High-absorptivity thin film battery assembly and manufacturing method thereof
By accurately matching the thickness of the first transparent conductive layer and the perovskite absorption layer in the thin film battery module, the problem of thickness mismatch between the TCO film and the battery's light absorption layer is solved, achieving high absorption rate and high photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202410734246.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-08
AI Technical Summary
The thickness mismatch between the TCO film and the light-absorbing layer of the battery affects the performance of the thin-film battery and affects the photoelectric conversion efficiency.
By accurately optimizing and matching the thickness of the first transparent conductive layer and the perovskite absorption layer, and regulating the film thickness of the first transparent conductive layer to match the perovskite absorption layer of different thicknesses, a thin film battery module with high absorption rate is formed. Make sure the light absorption rate is greater than 90%.
It improves the photoelectric conversion efficiency of thin film battery components and ensures the best light utilization and performance.
Smart Images

Figure CN118748894A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thin-film photovoltaic components, and in particular to a thin-film battery component with high absorption rate and a manufacturing method thereof. Background Art
[0002] TCO film can be used as the front electrode of thin-film battery and also has the function of anti-reflection film. Its thickness, conductivity and transmittance will directly affect the photoelectric conversion efficiency of thin-film battery. At the same time, since the light-absorbing layer of the battery is a thin-film battery, the change of thickness will affect the multiple reflection opportunities of light in the thin film, and the change of film thickness will also affect the amount of light penetrating the thin-film battery, which will also directly affect the photoelectric conversion efficiency of the battery. The thickness of TCO film and thin-film battery (battery light-absorbing layer) has a complex impact on the performance of solar cells, and is also the factor that most directly affects the performance of solar cells. Summary of the invention
[0003] The purpose of the present invention is to solve the problem that the performance of thin-film batteries is affected by the thickness mismatch between the TCO film and the battery light-absorbing layer, and to provide a thin-film battery component with a high absorption rate.
[0004] The present invention is achieved through the following technical solutions:
[0005] The present invention provides a thin-film battery assembly with high absorption rate, wherein the thin-film battery assembly comprises a front glass, a perovskite battery layer, a packaging layer and a back glass which are stacked in sequence, and the perovskite battery layer is stacked on the opposite side of the light-entering surface of the front glass; the absorption rate of the thin-film battery assembly is greater than 90%; the perovskite battery layer is stacked in sequence by a first transparent conductive layer, a first transmission layer, a perovskite absorption layer, a buffer layer, a second transmission layer and a second transparent conductive layer; the first transparent conductive layer is arranged on the opposite side of the light-entering surface of the front glass, and the refractive index of the first transparent conductive layer is set to 1.7-1.85; the refractive index of the perovskite absorption layer is set to 2.5-2.7;
[0006] Among them, when the thickness of the first transparent conductive layer is set to 160-170nm, the thickness of the perovskite absorption layer is set to 500-650nm; when the thickness of the first transparent conductive layer is set to 171-200nm, the thickness of the perovskite absorption layer is set to 400-600nm; when the thickness of the first transparent conductive layer is set to 201-210nm, the thickness of the perovskite absorption layer is set to 500-750nm; when the thickness of the first transparent conductive layer is set to 211-220nm, the thickness of the perovskite absorption layer is set to 600-850nm.
[0007] Specifically, in order to balance the effects of the thickness of the first transparent conductive layer (TCO film) and the perovskite absorption layer on the performance of the thin-film battery cell, the present invention achieves the best utilization of sunlight by the battery cell by deeply optimizing the thickness of the first transparent conductive layer and the perovskite absorption layer, thereby ensuring that the light absorption rate of the thin-film battery assembly can be greater than 90%.
[0008] Furthermore, a thin-film battery component with high absorption rate: the refractive index of the first transmission layer is set to 1.6-1.75, the thickness is set to 30-50nm, and it is made of NiOx or MoO3.
[0009] Furthermore, in a thin-film battery assembly with high absorptivity, the refractive index of the buffer layer is set to 2.1-2.4, and the thickness thereof is set to 20-40 nm.
[0010] Furthermore, a thin-film battery component with high absorption rate: the refractive index of the second transmission layer is set to 1.8-2.0, the thickness is set to 8-15nm, and the material is TiO2 or SnO2.
[0011] Furthermore, a thin-film battery component with high absorption rate: the refractive index of the second transparent conductive layer is set to 1.9-2.0, the thickness is set to 160-180nm, and the material is ITO, FTO or AZO.
[0012] The present invention also provides a method for manufacturing a thin-film battery assembly with a high absorption rate, the method comprising the following steps:
[0013] S1, depositing a TCO thin film material on the opposite side of the light incident surface of the front glass by magnetron sputtering, and then performing P1 laser scribing on the material to form the first transparent conductive layer;
[0014] S2. Forming the first transmission layer on the first transparent conductive layer using a vacuum coating device;
[0015] S3, after annealing / drying the first transmission layer, coating the perovskite absorption layer thereon;
[0016] S4, after annealing / drying the perovskite absorption layer, evaporating the buffer layer thereon;
[0017] S5, continuing to anneal / dry the buffer layer, and then forming the second transmission layer thereon;
[0018] S6, annealing / drying the second transmission layer, performing P2 laser scribing to form a plurality of perovskite sub-cells, then preparing a second transparent conductive layer on the second transmission layer using an RPD device, and continuing to perform P3 laser scribing and P4 edge cleaning to form a perovskite thin film battery assembly in which the sub-cells are connected in series;
[0019] S7. After the leads form a circuit loop, the encapsulation layer and the back glass are laid for lamination to obtain a thin-film battery module with a high absorption rate.
[0020] Beneficial effects of the present invention:
[0021] The present invention achieves the best light utilization effect by accurately optimizing and matching the thickness of the first transparent conductive layer (front transparent electrode) and the perovskite absorption layer in the thin-film battery assembly, and adjusting the film thickness of the first transparent conductive layer to match the perovskite absorption layers of different thicknesses, thereby effectively increasing the amount of incident light that can be received by a unit area of the thin-film battery assembly, ensuring that the light absorption rate of the thin-film battery assembly is greater than 90%, thereby improving the photoelectric conversion efficiency of the thin-film battery assembly. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0023] Figure 1 It is a layered schematic diagram of the thin-film battery assembly with high absorption rate of the present invention.
[0024] Markings in the figure: 1-front glass, 2-perovskite cell layer, 3-encapsulation layer, 4-back glass, 21-first transparent conductive layer, 22-first transmission layer, 23-perovskite absorption layer, 24-buffer layer, 25-second transmission layer, 26-second transparent conductive layer. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In the description of the present invention, it should be understood that the terms "upper", "lower", "left", "right", "top", "bottom", etc., indicating the position or positional relationship, are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Moreover, the terms "first", "second", etc. are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein.
[0027] Example 1
[0028] like Figure 1 As shown, a thin-film battery assembly with high absorption rate is provided, which includes a front glass 1, a perovskite battery layer 2, a packaging layer 3 and a back glass 4 which are stacked in sequence, and the perovskite battery layer 2 is stacked on the opposite side of the light incident surface of the front glass 1;
[0029] The perovskite battery layer 2 is formed by stacking a first transparent conductive layer 21, a first transmission layer 22, a perovskite absorption layer 23, a buffer layer 24, a second transmission layer 25 and a second transparent conductive layer 26 in sequence; the first transparent conductive layer 21 is arranged on the opposite side of the light incident surface of the front glass 1, and the refractive index of the first transparent conductive layer 21 is set to 1.8; the refractive index of the perovskite absorption layer 23 is set to 2.6; the thickness of the first transparent conductive layer 21 is set to 160nm, and the thickness of the perovskite absorption layer 23 is set to 500nm; by accurately matching the thickness of the first transparent conductive layer 21 and the perovskite absorption layer 23, it is ensured that the absorption rate of the thin film battery assembly is greater than 90%.
[0030] The method for manufacturing a thin-film battery assembly with a high absorption rate provided in the above-mentioned embodiment 1 comprises the following specific steps:
[0031] S1, depositing TCO thin film material on the opposite side of the light incident surface of the front glass 1 by magnetron sputtering, and performing P1 laser scribing on it after deposition to form a plurality of first transparent conductive layers 21 with a thickness of 160 nm;
[0032] S2. Forming a first transmission layer 22 with a thickness of 35 nm on the first transparent conductive layer 21 by using a vacuum coating device, wherein the material of the first transmission layer 22 is NiOx;
[0033] S3, after annealing / drying the first transmission layer 22, a 500 nm thick perovskite absorption layer 23 is coated thereon, the chemical formula of perovskite is ABX3, where A represents Cs + 、CH3NH3 + and HNCH(NH2) 2+ The positive ion selected from the group consisting of 2+ Sn 2+ The positive ion selected from the group consisting of - and I - Negative ions selected from the group consisting of;
[0034] S4, after annealing / drying the perovskite absorption layer 23, a buffer layer 24 with a thickness of 30 nm is formed thereon by evaporation, wherein the material of the buffer layer 24 is fullerene (C60);
[0035] S5, continue to anneal / dry the buffer layer 24, and then form a second transmission layer 25 with a thickness of 12 nm thereon, wherein the second transmission layer 25 is made of TiO2;
[0036] S6, annealing / drying the second transmission layer 25, and then performing P2 laser scribing to form a plurality of perovskite sub-cells, and then using RPD equipment to prepare a second transparent conductive layer 26 (ITO material) with a thickness of 165 nm on the second transmission layer 25, and continuing to perform P3 laser scribing and P4 edge cleaning to form a perovskite thin film battery assembly with sub-cells connected in series;
[0037] S7. The leads form a circuit loop, and the packaging layer 3 and the back glass 4 are laid for lamination to obtain a thin film battery assembly with high absorption rate. The light absorption rate of the obtained thin film battery assembly is 90.21%.
[0038] Example 2
[0039] Provided is a thin-film battery assembly with a high absorption rate, the thin-film battery assembly comprising a front glass 1, a perovskite battery layer 2, an encapsulation layer 3 and a back glass 4 which are stacked in sequence, and the perovskite battery layer 2 is stacked on the opposite side of the light incident surface of the front glass 1;
[0040] The perovskite battery layer 2 is composed of a first transparent conductive layer 21, a first transmission layer 22, a perovskite absorption layer 23, a buffer layer 24, a second transmission layer 25 and a second transparent conductive layer 26 stacked in sequence; the thickness of the first transparent conductive layer 21 is set to 180nm, and the thickness of the perovskite absorption layer 23 is set to 410nm; the absorption rate of the thin film battery assembly is 90.57%.
[0041] The difference between Example 2 and Example 1 is that the thickness settings of the first transparent conductive layer 21 and the perovskite absorption layer 23 in Example 2 are different from those in Example 1, and the rest are the same.
[0042] Example 3
[0043] Provided is a thin-film battery assembly with a high absorption rate, the thin-film battery assembly comprising a front glass 1, a perovskite battery layer 2, an encapsulation layer 3 and a back glass 4 which are stacked in sequence, and the perovskite battery layer 2 is stacked on the opposite side of the light incident surface of the front glass 1;
[0044] The perovskite battery layer 2 is composed of a first transparent conductive layer 21, a first transmission layer 22, a perovskite absorption layer 23, a buffer layer 24, a second transmission layer 25 and a second transparent conductive layer 26 stacked in sequence; the thickness of the first transparent conductive layer 21 is set to 205nm, and the thickness of the perovskite absorption layer 23 is set to 595nm; the absorption rate of the thin film battery assembly is 91.16%.
[0045] The difference between Example 3 and Example 1 is that the thickness settings of the first transparent conductive layer 21 and the perovskite absorption layer 23 in Example 3 are different from those in Example 1, and the rest are the same.
[0046] Example 4
[0047] Provided is a thin-film battery assembly with a high absorption rate, the thin-film battery assembly comprising a front glass 1, a perovskite battery layer 2, an encapsulation layer 3 and a back glass 4 which are stacked in sequence, and the perovskite battery layer 2 is stacked on the opposite side of the light incident surface of the front glass 1;
[0048] The perovskite battery layer 2 is composed of a first transparent conductive layer 21, a first transmission layer 22, a perovskite absorption layer 23, a buffer layer 24, a second transmission layer 25 and a second transparent conductive layer 26 stacked in sequence; the thickness of the first transparent conductive layer 21 is set to 215nm, and the thickness of the perovskite absorption layer 23 is set to 635nm; the absorption rate of the thin film battery assembly is 90.93%.
[0049] The difference between Example 4 and Example 1 is that the thickness settings of the first transparent conductive layer 21 and the perovskite absorption layer 23 in Example 4 are different from those in Example 1, and the rest are the same.
[0050] Example 5
[0051] Provided is a thin-film battery assembly with a high absorption rate, the thin-film battery assembly comprising a front glass 1, a perovskite battery layer 2, an encapsulation layer 3 and a back glass 4 which are stacked in sequence, and the perovskite battery layer 2 is stacked on the opposite side of the light incident surface of the front glass 1;
[0052] The perovskite battery layer 2 is composed of a first transparent conductive layer 21, a first transmission layer 22, a perovskite absorption layer 23, a buffer layer 24, a second transmission layer 25 and a second transparent conductive layer 26 stacked in sequence; the thickness of the first transparent conductive layer 21 is set to 180nm, and the thickness of the perovskite absorption layer 23 is set to 580nm; the absorption rate of the thin film battery assembly is 92.24%.
[0053] The difference between Example 5 and Example 2 is that the thickness setting of the perovskite absorption layer 23 in Example 5 is different from that in Example 2, and the rest are the same.
[0054] It can be seen from the data of Example 5 and Example 2 that within the matching range of the thickness of the first transparent conductive layer 21 and the perovskite absorption layer 23, as the thickness of the perovskite absorption layer 23 increases, the absorption rate of the thin film battery assembly will also increase.
[0055] Comparative Example 1
[0056] The difference between Comparative Example 1 and Example 1 is that in Comparative Example 1, the thickness of the first transparent conductive layer 21 is set to 150 nm, the thickness of the perovskite absorption layer 23 is set to 500 nm, and the rest is the same as Example 1; the absorption rate of the thin film battery assembly of Comparative Example 1 is 88.93%.
[0057] Comparative Example 2
[0058] The difference between Comparative Example 2 and Example 1 is that in Comparative Example 2, the thickness of the first transparent conductive layer 21 is set to 160 nm, the thickness of the perovskite absorption layer 23 is set to 680 nm, and the rest is the same as Example 1; the absorption rate of the thin film battery assembly of Comparative Example 2 is 88.54%.
[0059] Comparative Example 3
[0060] In Comparative Example 3, the thickness of the first transparent conductive layer 21 is set to 230 nm, the thickness of the perovskite absorption layer 23 is set to 680 nm, and the rest is the same as in Example 1; the absorption rate of the thin film battery assembly of Comparative Example 3 is 89.04%.
[0061] It can be seen from the absorption rates of the thin film battery assemblies of Comparative Examples 1 to 3 that since the thickness of the first transparent conductive layer 21 and the thickness of the perovskite absorption layer 23 in Comparative Examples 1 to 3 were not optimized for depth matching, their absorption rates decreased significantly.
[0062] The present invention adjusts the thickness of the first transparent conductive layer and the perovskite absorption layer to accurately match the thickness of the two, thereby improving the light utilization rate of the thin-film battery component and effectively improving the photoelectric conversion efficiency of the thin-film component.
[0063] The above are preferred embodiments of the present invention and are only used to explain the present invention, not to limit the present invention. Any obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A thin-film battery assembly with high absorption rate, characterized in that: The thin-film battery assembly comprises a front glass (1), a perovskite battery layer (2), a packaging layer (3) and a back glass (4) which are stacked in sequence, and the perovskite battery layer (2) is stacked on the side opposite to the light incident surface of the front glass (1); the absorption rate of the thin-film battery assembly is greater than 90%; The perovskite cell layer (2) is formed by stacking a first transparent conductive layer (21), a first transmission layer (22), a perovskite absorption layer (23), a buffer layer (24), a second transmission layer (25) and a second transparent conductive layer (26) in sequence; the first transparent conductive layer (21) is arranged on the side opposite to the light incident surface of the front glass (1), and the refractive index of the first transparent conductive layer (21) is set to 1.7-1.85; the refractive index of the perovskite absorption layer (23) is set to 2.5-2.7; Wherein, when the thickness of the first transparent conductive layer (21) is set to 160-170 nm, the thickness of the perovskite absorption layer (23) is set to 500-650 nm; When the thickness of the first transparent conductive layer (21) is set to 171-200 nm, the thickness of the perovskite absorption layer (23) is set to 400-600 nm; When the thickness of the first transparent conductive layer (21) is set to 201-210 nm, the thickness of the perovskite absorption layer (23) is set to 500-750 nm; When the thickness of the first transparent conductive layer (21) is set to 211-220 nm, the thickness of the perovskite absorption layer (23) is set to 600-850 nm.
2. A thin-film battery assembly with high absorption rate according to claim 1, characterized in that: The refractive index of the first transmission layer (22) is set to 1.6-1.75, and the thickness is set to 30-50 nm. The first transmission layer (22) is made of NiOx or MoO3.
3. A thin-film battery assembly with high absorption rate according to claim 1, characterized in that: The refractive index of the buffer layer (24) is set to 2.1-2.4, and the thickness thereof is set to 20-40 nm.
4. A thin-film battery assembly with high absorption rate according to claim 1, characterized in that: The refractive index of the second transmission layer (25) is set to 1.8-2.0, the thickness is set to 8-15 nm, and the material is TiO2 or SnO2.
5. A thin-film battery assembly with high absorption rate according to claim 1, characterized in that: The refractive index of the second transparent conductive layer (26) is set to 1.9-2.0, the thickness is set to 160-180 nm, and the material is ITO, FTO or AZO.
6. A method for manufacturing a thin-film battery assembly with high absorption rate according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: S1, depositing a TCO thin film material on the opposite side of the light incident surface of the front glass (1) by means of magnetron sputtering, and then performing P1 laser scribing on the material to form the first transparent conductive layer (21); S2, forming the first transmission layer (22) on the first transparent conductive layer (21) by using a vacuum coating device; S3, after annealing / drying the first transmission layer (22), coating the first transmission layer (22) thereon to form the perovskite absorption layer (23); S4, after annealing / drying the perovskite absorption layer (23), evaporating the buffer layer (24) thereon; S5, continuing to anneal / dry the buffer layer (24), and then forming the second transmission layer (25) thereon; S6, annealing / drying the second transmission layer (25), performing P2 laser scribing to form a plurality of perovskite sub-cells, and then preparing a second transparent conductive layer (26) on the second transmission layer (25) using an RPD device, and continuing to perform P3 laser scribing and P4 edge cleaning to form a perovskite thin film battery assembly in which the sub-cells are connected in series; S7. After the leads form a circuit loop, the packaging layer (3) and the back glass (4) are laid and laminated to obtain a thin-film battery assembly with a high absorption rate.