Figure 2C As shown, oxygen vacancies (Vo), hydrogen (H), and a state in which oxygen vacancies are bonded to hydrogen (VoH) may exist in the first metal oxide layer 108a and the second metal oxide layer 108b. When oxygen contained in the insulating layer 114a and the insulating layer 114b approaches oxygen vacancies in the first metal oxide layer 108a and the second metal oxide layer 108b, oxygen is captured by the oxygen vacancies and fills the oxygen vacancies. In addition, when oxygen approaches hydrogen, oxygen reacts with hydrogen to become water (H2O), and is separated from the first metal oxide layer 108a and the second metal oxide layer 108b as water molecules. In addition, when oxygen approaches VoH, oxygen fills oxygen vacancies. In addition, hydrogen contained in the VoH reacts with other oxygen to become water, and is separated from the first metal oxide layer 108a and the second metal oxide layer 108b as water. Thus, due to oxygen included in the insulating layers 114a and 114b, oxygen vacancies, hydrogen, and VoH in the first metal oxide layer 108a and the second metal oxide layer 108b can be reduced. Therefore, a transistor with excellent electrical characteristics and high reliability can be manufactured.
[0154] Here, the case where hydrogen is separated from the first metal oxide layer 108a and the second metal oxide layer 108b without providing the insulating layer 114 containing excess oxygen is considered. Sometimes, hydrogen contained in the first metal oxide layer 108a and the second metal oxide layer 108b is bonded with oxygen contained in the first metal oxide layer 108a and the second metal oxide layer 108b and separated as water molecules. In this case, oxygen contained in the first metal oxide layer 108a and the second metal oxide layer 108b is separated to generate oxygen vacancies, which is not preferable.
[0155] On the other hand, in a state where the insulating layer 114 containing excess oxygen is provided as shown in this embodiment, hydrogen is separated from the first metal oxide layer 108a and the second metal oxide layer 108b. The hydrogen contained in the first metal oxide layer 108a and the second metal oxide layer 108b reacts with the oxygen supplied from the insulating layer 114 and is separated as water molecules. The reaction of hydrogen with the oxygen supplied from the insulating layer 114 can suppress the generation of new oxygen vacancies in the first metal oxide layer 108a and the second metal oxide layer 108b, which is preferable.
[0156] By supplying oxygen from the insulating layers 114a and 114b to the first metal oxide layer 108a and the second metal oxide layer 108b, oxygen vacancies, hydrogen, and VoH in the first metal oxide layer 108a and the second metal oxide layer 108b can be reduced. In addition, generation of oxygen vacancies and VoH in the first metal oxide layer 108a and the second metal oxide layer 108b can be suppressed. By suppressing generation of oxygen vacancies and VoH, a transistor with good electrical characteristics and high reliability can be manufactured.
[0157] After forming the insulating layer 114a, the insulating layer 114b is preferably formed continuously in a vacuum so as not to expose the surface of the insulating layer 114a to the air. By forming the insulating layer 114b continuously, impurities derived from air components can be prevented from adhering to the surface of the insulating layer 114a.
[0158] The insulating layer 116 formed on the insulating layer 114b preferably uses an insulating film that is not easy to diffuse or permeate oxygen. In addition, the insulating layer 116 preferably uses an insulating film that releases less impurities and is not easy to diffuse or permeate impurities. In particular, the insulating layer 116 preferably contains hydrogen impurities that are not easy to diffuse or permeate impurities. By providing the insulating layer 116, the carrier density of the metal oxide layer 108 is reduced, thereby obtaining a transistor with good electrical characteristics and high reliability.
[0159] An insulating film containing silicon and nitrogen can be used as the insulating layer 116. In particular, an insulating film containing silicon and nitrogen as main components is preferably used. For example, a single layer or a stacked layer of silicon nitride, silicon nitride oxide, or the like can be used.
[0160] Alternatively, an oxide containing element X (X is one or more of aluminum, indium, gallium and zinc) can be used as the insulating layer 116. In particular, it is preferable to use an insulating film containing metal and oxygen as main components. For example, aluminum oxide or In-Ga-Zn oxide can be used as the insulating layer 116. It is more preferable to form the insulating layer 116 using a gas containing oxygen. By using a gas containing oxygen, oxygen can be supplied to the insulating layer 114b of the formed layer of the insulating layer 116, so it is preferred. The oxygen supplied to the insulating layer 114b can reduce oxygen vacancies, hydrogen and VoH in the metal oxide layer 108 as described above. Therefore, a transistor with good electrical characteristics and high reliability can be provided.
[0161] By performing the heat treatment in a state where the insulating films that release oxygen as the insulating layers 114a and 114b and the insulating film that does not diffuse and transmit oxygen as the insulating layer 116 are stacked, oxygen can be efficiently supplied to the metal oxide layer 108. As a result, oxygen vacancies in the metal oxide layer 108 and defects at the interface between the metal oxide layer 108 and the insulating layer 114 can be filled, thereby reducing defect levels. Therefore, a transistor with excellent electrical characteristics and high reliability can be manufactured.
[0162] The insulating layers 114a and 114b may have gaps 180 between the insulating layers 114a and 114b. Figure 3A As shown in FIG. 1 , particularly, gaps 180 are easily generated in the step portions of insulating layers 114a and 114b formed by conductive layers 112a and 112b. When gaps 180 exist in insulating layers 114a and 114b, impurities may diffuse from the outside or a layer formed later to metal oxide layer 108. Figure 3B As shown in FIG. 1 , by providing the insulating layer 116 over the insulating layer 114a and the insulating layer 114b, it is possible to suppress diffusion of impurities into the metal oxide layer 108. In addition, it is possible to suppress the release of oxygen from the metal oxide layer 108 and diffusion to the outside. By suppressing the diffusion of oxygen to the outside, it is possible to suppress the increase of oxygen vacancies, hydrogen, and VoH in the metal oxide layer 108, thereby manufacturing a transistor with excellent electrical characteristics and high reliability.
[0163] After forming the insulating layer 114b, it is preferable to continuously form the insulating layer 116 in a vacuum so that the surface of the insulating layer 114b is not exposed to the atmosphere. By continuously forming, it is possible to suppress the adhesion of impurities derived from atmospheric components to the surface of the insulating layer 114b. In addition, it is more preferable to continuously form the insulating layer 114a, the insulating layer 114b, and the insulating layer 116 in a vacuum because it is possible to suppress the adhesion of impurities derived from atmospheric components to the surfaces of the insulating layer 114a and the insulating layer 114b.
[0164] An insulating film into which impurities such as hydrogen and oxygen are not easily diffused can be used as the insulating layer 106. For example, an insulating film having a high barrier property such as a nitride insulating film can be used. In particular, an insulating film containing silicon and nitrogen as main components is preferably used.
[0165] The insulating layer 106 includes a region 106a near its top surface. Figure 1B and Figure 1C , the interface of the region 106a is shown by a dotted line. The region 106a is a region whose oxygen concentration is higher than that of other regions in the insulating layer 106. In addition, the region of the insulating layer 106 other than the region 106a preferably does not contain oxygen as a main component. In addition, the region 106a is preferably a region whose hydrogen concentration is lower than that of other regions in the insulating layer 106. The metal oxide layer 108 is provided in contact with the region 106a.
[0166] The thickness of the region 106 a may be greater than or equal to 1 nm and less than or equal to 10 nm.
[0167] By adopting a structure in which the region 106a containing a large amount of oxygen is in contact with the metal oxide layer 108, formation of defect levels at these interfaces can be suppressed. Therefore, by having a stacked structure including the region 106a and the metal oxide layer 108, the electrical characteristics of the transistor 100A can be improved.
[0168] By adopting a structure in which the metal oxide layer 108 is provided on the region 106a, the metal oxide layer 108 has an oxygen concentration gradient in the film thickness direction, and the oxygen concentration is sometimes higher on the region 106a side. In addition, as described above, the oxygen concentration is sometimes higher on the insulating layer 114 side of the metal oxide layer 108. That is, the metal oxide layer 108 sometimes has an oxygen concentration gradient in the film thickness direction, and the oxygen concentration is higher on the region 106a side and the insulating layer 114 side. As a method of elemental analysis, there are, for example, energy dispersive X-ray analysis (EDX), secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), and the like.
[0169] Furthermore, the transistor 100A has a structure in which the stacked structure of the region 106a, the metal oxide layer 108, and the insulating layer 114 is sandwiched by the insulating layers 106 and 116. Since the insulating layers 106 and 116 are layers in which water, hydrogen, oxygen, and the like are not easily diffused, water or hydrogen can be prevented from diffusing from the outside into the metal oxide layer 108 and oxygen can be prevented from diffusing (desorbing) from the metal oxide layer 108 to the outside. As a result, the electrical characteristics of the transistor 100A can be improved and the reliability can be improved.
[0170] For example, the existence of region 106a can be confirmed by performing elemental analysis of the region including the interface with the metal oxide layer 108 in the insulating layer 106. At this time, a large amount of oxygen may be detected in the region of the insulating layer 106 close to the metal oxide layer 108. In addition, a region with a high oxygen concentration is sometimes observed near the interface between the insulating layer 106 and the metal oxide layer 108. In addition, a region whose hydrogen concentration is lower than that of other parts may be observed in the region of the insulating layer 106 close to the metal oxide layer 108. As a method of elemental analysis, there are, for example, energy dispersive X-ray analysis (EDX), secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), etc. In addition, the existence of region 106a can sometimes be observed as a region of contrast different from other parts in a cross-sectional transmission electron microscope (TEM: Transmission Electron Microscopy) image, etc.
[0171] The above is the description of Structural Example 1.
[0172] Hereinafter, a structural example of a transistor having a part of a structure different from that of the structural example 1 described above will be described. In addition, the description of the parts repeated in the structural example 1 described above may be omitted below. In addition, in the drawings shown below, the parts having the same functions as those of the structural example 1 described above are denoted by the same hatching, and sometimes no reference numerals are attached.
[0173] <Structure Example 2>
[0174] Figure 4A A top view of a transistor 100B of a semiconductor device according to one embodiment of the present invention is shown. Figure 4B and Figure 4C A cross-sectional view thereof is shown. Figure 4B Equivalent to following Figure 4A The cross-sectional view cut along the dot-dash line X1-X2 shown in FIG. Figure 4C Equivalent to following Figure 4A A cross-sectional view taken along the dashed line Y1 - Y2 shown.
[0175] The transistor 100B is different from the transistor 100A shown in Structural Example 1 in that the metal oxide layer 108 includes a first metal oxide layer 108 a , a second metal oxide layer 108 b , and a third metal oxide layer 108 c .
[0176] like Figure 4A , Figure 4B and Figure 4CAs shown, the metal oxide layer 108 preferably has a stacked structure of a third metal oxide layer 108c, a first metal oxide layer 108a on the third metal oxide layer 108c, and a second metal oxide layer 108b on the first metal oxide layer 108a.
[0177] The first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c preferably include metal oxides, respectively. As the third metal oxide layer 108c, the material that can be used for the first metal oxide layer 108a and the second metal oxide layer 108b can be applied.
[0178] The first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c may also be formed using targets of different compositions, but it is particularly preferred to use a stacked film formed continuously using targets of the same composition without being exposed to the atmosphere. By forming the film continuously, in addition to being able to be processed in one film forming device, it is also possible to suppress impurities from remaining between the third metal oxide layer 108c and the first metal oxide layer 108a and between the first metal oxide layer 108a and the second metal oxide layer 108b. Since the impurities in the metal oxide layer may become a carrier source, by suppressing the increase of impurities, a transistor with good electrical characteristics and high reliability can be manufactured.
[0179] The third metal oxide layer 108c and the second metal oxide layer 108b preferably include a region having higher crystallinity than the first metal oxide layer 108a. When the third metal oxide layer 108c includes a region having high crystallinity, diffusion of impurities from the layers below the third metal oxide layer 108c (e.g., the insulating layer 106, the conductive layer 104, the substrate 102) to the first metal oxide layer 108a can be suppressed.
[0180] The first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c can be formed separately by, for example, making the film formation conditions different. For example, the first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c can have different flow rates of oxygen gas in the film formation gas.
[0181] At this time, as the film forming condition of the first metal oxide layer 108a, the ratio of the oxygen gas flow rate in the total gas flow rate (also referred to as the oxygen flow rate ratio or the oxygen partial pressure) is set to be greater than 0% and less than 30%, preferably greater than 5% and less than 15%. By adopting the oxygen flow rate ratio within the above range, the crystallinity of the first metal oxide layer 108a can be reduced.
[0182] On the other hand, as the film formation conditions of the second metal oxide layer 108b and the third metal oxide layer 108c, the oxygen flow rate ratio is set to be greater than 30% and less than 100%, preferably greater than 50% and less than 100%, and more preferably greater than 70% and less than 100%. By adopting the oxygen flow rate ratio within the above range, the crystallinity of the second metal oxide layer 108b and the third metal oxide layer 108c can be improved. In addition, the oxygen flow rate ratios of the second metal oxide layer 108b and the third metal oxide layer 108c can be the same or different.
[0183] Furthermore, by adopting the oxygen flow ratio within the above range, when the third metal oxide layer 108c is formed, oxygen is added to the insulating layer 106 on the surface where the third metal oxide layer 108c is formed. The oxygen added to the insulating layer 106 diffuses into the metal oxide layer 108 as excess oxygen. Therefore, oxygen vacancies, hydrogen, and VoH in the metal oxide layer can be reduced.
[0184] The substrate temperature when forming the first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c is preferably above room temperature (25°C) and below 200°C, and more preferably above room temperature and below 130°C. By adopting the substrate temperature in the above range, when a large-area glass substrate is used, the bending or distortion of the substrate can be suppressed. Here, by making the substrate temperatures of the first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c the same, productivity can be improved. In addition, for example, when the substrate temperatures of the first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c are different, the crystallinity of the second metal oxide layer 108b and the third metal oxide layer 108c can be further improved by increasing the substrate temperature when forming the second metal oxide layer 108b and the third metal oxide layer 108c.
[0185] For example, it is preferable to use a CAC-OS film as the first metal oxide layer 108 a , and to use a CAAC-OS film as the second metal oxide layer 108 b and the third metal oxide layer 108 c .
[0186] The thickness of the third metal oxide layer 108c is greater than 1 nm and less than 50 nm, preferably greater than 1 nm and less than 10 nm. In addition, the thickness of the first metal oxide layer 108a is greater than 1 nm and less than 50 nm, preferably greater than 5 nm and less than 20 nm. In addition, the thickness of the second metal oxide layer 108b is greater than 5 nm and less than 100 nm, preferably greater than 5 nm and less than 30 nm.
[0187] The boundaries (interfaces) among the first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c may not be clearly confirmed. Therefore, in the drawings for explaining one embodiment of the present invention, these boundaries are indicated by dotted lines.
[0188] <Structural Example 3>
[0189] Figure 5A A top view of a transistor 100C of a semiconductor device according to one embodiment of the present invention is shown. Figure 5B and Figure 5C A cross-sectional view thereof is shown. Figure 5B Equivalent to following Figure 5A The cross-sectional view cut along the dot-dash line X1-X2 shown in FIG. Figure 5C Equivalent to following Figure 5A A cross-sectional view taken along the dashed line Y1-Y2 shown.
[0190] The transistor 100C is different from the transistor 100A shown in Structural Example 1 in that the conductive layer 112a and the conductive layer 112b have a stacked-layer structure.
[0191] Conductive layer 112a has a stacked structure in which conductive layer 121a, conductive layer 122a, and conductive layer 123a are stacked in this order. Conductive layer 112b has a stacked structure in which conductive layer 121b, conductive layer 122b, and conductive layer 123b are stacked in this order.
[0192] The conductive layers 121a and 121b are provided in a manner covering the side surface of the first metal oxide layer 108a and the top surface and side surface of the metal oxide layer 108b. In addition, the conductive layers 121a and 121b are provided on and in contact with the region 106a of the insulating layer 106. The conductive layers 122a and 122b are provided on the conductive layers 121a and 121b, respectively. The conductive layers 122a and 122b are located on the inner side of the conductive layers 121a and 121b in a plane. The conductive layers 123a and 123b are provided on the conductive layers 122a and 122b, respectively. The conductive layers 123a and 123b are provided in a manner covering the top surface and side surface of the conductive layers 122a and 122b, respectively. In addition, a portion of the conductive layer 123a and the conductive layer 123b is provided in contact with the top surface of the conductive layer 121a and the conductive layer 121b, respectively. The ends of the conductive layer 121a and the conductive layer 123a are processed to be substantially consistent in a plane. The ends of the conductive layer 121b and the conductive layer 123b are processed to be substantially consistent in a plane.
[0193] By adopting the above structure, the conductive layer 122a can be surrounded by the conductive layer 121a and the conductive layer 123a. The conductive layer 122b can be surrounded by the conductive layer 121b and the conductive layer 123b. In other words, the structure can be such that the surfaces of the conductive layers 122a and 122b are not exposed. Thus, as the conductive layers 122a and 122b, materials whose components are easily diffused into the metal oxide layer 108 can be used.
[0194] The conductive layers 122a and 122b are preferably made of a material having a lower resistance than the conductive layers 121a, 121b, 123a, and 123b. In addition, the conductive layers 121a, 121b, 123a, and 123b may be made of a material whose components are less likely to diffuse into the metal oxide layer 108 than the conductive layers 122a and 122b.
[0195] Conductive layer 122a and conductive layer 122b may use a material having conductivity different from that of conductive layer 121a, conductive layer 121b, conductive layer 123a, and conductive layer 123b. In addition, conductive layer 121a, conductive layer 121b, conductive layer 123a, and conductive layer 123b may use different conductive materials. In particular, it is preferred that the conductive layer 121a, conductive layer 121b, conductive layer 123a, and conductive layer 123b use the same conductive material, so that a manufacturing device can be used in common and the contact resistance of the ends of these can be reduced.
[0196] For example, a titanium film or a molybdenum film is preferably used for the conductive layers 121a, 121b, 123a, and 123b. An aluminum film or a copper film is preferably used for the conductive layers 122a and 122b. By adopting the above structure, a transistor with good electrical characteristics can be realized while reducing the wiring resistance of the conductive layers 112a and 112b.
[0197] The above is the description of structural example 3.
[0198] <Structural Example 4>
[0199] Fig. 6A A top view of a transistor 100D of a semiconductor device according to one embodiment of the present invention is shown. Figure 6B and Figure 6C A cross-sectional view thereof is shown. Figure 6B Equivalent to following Fig. 6A The cross-sectional view cut along the dot-dash line X1-X2 shown in FIG. Figure 6C Equivalent to following Fig. 6A A cross-sectional view taken along the dashed line Y1-Y2 shown.
[0200] The transistor 100D is different from the transistor 100C shown in the above structural example 3 in that it includes a conductive layer 120a, a conductive layer 120b and a conductive layer 112c.
[0201] The conductive layer 120a is provided on the insulating layer 116 and includes a portion overlapping the metal oxide layer 108. In this case, the conductive layer 104 is used as a first gate electrode, and the conductive layer 120a is used as a second gate electrode. A portion of the insulating layer 106 is used as a first gate insulating layer, and a portion of the insulating layer 114 and the insulating layer 116 is used as a second gate insulating layer. The transistor 100D is a transistor including a pair of gate electrodes.
[0202] The transistor 100D is a so-called channel-etched dual-gate structure transistor.
[0203] Conductive layer 120b is electrically connected to conductive layer 123b of conductive layer 112b via connection portion 142b. In connection portion 142b, conductive layer 120b is electrically connected to conductive layer 123b of conductive layer 112b via an opening provided in insulating layer 116 and insulating layer 114.
[0204] like Figure 6C As shown, it is preferred that the conductive layer 120a is electrically connected to the conductive layer 104 through the connecting portion 142a. The conductive layer 121c, the conductive layer 122c and the conductive layer 123c are provided in the connecting portion 142a. In the connecting portion 142a, the conductive layer 120a is electrically connected to the conductive layer 123c through the openings provided in the insulating layer 114 and the insulating layer 116, and the conductive layer 121c is electrically connected to the conductive layer 104 through the openings provided in the insulating layer 106.
[0205] The metal oxide layer 108 in the transistor 100D is sandwiched between the conductive layer 104 and the conductive layer 120a. The lengths of the conductive layer 104 and the conductive layer 120a in the channel length direction and the channel width direction are longer than the lengths of the metal oxide layer 108 in the channel length direction and the channel width direction. Therefore, the metal oxide layer 108 is covered by the conductive layer 104 and the conductive layer 120a with the insulating layer 106, the insulating layer 114, and the insulating layer 116 sandwiched therebetween. In other words, the conductive layer 104 and the conductive layer 120a surround the metal oxide layer 108 in the channel width direction of the transistor 100D.
[0206] By adopting such a structure, the metal oxide layer 108 included in the transistor 100D can be electrically surrounded by the electric field of the conductive layer 104 and the conductive layer 120a. A device structure of a transistor in which a metal oxide layer having a channel region is electrically surrounded by the electric field of the conductive layer 104 and the conductive layer 120a, such as the transistor 100D, is referred to as a surrounded channel (S-channel) structure.
[0207] Since the transistor 100D has an S-channel structure, an electric field for causing a channel can be effectively applied to the metal oxide layer 108 using the conductive layer 104 and the conductive layer 120a. As a result, the driving capability of the transistor 100D is improved, so that a high on-state current characteristic can be obtained. In addition, since the on-state current can be increased, the transistor 100D can be miniaturized. In addition, since the transistor 100D has a structure in which the metal oxide layer 108 is surrounded by the conductive layer 104 and the conductive layer 120a, the mechanical strength of the transistor 100D can be improved.
[0208] By adopting the above structure, in the metal oxide layer 108, the region where carriers flow is formed on both the conductive layer 104 side of the metal oxide layer 108 and the conductive layer 120a side of the metal oxide layer 108, and the carriers flow through a wide region, so the amount of carrier mobility of the transistor 100D is increased. As a result, compared with the case where a predetermined potential is supplied to either the conductive layer 104 or the conductive layer 120a, the on-state current of the transistor 100D can be increased.
[0209] like Fig. 7A , Figure 7B and Figure 7C In the transistor 100E shown, the metal oxide layer 108 may also have a stacked structure of a third metal oxide layer 108c, a first metal oxide layer 108a on the third metal oxide layer 108c, and a second metal oxide layer 108b on the first metal oxide layer 108a.
[0210] like Fig. 8A , Figure 8B and Figure 8C The transistor 100F shown in the figure may not include the conductive layer 112 c. In the connecting portion 142 a , the conductive layer 120 a is electrically connected to the conductive layer 104 through the insulating layer 106 , the insulating layer 114 , and the opening provided in the insulating layer 116 .
[0211] The above is the description of structural example 4.
[0212] <Structural Example 5>
[0213] Fig.9AA top view of a transistor 100G of a semiconductor device according to one embodiment of the present invention is shown. Fig. 9B and Fig. 9C A cross-sectional view thereof is shown. Fig. 9B Equivalent to following Fig.9A The cross-sectional view cut along the dot-dash line X1-X2 shown in FIG. Fig. 9C Equivalent to following Fig.9A A cross-sectional view taken along the dashed line Y1-Y2 shown.
[0214] The transistor 100G is different from the transistor 100F shown in the above structural example 4 in that an insulating layer 150 is included between the metal oxide layer 108 and the conductive layers 120a and 120b.
[0215] The insulating layer 150 is provided to cover the top and side surfaces of the metal oxide layer 108 and the insulating layer 106. The insulating layer 150 is used as a channel protection layer for protecting the metal oxide layer 108 when the conductive layers 112a and 112b are processed.
[0216] The transistor 100G is a so-called channel protection type double-gate structure transistor.
[0217] The insulating layer 150 can be made of the same material as that of the insulating layer 114 a described above.
[0218] The conductive layer 112a and the conductive layer 112b are respectively provided on the insulating layer 150. The conductive layer 112a is electrically connected to the metal oxide layer 108 through the connecting portion 152a. In the connecting portion 152a, the conductive layer 112a is electrically connected to the metal oxide layer 108 through an opening provided in the insulating layer 150. The conductive layer 112b is electrically connected to the metal oxide layer 108 through the connecting portion 152b. In the connecting portion 152b, the conductive layer 112b is electrically connected to the metal oxide layer 108 through an opening provided in the insulating layer 150.
[0219] By adopting the above structure, the etching step for processing the conductive layer 112a and the conductive layer 112b is performed in a state where the metal oxide layer 108 is covered by the insulating layer 150, so that the metal oxide layer 108 can be less easily damaged by etching. In addition, by adopting the above structure, the range of material selection for the conductive layer 112a and the conductive layer 112b can be expanded, which is preferable.
[0220] Note that the insulating layer 150 covers not only the top surface but also the side surface of the metal oxide layer 108, but is not limited to this. For example, the insulating layer 150 may be processed into an island shape and located on the channel formation region of the metal oxide layer 108.
[0221] The above is the description of structural example 5.
[0222] <Components of a semiconductor device>
[0223] Next, components included in the semiconductor device of this embodiment will be described in detail.
[0224] [Substrate]
[0225] Although there is no particular limitation on the material of the substrate 102, it is at least required to have heat resistance that can withstand the subsequent heat treatment. For example, as the substrate 102, a glass substrate, a ceramic substrate, a quartz substrate, a sapphire substrate, etc. can be used. In addition, a single crystal semiconductor substrate or a polycrystalline semiconductor substrate made of silicon or silicon carbide, a compound semiconductor substrate made of silicon germanium, etc., an SOI (Silicon On Insulator) substrate, etc. can also be used, and a substrate having a semiconductor element provided on these substrates can also be used as the substrate 102. When a glass substrate is used as the substrate 102, a large display device can be manufactured by using a large-area substrate of the 6th generation (1500mm×1850mm), the 7th generation (1870mm×2200mm), the 8th generation (2200mm×2400mm), the 9th generation (2400mm×2800mm), the 10th generation (2950mm×3400mm), etc.
[0226] As the substrate 102, a flexible substrate may be used, and a transistor may be directly formed on the flexible substrate. Alternatively, a peeling layer may be provided between the substrate 102 and the transistor. The peeling layer may be used in the case where a part or all of a semiconductor device is manufactured on the peeling layer, and then the semiconductor device is separated from the substrate 102 and transferred to another substrate. In this case, the transistor may also be transferred to a substrate with low heat resistance or a flexible substrate.
[0227] [Conductive layer]
[0228] The conductive layer 104, the conductive layer 112a, the conductive layer 112b, the conductive layer 120a, and the conductive layer 120b can be formed using a metal element selected from chromium, copper, aluminum, gold, silver, zinc, molybdenum, tantalum, titanium, tungsten, manganese, nickel, iron, and cobalt, an alloy containing the above metal elements, or an alloy combining the above metal elements.
[0229] In addition, as the conductive layer 104, the conductive layer 112a, the conductive layer 112b, the conductive layer 120a, and the conductive layer 120b, an oxide conductor or oxide semiconductor such as an oxide containing indium and tin (In-Sn oxide), an oxide containing indium and tungsten (In-W oxide), an oxide containing indium, tungsten and zinc (In-W-Zn oxide), an oxide containing indium and titanium (In-Ti oxide), an oxide containing indium, titanium and tin (In-Ti-Sn oxide), an oxide containing indium and zinc (In-Zn oxide), an oxide containing indium, tin and silicon (In-Sn-Si oxide), or an oxide containing indium, gallium and zinc (In-Ga-Zn oxide) can also be used.
[0230] Here, an oxide conductor is described. In this specification, etc., an oxide conductor may also be referred to as an OC (Oxide Conductor). For example, an oxide conductor is obtained by the following steps: oxygen vacancies are formed in a metal oxide having semiconductor properties, and hydrogen is added to the oxygen vacancies to form donor energy levels near the conduction band. As a result, the conductivity of the metal oxide increases, and it becomes a conductor. The metal oxide that can become a conductor is called an oxide conductor. In general, since the energy gap of a metal oxide having semiconductor properties is large, it is transparent to visible light. On the other hand, an oxide conductor is a metal oxide having a donor energy level near the conduction band. Therefore, in an oxide conductor, the influence caused by the absorption of the donor energy level is small, and it has substantially the same light transmittance to visible light as a metal oxide having semiconductor properties.
[0231] In addition, a Cu-X alloy film (X is Mn, Ni, Cr, Fe, Co, Mo, Ta or Ti) may be applied as the conductive layer 104, the conductive layer 112a, and the conductive layer 112b. By using the Cu-X alloy film, processing can be performed by a wet etching process, thereby reducing manufacturing costs.
[0232] In addition, the conductive layers 112a and 112b preferably contain one or more of the above-mentioned metal elements, copper, titanium, tungsten, tantalum, and molybdenum. In addition, when a copper film or an aluminum film is used as the conductive layers 112a and 112b, the resistance of the conductive layers 112a and 112b can be reduced, which is preferred.
[0233] [Insulation layer]
[0234] As the insulating layer 106 used as a gate insulating layer, one or more insulating layers including a silicon nitride oxide film, a silicon nitride film, an aluminum nitride film, an aluminum nitride oxide film, etc. formed by a plasma enhanced chemical vapor deposition (PECVD) method, a sputtering method, etc. can be used. In addition, the insulating layer 106 may have a stacked structure of two or more layers.
[0235] As the insulating layer 114a and the insulating layer 114b provided on the metal oxide layer 108, one or more insulating layers including a silicon oxide film, a silicon oxynitride film, an aluminum oxide film, a hafnium oxide film, a yttrium oxide film, a zirconium oxide film, a gallium oxide film, a tantalum oxide film, a magnesium oxide film, a lanthanum oxide film, a cerium oxide film, and a neodymium oxide film formed by a PECVD method, a sputtering method, an ALD (Atomic Layer Deposition) method, etc. can be used. In particular, a silicon oxide film or a silicon oxynitride film formed by a PECVD method is preferably used.
[0236] As the insulating layer 114 a , an insulating film having a thickness of 5 nm to 150 nm, preferably 5 nm to 50 nm, can be appropriately used.
[0237] Furthermore, the number of defects in the insulating layer 114a is preferably small. Typically, the spin density of a signal at g=2.001 due to dangling bonds of silicon measured by ESR (Electron Spin Resonance) is preferably 3×10 17 spins / cm 3 This is because, if the defect density of the insulating layer 114a is high, oxygen is bonded to the defects, thereby reducing the oxygen permeability in the insulating layer 114a.
[0238] In the insulating layer 114a, sometimes, not all of the oxygen that enters the insulating layer 114a from the outside moves to the outside of the insulating layer 114a, but a part of it remains inside the insulating layer 114a. In addition, sometimes, when oxygen enters the insulating layer 114a, oxygen contained in the insulating layer 114a moves to the outside of the insulating layer 114a, and oxygen movement occurs in the insulating layer 114a. When an insulating film that allows oxygen to pass is formed as the insulating layer 114a, oxygen that has been separated from the insulating layer 114b provided on the insulating layer 114a can be moved to the metal oxide layer 108a and the metal oxide layer 108b through the insulating layer 114a.
[0239] In addition, the insulating layer 114a can be formed using an insulating film having a low state density due to nitride oxide. Note that the state density due to nitride oxide is sometimes formed between the energy (Ev_os) of the valence band top of the metal oxide film and the energy (Ec_os) of the conduction band bottom of the metal oxide. As the insulating film, a silicon oxynitride film having a low release amount of nitride oxide or an aluminum oxynitride film having a low release amount of nitride oxide can be used.
[0240] In addition, in thermal desorption spectroscopy (TDS), the silicon oxynitride film with a small amount of nitrogen oxide release is a film that releases more ammonia than nitrogen oxide. Typically, the amount of ammonia released is 1×10 18 cm / 3 Above and 5×10 19 cm / 3 Note that the amount of ammonia released is the amount released when the film surface temperature is heated to a temperature of 50° C. to 650° C., preferably 50° C. to 550° C.
[0241] Nitrogen oxides (NO x , x is greater than 0 and less than 2, preferably greater than 1 and less than 2), typically NO2 or NO, forming an energy level in the insulating layer 114a, etc. This energy level is located in the energy gap between the metal oxide layer 108a and the metal oxide layer 108b. Therefore, when the nitrogen oxide diffuses to the interface between the insulating layer 114a and the metal oxide layer 108b, sometimes this energy level captures electrons on the insulating layer 114a side. As a result, the captured electrons remain near the interface between the insulating layer 114a and the metal oxide layer 108b, thereby causing the threshold voltage of the transistor to drift in the positive direction.
[0242] In addition, when heat treatment is performed, nitrogen oxide reacts with ammonia and oxygen. When heat treatment is performed, nitrogen oxide included in the insulating layer 114a reacts with ammonia included in the insulating layer 114b, thereby reducing nitrogen oxide included in the insulating layer 114a. Therefore, electrons are not easily captured at the interface between the insulating layer 114a and the metal oxide layer 108b.
[0243] By using the above insulating film as the insulating layer 114 a , a drift of a threshold voltage of the transistor can be reduced, thereby reducing variations in electrical characteristics of the transistor.
[0244] The nitrogen concentration of the insulating film measured by SIMS was 6×10 20 atoms / cm 3 the following.
[0245] By forming the insulating film by a PECVD method using silane and nitrous oxide at a substrate temperature of 220° C. to 350° C., a dense film with high hardness can be formed.
[0246] The insulating layer 114b is an insulating film containing oxygen exceeding the stoichiometric composition. The insulating film is heated and part of the oxygen is released. The insulating film includes an oxygen release amount of 1.0×10 19 atoms / cm 3 Above, preferably 3.0×10 20 atoms / cm 3 The oxygen release amount is the total amount in the range of the heat treatment temperature of 50°C to 650°C or 50°C to 550°C in TDS analysis. The oxygen release amount is the total amount converted to oxygen atoms in TDS.
[0247] As the insulating layer 114 b , a silicon oxide film, a silicon oxynitride film, or the like can be used with a thickness of greater than or equal to 30 nm and less than or equal to 500 nm, preferably greater than or equal to 50 nm and less than or equal to 400 nm.
[0248] Furthermore, the amount of defects in the insulating layer 114 b is preferably small. Typically, the spin density of the signal at g=2.001 due to dangling bonds of silicon measured by ESR is less than 1.5×10 18 spins / cm 3 , more preferably 1×10 18 spins / cm 3 Since the insulating layer 114b is farther from the metal oxide layer 108a and the metal oxide layer 108b than the insulating layer 114a, the defect density of the insulating layer 114b can also be higher than that of the insulating layer 114a.
[0249] The insulating layer 116 used as a protective layer can use the above-mentioned materials. The insulating layer 116 may also have a stacked structure of two or more layers. It is preferable that an insulating film that does not easily diffuse or permeate oxygen is used for the insulating layer 116. In addition, it is preferable that an insulating film that does not easily diffuse or permeate impurities is used for the insulating layer 116. In particular, it is preferable that the insulating layer 116 contains hydrogen impurities that do not easily diffuse or permeate impurities.
[0250] As the insulating layer 116 , an insulating film having a thickness of 5 nm to 200 nm, preferably 10 nm to 150 nm, can be appropriately used.
[0251] [Semiconductor layer]
[0252] The first metal oxide layer 108 a , the second metal oxide layer 108 b , and the third metal oxide layer 108 c can use the above-mentioned materials.
[0253] When the first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c are In-M-Zn oxide, the atomic number ratio of the metal element of the sputtering target used to form the In-M-Zn oxide preferably satisfies In> M. Examples of the atomic number ratio of the metal element of such a sputtering target include In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=2:1:3, In:M:Zn=3:1:2, In:M:Zn=4:2:4.1, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5, and the like.
[0254] In addition, when the first metal oxide layer 108a, the second metal oxide layer 108b and the third metal oxide layer 108c are In-M-Zn oxide, it is preferable to use a target containing polycrystalline In-M-Zn oxide as a sputtering target. By using a target containing polycrystalline In-M-Zn oxide, it is easy to form a metal oxide layer 108 having crystallinity. Note that the atomic number ratio of the formed metal oxide layer 108 varies within the range of ±40% of the atomic number ratio of the metal element contained in the above-mentioned sputtering target. For example, when the composition of the sputtering target for the metal oxide layer 108 is In:Ga:Zn=4:2:4.1 [atomic number ratio], sometimes the composition of the formed metal oxide layer 108 is near In:Ga:Zn=4:2:3 [atomic number ratio].
[0255] The energy gap of the first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c is greater than or equal to 2 eV, and preferably greater than or equal to 2.5 eV. Thus, by using metal oxides with a wider energy gap, the off-state current of the transistor can be reduced.
[0256] The first metal oxide layer 108a, the second metal oxide layer 108b, and the third metal oxide layer 108c preferably have a non-single-crystal structure. The non-single-crystal structure includes, for example, CAAC-OS (C Axis Aligned Crystalline Oxide Semiconductor), a polycrystalline structure, a microcrystalline structure, or an amorphous structure. Among the non-single-crystal structures, the amorphous structure has the highest defect state density, while the CAAC-OS has the lowest defect state density.
[0257] <Method 1 for manufacturing transistor>
[0258] Next, an example of a method for manufacturing a transistor according to one embodiment of the present invention will be described. Here, the transistor 100C shown in the above-mentioned structural example 3 will be described as an example.
[0259] Thin films (insulating films, semiconductor films, conductive films, etc.) constituting semiconductor devices can be formed by sputtering, chemical vapor deposition (CVD: Chemical Vapor Deposition) method, vacuum evaporation method, pulse laser deposition (PLD: Pulse Laser Deposition) method, atomic layer deposition (ALD: Atomic Layer Deposition) method, etc. CVD methods include plasma enhanced chemical vapor deposition (PECVD: Plasma Enhanced CVD) method, thermal CVD method, etc. In addition, as one of the thermal CVD methods, there is metal organic chemical vapor deposition (MOCVD: Metal Organic CVD) method.
[0260] When forming a thin film (insulating film, semiconductor film, conductive film, etc.) that constitutes a semiconductor device, methods such as spin coating, dipping, spraying, droplet injection (inkjet, etc.), printing (screen printing, offset printing, etc.) and tools such as scrapers, roll coaters, curtain coaters, and knife coaters can be used.
[0261] When processing a thin film constituting a semiconductor device, it can be processed by photolithography or the like. In addition to the above methods, the thin film can also be processed by nanoimprinting, sandblasting, lift-off, etc. In addition, an island-shaped thin film can be directly formed by a film forming method using a shielding mask such as a metal mask.
[0262] There are two typical photolithography methods. One is to form a resist mask on a thin film to be processed, process the thin film by etching, etc., and remove the resist mask. The other is to form a photosensitive thin film, then perform exposure and development to process the thin film into a desired shape.
[0263] In the photolithography method, as the light used for exposure, for example, i-line (wavelength of 365nm), g-line (wavelength of 436nm), h-line (wavelength of 405nm) or a mixture of these lights can be used. In addition, ultraviolet light, KrF laser or ArF laser, etc. can also be used. In addition, liquid immersion exposure technology can also be used for exposure. As the light used for exposure, extreme ultraviolet light (EUV: Extreme Ultra-Violet light) or X-rays can also be used. In addition, an electron beam can also be used instead of the light used for exposure. When extreme ultraviolet light, X-rays or electron beams are used, extremely fine processing can be performed, so it is preferred. In addition, when exposure is performed by scanning a light beam such as an electron beam, a photomask is not required.
[0264] As a method for etching the thin film, a dry etching method, a wet etching method, a sand blast method, or the like can be used.
[0265] FIG. 10A to FIG. 13B The drawings shown are diagrams for explaining a method for manufacturing the transistor 100C. In each drawing, the left side shows a cross section in the channel length direction, and the right side shows a cross section in the channel width direction.
[0266] [Formation of Conductive Layer 104]
[0267] A conductive film is formed over the substrate 102 and is processed by a photolithography step and an etching step, so that a conductive layer 104 serving as a gate electrode is formed.
[0268] [Formation of Insulating Layer 106]
[0269] Next, an insulating layer 106 ( Fig. 10A ). The insulating layer 106 can be formed by using a PECVD method, for example.
[0270] In this embodiment, a 400 nm-thick silicon nitride film can be used as the insulating layer 106. The silicon nitride film has a three-layer stacked structure including a first silicon nitride film, a second silicon nitride film, and a third silicon nitride film. An example of the three-layer stacked structure is as follows.
[0271] A first silicon nitride film with a thickness of 50 nm can be formed under the following conditions: for example, silane with a flow rate of 200 sccm, nitrogen with a flow rate of 2000 sccm, and ammonia with a flow rate of 100 sccm are used as source gases, the source gases are supplied into the reaction chamber of the PECVD device, the pressure in the reaction chamber is controlled to 100 Pa, and a high-frequency power supply of 27.12 MHz is used to supply 2000 W of power.
[0272] A second silicon nitride film with a thickness of 300 nm can be formed under the following conditions: silane with a flow rate of 200 sccm, nitrogen with a flow rate of 2000 sccm, and ammonia with a flow rate of 2000 sccm are used as source gases, the source gases are supplied into the reaction chamber of the PECVD device, the pressure in the reaction chamber is controlled to 100 Pa, and a high-frequency power supply of 27.12 MHz is used to supply 2000 W of power.
[0273] The third silicon nitride film may be formed to a thickness of 50 nm using the same film forming conditions as those for the first silicon nitride film.
[0274] In addition, the substrate temperature during formation of the first silicon nitride film, the second silicon nitride film, and the third silicon nitride film can be set to 350° C. or less.
[0275] By adopting the above three-layer stacked structure as the silicon nitride film, for example, when a conductive film containing copper is used as the conductive layer 104, the following effects can be achieved. The first silicon nitride film can suppress the diffusion of copper elements from the conductive layer 104. The second silicon nitride film has a function of releasing hydrogen, and can improve the withstand voltage of the insulating film used as a gate insulating film. The third silicon nitride film is a film that releases less hydrogen and can suppress the diffusion of hydrogen released from the second silicon nitride film.
[0276] [Formation of Region 106a]
[0277] Next, oxygen 130a is preferably added to the insulating layer 106 to form a region 106a containing oxygen near the surface ( Fig. 10B ).
[0278] Examples of the oxygen 130a added to the insulating layer 106 include oxygen radicals, oxygen atoms, oxygen atomic ions, and oxygen molecular ions. In addition, examples of the adding method include ion doping, ion implantation, and plasma treatment. Alternatively, after a film that suppresses the release of oxygen is formed on the insulating layer 106, the oxygen 130a may be added to the insulating layer 106 through the film. The film is preferably removed after the addition of the oxygen 130a.
[0279] The film for suppressing oxygen desorption can be a conductive film or a semiconductor film containing one or more of indium, zinc, gallium, tin, aluminum, chromium, tantalum, titanium, molybdenum, nickel, iron, cobalt and tungsten.
[0280] When oxygen 130a is added by plasma treatment, high-density oxygen plasma is generated by exciting oxygen by microwaves, thereby increasing the amount of oxygen added to the insulating layer 106. In addition, by performing plasma treatment in an atmosphere containing oxygen, water or hydrogen attached to the surface of the insulating layer 106 can be removed. Thus, water or hydrogen that may be present in the metal oxide layer 108 to be formed later or at the interface between the metal oxide layer 108 and the insulating layer 106 can be reduced.
[0281] When silicon nitride, silicon nitride oxide, or the like is used as the insulating layer 106, hydrogen may be contained in the insulating layer 106. In this case, by performing the above-described plasma treatment or the like, the hydrogen concentration in at least the region 106a in contact with the metal oxide layer 108 can be reduced.
[0282] Before adding oxygen 130a, heat treatment may be performed to remove water or hydrogen from the surface and film of the insulating layer 106. For example, heat treatment may be performed in a nitrogen atmosphere at a temperature of 300°C or higher and lower than the heat resistance temperature of the conductive layer 104, preferably 300°C or higher and 450°C or lower.
[0283] [Formation of Metal Oxide Layer 108]
[0284] Next, a metal oxide film 128a and a metal oxide film 128b are formed on the insulating layer 106 ( Fig. 10C ).
[0285] The metal oxide film 128 a and the metal oxide film 128 b are preferably formed by a sputtering method using a metal oxide target.
[0286] When the metal oxide film 128a and the metal oxide film 128b are formed, an inert gas (e.g., helium gas, argon gas, xenon gas, etc.) may be mixed in addition to the oxygen gas. In addition, the ratio of the oxygen gas to the entire film-forming gas when the metal oxide film is formed (hereinafter also referred to as the oxygen flow rate ratio) is greater than 0% and less than 100%, preferably greater than 5% and less than 20%.
[0287] By reducing the oxygen flow rate to form a metal oxide film with low crystallinity, a metal oxide film with high conductivity can be obtained. On the other hand, by increasing the oxygen flow rate to form a metal oxide film with high crystallinity, a metal oxide film with high etching resistance and electrical stability can be obtained.
[0288] For example, the formation conditions of the metal oxide film 128a and the metal oxide film 128b are as follows: the substrate temperature is set to be higher than room temperature and lower than 180° C., preferably, the substrate temperature is set to be higher than room temperature and lower than 140° C. When the substrate temperature is set to be higher than room temperature and lower than 140° C. during the formation of the metal oxide film, productivity is improved, so it is preferred.
[0289] More specifically, the oxygen flow rate ratio when forming the metal oxide film 128a is 0% or more and less than 50%, preferably 0% or more and 30% or less, more preferably 0% or more and 20% or less, and typically 10%. The thickness of the metal oxide film 128a is 1nm or more and 50nm or less, preferably 5nm or more and 30nm or less.
[0290] The oxygen flow rate ratio when forming the metal oxide film 128b is 50% or more and 100% or less, preferably 60% or more and 100% or less, more preferably 80% or more and 100% or less, further preferably 90% or more and 100% or less, and typically 100%. In addition, the conditions such as pressure, temperature, and power when forming the metal oxide film 128a and the metal oxide film 128b may be different. By making the conditions other than the oxygen flow rate ratio the same, the time required for the film forming process can be shortened, which is preferred. The thickness of the metal oxide film 128b is greater than 10nm and less than 100nm, preferably greater than 20nm and less than 50nm.
[0291] The compositions of the metal oxide film 128a and the metal oxide film 128b may be different from each other. In this case, when both the metal oxide film 128a and the metal oxide film 128b use In-Ga-Zn oxide, the metal oxide film 128a preferably uses an oxide target whose In composition is higher than that of the metal oxide film 128b.
[0292] Next, a resist mask is formed on the metal oxide film 128b, the metal oxide film 128a and the metal oxide film 128b are processed by etching, and then the resist mask is removed to form the metal oxide layer 108a and the metal oxide layer 108b ( Fig.11A ).
[0293] After the metal oxide layer 108a and the metal oxide layer 108b are formed, a heat treatment (hereinafter referred to as a first heat treatment) may be performed. By performing the first heat treatment, hydrogen, water, and the like contained in the metal oxide layer 108a and the metal oxide layer 108b can be reduced. In addition, the heat treatment for the purpose of reducing hydrogen, water, and the like may be performed before the metal oxide film 128a and the metal oxide film 128b are processed into an island shape. Note that the first heat treatment is one of the treatments for highly purifying the metal oxide layer.
[0294] The temperature of the first heat treatment is, for example, 150° C. or higher and lower than the strain point of the substrate, preferably 200° C. or higher and 450° C. or lower, and more preferably 250° C. or higher and 350° C. or lower.
[0295] In addition, the first heat treatment can use an electric furnace, an RTA device, etc. By using an RTA device, heat treatment can be performed at a temperature above the strain point of the substrate only in a short time. Thus, the heating time can be shortened. The first heat treatment can be performed in an atmosphere of nitrogen, oxygen, ultra-dry air (water content is less than 20ppm, preferably less than 1ppm, more preferably less than 10ppb of air) or a rare gas (argon, helium, etc.). The above-mentioned nitrogen, oxygen, ultra-dry air or rare gas preferably does not contain hydrogen, water, etc. In addition, after heat treatment under a nitrogen or rare gas atmosphere, heating can also be performed under an oxygen or ultra-dry air atmosphere. As a result, while hydrogen, water, etc. in the metal oxide layer can be detached, oxygen can be supplied to the metal oxide layer. As a result, oxygen vacancies in the metal oxide layer can be reduced.
[0296] [Formation of Conductive Layer 112a and Conductive Layer 112b]
[0297] Next, a conductive film 121 which will later become the conductive layer 121a and the conductive layer 121b and a conductive film 122 which will later become the conductive layer 122a and the conductive layer 122b are stacked.
[0298] Next, a resist mask 131 ( Fig. 11B The resist mask 131 is provided at intervals in the region where the channel of the metal oxide layer 108 may be formed.
[0299] Then, the conductive film 122 is processed by etching to form a conductive layer 122a and a conductive layer 122b ( Fig. 11C ). At this time, if Fig. 11C As shown in FIG. 1 , it is preferable to perform processing so that the ends of the conductive layer 122 a and the conductive layer 122 b are located inside the ends of the resist mask 131 .
[0300] Isotropic etching is preferably used for etching the conductive film 122. Preferably, a wet etching method can be used. In this way, etching can be performed so that the ends of the conductive layer 122a and the conductive layer 122b are recessed.
[0301] After the conductive layer 122a and the conductive layer 122b are formed, the resist mask 131 is removed.
[0302] Next, the conductive film 123 is formed so as to cover the conductive layer 121a, the conductive layer 122a, and the conductive layer 122b. The conductive film 123 is a conductive film that will later become the conductive layer 123a and the conductive layer 123b.
[0303] Next, a resist mask 132 ( Fig. 12A). At this time, the resist mask 132 can be formed using the same photomask as the resist mask 131. Thus, since the same photomask can be used, the manufacturing cost can be suppressed.
[0304] Next, the conductive films 121 and 123 are processed by etching to form the conductive layers 121a, 121b, 123a, and 123b. At this time, it is preferable to process the conductive layers 121a and 123a so that the ends of the conductive layers 122a are in contact with each other and the conductive layer 122a is not exposed. At this time, it is preferable to process the conductive layers 121b and 123b so that the ends of the conductive layers 122b are in contact with each other and the conductive layer 122b is not exposed.
[0305] Anisotropic etching is preferably used for etching the conductive film 121 and the conductive film 123. Preferably, dry etching is used. Thus, the conductive layer 121a, the conductive layer 121b, the conductive layer 123a, and the conductive layer 123b can be processed in a manner that does not cause the ends of the conductive layer 121a, the conductive layer 121b, the conductive layer 123a, and the conductive layer 123b to recede. Thus, the conductive layer 121a and the conductive layer 123a can be formed in a manner that surrounds the conductive layer 122a. The conductive layer 121b and the conductive layer 123b can be formed in a manner that surrounds the conductive layer 122b. In addition, the deviation of the channel length of the transistor can be suppressed.
[0306] By using the same conductive film as the conductive layers 121a, 121b, 123a, and 123b, etching can be easily performed. This is preferred because it is difficult to form projections and recesses at the ends of the conductive layers 121a, 121b, 123a, and 123b.
[0307] Then, the resist mask 132 is removed. Through the above steps, the conductive layer 112a and the conductive layer 112b ( Fig. 12B ).
[0308] [Formation of Insulating Layers 114 and 116]
[0309] Next, the insulating layer 114 and the insulating layer 116 are formed so as to cover the conductive layer 112 a , the conductive layer 112 b , the metal oxide layer 108 , and the like.
[0310] The insulating layer 114 is preferably formed in an atmosphere containing oxygen, for example, and is preferably formed using a PECVD method.
[0311] As the insulating layer 114, for example, it is preferred to form an oxide film such as a silicon oxide film or a silicon oxynitride film using a PECVD device in an oxygen-containing atmosphere. In this way, an insulating layer 114 with few defects can be formed. At this time, as source gases, it is preferred to use a deposition gas containing silicon and an oxidizing gas. Typical examples of deposition gases containing silicon include silane, disilane, trisilane, and fluorinated silane. Oxidizing gases include oxygen, ozone, nitrous oxide, nitrogen dioxide, and the like.
[0312] The insulating layer 114 can have a stacked-layer structure including an insulating layer 114 a and an insulating layer 114 b over the insulating layer 114 a .
[0313] When forming the insulating layer 114a, the flow rate of the oxidizing gas relative to the above-mentioned deposition gas is greater than 20 times and less than 100 times, preferably greater than 40 times and less than 80 times, and the pressure in the processing chamber is less than 100Pa, preferably less than 50Pa.
[0314] In this embodiment, a silicon oxynitride film is formed as the insulating layer 114a by a PECVD method under the following conditions: the temperature of the substrate 102 is maintained at 220°C, silane with a flow rate of 50 sccm and nitrous oxide with a flow rate of 2000 sccm are used as source gases, the pressure in the processing chamber is 20 Pa, and the high-frequency power supplied to the parallel plate electrodes is 13.56 MHz, 100 W (power density is 1.6×10 -2 W / cm 2 ).
[0315] As the insulating layer 114b, a silicon oxide film or a silicon oxynitride film is formed under the following conditions: the substrate temperature in the processing chamber of the PECVD device which is vacuum-evacuated is maintained at 180°C to 280°C, preferably 200°C to 240°C, a source gas is introduced into the processing chamber and the pressure in the processing chamber is set to 100 Pa to 250 Pa, preferably 100 Pa to 200 Pa, and 0.17 W / cm2 is supplied to the electrode in the processing chamber. 2 Above and 0.5W / cm 2 Below, preferably 0.25W / cm 2 Above and 0.35W / cm 2 The following high frequency power.
[0316] In the film formation conditions of the insulating layer 114b, the high frequency power having the power density described above is supplied to the reaction chamber having the pressure described above, thereby improving the decomposition efficiency of the source gas in the plasma, increasing the oxygen radicals, and promoting the oxidation of the source gas, so that the oxygen content in the insulating layer 114b exceeds the stoichiometric composition. On the other hand, in the film formed at the substrate temperature within the temperature range described above, since the bonding force between silicon and oxygen is weak, part of the oxygen in the film is released by the heat treatment in the subsequent process. As a result, an insulating film having an oxygen content exceeding the stoichiometric composition and part of the oxygen released by heating can be formed.
[0317] In the step of forming the insulating layer 114b, the insulating layer 114a is used as a protective film for the metal oxide layer 108. Therefore, the insulating layer 114b can be formed using high-frequency power with high power density while reducing damage to the metal oxide layer 108.
[0318] In addition, in the film formation conditions of the insulating layer 114b, by increasing the flow rate of the deposition gas containing silicon relative to the oxidizing gas, the amount of defects in the insulating layer 114b can be reduced. As a result, the reliability of the transistor can be improved.
[0319] In the above description, the insulating layer 114 has a two-layer structure of the insulating layer 114a and the insulating layer 114b, but one embodiment of the present invention is not limited to this. For example, the insulating layer 114 may also have a single-layer structure of one of the insulating layer 114a and the insulating layer 114b. By making the insulating layer 114 have a single-layer structure, productivity can be improved, so it is preferred. In addition, the insulating layer 114 may also have a stacked structure of three or more layers.
[0320] Next, the insulating layer 116 is formed so as to cover the insulating layer 114b. The insulating layer 116 can be formed by the same method as that of the insulating layer 106.
[0321] As the insulating layer 116, for example, a silicon nitride film is preferably used. The insulating layer 116 can be formed, for example, by a sputtering method or a PECVD method. For example, when the insulating layer 116 is formed by a PECVD method, the substrate temperature is set to be lower than 400°C, preferably lower than 375°C, and more preferably higher than 180°C and lower than 350°C. By setting the substrate temperature during the formation of the insulating layer 116 to the above range, a dense film can be formed, so it is preferred. In addition, by setting the substrate temperature during the formation of the insulating layer 116 to the above range, oxygen or excess oxygen in the insulating layer 114a and the insulating layer 114b can be moved to the metal oxide layer 108.
[0322] When a silicon nitride film is formed as the insulating layer 116 using the PECVD method, a silicon-containing deposition gas, nitrogen and ammonia are preferably used as source gases. By using less ammonia than nitrogen, ammonia dissociates in the plasma to generate active species. The active species will cut the bond between silicon and hydrogen and the triple bond between nitrogen molecules included in the silicon-containing deposition gas. As a result, the bonding between silicon and nitrogen can be promoted, and a silicon nitride film with less bonding between silicon and hydrogen, fewer defects and greater density can be formed. On the other hand, when the amount of ammonia is greater than the amount of nitrogen, the decomposition of the silicon-containing deposition gas and nitrogen does not progress, and the bonding between silicon and hydrogen will remain, resulting in the formation of a silicon nitride film with more hydrogen and defects and less density. Therefore, in the source gas, the nitrogen flow ratio relative to ammonia is set to be greater than 5 times and less than 50 times, preferably greater than 10 times and less than 50 times. By adopting the above flow ratio, a silicon nitride with less hydrogen and defects and greater density can be formed.
[0323] In this embodiment, as the insulating layer 116, a silicon nitride film with a thickness of 100 nm is formed by using a PECVD device and using silane, nitrogen and ammonia as source gases. The flow rate of silane is 50 sccm, the flow rate of nitrogen is 5000 sccm, and the flow rate of ammonia is 100 sccm. The pressure of the processing chamber is set to 100 Pa, the substrate temperature is set to 350°C, and a high-frequency power of 1000 W is supplied to the parallel plate electrodes using a high-frequency power supply of 27.12 MHz. The PECVD device has an electrode area of 6000 cm 2 The parallel plate PECVD device is used, and the power supplied is converted into power per unit area (power density) of 1.7×10 -1 W / cm 2 .
[0324] The film formation temperature of the insulating layer 116 can be set higher than the film formation temperature of the insulating layer 114a and the insulating layer 114b. By setting the temperature to a high level, impurities such as hydrogen in the insulating layer 116 can be reduced. In addition, the substrate temperature when forming the insulating layer 116 can be set to the same temperature as the insulating layer 114a and the insulating layer 114b. By setting the same temperature, productivity can be improved.
[0325] It is preferred that after forming the insulating layer 114a, the insulating layer 114b is continuously formed in a vacuum in a manner that does not expose the surface of the insulating layer 114a to the atmosphere. By continuously forming, it is possible to suppress the adhesion of impurities derived from atmospheric components to the surface of the insulating layer 114a. It is preferred that after forming the insulating layer 114b, the insulating layer 116 is continuously formed in a vacuum in a manner that does not expose the surface of the insulating layer 114b to the atmosphere. By continuously forming, it is possible to suppress the adhesion of impurities derived from atmospheric components to the surface of the insulating layer 114b. It is more preferred that the insulating layer 114a, the insulating layer 114b, and the insulating layer 116 are continuously formed. By continuously forming, it is possible to suppress the adhesion of impurities derived from atmospheric components to the surfaces of the insulating layers 114a and 114b.
[0326] After forming the insulating layers 114a, 114b, and 116, heat treatment (hereinafter referred to as second heat treatment) is preferably performed. The second heat treatment can reduce nitrogen oxides contained in the insulating layers 114a, 114b, and 116. Alternatively, the second heat treatment can move part of oxygen in the insulating layers 114a and 114b to the metal oxide layer 108, so that oxygen vacancies and VoH in the metal oxide layer 108 can be reduced.
[0327] For example, the temperature of the second heat treatment is typically set to lower than 400°C, preferably lower than 375°C, and more preferably 150°C to 350°C.
[0328] The second heat treatment can be carried out in an atmosphere of nitrogen, oxygen, ultra-dry air (air with a water content of 20 ppm or less, preferably 1 ppm or less, preferably 10 ppb or less) or a rare gas (argon, helium, etc.). The nitrogen, oxygen, ultra-dry air or rare gas preferably does not contain hydrogen, water, etc. The heat treatment can be carried out using an electric furnace, RTA, etc.
[0329] Through the above-described steps, the transistor 100C can be manufactured.
[0330] <Method for manufacturing transistor 2>
[0331] Hereinafter, a method for manufacturing the transistor 100C which is different from the method for manufacturing the transistor 1 will be described. The steps until the formation of the conductive layer 112a and the conductive layer 112b are the same as those of the method for manufacturing the transistor 1 (see FIG. 1 ). Fig. 12B ).
[0332] [Formation of Insulating Layer 114]
[0333] Next, an insulating layer 114 is formed so as to cover the conductive layer 112a, the conductive layer 112b, the metal oxide layer 108, and the like. Fig.13A). Regarding the method for forming the insulating layer 114, reference can be made to the description of the transistor manufacturing method 1, so its detailed description can be omitted. In addition, the insulating layer 114 may also have a two-layer structure of an insulating layer 114a and an insulating layer 114b. One embodiment of the present invention is not limited to this, for example, it may also have a single-layer structure of one of the insulating layer 114a and the insulating layer 114b. By making the insulating layer 114 have a single-layer structure, productivity can be improved, so it is preferred. In addition, the insulating layer 114 may also have a stacked structure with more than three layers.
[0334] [Heat treatment]
[0335] Heat treatment is performed after forming the insulating layer 114. By performing heat treatment after forming the insulating layer 114, nitrogen oxides included in the insulating layer 114 can be reduced. In addition, by the heat treatment, part of oxygen in the insulating layer 114 can be moved to the metal oxide layer 108, so that oxygen vacancies and VoH in the metal oxide layer 108 can be reduced.
[0336] For example, the temperature of the heat treatment is typically set to lower than 400°C, preferably lower than 375°C, and more preferably 150°C to 350°C.
[0337] The heat treatment can be carried out in an atmosphere of nitrogen, oxygen, ultra-dry air (air with a water content of 20 ppm or less, preferably 1 ppm or less, preferably 10 ppb or less) or a rare gas (argon, helium, etc.). The nitrogen, oxygen, ultra-dry air or rare gas preferably does not contain hydrogen, water, etc. The heat treatment can be carried out using an electric furnace, RTA, etc.
[0338] [Formation of Insulating Layer 116]
[0339] Next, the insulating layer 116 is formed so as to cover the insulating layer 114. For the method of forming the insulating layer 116, the description of the transistor manufacturing method 1 can be referred to, and thus a detailed description thereof is omitted.
[0340] Regarding the heat treatment after forming the insulating layer 116 , the description of the transistor manufacturing method 1 can be referred to, and thus a detailed description thereof is omitted.
[0341] Through the above-described steps, the transistor 100C can be manufactured.
[0342] <Method for manufacturing transistor 3>
[0343] Hereinafter, a method for manufacturing the transistor 100C which is different from the method for manufacturing the transistor 1 will be described. The steps of forming the conductive layers 112a and 112b are the same as those of the method for manufacturing the transistor 1 (see FIG. 1 ). Fig. 12B ).
[0344] [Formation of Insulating Layer 114]
[0345] Next, insulating layers 114a and 114b are formed so as to cover the conductive layer 112a, the conductive layer 112b, the metal oxide layer 108, and the like. Fig.13A ) Regarding the method for forming the insulating layer 114a and the insulating layer 114b, reference can be made to the description of the transistor manufacturing method 1, and thus a detailed description thereof will be omitted.
[0346] After forming the insulating layer 114a, the insulating layer 114b is preferably formed continuously in a vacuum so as not to expose the surface of the insulating layer 114a to the air. By forming the insulating layer 114b continuously, impurities derived from air components can be prevented from adhering to the surface of the insulating layer 114a.
[0347] [Formation of Insulating Layer 116]
[0348] Next, the insulating layer 116 is formed so as to cover the insulating layer 114 .
[0349] The insulating layer 116 may be made of the above-mentioned materials. For example, aluminum oxide may be used for the insulating layer 116. In addition, for example, In-Ga-Zn oxide may be used for the insulating layer 116. When the ratio of gallium in the composition of In-Ga-Zn oxide is larger than that of indium (for example, the atomic ratio is In:Ga:Zn=1:3:2), the band gap of the insulating layer 116 is large, so it is preferred. The insulating layer 116 can be formed using a sputtering device. Fig. 13B A schematic cross-sectional view of the interior of the film forming apparatus when the insulating layer 116 is formed on the insulating layer 114 b is shown. Fig. 13B A target 191 disposed inside a sputtering device and a plasma 192 generated below the target 191 are schematically shown.
[0350] First, when forming the insulating layer 116, plasma discharge is performed in an atmosphere containing an oxygen gas. At this time, oxygen 130b is added to the insulating layer 114b, which is the surface on which the insulating layer 116 is formed. In addition, when forming the insulating layer 116, an inert gas (for example, helium gas, argon gas, xenon gas, etc.) may be mixed in addition to the oxygen gas. Oxygen 130b is sometimes supplied to the insulating layer 114a and the insulating layer 114b.
[0351] The ratio of the oxygen gas in the entire film-forming gas during formation of the insulating layer 116 is greater than 0% and less than 100%, preferably greater than 10% and less than 100%, and more preferably greater than 30% and less than 100%.
[0352] It is preferred that after forming the insulating layer 114a, the insulating layer 114b is continuously formed in a vacuum in a manner that does not expose the surface of the insulating layer 114a to the atmosphere. By continuously forming, it is possible to suppress the adhesion of impurities derived from atmospheric components to the surface of the insulating layer 114a. It is preferred that after forming the insulating layer 114b, the insulating layer 116 is continuously formed in a vacuum in a manner that does not expose the surface of the insulating layer 114b to the atmosphere. By continuously forming, it is possible to suppress the adhesion of impurities derived from atmospheric components to the surface of the insulating layer 114b. It is more preferred that the insulating layer 114a, the insulating layer 114b, and the insulating layer 116 are continuously formed. By continuously forming, it is possible to suppress the adhesion of impurities derived from atmospheric components to the surfaces of the insulating layers 114a and 114b.
[0353] After forming the insulating layers 114a, 114b, and 116, heat treatment is preferably performed. The heat treatment can reduce nitrogen oxides contained in the insulating layers 114a, 114b, and 116. Alternatively, the heat treatment can move part of oxygen in the insulating layers 114a and 114b to the metal oxide layer 108, so that oxygen vacancies and VoH in the metal oxide layer 108 can be reduced.
[0354] Regarding the heat treatment after forming the insulating layer 116 , the description of the transistor manufacturing method 1 can be referred to, and thus a detailed description thereof is omitted.
[0355] Through the above-described steps, the transistor 100C can be manufactured.
[0356] <Method for manufacturing transistor 4>
[0357] Hereinafter, a method for manufacturing the transistor 100C which is different from the manufacturing methods described in the transistor manufacturing methods 1 and 3 will be described. The steps until the conductive layers 112a and 112b are formed are the same as those in the transistor manufacturing method 1 (see FIG. 1 ). Fig. 12B ).
[0358] [Formation of Insulating Layer 114]
[0359] Next, insulating layers 114a and 114b are formed so as to cover the conductive layer 112a, the conductive layer 112b, the metal oxide layer 108, and the like. Fig.13A ) Regarding the method for forming the insulating layer 114a and the insulating layer 114b, reference can be made to the description of the transistor manufacturing method 1, and thus a detailed description thereof will be omitted.
[0360] After forming the insulating layer 114a, the insulating layer 114b is preferably formed continuously in a vacuum so as not to expose the surface of the insulating layer 114a to the air. By forming the insulating layer 114b continuously, impurities derived from air components can be prevented from adhering to the surface of the insulating layer 114a.
[0361] Heat treatment may be performed after the insulating layer 114b is formed. The heat treatment can reduce nitrogen oxides contained in the insulating layers 114a and 114b. In addition, the heat treatment can move part of oxygen contained in the insulating layers 114a and 114b to the metal oxide layer 108 to reduce oxygen vacancies and VoH contained in the metal oxide layer 108.
[0362] The temperature of the heat treatment is typically set to be above 150°C and below 400°C, preferably above 300°C and below 400°C, more preferably above 320°C and below 370°C. The heat treatment can be carried out in an atmosphere of nitrogen, oxygen, ultra-dry air (water content is below 20ppm, preferably below 1ppm, more preferably below 10ppb) or a rare gas (argon, helium, etc.). The above-mentioned nitrogen, oxygen, ultra-dry air or rare gas preferably does not contain hydrogen, water, etc. The heat treatment can be carried out using an electric furnace, an RTA device, etc.
[0363] [Oxygen supply treatment]
[0364] Next, a conductive film 134 ( Fig.14A ).
[0365] A metal oxide film, a metal film, or an alloy film can be used as the conductive film 134. The conductive film 134 is preferably extremely thin, for example, 1 nm to 20 nm, preferably 2 nm to 15 nm, more preferably 3 nm to 10 nm, and typically about 5 nm.
[0366] Examples of metal oxides that can be used for the conductive film 134 include In-Sn oxide, In-W oxide, In-W-Zn oxide, In-Ti oxide, In-Ti-Sn oxide, In-Zn oxide, In-Sn-Si oxide, and In-Ga-Zn oxide.
[0367] As the conductive film 134, a metal film or an alloy film containing aluminum, titanium, chromium, iron, cobalt, nickel, copper, zinc, gallium, molybdenum, silver, indium, tin, tantalum, tungsten, or the like can be used.
[0368] Alternatively, as the conductive film 134 , a semiconductor film made of a compound semiconductor, an oxide semiconductor, or the like other than silicon, germanium, or the like may be used.
[0369] Here, it is preferable to form the conductive film 134 using a metal oxide by a sputtering method or the like in an atmosphere containing oxygen because oxygen can be supplied to the insulating layer 114a and the insulating layer 114b during the formation.
[0370] The maximum temperature in the step of forming the conductive film 134 is 350° C. or lower, preferably 340° C. or lower, more preferably 330° C. or lower, and further preferably 300° C. or lower.
[0371] Next, a process of supplying oxygen 130c to the insulating layer 114a and the insulating layer 114b through the conductive film 134 (hereinafter also referred to as oxygen supply process) is performed. Fig. 14B ).
[0372] As oxygen supply treatment, plasma treatment in an oxygen atmosphere (also referred to as oxygen plasma treatment) is preferably used. By turning oxygen into plasma, oxygen radicals, oxygen atoms, or oxygen ions can be added to the insulating layer 114a and the insulating layer 114b through the conductive film 134. The higher the oxygen flow rate ratio in the gas introduced into the device, the better. The oxygen flow rate ratio is 50% or more and 100% or less, preferably 60% or more and 100% or less, more preferably 80% or more and 100% or less, and further preferably 100%.
[0373] In particular, it is preferable to use a processing device including a pair of parallel plate type electrodes as the processing device. In this case, by performing plasma processing with a bias voltage applied between the pair of electrodes, more oxygen can be supplied to the insulating layer 114a and the insulating layer 114b. The bias voltage is applied, for example, in such a way that oxygen ions in the oxygen plasma are easily moved to the substrate side. The oxygen ions in the oxygen plasma, for example, are charged with oxygen. + or 2+ Since the positive charges are equal, a bias voltage is applied so that the electrode located on the substrate side becomes a negative potential, and the oxygen ions tend to move to the substrate side.
[0374] Here, when the oxygen supply process is directly performed on the insulating layer 114a and the insulating layer 114b without providing the conductive film 134, a part of the oxygen supplied to the insulating layer 114a and the insulating layer 114b may be released to the outside again. However, in this manufacturing method example, by providing the conductive film 134 on the insulating layer 114a and the insulating layer 114b, the oxygen supplied to the insulating layer 114a and the insulating layer 114b can be prevented from being released to the outside again. In addition, by providing the conductive film 134, damage to the insulating layer 114a and the insulating layer 114b can be alleviated.
[0375] Furthermore, the conductive film 134 on the insulating layer 114a and the insulating layer 114b has an effect of easily attracting ionized oxygen when a bias voltage is applied between the pair of electrodes in the oxygen supply process. Therefore, by providing the conductive film 134, the effect of applying the bias voltage can be multiplied and enhanced.
[0376] In addition, when a dry etching device, an ashing device, a PECVD device, etc. is used as a processing device, it is preferable because the same device as other processing can be used. In particular, it is preferable to use an ashing device.
[0377] The oxygen supply treatment is preferably performed at a temperature of, for example, room temperature or higher and 350° C. or lower, preferably 150° C. or higher and lower than 350° C., and more preferably 200° C. or higher and 340° C. or lower.
[0378] When a bias voltage is applied between a pair of electrodes included in the processing device, the bias voltage may be set to, for example, 10 V or more and 1 kV or less. Alternatively, the power density of the bias voltage may be set to, for example, 1 W / cm 2 Above and 5W / cm 2 The following will do.
[0379] The oxygen supply treatment is not limited to the above-mentioned treatment, and a method that can supply oxygen to the insulating layer 114a and the insulating layer 114b through the conductive film 134 can be used. For example, oxygen can be supplied to the insulating film through the conductive film by an ion implantation method, an ion doping method, or a plasma immersion ion implantation method. Alternatively, heat treatment can be performed in an oxygen atmosphere. When such a treatment is used, the conductive film 134 can also be used as a capping film that prevents oxygen supplied to the insulating layer 114a and the insulating layer 114b from being separated and a mitigation layer that mitigates damage to the insulating layer 114a and the insulating layer 114b.
[0380] The conductive film 134 may become brittle due to the oxygen supply treatment. In addition, especially when a metal or an alloy is used as the conductive film 134, the conductive film 134 may be oxidized by the oxygen supply treatment to increase the resistance value or part of it may be etched to become thinner. In this case, the conductive film 134 is preferably removed by etching.
[0381] Fig. 14C A cross-sectional view is shown after the conductive film 134 is etched.
[0382] The maximum temperature in the etching step of the conductive film 134 is 350° C. or lower, preferably 340° C. or lower, more preferably 330° C. or lower, and further preferably 300° C. or lower.
[0383] As oxygen supply treatment, plasma treatment in an atmosphere containing oxygen may be performed without providing the conductive film 134. By not providing the conductive film 134, productivity can be improved.
[0384] [Formation of Insulating Layer 116]
[0385] Next, the insulating layer 116 is formed so as to cover the insulating layer 114. For the method of forming the insulating layer 116, the description of the transistor manufacturing method 1 can be referred to, and thus a detailed description thereof is omitted.
[0386] Through the above-described steps, the transistor 100C can be manufactured.
[0387] The above is the description of an example of a method for manufacturing a transistor.
[0388] At least a part of the structural examples, manufacturing method examples, and drawings corresponding to these examples described in this embodiment mode can be implemented in combination with other structural examples, manufacturing method examples, drawings, and the like as appropriate.
[0389] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0390] Implementation Method 2
[0391] In this embodiment, an example of a display device including the transistor described as an example in the above embodiment is described.
[0392] <Structure instance>
[0393] Fig.15A is a plan view showing an example of a display device. Fig.15A The display device 700 shown includes: a pixel portion 702 arranged on a first substrate 701; a source driver circuit portion 704 and a gate driver circuit portion 706 arranged on the first substrate 701; a sealant 712 arranged in a manner surrounding the pixel portion 702, the source driver circuit portion 704, and the gate driver circuit portion 706; and a second substrate 705 arranged in a manner opposite to the first substrate 701. Note that the first substrate 701 and the second substrate 705 are sealed by the sealant 712. In other words, the pixel portion 702, the source driver circuit portion 704, and the gate driver circuit portion 706 are sealed by the first substrate 701, the sealant 712, and the second substrate 705. Note that although in Fig.15A Although not shown in the figure, a display element is provided between the first substrate 701 and the second substrate 705.
[0394] In addition, in the display device 700, an FPC (Flexible printed circuit) terminal portion 708 electrically connected to the pixel portion 702, the source driver circuit portion 704, the gate driver circuit portion 706, and the gate driver circuit portion 706 is provided in a region on the first substrate 701 that is not surrounded by the sealant 712. In addition, the FPC terminal portion 708 is connected to the FPC 716, and various signals and the like are supplied to the pixel portion 702, the source driver circuit portion 704, and the gate driver circuit portion 706 through the FPC 716. In addition, the pixel portion 702, the source driver circuit portion 704, the gate driver circuit portion 706, and the FPC terminal portion 708 are each connected to a signal line 710. Various signals and the like supplied by the FPC 716 are supplied to the pixel portion 702, the source driver circuit portion 704, the gate driver circuit portion 706, and the FPC terminal portion 708 through the signal line 710.
[0395] In addition, a plurality of gate drive circuit units 706 may be provided in the display device 700. In addition, as the display device 700, although an example is shown in which the source drive circuit unit 704 and the gate drive circuit unit 706 are formed on the same first substrate 701 as the pixel unit 702, it is not limited to this structure. For example, only the gate drive circuit unit 706 may be formed on the first substrate 701, or only the source drive circuit unit 704 may be formed on the first substrate 701. In this case, a structure in which a substrate having a source drive circuit or a gate drive circuit, etc. (for example, a drive circuit substrate formed of a single crystal semiconductor film or a polycrystalline semiconductor film) is formed on the first substrate 701 may also be adopted. In addition, there is no particular limitation on the connection method of the separately formed drive circuit substrate, and a COG (Chip On Glass) method, a wire bonding method, etc. may be adopted.
[0396] The pixel portion 702 , the source driver circuit portion 704 , and the gate driver circuit portion 706 included in the display device 700 include a plurality of transistors, and transistors of the semiconductor device of one embodiment of the present invention can be applied as the transistors.
[0397] In addition, the display device 700 may include various elements. Examples of such elements include electroluminescent (EL) elements (including organic and inorganic EL elements, organic EL elements, inorganic EL elements, LEDs, etc.), light-emitting transistor elements (transistors that emit light according to current), electron emission elements, liquid crystal elements, electronic ink elements, electrophoretic elements, electrowetting elements, plasma display panels (PDPs), MEMS (micro-electromechanical systems), displays (e.g., grating light valves (GLVs), digital micromirror devices (DMDs), digital microshutter (DMS) elements, interferometric modulation (IMOD) elements, etc.), piezoelectric ceramic displays, etc.
[0398] In addition, as an example of a display device using EL elements, there are EL displays, etc. As an example of a display device using electron emission elements, there are field emission displays (FED) or SED flat-panel displays (SED: Surface-conduction Electron-emitter Display: surface conduction electron emission display), etc. As an example of a display device using liquid crystal elements, there are liquid crystal displays (transmissive liquid crystal displays, semi-transmissive liquid crystal displays, reflective liquid crystal displays, direct-view liquid crystal displays, projection liquid crystal displays), etc. As an example of a display device using electronic ink elements or electrophoretic elements, there are electronic paper, etc. Note that when a semi-transmissive liquid crystal display or a reflective liquid crystal display is implemented, part or all of the pixel electrode can have the function of a reflective electrode. For example, part or all of the pixel electrode can contain aluminum, silver, etc. In addition, at this time, a storage circuit such as SRAM can also be set under the reflective electrode. In this way, power consumption can be further reduced.
[0399] As a display mode of the display device 700, a progressive scanning mode or an interlaced scanning mode can be adopted. In addition, the color element controlled in the pixel when performing color display is not limited to the three colors of RGB (R represents red, G represents green, and B represents blue). For example, it can be composed of four pixels of R pixel, G pixel, B pixel and W (white) pixel. Or, as in the PenTile arrangement, one color element can be composed of two colors in RGB, and two different colors can be selected according to the color element. Or one or more colors such as yellow, cyan, magenta, etc. can be added to RGB. In addition, the size of the display area of each color element point can be different. However, the disclosed invention is not limited to a display device for color display, but can also be applied to a display device for black and white display.
[0400] In addition, in order to use white light (W) for backlight (organic EL element, inorganic EL element, LED, fluorescent lamp, etc.) to enable the display device to display in full color, a coloring layer (also called a filter) can also be used. As a coloring layer, for example, red (R), green (G), blue (B), yellow (Y), etc. can be used in appropriate combinations. By using a coloring layer, the color reproducibility can be further improved compared to the case where a coloring layer is not used. At this time, it is also possible to directly use white light in the area that does not include the coloring layer for display by setting an area including the coloring layer and an area that does not include the coloring layer. By partially setting an area that does not include the coloring layer, when displaying a bright image, the brightness reduction caused by the coloring layer can sometimes be reduced and the power consumption can be reduced by about 20% to 30%. However, when using self-luminous elements such as organic EL elements or inorganic EL elements for full-color display, R, G, B, Y, and W can also be emitted from elements with each luminous color. By using a self-luminous element, power consumption can sometimes be further reduced compared to the case where a coloring layer is used.
[0401] In addition, as a colorization method, in addition to a method of converting a portion of the emission from the above-mentioned white light into red, green and blue through a color filter (color filter method), a method of using red, green and blue emission respectively (three-color method) and a method of converting a portion of the emission from blue light into red or green (color conversion method or quantum dot method) can also be used.
[0402] Fig. 15B The display device 700A shown is a display device that can be suitably used in electronic devices having a large screen, for example, a television device, a monitor device, a digital signage, and the like.
[0403] The display device 700A includes a plurality of source driver ICs 721 and a pair of gate driver circuits 722 .
[0404] The plurality of source driver ICs 721 are mounted on FPCs 723. The plurality of FPCs 723 have one terminal connected to the substrate 701 and another terminal connected to a printed circuit board 724. The printed circuit board 724 is disposed on the back side of the pixel portion 702 by bending the FPC 723 and mounted in the electrical device.
[0405] On the other hand, the gate driver circuit 722 is formed on the substrate 701. Thus, an electronic device with a narrow frame can be realized.
[0406] By adopting the above structure, a large and high-definition display device can be realized. For example, it can be applied to a display device with a screen size of 30 inches or more, 40 inches or more, 50 inches or more, or 60 inches or more in diagonal. In addition, a display device with extremely high resolution such as full HD, 4K2K, 8K4K, etc. can be realized.
[0407] <Cross-section structure example>
[0408] Next, use Figures 16 to 18 A structure using a liquid crystal element and an EL element as a display element will be described. Fig.16 and Fig.17 It is along Fig.15A The cross-sectional view along the dot-dash line QR shown in FIG. 1 is a structure in which a liquid crystal element is used as a display element. Fig.18 It is along Fig.15A The cross-sectional view taken along the dashed line QR shown in the figure has a structure in which an EL element is used as a display element.
[0409] Below, first explain Figures 16 to 18 The common parts are shown, and then the different parts are described.
[0410] [Description of Common Parts of Display Devices]
[0411] Figures 16 to 18 The display device 700 shown includes: a routing wiring section 711; a pixel section 702; a source driver circuit section 704; and an FPC terminal section 708. In addition, the routing wiring section 711 includes a signal line 710. In addition, the pixel section 702 includes a transistor 750 and a capacitor 790. In addition, the source driver circuit section 704 includes a transistor 752.
[0412] The transistor described in Embodiment 1 can also be used as the transistor 750 and the transistor 752 .
[0413] The transistor used in this embodiment includes a highly purified oxide semiconductor film in which the formation of oxygen vacancies is suppressed. The transistor can reduce the off-state current. Therefore, the retention time of electrical signals such as image signals can be extended, and the writing interval can also be extended in the state where the power is turned on. Therefore, the frequency of refresh work can be reduced, thereby achieving the effect of suppressing power consumption.
[0414] In addition, the transistor used in this embodiment can obtain a higher field effect mobility and can therefore be driven at high speed. For example, by using such a transistor capable of high-speed driving in a display device, a switching transistor in a pixel portion and a driving transistor for a driving circuit portion can be formed on the same substrate. In other words, since a semiconductor device formed of a silicon wafer or the like does not need to be used separately as a driving circuit, the number of components of the semiconductor device can be reduced. In addition, a high-quality image can also be provided in the pixel portion by using a transistor capable of high-speed driving.
[0415] The capacitor 790 includes: a lower electrode formed by processing the same conductive film as the conductive film used as the first gate electrode included in the transistor 750; and an upper electrode formed by processing the same conductive film as the conductive film used as the second gate electrode included in the transistor 750. In addition, an insulating film formed by forming the same insulating film as the insulating film used as the first gate insulating film included in the transistor 750; and an insulating film formed by forming the same insulating film as the insulating film used as the protective insulating film on the transistor 750 are provided between the lower electrode and the upper electrode. That is, the capacitor 790 has a stacked structure in which an insulating film used as a dielectric film is sandwiched between a pair of electrodes.
[0416] In addition, Figures 16 to 18 In the embodiment, a planarization insulating film 770 is provided over the transistor 750, the transistor 752, and the capacitor 790.
[0417] exist Figures 16 to 18 7 shows a structure in which the transistor 750 included in the pixel unit 702 and the transistor 752 included in the source driver circuit unit 704 use transistors of the same structure, but is not limited to this. For example, the pixel unit 702 and the source driver circuit unit 704 may also use different transistors. Specifically, the pixel unit 702 uses a top-gate transistor, and the source driver circuit unit 704 uses a bottom-gate transistor, or the pixel unit 702 uses a bottom-gate transistor, and the source driver circuit unit 704 uses a top-gate transistor. In addition, the source driver circuit unit 704 may also be referred to as a gate driver circuit unit.
[0418] The signal line 710 is formed in the same process as a conductive film used as a source electrode and a drain electrode of the transistors 750 and 752. When a material containing copper is used as the signal line 710, for example, signal delay due to wiring resistance is reduced, and a large-screen display can be achieved.
[0419] In addition, the FPC terminal portion 708 includes a connection electrode 760, an anisotropic conductive film 780, and an FPC 716. The connection electrode 760 is formed in the same process as the conductive film used as the source electrode and the drain electrode of the transistors 750 and 752. In addition, the connection electrode 760 and the terminal included in the FPC 716 are electrically connected through the anisotropic conductive film 780.
[0420] Note that, for example, a glass substrate can be used as the first substrate 701 and the second substrate 705. Note that a flexible substrate can be used as the first substrate 701 and the second substrate 705. Examples of the flexible substrate include a plastic substrate.
[0421] In addition, a structure 778 is provided between the first substrate 701 and the second substrate 705. The structure 778 is a columnar spacer and is used to control the distance (cell gap) between the first substrate 701 and the second substrate 705. Alternatively, a spherical spacer may be used as the structure 778.
[0422] In addition, on the second substrate 705 side, a light-shielding film 738 used as a black matrix, a coloring film 736 used as a color filter, and an insulating film 734 in contact with the light-shielding film 738 and the coloring film 736 are provided.
[0423] [Structural Example of Display Device Using Liquid Crystal Element]
[0424] Fig.16 The display device 700 shown includes a liquid crystal element 775. The liquid crystal element 775 includes a conductive film 772, a conductive film 774, and a liquid crystal layer 776. The conductive film 774 is provided on the second substrate 705 side and functions as a counter electrode. Fig.16 The display device 700 shown can display an image by changing the alignment state of the liquid crystal layer 776 by applying a voltage between the conductive film 772 and the conductive film 774, thereby controlling the transmission and non-transmission of light.
[0425] The conductive film 772 is electrically connected to a conductive film used as a source electrode or a drain electrode of the transistor 750. The conductive film 772 is formed over the planarizing insulating film 770 and used as a pixel electrode, that is, one electrode of a display element.
[0426] As the conductive film 772, a conductive film that is translucent to visible light or a conductive film that is reflective to visible light can be used. As the conductive film that is translucent to visible light, for example, a material containing one selected from indium (In), zinc (Zn), and tin (Sn) is preferably used. As the conductive film that is reflective to visible light, for example, a material containing aluminum or silver is preferably used.
[0427] When the conductive film 772 is a conductive film that is reflective for visible light, the display device 700 is a reflective liquid crystal display device. In addition, when the conductive film 772 is a conductive film that is transmissive for visible light, the display device 700 is a transmissive liquid crystal display device. When a reflective liquid crystal display device is used, a polarizing plate is provided on the visible side. On the other hand, when a transmissive liquid crystal display device is used, a pair of polarizing plates that sandwich a liquid crystal element are provided.
[0428] By changing the structure on the conductive film 772, the driving method of the liquid crystal element can be changed. Fig.17 An example of this is shown. Fig.17The display device 700 shown is an example of a structure that uses a horizontal electric field method (for example, FFS mode) as a driving method for liquid crystal elements. Fig.17 In the case of the structure shown, an insulating film 773 is provided on the conductive film 772, and a conductive film 774 is provided on the insulating film 773. In this case, the conductive film 774 has a function as a common electrode, and the orientation state of the liquid crystal layer 776 can be controlled by the electric field generated between the conductive film 772 and the conductive film 774 via the insulating film 773.
[0429] Note that although Fig.16 and Fig.17 Although not shown in the figure, an alignment film may be provided on one or both of the conductive films 772 and 774 on the side in contact with the liquid crystal layer 776. Fig.16 and Fig.17 Although not shown in the figure, optical components (optical substrates) such as polarization components, phase difference components, and anti-reflection components may be appropriately provided. For example, circular polarization using a polarization substrate and a phase difference substrate may also be used. In addition, backlight, side light, etc. may also be used as a light source.
[0430] When a liquid crystal element is used as a display element, thermotropic liquid crystal, low molecular liquid crystal, polymer liquid crystal, polymer dispersed liquid crystal, ferroelectric liquid crystal, antiferroelectric liquid crystal, etc. These liquid crystal materials exhibit cholesteric phase, smectic phase, cubic phase, chiral nematic phase, homogeneous phase, etc. depending on the conditions.
[0431] In addition, when the lateral electric field method is adopted, liquid crystals exhibiting a blue phase without an alignment film can also be used. The blue phase is a type of liquid crystal phase, and refers to the phase that appears just before the transition from the cholesteric phase to the homogeneous phase when the temperature of the cholesteric liquid crystal is raised. Because the blue phase only appears in a narrow temperature range, a liquid crystal composition in which a chiral agent is mixed is used in the liquid crystal layer to expand the temperature range. Since the liquid crystal composition containing a liquid crystal exhibiting a blue phase and a chiral agent has a fast response speed and is optically isotropic. Therefore, the liquid crystal composition containing a liquid crystal exhibiting a blue phase and a chiral agent does not require an alignment treatment. In addition, since there is no need to set an alignment film and no friction treatment is required, electrostatic damage caused by the friction treatment can be prevented, thereby reducing defects and damage to the liquid crystal display device in the manufacturing process. In addition, the viewing angle dependence of the liquid crystal material exhibiting a blue phase is small.
[0432] When a liquid crystal element is used as a display element, a TN (Twisted Nematic) mode, an IPS (In-Plane-Switching) mode, an FFS (Fringe Field Switching) mode, an ASM (Axially Symmetric aligned Micro-cell) mode, an OCB (Optical Compensated Birefringence) mode, an FLC (Ferroelectric Liquid Crystal) mode, an AFLC (AntiFerroelectric Liquid Crystal) mode, or the like can be used.
[0433] In addition, the display device 700 may also use a normally black liquid crystal display device, such as a transmissive liquid crystal display device using a vertical alignment (VA) mode. As vertical alignment modes, several examples can be cited, such as MVA (Multi-Domain Vertical Alignment: multi-domain vertical alignment) mode, PVA (Patterned Vertical Alignment: vertical alignment configuration) mode, ASV (Advanced Super View: advanced super vision) mode, etc.
[0434] [Display device using light-emitting element]
[0435] Fig.18 The display device 700 shown includes a light-emitting element 782. The light-emitting element 782 includes a conductive film 772, an EL layer 786, and a conductive film 788. Fig.18 The display device 700 shown in the figure can display an image by emitting light from an EL layer 786 included in a light-emitting element 782 provided in each pixel. The EL layer 786 includes an organic compound or an inorganic compound such as quantum dots.
[0436] As materials that can be used for organic compounds, fluorescent materials or phosphorescent materials can be cited. In addition, as materials that can be used for quantum dots, colloidal quantum dot materials, alloy quantum dot materials, core-shell quantum dot materials, core-type quantum dot materials, etc. can be cited. In addition, materials containing element groups of Groups 12 and 16, Groups 13 and 15, or Groups 14 and 16 can also be used. Alternatively, quantum dot materials containing elements such as cadmium (Cd), selenium (Se), zinc (Zn), sulfur (S), phosphorus (P), indium (In), tellurium (Te), lead (Pb), gallium (Ga), arsenic (As), and aluminum (Al) can be used.
[0437] exist Fig.18 In the display device 700 shown in the figure, an insulating film 730 is provided on a planarizing insulating film 770 and a conductive film 772. The insulating film 730 covers a portion of the conductive film 772. The light-emitting element 782 adopts a top emission structure. Therefore, the conductive film 788 has light-transmitting properties and transmits light emitted by the EL layer 786. Note that although a top emission structure is illustrated in this embodiment mode, the present invention is not limited thereto. For example, a bottom emission structure that emits light to one side of the conductive film 772 or a double-sided emission structure that emits light to both the conductive film 772 side and the conductive film 788 side may also be applied.
[0438] In addition, a coloring film 736 is provided at a position overlapping with the light emitting element 782, and a light shielding film 738 is provided at a position overlapping with the insulating film 730, the routing wiring portion 711, and the source driver circuit portion 704. The coloring film 736 and the light shielding film 738 are covered by the insulating film 734. The space between the light emitting element 782 and the insulating film 734 is filled with the sealing film 732. Note that although the example is shown in Fig.18 The display device 700 shown in the figure has a structure in which the coloring film 736 is provided, but the present invention is not limited to this. For example, when the EL layer 786 is formed in an island shape in each pixel, that is, when the EL layer 786 is formed by coating, the coloring film 736 may not be provided.
[0439] [Configuration example of providing input / output device in display device]
[0440] Also available in Figures 16 to 18 An input-output device is provided in the display device 700 shown in the figure. Examples of the input-output device include a touch screen and the like.
[0441] Fig.19 Show Fig.17 The display device 700 shown in the figure is provided with a touch screen 791. Fig. 20 Show Fig.18 The display device 700 shown is provided with a touch screen 791 structure.
[0442] Fig.19 is Fig.17 The cross-sectional view of the display device 700 shown in FIG. Fig. 20 is Fig.18 The display device 700 is shown in a cross-sectional view in which a touch screen 791 is provided.
[0443] First, the following instructions Fig.19 and Fig. 20 Touch screen 791 is shown.
[0444] Fig.19 and Fig. 20 The touch panel 791 shown is a so-called In-Cell type touch panel provided between the substrate 705 and the coloring film 736. The touch panel 791 may be formed on the substrate 705 side before the light shielding film 738 and the coloring film 736 are formed.
[0445] The touch screen 791 includes a light shielding film 738, an insulating film 792, electrodes 793, electrodes 794, insulating films 795, electrodes 796, and insulating films 797. For example, a change in capacitance between the electrodes 793 and 794 caused by an approaching object such as a finger or a stylus pen can be detected.
[0446] In addition, Fig.19 and Fig. 20 The intersection of electrodes 793 and 794 is shown above the transistor 750. Electrode 796 is electrically connected to the two electrodes 793 sandwiching electrode 794 through an opening provided in an insulating film 795. Fig.19 and Fig. 20 7 shows a structure in which the region where the electrode 796 is provided is provided in the pixel portion 702 , but the present invention is not limited to this, and for example, the region where the electrode 796 is provided may also be formed in the source driver circuit portion 704 .
[0447] The electrode 793 and the electrode 794 are provided in the region overlapping with the light shielding film 738. Fig.19 As shown in FIG. 7 , the electrode 793 is preferably arranged so as not to overlap with the light emitting element 775. Fig. 20 As shown, the electrode 793 is preferably arranged in a manner that does not overlap with the liquid crystal element 782. In other words, the electrode 793 has an opening in the area overlapping with the light-emitting element 782 and the liquid crystal element 775. That is, the electrode 793 has a grid shape. By adopting this structure, the electrode 793 can have a structure that does not block the light emitted by the light-emitting element 782. Alternatively, the electrode 793 can also have a structure that does not block the light passing through the liquid crystal element 775. Therefore, since the brightness decrease caused by the configuration of the touch screen 791 is very small, a display device with high visibility and reduced power consumption can be realized. In addition, the electrode 794 can also have the same structure.
[0448] Electrodes 793 and 794 do not overlap with light emitting element 782, so metal materials with low visible light transmittance can be used for electrodes 793 and 794. Alternatively, electrodes 793 and 794 do not overlap with liquid crystal element 775, so metal materials with low visible light transmittance can be used for electrodes 793 and 794.
[0449] Therefore, compared with an electrode using an oxide material having high visible light transmittance, the resistance of the electrodes 793 and 794 can be reduced, thereby improving the sensor sensitivity of the touch screen.
[0450] For example, the electrodes 793, 794, and 796 may also use conductive nanowires. The average diameter of the nanowires may be greater than 1 nm and less than 100 nm, preferably greater than 5 nm and less than 50 nm, and more preferably greater than 5 nm and less than 25 nm. In addition, metal nanowires such as Ag nanowires, Cu nanowires, and Al nanowires, or carbon nanotubes may be used as the nanowires. For example, when Ag nanowires are used as any one or all of the electrodes 664, 665, and 667, a visible light transmittance of greater than 89% and a sheet resistance of greater than 40 Ω / square and less than 100 Ω / square may be achieved.
[0451] Although in Fig.19 and Fig. 20 , but the structure of the In-Cell touch screen is not limited thereto. For example, a so-called On-Cell touch screen formed on the display device 700 or a so-called Out-Cell touch screen attached to the display device 700 may be used.
[0452] In this way, the display device according to one embodiment of the present invention can be used in combination with touch panels of various embodiments.
[0453] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0454] Implementation 3
[0455] In this embodiment, refer to FIG. 21A to FIG. 21C A display device including a semiconductor device according to one embodiment of the present invention will be described.
[0456] <Circuit Structure of Display Device>
[0457] Fig.21AThe display device shown includes: a region having pixels of display elements (hereinafter referred to as pixel portion 502); a circuit portion arranged outside the pixel portion 502 and having a circuit for driving the pixels (hereinafter referred to as driving circuit portion 504); a circuit having a function of protecting the element (hereinafter referred to as protection circuit 506); and a terminal portion 507. In addition, a structure without providing the protection circuit 506 may be adopted.
[0458] A part or all of the driver circuit portion 504 is preferably formed on the same substrate as the pixel portion 502. Thus, the number of components or the number of terminals can be reduced. When a part or all of the driver circuit portion 504 is not formed on the same substrate as the pixel portion 502, a part or all of the driver circuit portion 504 can be mounted by COG or TAB (Tape Automated Bonding).
[0459] The pixel portion 502 includes a circuit (hereinafter referred to as a pixel circuit 501) for driving a plurality of display elements arranged in X rows (X is a natural number greater than or equal to 2) and Y columns (Y is a natural number greater than or equal to 2), and the driving circuit portion 504 includes a driving circuit such as a circuit for outputting a signal (scanning signal) for selecting a pixel (hereinafter referred to as a gate driver 504a), a circuit for supplying a signal (data signal) for driving the display element of the pixel (hereinafter referred to as a source driver 504b), and the like.
[0460] The gate driver 504a has a shift register, etc. The gate driver 504a is input with a signal for driving the shift register through the terminal portion 507 and outputs the signal. For example, the gate driver 504a is input with a start pulse signal, a clock signal, etc. and outputs a pulse signal. The gate driver 504a has a function of controlling the potential of the wiring (hereinafter referred to as the scanning lines GL_1 to GL_X) to which the scanning signal is supplied. In addition, a plurality of gate drivers 504a may be provided, and the scanning lines GL_1 to GL_X may be controlled respectively by the plurality of gate drivers 504a. Alternatively, the gate driver 504a has a function of being able to supply an initialization signal. However, it is not limited thereto, and the gate driver 504a may supply other signals.
[0461] The source driver 504b has a shift register, etc. In addition to the signal used to drive the shift register, the signal (image signal) as the basis of the data signal is also input to the source driver 504b through the terminal portion 507. The source driver 504b has a function of generating a data signal written to the pixel circuit 501 based on the image signal. In addition, the source driver 504b has a function of controlling the output of the data signal according to the pulse signal obtained by inputting a start pulse signal, a clock signal, etc. In addition, the source driver 504b has a function of controlling the potential of the wiring (hereinafter referred to as data lines DL_1 to DL_Y) supplied with the data signal. Alternatively, the source driver 504b has a function of being able to supply an initialization signal. However, it is not limited to this, and the source driver 504b can also supply other signals.
[0462] The source driver 504b is configured using, for example, a plurality of analog switches, etc. By sequentially turning on the plurality of analog switches, the source driver 504b can output a signal obtained by time-dividing an image signal as a data signal. Alternatively, the source driver 504b can be configured using a shift register, etc.
[0463] Each of the plurality of pixel circuits 501 is input with a pulse signal through one of the plurality of scanning lines GL supplied with a scanning signal, and is input with a data signal through one of the plurality of data lines DL supplied with a data signal. In addition, each of the plurality of pixel circuits 501 controls the writing and holding of data of the data signal through a gate driver 504a. For example, a pulse signal is input from the gate driver 504a to the pixel circuit 501 of the mth row and nth column through the scanning line GL_m (m is a natural number less than X), and a data signal is input from the source driver 504b to the pixel circuit 501 of the mth row and nth column through the data line DL_n (n is a natural number less than Y) according to the potential of the scanning line GL_m.
[0464] Fig.21A The protection circuit 506 shown is connected to, for example, a scanning line GL which is a wiring between the gate driver 504a and the pixel circuit 501. Alternatively, the protection circuit 506 is connected to a data line DL which is a wiring between the source driver 504b and the pixel circuit 501. Alternatively, the protection circuit 506 may be connected to a wiring between the gate driver 504a and the terminal portion 507. Alternatively, the protection circuit 506 may be connected to a wiring between the source driver 504b and the terminal portion 507. In addition, the terminal portion 507 refers to a portion provided with a terminal for inputting power, control signals, and image signals from an external circuit to the display device.
[0465] The protection circuit 506 is a circuit that causes conduction between the wiring connected thereto and other wirings when a potential outside a certain range is supplied to the wiring connected thereto.
[0466] like Fig.21A As shown, by providing a protection circuit 506 for each pixel portion 502 and a driving circuit portion 504, the resistance of the display device to overcurrent caused by ESD (Electro Static Discharge) and the like can be improved. However, the structure of the protection circuit 506 is not limited thereto, and for example, a structure in which the gate driver 504a is connected to the protection circuit 506 or a structure in which the source driver 504b is connected to the protection circuit 506 can also be adopted. Alternatively, a structure in which the terminal portion 507 is connected to the protection circuit 506 can also be adopted.
[0467] In addition, although Fig.21A , the example of forming the driver circuit portion 504 by the gate driver 504a and the source driver 504b is shown, but the present invention is not limited to this structure. For example, a structure in which only the gate driver 504a is formed and a separately prepared substrate (for example, a driver circuit substrate formed using a single crystal semiconductor film or a polycrystalline semiconductor film) having a source driver circuit is mounted may be adopted.
[0468] here, Fig. 22 Shown with Fig.21A Different structures. Fig. 22 In the embodiment, a pair of source lines (eg, source line DLa1 and source line DLb1) are arranged to surround a plurality of pixels arranged in the source line direction. In addition, two adjacent gate lines (eg, gate line GL_1 and gate line GL_2) are electrically connected to each other.
[0469] Furthermore, pixels connected to the gate line GL_1 are connected to one source line (source line DLa1, source line DLa2, etc.), and pixels connected to the gate line GL_2 are connected to another source line (source line DLb1, source line DLb2, etc.).
[0470] By adopting the above structure, two gate lines can be selected at the same time. Thus, the length of a horizontal period can be made Fig.21A This makes it easy to realize a high-definition and large-screen display device.
[0471] also, Fig.21A The plurality of pixel circuits 501 shown may be, for example, Fig.21B The structure shown.
[0472] Fig.21B The pixel circuit 501 shown includes a liquid crystal element 570, a transistor 550, and a capacitor 560. As the transistor 550, the transistor described in the above embodiment mode can be applied.
[0473] The potential of one of the pair of electrodes of the liquid crystal element 570 is appropriately set according to the specification of the pixel circuit 501. The orientation state of the liquid crystal element 570 is set according to the written data. In addition, a common potential may be supplied to one of the pair of electrodes of the liquid crystal element 570 included in each of the plurality of pixel circuits 501. In addition, different potentials may be supplied to one of the pair of electrodes of the liquid crystal element 570 included in each of the pixel circuits 501 of each row.
[0474] For example, the following modes may be used as a driving method for a display device having a liquid crystal element 570: TN mode; STN mode; VA mode; ASM (Axially Symmetric Aligned Micro-cell) mode; OCB (Optically Compensated Birefringence) mode; FLC (Ferroelectric Liquid Crystal) mode; AFLC (AntiFerroelectric Liquid Crystal) mode; MVA mode; PVA (Patterned Vertical Alignment) mode; IPS mode; FFS mode; or TBA (Transverse Bend Alignment) mode, etc. In addition to the above-mentioned driving methods, the display device may be driven by an ECB (Electrically Controlled Birefringence) mode, a PDLC (Polymer Dispersed Liquid Crystal) mode, a PNLC (Polymer Network Liquid Crystal) mode, a guest-host mode, etc. However, the present invention is not limited to this, and various liquid crystal elements and driving methods can be used as the liquid crystal element and the driving method thereof.
[0475] In the pixel circuit 501 at the mth row and the nth column, one of the source electrode and the drain electrode of the transistor 550 is electrically connected to the data line DL_n, and the other of the source electrode and the drain electrode is electrically connected to the other of the pair of electrodes of the liquid crystal element 570. In addition, the gate electrode of the transistor 550 is electrically connected to the scanning line GL_m. The transistor 550 has a function of controlling the writing of data of the data signal by turning on or off.
[0476] One of a pair of electrodes of the capacitor 560 is electrically connected to a wiring to which a potential is supplied (hereinafter referred to as a potential supply line VL), and the other is electrically connected to the other of a pair of electrodes of the liquid crystal element 570. In addition, the value of the potential of the potential supply line VL is appropriately set according to the specifications of the pixel circuit 501. The capacitor 560 is used as a storage capacitor for storing written data.
[0477] For example, in a Fig.21B In a display device of the pixel circuit 501, for example, by Fig.21A The gate driver 504 a shown in the figure sequentially selects the pixel circuits 501 of each row, and turns on the transistors 550 to write the data of the data signal.
[0478] When the transistor 550 is turned off, the pixel circuit 501 to which the data has been written is held. An image can be displayed by sequentially performing the above steps row by row.
[0479] Fig.21A The plurality of pixel circuits 501 shown may be, for example, Fig. 21C The structure shown.
[0480] in addition, Fig. 21C The pixel circuit 501 shown includes transistors 552 and 554, a capacitor 562, and a light-emitting element 572. The transistor described in the above embodiment can be applied to one or both of the transistor 552 and the transistor 554.
[0481] One of a source electrode and a drain electrode of the transistor 552 is electrically connected to a wiring (hereinafter referred to as a signal line DL_n) to which a data signal is supplied, and a gate electrode of the transistor 552 is electrically connected to a wiring (hereinafter referred to as a scanning line GL_m) to which a gate signal is supplied.
[0482] The transistor 552 has a function of controlling writing of a data signal by being turned on or off.
[0483] One of a pair of electrodes of the capacitor 562 is electrically connected to a wiring to which a potential is supplied (hereinafter referred to as a potential supply line VL_a), and the other is electrically connected to the other of a source electrode and a drain electrode of the transistor 552 .
[0484] The capacitor 562 is used as a storage capacitor for storing written data.
[0485] One of a source electrode and a drain electrode of the transistor 554 is electrically connected to the potential supply line VL_a, and a gate electrode of the transistor 554 is electrically connected to the other of a source electrode and a drain electrode of the transistor 552 .
[0486] One of the anode and the cathode of the light-emitting element 572 is electrically connected to the potential supply line VL_b, and the other is electrically connected to the other of the source electrode and the drain electrode of the transistor 554 .
[0487] As the light-emitting element 572, for example, an organic electroluminescent element (also referred to as an organic EL element) can be used. Note that the light-emitting element 572 is not limited to an organic EL element, and an inorganic EL element formed of an inorganic material may be used.
[0488] Furthermore, the high power supply potential VDD is applied to one of the potential supply line VL_a and the potential supply line VL_b, and the low power supply potential VSS is applied to the other.
[0489] For example, in a Fig. 21C In a display device of the pixel circuit 501, for example, by Fig.21A The gate driver 504a shown sequentially selects the pixel circuits 501 of each row, and turns on the transistors 552 to write the data of the data signal.
[0490] When the transistor 552 is turned off, the pixel circuit 501 in which the data is written is kept. Furthermore, the amount of current flowing between the source electrode and the drain electrode of the transistor 554 is controlled according to the potential of the written data signal, and the light-emitting element 572 emits light at a brightness corresponding to the amount of current flowing. By sequentially performing the above steps row by row, an image can be displayed.
[0491] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0492] Implementation 4
[0493] In this embodiment, an electronic device which is one embodiment of the present invention is described with reference to the drawings.
[0494] The electronic devices exemplified below are electronic devices that include a display device according to one embodiment of the present invention in a display portion, and thus can achieve high definition. In addition, they can achieve both high definition and a large screen.
[0495] The display unit of the electronic device of one embodiment of the present invention can display images with full HD, 4K2K, 8K4K, 16K8K or higher resolution. In addition, the screen size of the display unit can be greater than 20 inches diagonally, greater than 30 inches diagonally, greater than 50 inches diagonally, greater than 60 inches diagonally, or greater than 70 inches diagonally.
[0496] Electronic devices include, for example, television sets, desktop or notebook personal computers, displays for computers, etc., digital signage, large-scale game machines such as pinball machines, and other electronic devices with larger screens, as well as digital cameras, digital video cameras, digital photo frames, mobile phones, portable game consoles, portable information terminals, sound reproduction devices, etc.
[0497] The electronic device or lighting device of one embodiment of the present invention can be assembled along the curved surface of the inner wall or outer wall of a house or a building, or the interior or exterior of a car.
[0498] The electronic device of one embodiment of the present invention may also include an antenna. By receiving a signal through the antenna, an image or data can be displayed on the display unit. In addition, when the electronic device includes an antenna and a secondary battery, the antenna can be used for contactless power transmission.
[0499] An electronic device of one embodiment of the present invention may also include a sensor (the sensor has the function of measuring the following factors: force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substance, sound, time, hardness, electric field, current, voltage, electricity, radiation, flow, humidity, inclination, vibration, odor or infrared).
[0500] An electronic device of one embodiment of the present invention may have various functions. For example, it may have the following functions: a function of displaying various information (static images, dynamic images, text images, etc.) on a display unit; a function of a touch panel; a function of displaying a calendar, date, or time, etc.; a function of executing various software (programs); a function of wireless communication; a function of reading programs or data stored in a storage medium; etc.
[0501] Fig.23A 100 shows an example of a television set. In a television set 7100, a display portion 7000 is incorporated in a housing 7101. Here, a structure in which the housing 7101 is supported by a stand 7103 is shown.
[0502] The display device of one embodiment of the present invention can be applied to the display portion 7000 .
[0503] The operation switch provided in the housing 7101 and the remote control unit 7111 provided separately can be used to control Fig.23AThe television device 7100 shown in FIG. 7 is operated. In addition, the display portion 7000 may be provided with a touch sensor, and the display portion 7000 may be operated by touching the display portion 7000 with a finger or the like. In addition, the remote control unit 7111 may be provided with a display unit for displaying data output from the remote control unit 7111. By using the operation keys or the touch screen provided in the remote control unit 7111, the channel and volume can be operated, and the image displayed on the display portion 7000 can be operated.
[0504] In addition, the television device 7100 is provided with a receiver and a modem. General television broadcasts can be received by using the receiver. Furthermore, the television device is connected to a wired or wireless communication network via a modem to perform one-way (from a sender to a receiver) or two-way (between a sender and a receiver or between receivers, etc.) information communication.
[0505] Fig. 23B The notebook personal computer 7200 is shown. The notebook personal computer 7200 includes a housing 7211 , a keyboard 7212 , a pointing device 7213 , an external connection port 7214 , and the like. A display portion 7000 is incorporated in the housing 7211 .
[0506] The display device of one embodiment of the present invention can be applied to the display portion 7000 .
[0507] Fig.23C , Fig.23D An example of digital signage is shown.
[0508] Fig.23C The digital signage 7300 shown includes a housing 7301, a display unit 7000, a speaker 7303, etc. In addition, an LED lamp, operation keys (including a power switch or an operation switch), a connection terminal, various sensors, a microphone, etc. may be included.
[0509] Fig.23D The digital signage 7400 is shown to be disposed on a cylindrical pillar 7401. The digital signage 7400 includes a display unit 7000 disposed along a curved surface of the pillar 7401.
[0510] exist Fig.23C , Fig.23D In the embodiment of the present invention, a display device according to one embodiment of the present invention can be applied to the display portion 7000 .
[0511] The larger the display unit 7000 is, the more information the display device can provide at one time. The larger the display unit 7000 is, the easier it is to attract people's attention, for example, it can improve the advertising effect.
[0512] By using a touch screen for the display unit 7000, not only can a static image or a dynamic image be displayed on the display unit 7000, but the user can also intuitively operate it, which is preferred. In addition, when used for providing information such as route information or traffic information, the ease of use can be improved through intuitive operation.
[0513] like Fig.23C , Fig.23D As shown, the digital signage 7300 or the digital signage 7400 can be linked with the information terminal device 7311 or the information terminal device 7411 such as a smartphone carried by the user preferably through wireless communication. For example, the advertisement information displayed on the display unit 7000 can be displayed on the screen of the information terminal device 7311 or the information terminal device 7411. In addition, by operating the information terminal device 7311 or the information terminal device 7411, the display of the display unit 7000 can be switched.
[0514] Furthermore, the game can be executed on the digital signage 7300 or the digital signage 7400 using the screen of the information terminal device 7311 or the information terminal device 7411 as an operation unit (controller). Thus, an unspecified number of users can participate in the game at the same time and enjoy the game.
[0515] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.
[0516] Implementation method 5
[0517] In this embodiment, an example of a television device to which a display device according to one embodiment of the present invention can be applied will be described with reference to the drawings.
[0518] Fig.24A A block diagram of a television apparatus 600 is shown.
[0519] The block diagrams in this specification show constituent elements classified according to their functions in independent blocks; however, actual constituent elements are difficult to be clearly divided according to their functions, and one constituent element may have a plurality of functions.
[0520] The television device 600 includes a control unit 601 , a storage unit 602 , a communication control unit 603 , an image processing circuit 604 , a decoder circuit 605 , a video signal receiving unit 606 , a timing controller 607 , a source driver 608 , a gate driver 609 , a display panel 620 , and the like.
[0521] The display device shown in the above embodiment can be applied to Fig.24A The display panel 620 in the embodiment of the present invention can be realized. Thus, a large-scale, high-resolution, and highly visible television device 600 can be realized.
[0522] The control unit 601 may be used as a central processing unit (CPU), for example, and has a function of controlling components such as the storage unit 602 , the communication control unit 603 , the image processing circuit 604 , the decoder circuit 605 , and the video signal receiving unit 606 via the system bus 630 .
[0523] Signals are transmitted between the control unit 601 and each component via the system bus 630. In addition, the control unit 601 has a function of processing signals input from each component connected via the system bus 630, a function of generating signals output to each component, and the like, thereby being able to control each component connected to the system bus 630 as a whole.
[0524] The storage unit 602 is used as a register, a cache memory, a main memory, a secondary memory, or the like that can be accessed by the control unit 601 and the image processing circuit 604 .
[0525] As a storage device that can be used as a secondary memory, for example, a storage device using a rewritable nonvolatile storage element can be used. For example, a flash memory, MRAM (Magnetoresistive Random Access Memory), PRAM (Phase change RAM), ReRAM (Resistive RAM), FeRAM (Ferroelectric RAM), etc. can be used.
[0526] As a storage device that can be used as a temporary memory such as a register, a cache memory, or a main memory, a nonvolatile storage element such as a DRAM (Dynamic RAM) or an SRAM (Static Random Access Memory) may be used.
[0527] For example, the RAM provided in the main memory, such as DRAM, is virtually allocated and used as a storage space for the work space of the control unit 601. The operating system, application program, program module, program data, etc. stored in the storage unit 602 are loaded into the RAM when executed. These data, programs, or program modules loaded into the RAM are directly accessed and operated by the control unit 601.
[0528] On the other hand, BIOS (Basic Input / Output System) or firmware that does not need to be rewritten can be stored in the ROM. As ROM, mask ROM, OTPROM (One Time Programmable Read Only Memory), EPROM (Erasable Programmable Read Only Memory), etc. can be used. As EPROM, UV-EPROM (Ultra-Violet Erasable Programmable Read Only Memory) that can erase stored data by ultraviolet irradiation, EEPROM (Electrically Erasable Programmable Read Only Memory), and flash memory can be cited.
[0529] In addition, a structure that can connect a removable storage device in addition to the storage unit 602 can be adopted. For example, it is preferable to include a terminal for connecting to a recording medium drive such as a hard disk drive (HDD) or a solid state drive (SSD) used as a storage device, a flash memory, a Blu-ray disc, a DVD, etc. Thus, images can be recorded.
[0530] The communication control unit 603 has a function of controlling communication through a computer network. For example, the control unit 601 controls a control signal for connecting to a computer network according to an instruction from the control unit 601, and sends the signal to the computer network. Thus, it is possible to connect to a computer network such as the Internet, an intranet, an extranet, a PAN (Personal Area Network), a LAN (Local Area Network), a CAN (Campus Area Network), a MAN (Metropolitan Area Network), a WAN (Wide Area Network), and a GAN (Global Area Network) based on the World Wide Web (WWW) to communicate.
[0531] The communication control unit 603 has a function of communicating with a computer network or other electronic devices using a communication standard such as Wi-Fi (registered trademark), Bluetooth (registered trademark), or ZigBee (registered trademark).
[0532] The communication control unit 603 may also have a function of communicating wirelessly. For example, an antenna and a high-frequency circuit (RF circuit) may be provided to transmit and receive RF signals. A high-frequency circuit is a circuit used to convert electromagnetic signals and electrical signals in the frequency bands specified by the laws of various countries and to communicate with other communication devices wirelessly using the electromagnetic signals. As a practical frequency band, a frequency band of tens of kHz to tens of GHz is generally used. The high-frequency circuit connected to the antenna has a high-frequency circuit unit corresponding to multiple frequency bands, and the high-frequency circuit unit may have an amplifier, a mixer, a filter, a DSP, an RF transceiver, etc.
[0533] The image signal receiving unit 606 includes, for example, an antenna, a demodulation circuit, and an AD conversion circuit (analog-digital conversion circuit). The demodulation circuit has a function of demodulating a signal input from the antenna. In addition, the AD conversion circuit has a function of converting the demodulated analog signal into a digital signal. The signal processed by the image signal receiving unit 606 is sent to the decoder circuit 605.
[0534] The decoder circuit 605 has the following functions: decode the image data included in the digital signal input from the image signal receiving unit 606 according to the transmitted broadcast standard, and generate a signal to be sent to the image processing circuit. For example, as a broadcast standard for 8K broadcasting, there is H.265|MPEG-H High Efficiency Video Coding (abbreviated as: HEVC) and the like.
[0535] As broadcast waves that the antenna included in the image signal receiving unit 606 can receive, there can be terrestrial broadcasts or waves sent from satellites, etc. In addition, as broadcast waves that the antenna can receive, there are analog broadcasts, digital broadcasts, etc., as well as broadcasts of images and sounds or broadcasts of sound only, etc. For example, broadcast waves transmitted in a specified frequency band in the UHF band (approximately 300MHz to 3GHz) or the VHF band (30MHz to 300MHz) can be received. For example, by using multiple data received in multiple frequency bands, the transmission rate can be increased, so that more information can be obtained. Thus, an image with a resolution exceeding full HD can be displayed on the display panel 620. For example, an image with a resolution of 4K2K, 8K4K, 16K8K or higher can be displayed.
[0536] In addition, the image signal receiving unit 606 and the decoder circuit 605 may also have a structure in which broadcast data transmitted through a computer network data transmission technology is used to generate a signal to be transmitted to the image processing circuit 604. In this case, when the received signal is a digital signal, the image signal receiving unit 606 may not include a demodulation circuit and an AD conversion circuit.
[0537] The image processing circuit 604 has a function of generating an image signal to be input to the timing controller 607 based on the image signal input from the decoder circuit 605 .
[0538] The timing controller 607 has the function of generating and outputting signals (clock signals, start pulse signals, etc.) to the gate driver 609 and the source driver 608 based on the synchronization signals in the image signal etc. processed by the image processing circuit 604. In addition, the timing controller 607 has the function of generating video signals to be output to the source driver 608 in addition to the above-mentioned signals.
[0539] The display panel 620 includes a plurality of pixels 621. Each pixel 621 is driven by a signal supplied from a gate driver 609 and a source driver 608. Here, an example of a display panel having a resolution corresponding to 8K4K specifications and having a pixel count of 7680×4320 is shown. In addition, the resolution of the display panel 620 is not limited thereto, and may also be a resolution corresponding to specifications such as full HD (pixel count of 1920×1080) or 4K2K (pixel count of 3840×2160).
[0540] As Fig.24A The structure of the control unit 601 or the image processing circuit 604 shown in the figure may, for example, be a structure including a processor. For example, the control unit 601 may use a processor used as a central processing unit (CPU). In addition, as the image processing circuit 604, for example, other processors such as a DSP (Digital Signal Processor) and a GPU (Graphics Processing Unit) may be used. In addition, the control unit 601 or the image processing circuit 604 may also have a structure in which such a processor is implemented by a PLD (Programmable Logic Device) such as an FPGA (Field Programmable Gate Array) or an FPAA (Field Programmable Analog Array).
[0541] The processor performs various data processing or program control by interpreting and executing instructions from various programs. The program that may be executed by the processor may be stored in a memory area in the processor or in a separately provided storage device.
[0542] It is also possible to integrate two or more functions of the control unit 601, the storage unit 602, the communication control unit 603, the image processing circuit 604, the decoder circuit 605, the image signal receiving unit 606, and the timing controller 607 on one IC chip to form a system LSI. For example, a system LSI including a processor, a decoder circuit, a tuner circuit, an AD conversion circuit, a DRAM, an SRAM, etc. may be used.
[0543] In addition, a transistor that uses an oxide semiconductor in the channel formation region to achieve an extremely small off-state current can also be used for the control unit 601 or an IC included in other components. Since the off-state current of the transistor is extremely small, a longer data retention period can be ensured by using the transistor as a switch to maintain the charge (data) flowing into the capacitor used as a storage element. By using this characteristic for a register or cache memory such as the control unit 601, the control unit 601 can be operated only when necessary, and the previous processing information can be stored in the storage element in other cases, thereby achieving normally off computing. Thus, low power consumption of the television device 600 can be achieved.
[0544] Notice, Fig.24A The structure of the television device 600 shown is an example, and does not necessarily include all the components. Fig.24A The television device 600 may include the required components among the components shown. Fig.24A Constituent elements other than those shown in the figure.
[0545] For example, the television device 600 may also have Fig.24A The structure shown in the figure adds the structure of external interface, sound output part, touch screen unit, sensor unit, camera unit, etc. For example, as the external interface, there are external connection terminals such as USB (Universal Serial Bus) terminal, LAN (Local Area Network) connection terminal, power receiving terminal, sound output terminal, sound input terminal, video output terminal, video input terminal, etc., optical communication transceiver using infrared, visible light, ultraviolet light, etc., physical button provided in the housing, etc. In addition, as the sound input and output part, there are sound controller, microphone, speaker, etc.
[0546] Next, the image processing circuit 604 will be described in more detail.
[0547] The image processing circuit 604 preferably has a function of executing image processing based on the video signal input from the decoder circuit 605 .
[0548] As the image processing, for example, there can be mentioned noise removal processing, grayscale conversion processing, tone correction processing, brightness correction processing, etc. As the tone correction processing or brightness correction processing, there is gamma correction, etc., for example.
[0549] In addition, the image processing circuit 604 preferably has a function of executing inter-pixel complementation processing accompanying up-conversion of resolution and inter-frame complementation processing accompanying up-conversion of frame frequency.
[0550] For example, in the noise removal process, various noises are removed, such as mosquito noise generated near the outline of text, block noise generated in high-speed dynamic images, random noise that generates flicker, and point noise caused by up-conversion of resolution.
[0551] Grayscale conversion processing refers to processing for converting the grayscale of an image into a grayscale corresponding to the output characteristics of the display panel 620. For example, when increasing the grayscale number, by supplementing an image input with a smaller grayscale number and assigning grayscale values corresponding to each pixel, a histogram smoothing process can be performed. In addition, high dynamic range (HDR) processing for expanding the dynamic range is also included in grayscale change processing.
[0552] The inter-pixel complementation process complements data that does not exist when up-converting the resolution. For example, the pixel near the target pixel is referenced and the data is complemented to display the intermediate color of the pixel.
[0553] The color tone correction process refers to the process of correcting the color tone of the image. In addition, the brightness correction process refers to the process of correcting the brightness (brightness contrast) of the image. For example, the type, brightness or color purity of the lighting in the space where the television device 600 is installed is detected, and the brightness or color tone of the image displayed on the display panel 620 is corrected to the most suitable brightness or color tone based on this information. Alternatively, it is also possible to have a function of comparing the displayed image with the images of various scenes in the pre-stored image list, and correcting the displayed image to the brightness or color tone of the image suitable for the closest scene.
[0554] In inter-frame supplementation, when the frame frequency of the displayed image is increased, an image of a frame (supplementary frame) that does not originally exist is generated. For example, the difference between two images is used to generate an image of a supplementary frame inserted between the two images. Alternatively, multiple supplementary frame images can be generated between the two images. For example, when the frame frequency of the image signal input from the decoder circuit 605 is 60 Hz, by generating multiple supplementary frames, the frame frequency of the image signal input to the timing controller 607 can be increased to twice 120 Hz, four times 240 Hz, or eight times 480 Hz, etc.
[0555] The image processing circuit 604 preferably has a function of performing image processing using a neural network. Fig.24A An example in which the image processing circuit 604 includes a neural network 610 is shown.
[0556] For example, features may be extracted from image data included in an image by using the neural network 610. In addition, the image processing circuit 604 may select the most suitable correction method or select parameters for correction based on the extracted features.
[0557] Alternatively, the neural network 610 itself may have a function of performing image processing. In other words, a structure may be adopted in which image data before image processing is input to the neural network 610, and image data after image processing is output.
[0558] In addition, the data of the weight coefficients used for the neural network 610 is stored as a data table in the storage unit 602. The data table including the weight coefficients is updated to the latest data table via the computer network by using the communication control unit 603, for example. Alternatively, the image processing circuit 604 has a learning function and can update the data table including the weight coefficients.
[0559] Fig. 24B A schematic diagram showing a neural network 610 included in the image processing circuit 604 is shown.
[0560] In this specification, etc., a neural network refers to a neural circuit network that simulates a living being, and all models that have problem-solving capabilities by learning to determine the strength of the connection between neurons. A neural network includes an input layer, an intermediate layer (also called a hidden layer), and an output layer. A neural network that includes more than two intermediate layers in a neural network is called deep learning (or deep neural network (DNN)).
[0561] In addition, in this specification, when describing a neural network, sometimes determining the strength of connection between neurons (also called weight coefficient) based on existing information is called "learning". In addition, in this specification, sometimes constructing a neural network using the connection strength obtained through learning and deriving a new conclusion from the structure is called "inference".
[0562] The neural network 610 includes an input layer 611, one or more intermediate layers 612, and an output layer 613. Input data is input to the input layer 611, and output data is output from the output layer 613.
[0563] The input layer 611, the intermediate layer 612, and the output layer 613 each include a neuron 615. Here, the neuron 615 refers to a circuit element (a product-sum operation element) that can perform a product-sum operation. Fig. 24B The arrows in FIG. 1 show the data input and output directions between two neurons 615 included in the two layers.
[0564] The operation processing of each layer is performed by the product-sum operation of the output of the neuron 615 included in the previous layer and the weight coefficient. For example, the output of the i-th neuron in the input layer 611 is x i , and output x i The strength of the connection (weight coefficient) with the jth neuron in the next intermediate layer 612 is w ji When the output of the jth neuron in the middle layer is y j =f(Σw ji ·x i ). Note that i and j are integers greater than 1. Here, f(x) is an activation function, and a sigmoid function, a threshold function, etc. can be used as the activation function. In the following, similarly, the output of the neuron 615 of each layer is the value obtained by calculating the product and calculation result of the output of the neuron 615 of the previous layer and the weight coefficient using the activation function. In addition, the connection between layers can be a full connection in which all neurons are connected to each other, or a partial connection in which some neurons are connected to each other.
[0565] Fig. 24B An example including three intermediate layers 612 is shown. In addition, the number of intermediate layers 612 is not limited thereto, and more than one intermediate layer may be included. In addition, the number of neurons included in one intermediate layer 612 may be appropriately changed according to the specification. For example, the number of neurons 615 included in one intermediate layer 612 may be more than the number of neurons 615 included in the input layer 611 or the output layer 613, or may be less than the number of neurons 615 included in the input layer 611 or the output layer 613.
[0566] The weight coefficient of the index of the strength of the connection between neurons 615 is determined by learning. The learning can be performed by a processor included in the television device 600, preferably by a computer with high computing processing power such as a dedicated server or cloud. The weight coefficient determined by learning is stored as a table in the above-mentioned storage unit 602, and is read out and used by the image processing circuit 604. In addition, the table can be updated through the computer network as needed.
[0567] The above is the description of the neural network.
[0568] At least a part of this embodiment can be implemented in appropriate combination with other embodiments described in this specification.
[0569] Example 1
[0570] In this example, an insulating layer of one aspect of the present invention is evaluated. In this example, Samples A1, A2, and A3 are manufactured. Samples A1 and A2 are insulating layers of one aspect of the present invention, corresponding to the insulating layer 106 and the region 106a shown in the embodiment. Sample A3 is an insulating layer for comparison.
[0571] <Samples A1, A2, A3>
[0572] First, each sample manufactured in this example will be described.
[0573] For Samples A1, A2, and A3, a silicon nitride film with a thickness of 400 nm is formed on a glass substrate using a PECVD apparatus. The film formation conditions for the silicon nitride film are as follows: the substrate temperature is 350°C; silane gas with a flow rate of 200 sccm, nitrogen gas with a flow rate of 2000 sccm, and ammonia gas with a flow rate of 100 sccm are introduced into the chamber; the pressure is 100 Pa; and 2000 W of RF power is supplied between parallel plate electrodes provided in the PECVD apparatus to form a silicon nitride film with a thickness of 50 nm. Then, the ammonia gas flow rate is changed to 2000 sccm to form a silicon nitride film with a thickness of 300 nm. Then, the ammonia gas flow rate is changed to 100 sccm to form a silicon nitride film with a thickness of 50 nm.
[0574] Next, plasma treatment is performed in an oxygen-containing atmosphere. The conditions for the plasma treatment of Sample A1 are as follows: the temperature is 350°C; the pressure is 40 Pa; the power supply power is 3000 W; the oxygen flow rate is 3000 sccm; the treatment time is 300 seconds. The conditions for the plasma treatment of Sample A2 are as follows: the temperature is 350°C; the pressure is 40 Pa; the power supply power is 3000 W; the nitrous oxide flow rate is 3000 sccm; the treatment time is 300 seconds. Plasma treatment is not performed on Sample A3. In addition, plasma treatment is continuously performed on Samples A1 and A2 in a vacuum after the formation of the silicon nitride film.
[0575] The size of the glass substrate used for each of the above samples is 600 mm × 720 mm.
[0576] <X-ray photoelectron spectroscopy>
[0577] Next, X-ray photoelectron spectroscopy (XPS) was performed on sample A1, sample A2, and sample A3.
[0578] Fig.25 The spectra of Si2p, O1s, and N1s obtained by XPS measurement are shown. In Fig.25 the horizontal axis shows the binding energy [eV], and the vertical axis shows the intensity of photoelectrons (in arbitrary units).
[0579] In the XPS measurement, a Quantera SXM manufactured by ULVAC-PHI was used. Monochromatic Al Kα line (1486.6 eV) was used as the X-ray source. The detection area was 100 μmφ. The extraction angle was 45°. The detection depth was considered to be approximately 4 nm to 5 nm.
[0580] As Fig.25 shown, it can be seen that compared with sample A3, the peaks derived from Si-N bonding in sample A1 and sample A2 are small, and the peaks derived from Si-O bonding are large. Therefore, it was confirmed that the surfaces of sample A1 and sample A2 near the silicon nitride film were oxidized by the above plasma treatment, forming regions with a higher oxygen content than silicon nitride.
[0581] <TEM Observation>
[0582] Next, samples A1 to A3 were thinned using a focused ion beam (FIB), and the cross-sections of the samples were observed by TEM. The TEM observation was performed using a transmission electron microscope H-9500 manufactured by Hitachi High-Technologies Corporation, and the acceleration voltage was 300 kV.
[0583] Fig.26A The cross-sectional TEM image of sample A1 is shown, Fig.26B The cross-sectional TEM image of sample A2 is shown, Fig.26C The cross-sectional TEM image of sample A3 is shown. FIG. 26A to FIG. 26C It is a transmission electron image (TE image: Transmission Electron Image) at a magnification of 2 million times.
[0584] As Fig.26A and Fig.26B shown, regions with different concentrations (brightness) of the TEM image were confirmed near the surfaces of sample A1 and sample A2. Considering the above XPS measurement results, it is considered that the surfaces of silicon nitride in sample A1 and sample A2 were oxidized, forming regions with a higher oxygen content than silicon nitride (hereinafter referred to as oxidation regions). In addition, no layer with different concentrations (brightness) of the TEM image was confirmed near the surface of sample A3.
[0585] The thickness of the oxidized regions of Sample A1 and Sample A2 were measured. Fig.27A The length measurement portion of sample A1 is shown. Fig.27B The length measurement section of sample A2 is shown. Fig.27A and Fig.27B In the figure, the measured length is indicated by an arrow. The three regions of sample A1 and sample A2 were measured. Table 1 shows the measurement results. In Table 1, the column recorded as "oxidized region" shows the value of each measured length. The column recorded as "average" shows the average value of each sample. In addition, it can be seen that the thickness of the oxidized region of sample A1 and sample A2 is about 6nm.
[0586] [Table 1]
[0587]
[0588]
[0589] The structure described in this embodiment can be implemented in combination with the structures described in other embodiment modes or other embodiments as appropriate.
[0590] Example 2
[0591] In this example, the crystallinity of a metal oxide film of one embodiment of the present invention was evaluated. In addition, in this example, samples B1 to B29 and samples C1 to C25 were manufactured. In addition, samples B1 to B29 and samples C1 to C25 are metal oxide films of one embodiment of the present invention.
[0592] <Samples B1 to B29, Samples C1 to C25>
[0593] First, each sample produced in this example will be described.
[0594] Samples B1 to B29 have a structure in which a metal oxide film with a thickness of 100 nm is formed on a glass substrate. The metal oxide film is formed using a sputtering device, and In-Ga-Zn oxide (In:Ga:Zn=4:2:3 [atomic number ratio]) is used as a sputtering target. During the sputtering process, the pressure is controlled to 0.6 Pa, and an AC power of 2500 W is applied. The substrate temperature (Tsub.), Ar flow rate, and O2 flow rate during film formation are different for samples B1 to B29. Table 2 shows the main contents of the film formation conditions.
[0595] Samples C1 to C25 have a structure in which a metal oxide film with a thickness of 100 nm is formed on a glass substrate. The metal oxide film is formed using a sputtering device, and In-Ga-Zn oxide (In:Ga:Zn=1:1:1.2 [atomic number ratio]) is used as a sputtering target. During the sputtering process, the pressure is controlled to 0.6 Pa, and an AC power of 2500 W is applied. The substrate temperature (Tsub.), Ar flow rate, and O2 flow rate during film formation are different for samples C1 to C25. Table 3 shows the main contents of the film formation conditions.
[0596] In Tables 2 and 3, the description of room temperature (RT) in the item of substrate temperature (Tsub.) means that the substrate is not heated during film formation. In addition, the column describing the oxygen flow rate ratio shows the ratio of the O2 flow rate to the total gas flow rate (the sum of the Ar flow rate and the O2 flow rate).
[0597] Samples B1 to B29 and samples C1 to C25 were all formed using a parallel plate sputtering device. AC power was used as a power source applied to the target during film formation of each of the above samples. In addition, the size of the glass substrate used for each of the above samples was 600 mm×720 mm.
[0598] [Table 2]
[0599]
[0600]
[0601] [Table 3]
[0602]
[0603] <Crystallinity Evaluation by XRD Measurement>
[0604] Next, X-ray analysis (XRD) was performed on samples B1 to B29 and samples C1 to C25. Fig.28 The coordinates of the glass substrate on which XRD was performed are shown. Fig.28 The coordinates of the portion where XRD was performed in a glass substrate of 600 mm x 720 mm size are shown. Fig.28 In FIG. 1 , B, E, and H indicated by white circles show coordinates for performing XRD analysis.
[0605] Fig.29 The XRD spectra of samples B1 to B17 are shown. Fig.30 Samples B18 to B29 are shown. Fig.31 The XRD spectra of samples C1 to C15 are shown. Fig.32 XRD spectra of samples C16 to C25 are shown.
[0606] Figure 29 to Figure 32 The spectrum obtained by the θ-2θ scanning method, which is a type of out-of-plane method, is shown, with the horizontal axis showing the diffraction intensity 2θ [deg.] and the vertical axis showing the diffraction X-ray intensity (arbitrary unit). The θ-2θ scanning method is a method in which the X-ray diffraction intensity is measured while changing the incident angle of the X-ray and making the angle of the detector set opposite to the X-ray source the same as the incident angle. The θ-2θ scanning method is sometimes called the powder method.
[0607] In the XRD measurement, an X-ray diffractometer D8 ADVANCE manufactured by Bruker AXS was used. As the X-ray source, CuKα line with a wavelength of 0.15418 nm was used, the scanning range was 2θ=15 degrees to 50 degrees, the step width was 0.01 degrees, and the scanning speed was 6.0 degrees / minute.
[0608] like Fig.29 and Fig.30 As shown, a peak near 2θ=31° indicating CAAC-OS was confirmed in samples B2 to B29. This shows that samples B2 to B29 have good crystallinity. No clear peak near 2θ=31° was confirmed in sample B1. This shows that the crystallinity of sample B1 is lower than that of samples B2 to B29.
[0609] like Fig.29 and Fig.30 As shown, the higher the substrate temperature or oxygen gas flow rate during film formation, the greater the peak intensity near 2θ=31°. In addition, no peak near 2θ=36°, which is believed to be derived from the spinel phase, was confirmed in samples B1 to B29.
[0610] like Fig.31 and Fig.32 As shown, a peak near 2θ=31° indicating CAAC-OS was confirmed in samples C3 to C5, samples C7 to C10, and samples C12 to C25. It can be seen that samples C3 to C5, samples C7 to C10, and samples C12 to C25 have good crystallinity. In addition, a tiny peak near 2θ=31° indicating CAAC-OS was confirmed in samples C2 and C11. It can be seen that samples C2 and C11 also have crystallinity. No clear peak near 2θ=31° was confirmed in samples C1 and C6. It can be seen that the crystallinity of samples C1 and C6 is lower than that of samples C2 to C5 and samples C7 to C25.
[0611] like Fig.31 and Fig.32As shown, the higher the substrate temperature or oxygen gas flow rate ratio during film formation, the greater the peak intensity near 2θ = 31°. In addition, a peak near 2θ = 36°, which can be considered to be derived from the spinel phase, was confirmed in samples C3 to C5, samples C8 to C10, samples C12 to C15, samples C17 to C20, and samples C22 to C25.
[0612] The structure described in this embodiment can be implemented in combination with the structures described in other embodiment modes or other embodiments as appropriate.
[0613] Example 3
[0614] In this embodiment, a transistor is manufactured and the electrical characteristics of the transistor are evaluated. In this embodiment, samples D1 to D4 shown below are manufactured and evaluated. The structure of the metal oxide layer 108 of samples D1 to D4 is different. In addition, in samples D1 to D4, the channel width W of the transistor is 50 μm, and the channel length L is 2 μm and 3 μm. In samples D1 to D4, 10 transistors are formed as transistors for each channel length L.
[0615] <Method for producing sample D1>
[0616] First, the conductive layer 104 is formed on the substrate 102. A glass substrate is used as the substrate 102. Furthermore, a tungsten film with a thickness of 100 nm is formed using a sputtering device, and the film is processed to form the conductive layer 104.
[0617] Next, an insulating layer 106 is formed on the substrate 102 and the conductive layer 104. As the insulating layer 106, a 400 nm thick silicon nitride film and a 5 nm thick silicon oxynitride film on the silicon nitride are formed using a PECVD apparatus.
[0618] The film forming conditions of the insulating layer 106 are as follows: the substrate temperature is 350° C.; silane gas with a flow rate of 200 sccm, nitrogen gas with a flow rate of 2000 sccm, and ammonia gas with a flow rate of 100 sccm are introduced into the chamber; the pressure is 100 Pa; and 2000 W of RF power is supplied between the parallel plate electrodes set in the PECVD device to form a silicon nitride film with a thickness of 50 nm, then the ammonia gas flow rate is changed to 2000 sccm to form a silicon nitride film with a thickness of 300 nm, and then the ammonia gas flow rate is changed to 100 sccm to form a silicon nitride film with a thickness of 50 nm. After the silicon nitride film is formed, a silicon oxynitride film is continuously formed in the chamber of the PECVD device. The film formation conditions of the silicon oxynitride film are as follows: the substrate temperature is 350°C; silane gas with a flow rate of 20 sccm and nitrous oxide gas with a flow rate of 3000 sccm are introduced into the chamber; the pressure is 40 Pa; and 500 W of RF power is supplied to the parallel plate electrodes arranged in the PECVD device.
[0619] Next, a metal oxide layer 108 is formed on the insulating layer 106. In addition, the metal oxide layer 108 of the sample D1 has a stacked structure of a first metal oxide layer IGZOa1 and a second metal oxide layer IGZOb1 on the first metal oxide layer IGZOa1. The first metal oxide layer IGZOa1 and the second metal oxide layer IGZOb1 are continuously formed in a vacuum using a sputtering device. The stacked metal oxide layers are processed to obtain the metal oxide layer 108.
[0620] As IGZOa1, an In-Ga-Zn oxide film with a thickness of 20 nm was formed. In addition, the film formation conditions of IGZOa1 were as follows: the substrate temperature was room temperature; an argon gas with a flow rate of 180 sccm and an oxygen gas with a flow rate of 20 sccm (oxygen flow rate ratio of 10%) were introduced into the chamber; the pressure was 0.6 Pa; and an AC power of 2500 W was applied to the polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0621] As IGZOb1, an IGZO film with a thickness of 30 nm was formed. In addition, the film forming conditions of IGZOb1 were as follows: the substrate temperature was room temperature; an argon gas with a flow rate of 100 sccm and an oxygen gas with a flow rate of 100 sccm (oxygen flow ratio of 50%) were introduced into the chamber; the pressure was 0.6 Pa; and an AC power of 2500 W was applied to the polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0622] Next, heat treatment was performed at 350° C. for one hour in a nitrogen atmosphere, and then heat treatment was performed at 350° C. for one hour in a mixed gas atmosphere of nitrogen and oxygen.
[0623] Next, a conductive film is formed on the insulating layer 106 and the metal oxide layer 108, and the conductive film is processed to form the conductive layer 112a and the conductive layer 112b. Here, as the conductive film, a first titanium film with a thickness of 30 nm and a copper film with a thickness of 200 nm are sequentially formed using a sputtering device. Next, the copper film is etched by photolithography, and then a second titanium film with a thickness of 100 nm is formed using a sputtering device. Next, the first titanium film and the second titanium film are etched by photolithography, thereby forming the conductive layer 112a and the conductive layer 112b.
[0624] Next, the exposed surface (back channel side) of the metal oxide layer 108 was washed with phosphoric acid. In the phosphoric acid washing, an aqueous solution of phosphoric acid having a concentration of 85 weight % was diluted to 1 / 100, and the treatment was performed at room temperature for 15 seconds.
[0625] Next, a first plasma treatment is performed in an atmosphere containing an oxygen gas. A PECVD device is used in the first plasma treatment. The conditions of the first plasma treatment are as follows: a temperature of 350°C; a pressure of 40 Pa; a power supply of 3000 W; an oxygen flow rate of 3000 sccm (oxygen flow rate ratio of 100%); and a treatment time of 300 seconds.
[0626] Next, the insulating layer 114 is formed over the insulating layer 106, the metal oxide layer 108, the conductive layer 112a, and the conductive layer 112b. As the insulating layer 114, a silicon oxynitride film is formed to a thickness of 50 nm using a PECVD apparatus.
[0627] The film formation conditions of the insulating layer 114 are as follows: the substrate temperature is 350°C; silane gas with a flow rate of 100 sccm and nitrous oxide gas with a flow rate of 2500 sccm are introduced into the chamber; the pressure is 400 Pa; and 500 W of RF power is supplied between the parallel plate electrodes arranged in the PECVD device.
[0628] After forming the insulating layer 114, a second plasma treatment is continuously performed in the chamber of the PECVD device. The conditions of the second plasma treatment are as follows: temperature of 350° C., pressure of 40 Pa, power of 3000 W, oxygen flow rate of 3000 sccm (oxygen flow rate ratio of 100%), and treatment time of 600 seconds.
[0629] Next, a third plasma treatment is performed in an atmosphere containing an oxygen gas. A PECVD device is used in the third plasma treatment. The conditions of the third plasma treatment are as follows: a temperature of 220° C.; a pressure of 40 Pa; a power supply of 3000 W; an oxygen flow rate of 3000 sccm (oxygen flow rate ratio of 100%); and a treatment time of 600 seconds.
[0630] Next, the insulating layer 116 is formed on the insulating layer 114. As the insulating layer 116, a silicon nitride film is formed to a thickness of 100 nm using a PECVD apparatus.
[0631] In addition, the film formation conditions of the insulating layer 116 are as follows: the substrate temperature is 350°C; silane gas with a flow rate of 50sccm, nitrogen gas with a flow rate of 5000sccm, and ammonia gas with a flow rate of 100sccm are introduced into the chamber; the pressure is 100Pa; and 1000W of RF power is supplied between the parallel plate electrodes arranged in the PECVD device.
[0632] Then, an acrylic resin film with a thickness of about 1.5 μm is formed on the insulating layer 116, and the film is processed to obtain a planarized film. The acrylic resin film is formed by firing an acrylic photosensitive resin at 250° C. for one hour in a nitrogen atmosphere. Then, a heat treatment is performed at 250° C. for one hour in a nitrogen atmosphere.
[0633] The sample D1 of this example was manufactured through the above-mentioned process.
[0634] <Method for producing sample D2>
[0635] The difference between sample D2 and sample D1 is the film forming conditions of the metal oxide layer 108. The other steps are the same as those of sample D1.
[0636] The metal oxide layer 108 of sample D2 has a stacked structure of a third metal oxide layer IGZOc2, a first metal oxide layer IGZOa2 on the third metal oxide layer IGZOc2, and a second metal oxide layer IGZOb2 on the first metal oxide layer IGZOa2. The third metal oxide layer IGZOc2, the first metal oxide layer IGZOa2, and the second metal oxide layer IGZOb2 are continuously formed in a vacuum using a sputtering device. The stacked metal oxide layers are processed to obtain the metal oxide layer 108.
[0637] As IGZOc2, an IGZO film with a thickness of 5 nm was formed. In addition, the film formation conditions of IGZOc2 were as follows: the substrate temperature was room temperature; an argon gas with a flow rate of 100 sccm and an oxygen gas with a flow rate of 100 sccm (oxygen flow ratio of 50%) were introduced into the chamber; the pressure was 0.6 Pa; and an AC power of 2500 W was applied to a polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0638] As IGZOa2, an In-Ga-Zn oxide film with a thickness of 20 nm was formed. In addition, the film formation conditions of IGZOa2 were as follows: the substrate temperature was room temperature; an argon gas with a flow rate of 180 sccm and an oxygen gas with a flow rate of 20 sccm (oxygen flow ratio of 10%) were introduced into the chamber; the pressure was 0.6 Pa; and an AC power of 2500 W was applied to the polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0639] As IGZOb2, an IGZO film with a thickness of 30 nm was formed. In addition, the film formation conditions of IGZOb2 were as follows: the substrate temperature was room temperature; an argon gas with a flow rate of 100 sccm and an oxygen gas with a flow rate of 100 sccm (oxygen flow ratio of 50%) were introduced into the chamber; the pressure was 0.6 Pa; and an AC power of 2500 W was applied to the polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0640] The sample D2 of this example was manufactured through the above-mentioned process.
[0641] <Method for producing sample D3>
[0642] The difference between the sample D3 and the sample D1 is the film forming conditions of the metal oxide layer 108. The other steps are the same as those of the sample D1.
[0643] The metal oxide layer 108 of sample D3 has a stacked structure of a first metal oxide layer IGZOa3 and a second metal oxide layer IGZOb3 on the first metal oxide layer IGZOa3. The first metal oxide layer IGZOa3 and the second metal oxide layer IGZOb3 are continuously formed in a vacuum using a sputtering device. The stacked metal oxide layers are processed to obtain the metal oxide layer 108.
[0644] As IGZOa3, an In-Ga-Zn oxide film with a thickness of 20 nm was formed. In addition, the film formation conditions of IGZOa3 were as follows: substrate temperature was 70°C; argon gas with a flow rate of 180 sccm and oxygen gas with a flow rate of 20 sccm (oxygen flow ratio of 10%) were introduced into the chamber; the pressure was 0.6 Pa; and 2500 W of AC power was applied to the polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0645] As IGZOb3, an IGZO film with a thickness of 30 nm was formed. In addition, the film formation conditions of IGZOb3 were as follows: substrate temperature was 70°C; argon gas with a flow rate of 100 sccm and oxygen gas with a flow rate of 100 sccm (oxygen flow ratio of 50%) were introduced into the chamber; the pressure was 0.6 Pa; and 2500 W of AC power was applied to the polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0646] The sample D3 of this example was manufactured through the above-mentioned process.
[0647] <Method for producing sample D4>
[0648] The difference between the sample D4 and the sample D1 is the film forming conditions of the metal oxide layer 108. The other steps are the same as those of the sample D1.
[0649] The metal oxide layer 108 of the sample D4 has a stacked structure of a third metal oxide layer IGZOc4, a first metal oxide layer IGZOa4 on the third metal oxide layer IGZOc4, and a second metal oxide layer IGZOb4 on the first metal oxide layer IGZOa4. The third metal oxide layer IGZOc4, the first metal oxide layer IGZOa4, and the second metal oxide layer IGZOb4 are continuously formed in a vacuum using a sputtering device. The stacked metal oxide layers are processed to obtain the metal oxide layer 108.
[0650] As IGZOc4, an IGZO film with a thickness of 5 nm was formed. In addition, the film forming conditions of IGZOc4 were as follows: substrate temperature was 70°C; argon gas with a flow rate of 100 sccm and oxygen gas with a flow rate of 100 sccm (oxygen flow ratio of 50%) were introduced into the chamber; the pressure was 0.6 Pa; and 2500 W of AC power was applied to the polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0651] As IGZOa4, an In-Ga-Zn oxide film with a thickness of 20 nm was formed. In addition, the film formation conditions of IGZOa4 were as follows: substrate temperature was 70°C; argon gas with a flow rate of 180 sccm and oxygen gas with a flow rate of 20 sccm (oxygen flow ratio of 10%) were introduced into the chamber; the pressure was 0.6 Pa; and 2500 W of AC power was applied to the polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0652] As IGZOb4, an IGZO film with a thickness of 30 nm was formed. In addition, the film formation conditions of IGZOb4 were as follows: substrate temperature was 70°C; argon gas with a flow rate of 100 sccm and oxygen gas with a flow rate of 100 sccm (oxygen flow ratio of 50%) were introduced into the chamber; the pressure was 0.6 Pa; and 2500 W of AC power was applied to the polycrystalline metal oxide sputtering target (In:Ga:Zn=1:1:1.2 [atomic number ratio]).
[0653] The sample D4 of this example was manufactured through the above-mentioned process.
[0654] <Electrical Characteristics of Transistors>
[0655] Next, the Id-Vg characteristics of the transistors of the samples manufactured above were measured. As the measurement conditions of the Id-Vg characteristics of the transistors, the gate voltage (Vg) was changed from -15V to +20V at intervals of 0.25V. In addition, the source voltage (Vs) was set to 0V, and the drain voltage (Vd) was set to 0.1V and 15V. In addition, the number of samples measured was 10.
[0656] Next, the Id-Vg characteristics of the samples D1 to D4 manufactured as described above were measured. Fig.33A and Fig.33B The Id-Vg characteristic results of sample D1 are shown. Fig.34A and Fig.34B The Id-Vg characteristic results of sample D2 are shown. Fig.35A and Fig.35B The Id-Vg characteristic results of sample D3 are shown. Fig.36A and Fig.36B The Id-Vg characteristic results of sample D4 are shown. Fig.33A , Fig.34A , Fig.35A and Fig.36A The measurement results of a transistor having a channel length L of 2 μm and a channel width W of 50 μm are shown. Fig.33B , Fig.34B , Fig.35B and Fig.36B The measurement results of a transistor with a channel length L of 3 μm and a channel width W of 50 μm are shown. Fig.33A , Fig.33B , Fig.34A , Fig.34B , Fig.35A , Fig.35B , Fig.36A and Fig.36B In the figure, the first vertical axis represents Id [A], and the second vertical axis represents μFE [cm 2 / Vs], and the horizontal axis represents Vg[V].
[0657] like Fig.33A , Fig.33B , Fig.34A , Fig.34B , Fig.35A , Fig.35B , Fig.36A and Fig.36B As shown, when the channel length L of samples D1 to D4 was 3 μm, good electrical characteristics with little variation were confirmed. Also, when the channel length L of samples D2 and D4 was 2 μm, good electrical characteristics with little variation were confirmed.
[0658] Next, the reliability evaluation was performed on the samples D1 to D4 manufactured as described above. A bias-thermal stress test (hereinafter referred to as GBT test) was used as the reliability evaluation.
[0659] The conditions of the GBT test of this embodiment are as follows: the gate voltage (Vg) is ±30V; the drain voltage (Vd) and the source voltage (Vs) are both 0V (comm); the stress temperature is 70°C; and the stress application time is one hour; the measurement conditions are two environments: a dark environment and a light irradiation environment (using a white LED to irradiate about 10000lx of light). That is, the potential of the source electrode and the drain electrode of the transistor is set to the same potential, and a different potential from the source electrode and the drain electrode is applied to the gate electrode for a certain period of time (here one hour). The channel length L of the transistor used for the GBT test is 3μm, and the channel width W is 50μm.
[0660] In addition, the case where the potential applied to the gate electrode is higher than the potential of the source electrode and the drain electrode is called positive stress, and the case where the potential applied to the gate electrode is lower than the potential of the source electrode and the drain electrode is called negative stress. Therefore, according to the stress situation and the measurement environment, reliability evaluation is performed under four conditions: positive GBT (darkness), negative GBT (darkness), positive GBT (light irradiation) and negative GBT (light irradiation). In addition, the positive GBT (darkness) is sometimes expressed as PBTS (Positive Bias Temperature Stress), the negative GBT (darkness) is expressed as NBTS (Negative Bias Temperature Stress), the positive GBT (light irradiation) is expressed as PBITS (Positive Bias Illumination Temperature Stress), and the negative GBT (light irradiation) is expressed as NBITS (Negative Bias Illumination Temperature Stress).
[0661] Fig.37 The GBT test results of samples D1 to D4 are shown. Fig.37In the graph, the vertical axis represents the amount of change in the threshold voltage of the transistor (ΔVth), and the horizontal axis represents the sample name.
[0662] like Fig.37 As shown, the amount of change (ΔVth) in the threshold voltage of each of samples D1 to D4 in the GBT test was within ±2 V. Therefore, it was confirmed that the transistor including the metal oxide film according to one embodiment of the present invention had high reliability.
[0663] The structure described in this embodiment can be implemented in combination with the structures described in other embodiment modes or other embodiments as appropriate.
[0664] Explanation of symbols
[0665] 100A transistor
[0666] 100B transistor
[0667] 100C transistor
[0668] 100D transistor
[0669] 100E transistor
[0670] 100F transistor
[0671] 100G transistor
[0672] 102 substrate
[0673] 104 conductive layer
[0674] 106 insulation layer
[0675] Area 106a
[0676] 108 Metal Oxide Layer
[0677] 108a Metal oxide layer
[0678] 108b Metal oxide layer
[0679] 108c Metal oxide layer
[0680] 112a Conductive layer
[0681] 112b Conductive layer
[0682] 112c conductive layer
[0683] 114 Insulation layer
[0684] 114a Insulation layer
[0685] 114b insulation layer
[0686] 116 insulation layer
[0687] 120a Conductive layer
[0688] 120b conductive layer
[0689] 121 Conductive film
[0690] 121a Conductive layer
[0691] 121b Conductive layer
[0692] 121c Conductive layer
[0693] 122 Conductive film
[0694] 122a Conductive layer
[0695] 122b Conductive layer
[0696] 122c conductive layer
[0697] 123 Conductive film
[0698] 123a Conductive layer
[0699] 123b Conductive layer
[0700] 123c conductive layer
[0701] 128a Metal oxide film
[0702] 128b Metal oxide film
[0703] 130a oxygen
[0704] 130b oxygen
[0705] 130c oxygen
[0706] 131 resist mask
[0707] 132 resist mask
[0708] 134 Conductive film
[0709] 142a Connecting part
[0710] 142b Connection
[0711] 150 insulation layer
[0712] 152aConnection
[0713] 152b Connection
[0714] 180 gap
[0715] 501 pixel circuit
[0716] 502 pixel unit
[0717] 504 drive circuit unit
[0718] 504a Gate Driver
[0719] 504b source driver
[0720] 506 protection circuit
[0721] 507 terminal part
[0722] 550 transistors
[0723] 552 transistor
[0724] 554 transistor
[0725] 560 capacitor element
[0726] 562 capacitor element
[0727] 570 LCD components
[0728] 572 light emitting element
[0729] 600 TV sets
[0730] 601 Control Department
[0731] 602 Storage Department
[0732] 603 Communication Control Unit
[0733] 604 image processing circuit
[0734] 605 decoder circuit
[0735] 606 Image signal receiving unit
[0736] 607 Timing Controller
[0737] 608 source driver
[0738] 609 Gate Driver
[0739] 610 Neural Network
[0740] 611 Input layer
[0741] 612 middle layer
[0742] 613 Output layer
[0743] 615 Neurons
[0744] 620 display panel
[0745] 621 pixels
[0746] 630 system bus
[0747] 664 Electrode
[0748] 665 electrode
[0749] 667 electrode
[0750] 700 display device
[0751] 700A Display Device
[0752] 701 substrate
[0753] 702 pixel unit
[0754] 704 source driver circuit
[0755] 705 substrate
[0756] 706 Gate drive circuit unit
[0757] 708FPC terminal part
[0758] 710 signal line
[0759] 711 Wiring Department
[0760] 712 sealant
[0761] 716FPC
[0762] 721 Source Driver IC
[0763] 722 Gate Driver Circuit
[0764] 723FPC
[0765] 724 printed circuit board
[0766] 730 insulation film
[0767] 732 Sealing Film
[0768] 734 Insulation Film
[0769] 736 Coloring Film
[0770] 738 shading film
[0771] 750 transistors
[0772] 752 transistors
[0773] 760 connection electrode
[0774] 770 planarization insulating film
[0775] 772 conductive film
[0776] 773 insulation film
[0777] 774 Conductive film
[0778] 775 Liquid Crystal Components
[0779] 776 Liquid crystal layer
[0780] 778 Structure
[0781] 780 Anisotropic Conductive Film
[0782] 782 light emitting element
[0783] 786EL layer
[0784] 788 conductive film
[0785] 790 capacitor element
[0786] 791 Touch Screen
[0787] 792 insulation film
[0788] 793 Electrode
[0789] 794 Electrode
[0790] 795 insulation film
[0791] 796 Electrode
[0792] 797 Insulation Film
[0793] 7000 Display Unit
[0794] 7100 TV Set
[0795] 7101 housing
[0796] 7103 bracket
[0797] 7111 Remote Control Machine
[0798] 7200 Notebook PC
[0799] 7211 housing
[0800] 7212 Keyboard
[0801] 7213 pointing device
[0802] 7214 External connection port
[0803] 7300 Digital Signage
[0804] 7301 housing
[0805] 7303 Speaker
[0806] 7311 Information terminal equipment
[0807] 7400 Digital Signage
[0808] 7401 Pillar
[0809] 7411 Information terminal equipment
Claims
1. A semiconductor device comprising: a first conductive layer; a first insulating layer on the first conductive layer; a second insulating layer on the first insulating layer; a metal oxide layer on the second insulating layer; a third insulating layer on the metal oxide layer; a second conductive layer in contact with the metal oxide layer; a third conductive layer in contact with the metal oxide layer; a fourth insulating layer on the third insulating layer, the second conductive layer and the third conductive layer; and a fourth conductive layer on the third insulating layer, wherein the metal oxide layer includes a channel formation region, The channel formation region includes a region overlapping the first conductive layer with the first insulating layer and the second insulating layer interposed therebetween. The channel formation region includes a region overlapping the fourth conductive layer with the third insulating layer interposed therebetween. The first conductive layer comprises copper and titanium, The second conductive layer and the third conductive layer each include an oxide including indium and tin, The fourth conductive layer comprises copper and titanium, and The fourth insulating layer includes a gap portion.
2. A semiconductor device comprising: a first insulating layer; a second insulating layer on the first insulating layer; a metal oxide layer on the second insulating layer; a third insulating layer on the metal oxide layer; a first conductive layer on and in contact with the metal oxide layer; a second conductive layer on and in contact with the metal oxide layer; a fourth insulating layer on the third insulating layer, the first conductive layer and the second conductive layer; and a third conductive layer on the third insulating layer, wherein the metal oxide layer includes a channel formation region, The channel formation region includes a region overlapping the third conductive layer with the third insulating layer interposed therebetween. The first conductive layer comprises copper and titanium, The first conductive layer and the second conductive layer each include an oxide including indium and tin, The third conductive layer comprises copper and titanium, and The fourth insulating layer includes a gap portion.