Solder alloy, bonded power, bonded material, solder paste, bonded structure, and
By adjusting the proportions of Bi, Sb and Ag in the solder alloy and adding specific elements to form fine intermetallic compounds, the problem of the solder alloy's resistance to thermal cycles and drop impacts is solved, and the high heat resistance of the joint is achieved. Cycling resistance and drop impact resistance avoid peeling and cracking.
Patent Information
- Application Number
- CN202380016098.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-24
- Publication Date
- 2024-10-08
AI Technical Summary
Existing solder alloys are prone to thermal fatigue damage, cracks and peeling under repeated thermal cycles and drop impacts, and Bi reduces ductility, resulting in uneven joint strength and ductility, making it difficult to prevent external force damage.
A solder alloy composed of 35-65 mass% Bi, 0.1-0.65 mass% Sb, 0.05-2 mass% Ag and the balance Sn is used, and P, Ga and Ge are added to the joining material and solder paste. , Mn, Ti, Al, Cr, V, Fe, Mg, Pd, Pb, Mo and other elements to form fine intermetallic compounds to improve thermal cycle resistance and drop impact resistance.
While containing Bi, it significantly improves the thermal cycle resistance and drop impact resistance of the joint, suppresses the occurrence of cracks and peeling, provides balanced strength and ductility, and enhances the reliability of the joint.
Smart Images

Figure CN118748957A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a solder alloy, a joint portion, a joint material, a solder paste, a joint structure and an electronic control device. Background Art
[0002] The joining conditions of the materials to be joined (for example, a printed circuit board and electronic components), such as the heating temperature and heating time, are set according to the purpose of the electronic device and the material and heat resistance of the components constituting the electronic device. Usually, a solder alloy that melts below the set heating temperature is used as the joining material.
[0003] Furthermore, as a method of lowering the melting temperature (in this specification, "melting point" or "liquidus temperature") of the solder alloy, a method of adding Bi to the solder alloy is provided. However, Bi is hard and brittle, and therefore reduces the ductility of the solder alloy.
[0004] Therefore, as a solder alloy containing Bi with improved ductility, for example, the following solder alloy is provided.
[0005] A solder alloy characterized by having the following alloy composition: in terms of mass %, Bi: 35-68%, Sb: 0.1-2.0%, Ni: 0.01-0.10%, and the balance being Sn (Patent Document 1).
[0006] A lead-free solder alloy comprising: 32 mass % or more and 40 mass % or less of Bi, 0.1 mass % or more and 1.0 mass % or less of Sb, 0.1 mass % or more and 1.0 mass % or less of Cu, 0.001 mass % or more and 0.1 mass % or less of Ni, the balance consisting of Sn and unavoidable impurities (Patent Document 2).
[0007] A SnBiSb-based low-temperature lead-free solder, characterized in that the lead-free solder is composed of 32.8-56.5% Bi, 0.7-2.2% Sb, and the remainder Sn in mass percentage, and the mass percentages of Bi and Sb satisfy the relationship b=0.006a2-0.672a+19.61+c, a represents the mass percentage of Bi, b represents the mass percentage of Sb, and c is in the range of -1.85≤c≤1.85. It also contains one or more metal elements of 0.01-2.5% Ce, 0.05-2.0% Ti, 0.5-0.8% Ag, and 0.05-1% In in mass percentage (Patent Document 3).
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent No. 6477965
[0011] Patent Document 2: Japanese Patent No. 6804126
[0012] Patent Document 3: Japanese Patent No. 6951438 Summary of the invention
[0013] Problem that the invention aims to solve
[0014] Depending on the type of electronic device, the joint structure (in this specification, a structure in which a plurality of joined materials are joined via a joint) in the electronic device is sometimes placed in an environment of repeated thermal cycles. This thermal cycle causes thermal fatigue damage (cracks) in the joint. Moreover, as mentioned above, Bi reduces the ductility of the solder alloy, so the above-mentioned cracks are easily generated in the joint formed by the solder alloy containing Bi.
[0015] In addition, if an electronic device is subjected to a strong impact caused by falling or the like, a strong external force will be applied to the joined materials and the joints instantly and concentratedly. In order to prevent the joints from being damaged by the external force, it is necessary to improve the strength and ductility of the solder alloy in a well-balanced manner. However, as mentioned above, Bi reduces the ductility of the solder alloy, and therefore, in the joints formed by the solder alloy containing Bi, damage caused by the external force mentioned above is easily generated.
[0016] In addition, when using an electronic component with a terminal as a material to be joined, the following method (through-hole mounting method) is used: a through-hole is provided in the printed circuit board, the terminal of the electronic component is inserted into the through-hole, and the two are joined, and the terminal of the electronic component in the through-hole is joined to the pad (electrode) of the printed circuit board with the aid of a joining portion (solder fillet) formed on the printed circuit board.
[0017] In this joining method, the molten solder solidifies from the through-hole side to the printed circuit board side when cooling, so the residual stress in the formed joint is easily concentrated on the pad side. In addition, the printed circuit board also shrinks thermally in the longitudinal direction. Therefore, in this case, it is easy to produce the phenomenon that the joint will peel off from the pad (peeling). This peeling is particularly easy to occur when a solder alloy containing Bi is used for joining.
[0018] Moreover, Patent Documents 1 to 3 neither disclose nor suggest a solder alloy having resistance to the above-mentioned cracks (hereinafter referred to as "thermal cycle resistance" in this specification) and resistance to the above-mentioned external forces (hereinafter referred to as "drop impact resistance" in this specification) and suppressing the occurrence of peeling.
[0019] An object of the present invention is to solve the above-mentioned problems and to provide a solder alloy, a bonding material, and a solder paste that can form a bonding portion that contains Bi and has heat cycle resistance and drop impact resistance and suppresses the occurrence of peeling.
[0020] Solutions for solving problems
[0021] (1) The solder alloy of the present invention contains 35 mass % to 65 mass % of Bi, 0.1 mass % to 0.65 mass % of Sb, and 0.05 mass % to 2 mass % of Ag, with the balance being Sn and unavoidable impurities.
[0022] (2) The solder alloy of the present invention preferably further contains 0.001 mass % or more and 0.05 mass % or less in total of one or more selected from the group consisting of P, Ga, and Ge.
[0023] (3) The solder alloy of the present invention preferably further contains at least one selected from the group consisting of Mn, Ti, Al, Cr, V, Fe, Mg, Pd, Pb and Mo in an amount of 0.001 mass % to 0.05 mass % in total.
[0024] (4) The bonding material of the present invention includes the solder alloy described in any one of (1) to (3) above.
[0025] (5) The solder paste of the present invention comprises: the solder alloy according to any one of (1) to (3) above in powder form; and a flux containing a base resin, a thixotropic agent, an activator, and a solvent.
[0026] (6) The joint portion of the present invention is formed of the solder alloy described in any one of (1) to (3) above.
[0027] (7) The joining portion of the present invention is formed of the joining material described in (4) above.
[0028] (8) The bonding portion of the present invention is formed by the solder paste described in (5) above.
[0029] (9) The joining structure of the present invention comprises: a first material to be joined, a joining portion and a second material to be joined, wherein the joining portion is the joining portion described in any one of (6) to (8) above, and the first material to be joined and the second material to be joined are joined by means of the joining portion.
[0030] (10) The electronic control device of the present invention includes the joint structure described in (9) above.
[0031] Effects of the Invention
[0032] The solder alloy, the bonding material, and the solder paste of the present invention can form a bonding portion which contains Bi, has heat cycle resistance and drop impact resistance, and can suppress the occurrence of peeling. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 (1) This is a plan view showing the shape of a test piece used in the tensile test. DETAILED DESCRIPTION
[0034] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to the following embodiments.
[0035] 1. Solder alloy
[0036] The solder alloy of the present embodiment contains 35 mass % to 65 mass % of Bi, 0.1 mass % to 0.65 mass % of Sb, and 0.05 mass % to 2 mass % of Ag, with the balance being Sn and inevitable impurities.
[0037] The solder alloy of the present embodiment contains Bi, Sb, Ag, and Sn in predetermined amounts, respectively, so that the strength and ductility of the solder alloy can be improved in a well-balanced manner while containing Bi.
[0038] Therefore, the solder alloy of the present embodiment can suppress plastic deformation and sliding deformation at the crack tip even when cracks due to repeated thermal cycles occur in the joint and stress concentrates in the cracks, thereby suppressing crack propagation.
[0039] In addition, the solder joint of the present embodiment can thereby suppress damage to the joint portion caused by the instantaneous and concentrated strong external force (hereinafter simply referred to as "external force") acting on the joint portion due to the falling of the electronic device, etc.
[0040] As mentioned above, in order to suppress the development of cracks generated in the joint, it is important that the joint is not prone to plastic deformation and sliding deformation. On the other hand, the joint that is not prone to plastic deformation absorbs less impact energy generated by the above external force, and the impact energy that is not completely absorbed will damage the joint. In addition, the above external force acts on the joint from multiple directions (at least two of tension, compression, shear, bending and twisting).
[0041] Therefore, in order to prevent the damage of the joint caused by the impact energy / stress of the external force, it is required to improve the balance between the strength and ductility of the solder alloy, that is, to improve the yield stress, tensile stress and fracture strain of the joint in a balanced manner. Moreover, as described above, the solder alloy of the present embodiment can form a joint with good strength and ductility in a balanced manner through the above-mentioned configuration, so that a joint with good resistance to the external force, that is, good resistance to drop impact, can be provided.
[0042] In addition, the solder alloy of the present embodiment can thereby easily relax the residual stress generated in the joint when the solder solidifies, and can suppress the occurrence of cracks in the joint due to the residual stress and the above-mentioned peeling.
[0043] (1)Bi
[0044] The solder alloy of this embodiment contains Bi in an amount of 35% by mass or more and 65% by mass or less. This lowers the melting temperature of the solder alloy and suppresses the reduction in ductility of the solder alloy. In addition, the solid solution of Bi in Sn can strengthen the joint, thereby improving the strength and ductility of the joint in a well-balanced manner.
[0045] On the other hand, when the Bi content is out of the above range, there is a concern that the strength and ductility of the solder alloy may be reduced.
[0046] The preferred content of Bi is 35% by mass or more and 60% by mass or less. In addition, the further preferred content of Bi is 40% by mass or more and 59% by mass or less. The preferred content of Bi can be set to 50% by mass or more, or 54% by mass or more, or can be set to 58% by mass or less, 56.5% by mass or less, or 56% by mass or less. By making the content of Bi within this range, the ductility and strength of the joint can be further improved.
[0047] (2) Sb
[0048] The solder alloy of this embodiment contains Sb in an amount of not less than 0.1 mass % and not more than 0.65 mass %. Thus, the solid solution strengthening of the joint is achieved by the solid solution of Sb in Sn, and the strengthening and ductility of the joint can be improved by the precipitation and dispersion of fine β-SnSb intermetallic compounds, thereby improving the strength and ductility of the joint in a well-balanced manner.
[0049] On the other hand, when the Sb content is less than 0.1 mass %, there is a concern that the strengthening of the joint becomes insufficient. In addition, when the Sb content exceeds 0.65 mass %, coarse β-SnSb intermetallic compounds as primary crystals crystallize, thereby hindering the ductility of the joint.
[0050] The preferred content of Sb is 0.2 mass % or more and 0.65 mass % or less. In addition, the more preferred content of Sb is 0.3 mass % or more and 0.65 mass % or less. By making the content of Sb within this range, the ductility and strength of the joint can be further improved.
[0051] (3) Ag
[0052] The solder alloy of this embodiment contains Ag in an amount of not less than 0.05 mass % and not more than 2 mass %. Thus, the melting temperature of the solder alloy is lowered, and the strengthening and ductility of the joint can be improved by precipitation and dispersion of fine Ag3Sn intermetallic compounds, thereby improving the strength and ductility of the joint in a well-balanced manner.
[0053] On the other hand, if the Ag content is less than 0.05 mass %, there is a concern that precipitation strengthening of the joint may become insufficient. In addition, if the Ag content exceeds 2 mass %, the Ag3Sn intermetallic compound coarsens, thereby hindering the ductility of the joint.
[0054] The preferred content of Ag is 0.1 mass % or more and 1.5 mass % or less. The preferred content of Ag can be set to 1 mass % or less, 0.8 mass % or less, or 0.5 mass % or less. In addition, the further preferred content of Ag is 0.2 mass % or more and 0.4 mass % or less. By making the content of Ag within this range, the ductility and strength of the joint can be further improved.
[0055] The solder alloy of the present embodiment may further contain a total of 0.001 mass % or more and 0.05 mass % or less of one or more selected from the group of P, Ga and Ge. By adding one or more selected from the group of P, Ga and Ge to the solder alloy, oxidation of the solder alloy can be suppressed, and wettability of the solder alloy can be improved, thereby providing a highly reliable joint.
[0056] On the other hand, if the total content of one or more selected from the group consisting of P, Ga, and Ge exceeds 0.05 mass %, voids may be generated in the joint portion, and the thermal cycle resistance of the joint portion may be deteriorated.
[0057] The solder alloy of the present embodiment may further contain 0.001 mass % to 0.05 mass % in total of one or more selected from the group consisting of Mn, Ti, Al, Cr, V, Fe, Mg, Pd, Pb, and Mo.
[0058] By adding one or more selected from the group consisting of Mn, Ti, Al, Cr, V, Fe, Mg, Pd, Pb and Mo to the solder alloy, the intermetallic compounds in the joint are further refined, so the progress of cracks can be suppressed and good thermal cycle resistance can be achieved. On the other hand, if the total content of one or more selected from the group consisting of Mn, Ti, Al, Cr, V, Fe, Mg, Pd, Pb and Mo exceeds 0.05 mass%, voids are generated in the joint, and there is a concern that the thermal cycle resistance will deteriorate.
[0059] In addition, when Fe is added to the solder alloy of the present embodiment, if the Fe content exceeds 0.05 mass %, there is a concern that needle-shaped substances are easily generated in the solder alloy during the manufacturing process of the solder alloy. Here, when the solder alloy containing the needle-shaped substance is pulverized into a spherical shape, the presence of the needle-shaped substance hinders the spherical shape, and therefore, there is a concern that the spherical shape pulverization becomes difficult.
[0060] The solder alloy of the present embodiment has a balance consisting of Sn and inevitable impurities. That is, the solder alloy of the present embodiment may contain alloy elements other than the above-mentioned alloy elements as inevitable impurities.
[0061] 2. Bonding materials
[0062] The bonding material of the present embodiment includes the solder alloy of the present embodiment, and can be used in the form of solder paste, solder ball, wire, preformed solder, core solder, etc. The form of the bonding material can be appropriately selected according to the size, type and use of the materials to be bonded, the solder bonding method, etc.
[0063] Furthermore, the bonding material of the present embodiment includes the solder alloy of the present embodiment, and thus the melting temperature is lowered by adding Bi, and a bonding portion having heat cycle resistance and drop impact resistance and suppressing the occurrence of peeling can be formed.
[0064] 3. Solder paste
[0065] The solder paste of the present embodiment includes the solder alloy of the present embodiment in powder form (hereinafter referred to as “alloy powder”), and is produced, for example, by kneading the alloy powder and flux into a paste.
[0066] <Flux>
[0067] The aforementioned soldering flux may include, for example, a base resin, a thixotropic agent, an activator, and a solvent.
[0068] Examples of the base resin include rosin resins; acrylic resins obtained by polymerizing at least one monomer selected from acrylic acid, methacrylic acid, various esters of acrylic acid, various esters of methacrylic acid, crotonic acid, itaconic acid, maleic acid, maleic anhydride, maleic acid esters, maleic anhydride esters, acrylonitrile, methacrylonitrile, acrylamide, methacrylamide, vinyl chloride, vinyl acetate, etc.; epoxy resins; phenolic resins, etc. These can be used alone or in combination.
[0069] Examples of the thixotropic agent include hydrogenated castor oil, hydrogenated castor oil, bisamide thixotropic agents (saturated fatty acid bisamide, unsaturated fatty acid bisamide, aromatic bisamide, etc.), oxy fatty acids, dimethyldibenzylidene sorbitol, etc. These may be used alone or in combination of two or more.
[0070] Examples of the activator include organic acids (monocarboxylic acids, dicarboxylic acids, and other organic acids), halogen-containing compounds, and amine-based activators, etc. These may be used alone or in combination of two or more.
[0071] Examples of the solvent include alcohol-based, butyl cellosolve-based, glycol ether-based, and ester-based solvents, and these solvents may be used alone or in combination of two or more.
[0072] The soldering flux may contain an antioxidant, for example, a hindered phenol antioxidant, a phenol antioxidant, a bisphenol antioxidant, a polymer antioxidant, etc.
[0073] Furthermore, additives such as a matting agent and a defoaming agent may be added to the aforementioned flux.
[0074] When preparing the solder paste of the present embodiment, the alloy powder and flux blending ratio (mass %) can be 65:35 to 95:5 in terms of alloy powder:flux ratio. Alternatively, for example, the blending ratio can be 85:15 to 93:7 or 87:13 to 92:8.
[0075] It should be noted that the particle size of the alloy powder may be set to be 1 μm or more and 40 μm or less. Alternatively, the particle size may be set to be 5 μm or more and 35 μm or more and 10 μm or more and 30 μm or less. It should be noted that the particle size of the alloy powder may be changed as appropriate.
[0076] Furthermore, the solder paste of the present embodiment includes the alloy powder, and thus Bi is added to lower the melting temperature, and can form a joint portion having heat cycle resistance and drop impact resistance and suppressing the occurrence of peeling.
[0077] 4. Joint
[0078] The joining portion of the present embodiment is formed using the solder alloy of the present embodiment and a joining material (hereinafter, including solder paste unless otherwise specified) and joins materials to be joined.
[0079] The method for forming the joint portion of the present embodiment can be formed by using the solder alloy and the joint material of the present embodiment, and any method such as reflow soldering and flow soldering can be adopted. In addition, the form of the joint material to be used can also be appropriately selected according to the size, type and purpose of the materials to be joined, and the method for forming the joint portion.
[0080] 5. Joining structures
[0081] The joined structure of the present embodiment includes a first material to be joined, a joining portion, and a second material to be joined. The joining portion is a joining portion of the present embodiment, and the first material to be joined and the second material to be joined are joined via the joining portion.
[0082] As the first material to be joined and the second material to be joined, for example, a substrate (a surface formed of any of ceramic, metal, alloy or resin, and not formed with an electronic circuit), a printed circuit board (a substrate formed with an electronic circuit, and not equipped with electronic components, etc.), a printed circuit board (a printed circuit board equipped with electronic components, etc.), an electronic component, a silicon wafer, a semiconductor package, a semiconductor chip, etc. can be used. Different types of materials to be joined can be combined, and the same type of materials to be joined can also be combined.
[0083] Specific examples of the combination include a printed circuit board and an electronic component, a printed circuit board and a semiconductor chip, a semiconductor package and a printed circuit board, and a printed circuit board and a printed circuit board.
[0084] In addition, the joined structure of the present embodiment is produced, for example, by the following method.
[0085] When a printed circuit board is used as the first material to be joined and an electronic component is used as the second material to be joined, first, the joining material of the present embodiment is placed (applied in the case of solder paste) at a predetermined position of the first material to be joined, such as an electronic circuit, and the second material to be joined is placed on the joining material. Then, they are reflowed at a predetermined heating temperature, such as a peak temperature of 200°C, to form a joining portion where the first material to be joined is joined to the second material to be joined. Thus, the joining structure (printed circuit board) of the present embodiment can be manufactured.
[0086] It should be noted that when using a preform solder as the aforementioned joining material, the preform solder with flux applied on the surface is placed at a predetermined position of the aforementioned first joining material, and the aforementioned second joining material is placed on the aforementioned preform solder and heated.
[0087] In addition, when an electronic component having solder balls such as a Ball Grid Array (BGA) is used as the second material to be joined, solder paste is applied to the surface of the BGA and at a specified position of the first material to be joined, and the second material to be joined is placed on a specified position of the first material to be joined and heated.
[0088] Then, the bonded structure of the present embodiment has the bonded portion of the present embodiment. Thus, the bonded structure of the present embodiment has heat cycle resistance and drop impact resistance, and is less likely to peel off, thereby maintaining high reliability.
[0089] 6. Electronic control device
[0090] The electronic control device of the present embodiment includes the joint structure of the present embodiment, and is formed by placing a printed circuit board in which an electronic component and a printed circuit board are joined, for example, in a casing, and controls the operation of components constituting the electronic device.
[0091] Furthermore, the electronic control device of the present embodiment includes the joint structure of the present embodiment. Therefore, the electronic control device of the present embodiment has heat cycle resistance and drop impact resistance, and is less likely to peel off, thereby maintaining high reliability.
[0092] Example
[0093] Hereinafter, the present invention will be described in detail with reference to Examples and Comparative Examples, but it should be noted that the present invention is not limited to these Examples.
[0094] [Table 1]
[0095]
[0096] [Table 2]
[0097]
[0098] [Table 3]
[0099]
[0100] (1) Tensile test
[0101] For each solder alloy shown in Tables 1 to 3, Figure 1 The test piece 10 is shown.
[0102] It should be noted that the test piece 10 is parallel to the central part ( Figure 1 between G1 and G2) is produced in the following manner.
[0103] · Length of the central parallel section ( Figure 1 L): 12mm
[0104] Width of the central parallel section ( Figure 1 W): 2mm
[0105] ·Thickness of central parallel part: 4mm
[0106] Then, a tensile test was performed on the test piece 10 according to the following procedure.
[0107] The test piece 10 was stretched in the X direction at room temperature with a stroke of 0.72 mm / min until it broke using a desktop precision universal testing machine (product name: Autograph AG-50kNX plus, manufactured by Shimadzu Corporation).
[0108] Then, the elongation of the test piece 10 was calculated based on the following formula, with the stroke distance when the test piece 10 was broken being GL1 and the length L of the central parallel portion of the test piece before being stretched being GL0.
[0109] Elongation (%) = (GL1-GL0) / GL0×100
[0110] Five test pieces 10 were prepared for one solder alloy, and the elongation and the average value of the elongation were calculated according to the above-mentioned procedure, and the test pieces were evaluated based on the following criteria. The results are shown in Tables 4 to 6.
[0111] ◎: The average elongation is 35% or more
[0112] ○: The average elongation is 30% or more and less than 35%
[0113] △: The average elongation is 25% or more and less than 30%
[0114] ×: The average elongation is less than 25%
[0115] (2) Drop impact test
[0116] The fluxes kneaded with the following components were kneaded with solder alloy powders (powder particle size 20 μm to 38 μm) shown in Tables 1 to 3 at the following blending ratios (mass %) to prepare solder pastes. The solder alloy powders were prepared by an atomization method.
[0117] Solder alloy powder: flux = 89:11
[0118] <Composition of flux>
[0119] Hydrogenated acid-modified rosin (product name: KE-604, manufactured by Arakawa Chemical Industries, Ltd.): 49 mass%
[0120] · Surfactant (glutaric acid: 0.3 mass%, suberic acid: 2 mass%, malonic acid: 0.5 mass%, dodecanedioic acid: 2 mass%, dibromobutylene glycol: 2 mass%)
[0121] Fatty acid amide (product name: SLIPAX ZHH, manufactured by Nippon Chemical Industries, Ltd.): 6% by mass
[0122] ·Diethylene glycol monohexyl ether: 35.2 mass%
[0123] Hindered phenol antioxidant (product name: Irganox 245, manufactured by BASF Japan): 3% by mass
[0124] In addition, prepare the following tools.
[0125] LGA (Land Grid Array, pitch width: 0.5mm, size: length 12mm × width 12mm × thickness 1mm, number of terminals: 228 pins)
[0126] Glass epoxy substrate (base material: FR-4, surface treatment: Cu-OSP, thickness: 1.0mm, with pattern that can mount the above LGA)
[0127] Metal mask (thickness: 100 μm, corresponding to the above pattern)
[0128] For each solder paste, 5 sheets of the aforementioned glass epoxy substrates and 20 LGAs were used.
[0129] Then, using the above-mentioned tools and each solder paste, each test substrate was prepared according to the following procedure, and a drop impact test was performed.
[0130] First, solder paste is printed on a glass epoxy substrate using a metal mask. Then, four LGAs are placed on one glass epoxy substrate at predetermined positions on the printed solder paste. It should be noted that the printed film thickness of the solder paste is adjusted according to the metal mask.
[0131] Then, the glass epoxy substrate on which the LGA was mounted was reflowed in a reflow furnace (product name: TNV-M6110CR, manufactured by TAMURA Corporation) to prepare a test substrate having the LGA, the glass epoxy substrate, and a joint portion where these were joined.
[0132] It should be noted that the reflow soldering is as follows: preheating is set to 100°C to 120°C, peak temperature is set to 200°C, time above 150°C is set to 60 seconds, cooling rate from peak temperature to 100°C is set to 1°C to 4°C / second. In addition, oxygen concentration is set to 200±100 ppm.
[0133] Next, a drop impact test was performed on the prepared test substrate under the following conditions using a drop impact tester (product name: HDST-150J, SHINYEI Technology Co., Ltd.).
[0134] That is, according to JEDEC standard JESD22-B111, the test substrate is repeatedly dropped freely from a height with a shock waveform of 1500G acceleration and 0.5ms width. During the drop shock test, the resistance of each joint of the test substrate is observed at any time, and when the resistance value exceeds 1000Ω, it is judged to be broken, and the number of drops until the break is measured.
[0135] It should be noted that 5 test substrates were prepared for each solder paste, and for a total of 20 LGAs, the above measurement results were plotted as Weibull curves, and the number of drops at a cumulative failure rate of 63.2% was estimated as the characteristic life, and the evaluation was performed according to the following criteria. The results are shown in Tables 4 to 6.
[0136] ◎: Characteristic life is more than 110 times
[0137] ○: Characteristic life is 90 times or more and less than 110 times
[0138] △: Characteristic life is 70 times or more and less than 90 times
[0139] ×: Characteristic life is less than 70 times
[0140] (3) Thermal cycle test
[0141] Prepare the following utensils.
[0142] Chip components (3.2mm×1.6mm)
[0143] Glass epoxy substrate (base material: FR-4, surface treatment: Cu-OSP, thickness: 1.2mm, with pattern that can mount the above chip components)
[0144] Metal mask (thickness: 120 μm, corresponding to the above pattern)
[0145] For each solder paste, three sheets of the aforementioned glass epoxy substrates and 30 chip components were used.
[0146] Then, using the above-mentioned tools and each solder paste, each test substrate was prepared according to the following procedure and a heat cycle test was performed.
[0147] First, solder paste is printed on a glass epoxy substrate using a metal mask. Then, 10 chip components are placed on one glass epoxy substrate at predetermined positions on the printed solder paste. It should be noted that the printed film thickness of the solder paste is adjusted according to the metal mask.
[0148] Then, the glass epoxy substrate on which the chip components were mounted was reflowed in a reflow furnace (product name: TNV-M6110CR, manufactured by TAMURA Corporation) to prepare three mounting substrates having the chip components, the glass epoxy substrate, and a junction between them.
[0149] It should be noted that the reflow soldering is as follows: preheating is set to 100°C to 120°C, peak temperature is set to 200°C, time above 150°C is set to 60 seconds, cooling rate from peak temperature to 100°C is set to 1°C to 4°C / second. In addition, oxygen concentration is set to 200±100 ppm.
[0150] Next, using a thermal shock tester (product name: ES-76LMS, manufactured by Hitachi Appliances Weibull Curve Techno Service, Ltd.), each mounted substrate was exposed to a thermal shock cycle as described below under the setting conditions of -40°C (30 minutes) to 125°C (30 minutes) as one cycle to produce test substrates a to c.
[0151] a: Test substrate exposed to the environment where the above thermal shock cycle is repeated 2000 times
[0152] b: Test substrate exposed to the environment where the above thermal shock cycle is repeated 2250 times
[0153] c: Test substrate exposed to the environment where the above thermal shock cycle is repeated 2500 times
[0154] The target portion of each of the test substrates a to c was cut out and sealed with an epoxy resin (product name: HERZOG Epo low-viscosity resin (main agent and curing agent), manufactured by HERZOG Co., Ltd.).
[0155] Then, a wet grinder (product name: TegraPol-25, manufactured by STRUERS) was used to form a state of the central cross section of each chip component mounted on each test substrate, and a scanning electron microscope (product name: TM-1000, manufactured by Hitachi High-Tech Corporation) was used to observe the state of each joint on each test substrate a to c, confirm the presence or absence of cracks that completely cross the joint, and evaluate according to the following criteria. The results are shown in Tables 4 to 6.
[0156] ◎: No cracks completely crossing the joint occurred in any of the test substrates a to c.
[0157] ○: In the test substrates a and b, no cracks completely crossing the joint occurred
[0158] △: In the test substrate a, no cracks completely crossing the joint occurred
[0159] ×: Cracks that completely penetrated the joint occurred in all of the test substrates a to c.
[0160] (5) Peeling Occurrence Confirmation Test
[0161] Prepare the following utensils.
[0162] ・Connector parts (Product name: S15B-EH (LF) (SN), manufactured by Nippon Terminal Manufacturing Co., Ltd.)
[0163] Glass epoxy substrate (base material: FR-4, surface treatment: Cu-OSP, size: 50 mm × 50 mm, thickness: 1.6 mm, with 1.6 mm diameter pads and 1.0 mm diameter through holes at 2.5 mm intervals)
[0164] A metal mask with a thickness of 200 μm and an opening pattern with a diameter of 3 mm at 5 mm intervals
[0165] Then, using the above-mentioned tools and each solder paste, each test substrate was prepared in the following steps, and a peeling occurrence confirmation test was performed.
[0166] First, solder paste was printed on a glass epoxy substrate using a metal mask. Then, the terminals of the connector components were inserted into the prescribed through holes provided in the glass epoxy substrate, and reflow was performed in a reflow oven (product name: TNP-538EM, manufactured by Tamura Manufacturing Co., Ltd.) to prepare a test substrate having a solder joint (solder fillet) connecting the connector component to the glass epoxy substrate. It should be noted that the reflow was performed under the same conditions as in the drop impact test (2).
[0167] Next, the target portion of each test substrate was cut out and sealed with an epoxy resin (product name: Epomount (main agent and curing agent), manufactured by Refine Tec Co., Ltd.). A wet grinder (product name: TegraPol-25, manufactured by Marumoto Struers Co., Ltd.) was further used to form a central cross-section of the terminal of each connector component installed on each test substrate, and the state was observed with a scanning electron microscope (product name: TM-1000, manufactured by Hitachi-High-Technologies-Corporation), and evaluated according to the following criteria. It should be noted that the number of evaluation terminals was set to 8. The results are shown in Tables 4 to 6.
[0168] ○: No peeling occurred
[0169] ×: Peeling occurs
[0170] (5) Needle-like substance generation confirmation test
[0171] A solder ingot made of each solder alloy was prepared. Then, solder alloy powder was prepared from each solder ingot under the following conditions.
[0172] First, 50 g of the solder ingot, 890 g of castor oil, and 10 g of hydrogenated acid-modified rosin (product name: KE-604, manufactured by Arakawa Chemical Industries, Ltd.) were placed in a 2 L stainless steel beaker and then continuously heated with a hooded heater.
[0173] When the temperature of the contents in the stainless steel beaker reached 100° C., stirring of the contents in the stainless steel beaker was started using a homogenizer (manufactured by SMT Co., Ltd.) at a rotation speed of 2000 rpm. During stirring, heating by the hooded heater was continued.
[0174] Then, when the temperature of the contents in the stainless steel beaker reached 200° C., heating was stopped, the rotation of the homogenizer was changed to 10,000 rpm, and the contents in the stainless steel beaker were stirred for 5 minutes. After the stirring was completed, the temperature of the contents in the stainless steel beaker was cooled to room temperature.
[0175] Then, the solder alloy powder precipitated in the castor oil was taken out from the stainless steel beaker, washed with ethyl acetate, and after removing the attached matter, the state of the solder alloy powder was observed with a digital microscope at 200 times. The observation results were evaluated based on the following criteria. The results are shown in Tables 4 to 6.
[0176] ○: No needle-like substances are generated in the solder alloy powder
[0177] ×: Needle-shaped substances were generated in the solder alloy powder [Table 4]
[0178]
[0179] [Table 5]
[0180]
[0181] [Table 6]
[0182]
[0183] As described above, the solder alloy of this embodiment contains Bi, Sb, Ag and Sn in predetermined amounts, thereby forming a joint portion that shows good results in any of the above (1) to (4) while containing Bi. In addition, the solder alloy of this embodiment can also suppress the generation of needle-shaped substances when Fe is added.
[0184] Here, the strain rate when the car collides with the object is said to be 10 -3 (s -1 )~10 3 (s -1 ). In addition, in the (1) tensile test, the test piece with a GL0 of 12 mm was stretched at a stroke of 0.72 mm / min, so when it is converted into a strain rate, it becomes 10 -3 (s -1 ).
[0185] As described above, it is found that the solder alloy of the present example can form a joint portion having excellent resistance, that is, excellent strength and ductility, even when a load comparable to the strain rate when a car collides with an object is applied.
[0186] As described above, the solder alloy of this embodiment can form a joint portion that contains Bi and has heat cycle resistance and drop impact resistance, and suppresses the occurrence of peeling. In addition, an electronic control device and an electronic device having such a joint portion can exhibit high reliability.
[0187] Description of Reference Numerals
[0188] 10 test pieces
Claims
1. A solder alloy comprising: 35 mass % or more and 65 mass % or less of Bi, 0.1 mass % or more and 0.65 mass % or less of Sb, and 0.05 mass % or more and 2 mass % or less of Ag, with the balance being Sn and unavoidable impurities. 2 . The solder alloy according to claim 1 , further comprising 0.001 mass % or more and 0.05 mass % or less in total of one or more selected from the group consisting of P, Ga and Ge.
3. The solder alloy according to claim 1 or claim 2, further comprising a total of 0.001 mass % to 0.05 mass % or less of one or more selected from the group consisting of Mn, Ti, Al, Cr, V, Fe, Mg, Pd, Pb and Mo. 4 . A bonding material comprising the solder alloy according to claim 1 .
5. A solder paste comprising: the solder alloy according to any one of claims 1 to 3 in powder form; and A flux containing a base resin, a thixotropic agent, an activator and a solvent. 6 . A joint portion formed of the solder alloy according to claim 1 . 7 . A joining portion formed of the joining material according to claim 4 .
8. A joint portion formed by the solder paste according to claim 5.
9. A joined structure comprising: a first joined material, a joining portion, and a second joined material, The joining portion is a joining portion as claimed in any one of claims 6 to 8, The first material to be joined and the second material to be joined are joined via the joining portion. 10 . An electronic control device comprising the joint structure according to claim 9 .