Nitrogen-doped mesoporous carbon supported platinum catalyst and preparation method thereof
The nitrogen-doped mesoporous carbon support was prepared by ultrasonic mixing method, which solved the problem of Pt particles agglomerating and falling off in the fuel cell, improved the stability and efficiency of the catalyst, simplified the preparation process and reduced the cost, and realized an efficient fuel cell. catalyst.
Patent Information
- Application Number
- CN202410808946.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-08
AI Technical Summary
Pt particles in existing fuel cell catalysts are easy to agglomerate and fall off, resulting in low utilization rate. In addition, a large amount of organic solvents and high-cost sodium chloride and zinc chloride are used in the preparation process of traditional carbon carrier materials, which affects the stability and efficiency of the catalyst. .
Nitrogen-doped mesoporous carbon carriers were prepared using ultrasonic mixing of metal salts and imidazole. Carbon carriers with excellent pore structures were formed through heat treatment and acid solution treatment, and MOF-derived carbon materials were optimized to improve the dispersion of Pt particles and the electrocatalyst. chemical activity.
It achieves uniform distribution and efficient utilization of Pt particles, improves the electrochemical activity and stability of the fuel cell catalyst, simplifies the preparation process, reduces costs, and the process is environmentally friendly and easy to produce on a large scale.
Smart Images

Figure CN118748256A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a nitrogen-doped mesoporous carbon-supported platinum catalyst and a preparation method thereof. Background Art
[0002] With the increasing severity of environmental pollution and the accelerated depletion of traditional fossil resources, it is urgent to develop sustainable new alternative energy storage and conversion equipment. New energy systems represented by fuel cells have the advantages of high energy conversion efficiency and clean and pollution-free, and are expected to replace traditional energy systems to a certain extent. In the fuel cell system, the mechanism of the cathode oxygen reduction reaction (ORR) is complex and the reaction kinetics are slow, so an efficient catalyst is needed to accelerate this reaction. At present, the commercial catalyst is mainly Pt / C catalyst, whose structure is mainly active Pt particles loaded on the surface of carbon carrier. The specific surface area and porosity of the carbon carrier are crucial to the stability and dispersibility of platinum particles, and are also conducive to mass transfer in the system reaction process. In traditional carbon carrier materials, Pt particles are mainly loaded on the surface of carbon materials. In the reaction conditions of fuel cells, Pt particles are prone to agglomeration and shedding, which reduces the utilization rate of Pt and affects the overall efficiency of the system.
[0003] Metal organic framework materials (MOFs) are hybrid materials with periodic network structures formed by self-assembly of metal ions and organic ligands. They have advantages such as high specific surface area and rich pore structure. Therefore, the preparation of carbon materials with MOF as a precursor can inherit its excellent structural characteristics and obtain carbon materials with adjustable pore size. The preparation of mesoporous carbon carriers with specific pore size structures can provide more sites for Pt particles, improve the utilization rate of Pt, and enhance the reaction activity. At the same time, the use of nitrogen-containing organic ligands as MOF precursors can be in-situ doped with nitrogen to obtain nitrogen-doped carbon carriers. The introduction of nitrogen is beneficial to improve the hydrophilicity and conductivity of the carrier, and has a certain help to the activity of the catalyst. Therefore, the development of a new type of carrier material with a specific pore structure and nitrogen functionality plays a vital role in improving the activity and stability of fuel cell catalysts and accelerating the large-scale industrial application of fuel cells.
[0004] The invention application document with publication number CN113745553A discloses a technical solution for preparing a carbon carrier by calcining ZIF-8 in molten salt, dissolving metal salt and imidazole organic ligand into organic solvent respectively, heat treating in inert gas, and acid washing and water washing. In the invention, a large amount of organic solvent methanol is used to prepare ZIF-8, which is not in line with the environmentally friendly strategy. In addition, sodium chloride and zinc chloride are added during the heat treatment process, which also increases the additional preparation cost.
[0005] The patent application document with publication number CN114094113A discloses a carbon carrier for hydrogen fuel cells, a preparation method and a prepared battery catalyst. The preparation method includes: pre-mixing and dispersing the carbon carrier, pickling with an oxidizing acid solution and filtering and rinsing steps, and then functionalizing the carbon carrier by crushing and screening, purging with a mixed gas containing ammonia, and heating in a plasma-enhanced rotary kiln, while starting a plasma generator to finally obtain a functionalized carbon carrier. Although the invention can produce Pt nanoparticles with smaller and more uniform particle sizes, the nitrogen source used in its preparation process is cumbersome and dangerous, and the highest electrochemical activity measured is 218mA / mg Pt .
[0006] The invention application document with publication number CN113013427A discloses a high-performance electrocatalyst carrier derived from a metal organic framework (MOF) material and a preparation method thereof, which effectively controls the graphitization degree and stability of the carrier and obtains uniform Pt-based nanoparticles. However, the preparation of the MOF precursor in the patent involves the use of a large amount of organic solvents, and secondly, the patent does not focus on the effect of adjusting the pore size of the carbon carrier on the Pt-loaded catalyst.
[0007] The invention with publication number CN108441884A also prepares a mixed solution of zinc salt and dimethylimidazole, stirs and separates to obtain ZIF-8, and the obtained product is subjected to high temperature calcination, acid washing and water washing to obtain a carbon material. The obtained carbon is combined with molybdenum disulfide to construct a new composite structure to improve the electrocatalytic hydrogen evolution activity and stability of molybdenum disulfide. The invention mainly uses carbon derived from a metal organic framework and molybdenum disulfide to construct an electrocatalytic hydrogen evolution material, and does not pay attention to the regulatory effect of the types of zinc salts, solvents, etc. and the optimization of specific conditions on the pore size of the carbon carrier, and carbon carriers with different pore sizes and specific surface areas are very important for carrying Pt in fuel cells.
[0008] Therefore, how to prepare a mesoporous carbon carrier with adjustable pore size suitable for fuel cells through a simple process to achieve uniform distribution and efficient utilization of Pt particles is one of the practical problems for the engineering application of PEMFC. Summary of the invention
[0009] In order to solve the above technical problems, the present invention provides a nitrogen-doped mesoporous carbon-supported platinum catalyst and a preparation method thereof.
[0010] In a first aspect, the present invention provides a method for preparing nitrogen-doped mesoporous carbon, comprising: 1) ultrasonically mixing the metal salt solution and the imidazole solution, stirring for reaction, and then centrifuging, washing and drying the obtained crystals to obtain a carbon carrier precursor; 2) heat-treating the carbon carrier precursor obtained in step 1) under an inert atmosphere to obtain a carbon carrier powder; 3) heating, stirring and refluxing the carbon support powder obtained in step 2) in an acid solution, and then washing and drying the carbon support powder to obtain a carbon support material; The metal salt is selected from one or more of zinc sulfate heptahydrate, zinc acetate dihydrate, zinc chloride, and zinc oxide; and the solvents used in the metal salt solution and the imidazole solution are selected from one or more of anhydrous ethanol, NN dimethylformamide, and deionized water.
[0011] In the present invention, a certain type of metal salt, imidazole and solvent are stirred under certain conditions, and the obtained precursor is heat-treated and activated by heating, stirring and refluxing in an acid solution to obtain a carbon support material with excellent pore structure characteristics, which can make the fuel cell Pt / C catalyst have excellent electrochemical activity and stability.
[0012] Preferably, in step 1), the metal salt is zinc acetate dihydrate.
[0013] Preferably, in step 1), the imidazole is dimethylimidazole.
[0014] In the present invention, by using zinc acetate dihydrate and dimethylimidazole, nitrogen-doped mesoporous carbon with excellent pore structure can be formed, Pt particles can be better dispersed, and the catalyst activity is improved. By optimizing the synergistic effect of zinc acetate dihydrate and dimethylimidazole, the structure and performance of MOF-derived nitrogen-doped mesoporous carbon are significantly improved, and a carbon-supported platinum catalyst with excellent electrochemical activity and stability is prepared.
[0015] Preferably, in step 1), the molar ratio of the metal salt to the imidazole is 1:6 to 1:12.
[0016] Further preferably, in step 1), the molar ratio of the metal salt to the imidazole is 1:9 to 1:11, preferably 1:10. By optimizing the ratio of the above metal salt to imidazole, the pore structure of MOF can be regulated, and a specific molar ratio helps to form a MOF material with a specific pore size. When zinc acetate dihydrate and dimethylimidazole are used in the preferred dosage ratio, under certain treatment conditions, mesoporous carbon with a more ideal pore size distribution can be obtained, which improves the uniform distribution and utilization efficiency of Pt particles in the material, and makes the fuel cell Pt / C catalyst have better electrochemical activity and stability, which helps to further improve the comprehensive performance of the carrier and catalyst.
[0017] Preferably, in step 1), the solvent is deionized water. The present invention has found that when deionized water is used as the solvent, it is beneficial for the reaction to form a high-purity, high-quality MOF precursor.
[0018] Preferably, in step 1), the concentration ratio of the metal salt solution to the imidazole solution is 1:6 to 1:12, for example, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, etc.
[0019] Preferably, in step 1), the stirring reaction time is 8 to 48 hours, for example, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 24 hours, 28 hours, 32 hours, 36 hours, 40 hours, 44 hours, etc.
[0020] Preferably, in step 1), the stirring rate is 300 to 1000 rpm; the centrifugal speed is 6000 to 10000 rpm. For example, the stirring rate can be 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm, etc., and the centrifugal speed can be 6000 rpm, 7000 rpm, 8000 rpm, 9000 rpm, 10000 rpm, etc.
[0021] Preferably, in step 1), the drying method is vacuum drying, the vacuum temperature is 40 to 80° C., and the drying time is 8 to 24 hours.
[0022] Preferably, in step 2), the inert atmosphere is nitrogen or argon.
[0023] Preferably, in step 2), the heat treatment temperature is 800-1100°C, and the heat treatment time is 2-5 hours. For example, the heat treatment temperature can be 850°C, 900°C, 950°C, 1000°C, 1050°C, etc.
[0024] Preferably, in step 3), the acid solution is selected from one or more of sulfuric acid, nitric acid and hydrochloric acid; and the concentration of the acid solution is 0.1-1 mol / L.
[0025] Preferably, in step 3), the heating temperature is 60-100° C.; the stirring speed is 300-1000 rpm; and the reflux treatment time is 0.5-8 h.
[0026] Preferably, in step 3), the centrifugal separation speed during the water washing process is 6000-10000 rpm; the drying is vacuum drying at a temperature of 40-80°C and a drying time of 8-24h. In the present invention, by adopting heat treatment, acid treatment and other subsequent treatments under the above conditions, it is helpful to better form a mesoporous carbon skeleton, further optimize the pore structure and surface chemical properties, and help improve the comprehensive performance of the MOF-derived nitrogen-doped mesoporous carbon-supported platinum catalyst, such as activity and stability.
[0027] In a second aspect, the present invention provides MOF-derived nitrogen-doped mesoporous carbon obtained by the above-mentioned preparation method of nitrogen-doped mesoporous carbon.
[0028] In a third aspect, the present invention provides a nitrogen-doped mesoporous carbon-supported platinum catalyst, including the nitrogen-doped mesoporous carbon obtained by the above-mentioned preparation method of nitrogen-doped mesoporous carbon or the above-mentioned nitrogen-doped mesoporous carbon, and the platinum loading rate is 40% to 60%.
[0029] The carbon carrier prepared by the present invention using a specific MOF precursor is a mesoporous carbon with adjustable pore size, which can effectively disperse Pt particles and improve the utilization rate of Pt; after the carbon carrier prepared by the present invention is loaded with 50wt% Pt nanoparticles, its mass activity can reach 0.4A / mg in electrochemical testing Pt .
[0030] In a fourth aspect, the present invention provides the use of the above-mentioned nitrogen-doped mesoporous carbon-supported platinum catalyst in a fuel cell.
[0031] The beneficial effects of the present invention are at least: (1) The metal salt, imidazole and solvent used in the present invention are stirred under certain conditions, and the resulting precursor is heat treated and activated by heating, stirring and refluxing in an acid solution to obtain a carbon support material with excellent pore structure characteristics, which can make the fuel cell Pt / C catalyst have excellent electrochemical activity and stability.
[0032] (2) The carbon carrier prepared by the present invention introduces nitrogen atoms, which enhances the hydrophilicity of the carbon carrier and facilitates the dispersion of the carrier in the liquid phase.
[0033] (3) The carbon carrier prepared by the present invention is mesoporous carbon with a pore size of 3 to 6 nm. This pore size range is suitable for use as a carrier for fuel cell catalysts, so that Pt particles are evenly distributed and have a higher specific surface area. At the same time, after the carbon carrier is loaded with 50 wt% Pt nanoparticles, the mass activity can reach 0.4 A / mg Pt .
[0034] (4) The carbon carrier material prepared by the present invention has a simple and easy preparation method, does not require any surfactant, is environmentally friendly, and is easy to scale up for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 The pore size distribution diagram of the carbon supports prepared in the examples and comparative examples.
[0037] Figure 2 Graph showing the specific surface area of the carbon supports prepared in Examples and Comparative Examples.
[0038] Figure 3 TEM image of the Pt / C catalyst prepared in Example 1.
[0039] Figure 4 This is the TEM image of the Pt / C catalyst prepared in Comparative Example 1.
[0040] Figure 5 The electrochemical LSV curves of the Pt / C catalysts prepared in the examples and comparative examples. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] If no specific technology or conditions are specified in the embodiments of the present invention, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the devices, instruments, reagents, etc. is not specified, they are all conventional products that can be purchased through regular channels. The raw materials used in the present invention can be easily purchased in the domestic product market.
[0043] Example 1
[0044] 1) At room temperature, 0.6 mmol zinc acetate dihydrate and 6.0 mmol dimethylimidazole are weighed at a molar ratio of 1:10; they are dissolved in 50 mL deionized water to keep the metal salt solution: imidazole solution at a ratio of 1:10; the solutions are mixed and stirred for 12 hours, wherein the stirring rate is 500 rpm; the product is separated from the solvent by centrifugation at a speed of 10,000 rpm, and washed with water 4 times; and the obtained crystals are then vacuum dried at 60° C. for 12 hours to obtain a precursor of the carrier material.
[0045] 2) placing the precursor product obtained in step (1) in a tube furnace, treating it at 900° C. for 2 h in an inert atmosphere of argon to obtain a carbonized product.
[0046] 3) The product obtained in step (2) was placed in a flask containing 200 mL of 0.5 mol / L hydrochloric acid solution, heated, stirred and refluxed for 3 h, wherein the stirring rate was 500 rpm and the heating temperature was 80°C.
[0047] 4) The product obtained in step (3) was centrifuged and washed with water 4 times at a speed of 8000 rpm; the obtained crystals were then vacuum dried at 60° C. for 24 h to obtain a carbon carrier material. The pore size distribution and specific surface area of the prepared carbon carrier were as follows: Figure 1-2 As shown in the figure, the pore size is concentrated in the range of 3 to 6 nm through BET analysis, and the specific surface area reaches 1567 m 2 / g, which is a mesoporous carbon material. After the carbon carrier prepared in this embodiment is loaded with 50wt% Pt nanoparticles by impregnation method, the TEM image of the prepared Pt / C catalyst is as follows Figure 3 As shown in Figure 2, the electrochemical LSV curve of the Pt / C catalyst is Figure 5 As shown, electrochemical tests show that the mass activity can reach 0.4A / mg Pt .
[0048] Example 2
[0049] 1) At room temperature, 0.6 mmol zinc acetate dihydrate and 3.6 mmol dimethylimidazole are weighed respectively at a molar ratio of 1:6; they are dissolved in 50 mL deionized water to keep the metal salt solution: imidazole solution at a ratio of 1:6; the solutions are mixed and stirred for reaction for 12 hours, wherein the stirring rate is 500 rpm; the product is separated from the solvent by centrifugation at a speed of 10,000 rpm, and washed with water 4 times; and the obtained crystals are then vacuum dried at 60° C. for 12 hours to obtain a precursor of the carrier material.
[0050] 2) placing the precursor product obtained in step (1) in a tube furnace, treating it at 900° C. for 2 h in an inert atmosphere of argon to obtain a carbonized product.
[0051] 3) The product obtained in step (2) was placed in a flask containing 200 mL of 0.5 mol / L hydrochloric acid solution, heated, stirred and refluxed for 3 h, wherein the stirring rate was 500 rpm and the heating temperature was 80°C.
[0052] 4) The product obtained in step (3) was centrifuged and washed with water 4 times at a speed of 8000 rpm; the obtained crystals were then vacuum dried at 60° C. for 24 h to obtain a carbon carrier material. The pore size distribution and specific surface area of the prepared carbon carrier were as follows: Figure 1-2 As shown in the figure, the pore size is concentrated in the range of 3 to 6 nm through BET analysis, and the specific surface area reaches 1188 m 2 / g, which is a mesoporous carbon material.
[0053] Example 3
[0054] 1) At room temperature, 0.6 mmol zinc acetate dihydrate and 7.2 mmol dimethylimidazole are weighed at a molar ratio of 1:12; they are dissolved in 50 mL deionized water to keep the metal salt solution: imidazole solution at a ratio of 1:12; the solutions are mixed and stirred for 12 hours, wherein the stirring rate is 500 rpm; the product is separated from the solvent by centrifugation at a speed of 10,000 rpm, and washed with water 4 times; and the obtained crystals are then vacuum dried at 60° C. for 12 hours to obtain a precursor of the carrier material.
[0055] 2) placing the precursor product obtained in step (1) in a tube furnace, treating it at 1100° C. for 6 h in an inert atmosphere of argon to obtain a carbonized product.
[0056] 3) The product obtained in step (2) was placed in a flask containing 200 mL of 0.5 mol / L hydrochloric acid solution, heated, stirred and refluxed for 3 h, wherein the stirring rate was 500 rpm and the heating temperature was 80°C.
[0057] 4) The product obtained in step (3) was centrifuged and washed with water 4 times at a speed of 8000 rpm; the obtained crystals were then vacuum dried at 60° C. for 24 h to obtain a carbon carrier material. The pore size distribution and specific surface area of the prepared carbon carrier were as follows: Figure 1-2 As shown in the figure, the pore size is concentrated in the range of 3 to 6 nm through BET analysis, and the specific surface area reaches 1307 m 2 / g, which is a mesoporous carbon material.
[0058] Example 4
[0059] 1) At room temperature, 0.6 mmol zinc acetate dihydrate and 1.8 mmol dimethylimidazole are weighed at a molar ratio of 1:3; they are dissolved in 50 mL deionized water to keep the metal salt solution: imidazole solution at a ratio of 1:3; the solutions are mixed and stirred for 12 hours, wherein the stirring rate is 250 rpm; the product is separated from the solvent by centrifugation at a speed of 12000 rpm, and washed with water 4 times; and the obtained crystals are then vacuum dried at 60°C for 12 hours to obtain a precursor of the carrier material.
[0060] 2) placing the precursor product obtained in step (1) in a tube furnace, treating it at 900° C. for 2 h in an inert atmosphere of argon to obtain a carbonized product.
[0061] 3) The product obtained in step (2) was placed in a flask containing 200 mL of 0.5 mol / L hydrochloric acid solution, heated, stirred and refluxed for 3 h, wherein the stirring rate was 500 rpm and the heating temperature was 80°C.
[0062] 4) The product obtained in step (3) was centrifuged and washed with water 4 times at a speed of 8000 rpm; the obtained crystals were then vacuum dried at 60°C for 24 hours to obtain a carbon carrier material. The pore size distribution and specific surface area of the prepared carbon carrier are shown in the following table. Figure 1-2 As shown in the figure, the pore size is concentrated in the range of 3 to 5 nm through BET analysis, and the specific surface area is 908 m 2 / g, which is a mesoporous carbon material.
[0063] Example 5
[0064] 1) At room temperature, 0.6 mmol of zinc sulfate heptahydrate and 3.6 mmol of dimethylimidazole are weighed at a molar ratio of 1:10; they are dissolved in 50 mL of anhydrous ethanol to keep the metal salt solution: imidazole solution at a ratio of 1:10; the solutions are mixed and stirred for reaction for 12 hours, wherein the stirring rate is 500 rpm; the product is separated from the solvent by centrifugation at a speed of 10,000 rpm, and washed with water 4 times; and the obtained crystals are then vacuum dried at 60° C. for 12 hours to obtain a precursor of the carrier material.
[0065] 2) placing the precursor product obtained in step (1) in a tube furnace, treating it at 900° C. for 2 h in an inert atmosphere of argon to obtain a carbonized product.
[0066] 3) The product obtained in step (2) was placed in a flask containing 200 mL of 0.5 mol / L hydrochloric acid solution, heated, stirred and refluxed for 3 h, wherein the stirring rate was 500 rpm and the heating temperature was 80°C.
[0067] 4) The product obtained in step (3) was centrifuged and washed with water 4 times at a speed of 8000 rpm; the obtained crystals were then vacuum dried at 60° C. for 24 h to obtain a carbon carrier material. The specific surface area of the prepared carbon carrier was 883 m 2 / g.
[0068] Example 6
[0069] 1) At room temperature, 0.6 mmol of zinc sulfate heptahydrate and 3.6 mmol of dimethylimidazole are weighed at a molar ratio of 1:10; they are dissolved in 50 mL of deionized water to keep the metal salt solution: imidazole solution at a ratio of 1:10; the solutions are mixed and stirred for 12 hours, wherein the stirring rate is 500 rpm; the product is separated from the solvent by centrifugation at a speed of 10,000 rpm, and washed with water 4 times; and the obtained crystals are then vacuum dried at 60° C. for 12 hours to obtain a precursor of the carrier material.
[0070] 2) placing the precursor product obtained in step (1) in a tubular furnace, treating it at 600° C. for 2 h in an inert atmosphere of argon to obtain a carbonized product.
[0071] 3) The product obtained in step (2) was placed in a flask containing 200 mL of 0.5 mol / L hydrochloric acid solution, heated, stirred and refluxed for 3 h, wherein the stirring rate was 500 rpm and the heating temperature was 80°C.
[0072] 4) The product obtained in step (3) was centrifuged and washed with water 4 times at a speed of 8000 rpm; the obtained crystals were then vacuum dried at 60° C. for 24 h to obtain a carbon carrier material. The specific surface area of the prepared carbon carrier was 784 m 2 / g.
[0073] Example 7
[0074] 1) At room temperature, 0.6 mmol zinc acetate dihydrate and 3.6 mmol dimethylimidazole are weighed at a molar ratio of 1:10; they are dissolved in 50 mL deionized water to keep the metal salt solution: imidazole solution at a ratio of 1:10; the solutions are mixed and stirred for 12 hours, wherein the stirring rate is 500 rpm; the product is separated from the solvent by centrifugation at a speed of 10,000 rpm, and washed with water 4 times; and the obtained crystals are then vacuum dried at 60° C. for 12 hours to obtain a precursor of the carrier material.
[0075] 2) placing the precursor product obtained in step (1) in a tubular furnace, treating it at 1200° C. for 2 h in an inert atmosphere of argon to obtain a carbonized product.
[0076] 3) The product obtained in step (2) was placed in a flask containing 200 mL of 0.5 mol / L hydrochloric acid solution, heated, stirred and refluxed for 3 h, wherein the stirring rate was 500 rpm and the heating temperature was 80°C.
[0077] 4) The product obtained in step (3) was centrifuged and washed with water 4 times at a speed of 8000 rpm; the obtained crystals were then vacuum dried at 60° C. for 24 h to obtain a carbon carrier material. The specific surface area of the prepared carbon carrier was 1085 m 2 / g.
[0078] Example 8
[0079] 1) At room temperature, 0.6 mmol of zinc sulfate heptahydrate and 3.6 mmol of dimethylimidazole are weighed at a molar ratio of 1:10; they are dissolved in 50 mL of deionized water to keep the metal salt solution: imidazole solution at a ratio of 1:10; the solutions are mixed and stirred for 12 hours, wherein the stirring rate is 500 rpm; the product is separated from the solvent by centrifugation at a speed of 10,000 rpm, and washed with water 4 times; and the obtained crystals are then vacuum dried at 60° C. for 12 hours to obtain a precursor of the carrier material.
[0080] 2) placing the precursor product obtained in step (1) in a tube furnace, treating it at 900° C. for 2 h in an inert atmosphere of argon to obtain a carbonized product.
[0081] 3) The product obtained in step (2) was placed in a flask containing 200 mL of 2 mol / L hydrochloric acid solution, heated, stirred and refluxed for 6 h, wherein the stirring rate was 500 rpm and the heating temperature was 80°C.
[0082] 4) The product obtained in step (3) was centrifuged and washed with water 4 times at a speed of 8000 rpm; the obtained crystals were then vacuum dried at 60° C. for 24 h to obtain a carbon carrier material. The specific surface area of the prepared carbon carrier was 895 m 2 / g.
[0083] Example 9
[0084] 1) At room temperature, 0.6 mmol zinc acetate dihydrate and 3.6 mmol dimethylimidazole are weighed at a molar ratio of 1:10; they are dissolved in 50 mL deionized water to keep the metal salt solution: imidazole solution at a ratio of 1:10; the solutions are mixed and stirred for 12 hours, wherein the stirring rate is 500 rpm; the product is separated from the solvent by centrifugation at a speed of 10,000 rpm, and washed with water 4 times; and the obtained crystals are then vacuum dried at 60° C. for 12 hours to obtain a precursor of the carrier material.
[0085] 2) placing the precursor product obtained in step (1) in a tubular furnace, treating it at 1200° C. for 2 h in an inert atmosphere of argon to obtain a carbonized product.
[0086] 3) The product obtained in step (2) was placed in a flask containing 200 mL of 2 mol / L hydrochloric acid solution, heated, stirred and refluxed for 3 h, wherein the stirring rate was 250 rpm and the heating temperature was 50°C.
[0087] 4) The product obtained in step (3) was centrifuged and washed with water 4 times at a speed of 8000 rpm; the obtained crystals were then vacuum dried at 60° C. for 24 h to obtain a carbon carrier material. The specific surface area of the prepared carbon carrier was 1204 m 2 / g.
[0088] Comparative Example 1
[0089] The difference between this comparative example and Example 1 is that step (1) is to weigh 0.6 mmol zinc nitrate hexahydrate and 6.0 mmol dimethylimidazole at room temperature in a molar ratio of 1:10; respectively dissolve them in 50 mL of anhydrous methanol to keep the metal salt solution: imidazole solution at a ratio of 1:10; mix the solutions and stir to react for 24 hours, wherein the stirring rate is 500 rpm; separate the product from the solvent by centrifugation at a speed of 10,000 rpm, and wash it with water 4 times; then vacuum dry the obtained crystals at 60°C for 12 hours to obtain the precursor of the carrier material. The rest of the preparation method and parameters are consistent with Example 1. The pore size distribution and specific surface area results of the prepared carbon carrier are shown as follows: Figure 1-2 As shown in the figure, the measured structure shows that the average pore size of the carrier is less than 1.5nm, with only microporous structure and a specific surface area of 773m 2 / g. TEM images of prepared Pt / C catalysts are shown in Figure 4 As shown, it can be seen that the catalyst Pt particles prepared by this carrier are relatively large and partially agglomerated.
[0090] Comparative Example 2
[0091] The difference between this comparative example and Example 1 is that step (1) is to weigh 0.6 mmol zinc nitrate hexahydrate and 4.8 mmol dimethylimidazole at room temperature in a molar ratio of 1:8; respectively dissolve them in 50 mL of anhydrous methanol to keep the metal salt solution: imidazole solution at a ratio of 1:8; mix the solutions and stir to react for 48 hours, wherein the stirring rate is 250 rpm; separate the product from the solvent by centrifugation at a speed of 10,000 rpm, and wash it with water 4 times; then vacuum dry the obtained crystals at 60°C for 12 hours to obtain the precursor of the carrier material. The rest of the preparation method and parameters are consistent with Example 1. The pore size distribution and specific surface area results of the prepared carbon carrier are shown as follows: Figure 1-2 As shown in the figure, the measured structure shows that the average pore size of the carrier is less than 1.5nm, with only microporous structure and a specific surface area of 844m 2 / g.
[0092] Preparation of Pt / C catalyst: The carbon carrier obtained in the embodiment and the comparative example is prepared into a platinum-carbon catalyst. The preparation method of the platinum-carbon catalyst is a solution impregnation method, and the specific steps include: weighing 70 mg of the carbon carrier prepared in the above embodiment and the comparative example and ultrasonically dispersing it in 12 mL of ultrapure water; measuring 1.868 mL of chloroplatinic acid aqueous solution (concentration of 0.192 mol / L) and adding it to the above solution to prepare a suspension, and ultrasonicating it in an ice bath for 30 minutes; then heating at 70°C and continuously stirring magnetically to evaporate until most of the liquid disappears, and the whole is in a viscous yogurt-like state, and then placed in a freeze dryer for freeze drying for 15 hours; placing the dried sample in a crucible and reducing it in a 10% hydrogen-argon mixture at a reduction temperature of 100-300°C for 1-3 hours, and finally obtaining a Pt / C catalyst, and controlling the mass content of Pt metal to be 50%.
[0093] Performance of Pt / C catalyst: The catalysts prepared in Examples 1-4 and Comparative Examples 1-2 were prepared into slurries and subjected to electrochemical tests. The electrochemical LSV curves of the Pt / C catalysts are shown in FIG. Figure 5 The specific steps of electrochemical test are as follows.
[0094] 1) Add 50 μL of 5% Nafion solution, 2 mL of deionized water and 2 mL of isopropanol to the weighed catalyst in sequence; use ultrasonic wave with power not less than 200 W for 30 min to mix the slurry evenly. During the ultrasonic process, the water bath temperature should be kept not higher than 20°C.
[0095] 2) Grind the electrode with polishing powder for 3 minutes, and clean the polished electrode with ultrapure water and ethanol for later use. 2 ~200 μg / cm 2 , take an appropriate amount of the dispersed slurry and evenly add it twice to the smooth and clean surface of the disk electrode, let it dry naturally and completely, as the working electrode.
[0096] 3) The electrochemical test was carried out using a rotating disk electrode test system and an electrochemical workstation of PINE. The above-mentioned electrode was placed in an electrolytic cell as a working electrode, the reference electrode was a reversible hydrogen electrode (RHE), the counter electrode was a Pt sheet, and a three-electrode system was formed. The electrolyte was a 0.1 M perchloric acid solution saturated with N2.
[0097] 4) Electrode activation was performed, and the catalyst was activated at a scanning rate of 200 mV / s until the hydrogen desorption peak area no longer increased.
[0098] 5) Test the oxygen reduction linear scanning curve, the electrolyte was replaced with a 0.1M perchloric acid solution saturated with O2, the scanning speed was 10mV / s, the electrode speed was 1600rpm, and the scanning was performed for 3 circles. The potential scanning range was 0.025V to 1.2V (relative to RHE). The kinetic diffusion current was calculated according to the Koutecky-Levich formula, and finally the current value at a potential of 0.9V was taken to calculate MA, and the calculation formula is as follows: k =j d *j / (j d -j); where j is the experimentally measured current, j k is the dynamic current of the rotating disk, j d is the limiting current, MA = j k / m Pt (A / mg Pt ), m Pt is the amount of Pt loaded on the glassy carbon electrode, μg cm -2 .
[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing nitrogen-doped mesoporous carbon, characterized in that: include: 1) ultrasonically mixing the metal salt solution and the imidazole solution, stirring for reaction, and then centrifuging, washing and drying the obtained crystals to obtain a carbon carrier precursor; 2) heat-treating the carbon carrier precursor obtained in step 1) under an inert atmosphere to obtain a carbon carrier powder; 3) heating, stirring and refluxing the carbon support powder obtained in step 2) in an acid solution, and then washing and drying the carbon support powder to obtain a carbon support material; The metal salt is selected from one or more of zinc sulfate heptahydrate, zinc acetate dihydrate, zinc chloride, and zinc oxide, and the solvents used in the metal salt solution and the imidazole solution are selected from one or more of anhydrous ethanol, NN dimethylformamide, and deionized water.
2. The method for preparing nitrogen-doped mesoporous carbon according to claim 1, characterized in that: In step 1), the metal salt is zinc acetate dihydrate; And / or, the imidazole is dimethylimidazole; And / or, the molar ratio of the metal salt to the imidazole is 1:6 to 1:
12.
3. The method for preparing nitrogen-doped mesoporous carbon according to claim 2, characterized in that: In step 1), the solvent is deionized water; And / or, in step 1), the concentration ratio of the metal salt solution to the imidazole solution is 1:6 to 1:
12.
4. The method for preparing nitrogen-doped mesoporous carbon according to claim 3, characterized in that: In step 1), the stirring reaction time is 8 to 48 hours, and the stirring rate is 300 to 1000 rpm.
5. The method for preparing nitrogen-doped mesoporous carbon according to any one of claims 1 to 4, characterized in that: In step 1), the centrifugal speed is 6000-10000 rpm; and / or the drying method is vacuum drying, the vacuum temperature is 40-80° C., and the drying time is 8-24 hours.
6. The method for preparing nitrogen-doped mesoporous carbon according to any one of claims 1 to 5, characterized in that: In step 2), the inert atmosphere is nitrogen or argon; And / or, in step 2), the temperature of the heat treatment is 800-1100° C., and the time of the heat treatment is 2-5 hours.
7. The method for preparing nitrogen-doped mesoporous carbon according to any one of claims 1 to 6, characterized in that: In step 3), the acid solution is selected from one or more of sulfuric acid, nitric acid and hydrochloric acid, and the concentration of the acid solution is preferably 0.1 to 1 mol / L; And / or, in step 3), the heating temperature is 60-100° C.; the stirring speed is 300-1000 rpm; the reflux treatment time is 0.5-8 h; And / or, in step 3), the centrifugal separation speed during the water washing process is 6000-10000 rpm; the drying is vacuum drying at a temperature of 40-80° C. and a drying time of 8-24 h.
8. Nitrogen-doped mesoporous carbon obtained by the method for preparing nitrogen-doped mesoporous carbon according to any one of claims 1 to 7.
9. A nitrogen-doped mesoporous carbon-supported platinum catalyst, comprising platinum and the nitrogen-doped mesoporous carbon obtained by the preparation method of the nitrogen-doped mesoporous carbon according to any one of claims 1 to 7 or the nitrogen-doped mesoporous carbon according to claim 8, wherein the platinum loading rate is 40% to 60%.
10. Use of the nitrogen-doped mesoporous carbon-supported platinum catalyst according to claim 9 in a fuel cell.