Metal soldering paste and preparation method and application thereof
By mixing the flocculant composition and the alloy powder composition in the metal solder paste, the solder paste delamination problem is solved, the uniformity and bonding strength of the welding are improved, and the quality of active metal brazing is improved.
Patent Information
- Application Number
- CN202410567903.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2024-10-22
AI Technical Summary
Existing metal solder pastes are prone to delamination after standing, resulting in poor welding uniformity and insufficient adhesive strength, affecting the quality of active metal soldering.
The binder composition containing flocculant is mixed with the alloy powder composition to form a bridge effect through the flocculant to solve the stratification problem caused by inconsistent powder settling speed and improve the uniformity and welding strength of the solder paste.
It effectively solves the problem of solder paste delamination, improves the uniformity and bonding strength of welding, and improves the quality and yield rate of active metal soldering.
Smart Images

Figure CN118808982A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding, and in particular to a metal solder paste and a preparation method and application thereof. Background Art
[0002] In the process of active metal brazing, the existing technology mostly uses traditional solder pastes such as silver, copper and titanium. Such traditional solder pastes contain a variety of metal particles (such as silver and copper). Due to the influence of the physical and chemical properties of different metal particles, the solder paste will be stratified after standing. Moreover, when the stratified solder paste is used in screen printing, the uniformity of the metal solder paste on the screen printing sheet is poor, and the bonding strength between the materials after welding is poor, that is, the quality of active metal brazing is poor and the yield rate is low. Therefore, how to solve the stratification of solder paste and improve the uniformity of solder paste in the process has become the key. Summary of the invention
[0003] The purpose of the present invention is to provide a metal solder paste and a preparation method and application thereof, so as to solve the problems of poor uniformity and welding strength of the existing metal solder paste.
[0004] To achieve the purpose of the present invention, the present invention provides the following technical solutions:
[0005] In a first aspect, the present invention provides a metal solder paste comprising an alloy powder composition and a binder composition, wherein the binder composition comprises a flocculant.
[0006] In one embodiment, in the metal solder paste, the alloy powder composition accounts for 80% to 90% by mass, and the binder composition accounts for 10% to 20% by mass.
[0007] In one embodiment, the flocculant includes one or more of polybasic long alkyl chain carboxylic acids and derivatives thereof, polybasic carboxylic acid polymers and copolymers thereof.
[0008] In one embodiment, in the binder composition, the flocculant accounts for 1% to 10% by mass.
[0009] In one embodiment, the binder composition further comprises, by weight percentage, 1% to 10% of a dispersant, 1% to 10% of a thickener, and 80% to 95% of a solvent.
[0010] In one embodiment, the dispersant includes one or two of stearic acid and polyethylene glycol, the thickener includes one or more of ethyl cellulose, polyvinyl alcohol, and acrylic resin, and the solvent includes one or more of pineneol, tributyl citrate, diethylene glycol butyl ether, and diethylene glycol butyl ether acetate.
[0011] In one embodiment, the alloy powder composition includes 3% to 5% hydride and 95% to 97% copper-silver alloy in terms of mass percentage.
[0012] In one embodiment, the hydride includes one or both of titanium hydride and zirconium hydride, and the copper-silver alloy includes one or more of silver-copper, copper-phosphorus-silver, and copper-tin-phosphorus-silver.
[0013] In one embodiment, the particle size D50 of the hydride is 1 μm to 20 μm, and the particle size D50 of the copper-silver alloy is 5 μm to 50 μm.
[0014] In a second aspect, the present invention provides a method for preparing a metal solder paste, comprising: separately preparing an alloy powder composition and a binder composition, wherein the binder composition comprises a flocculant; and mixing the alloy powder composition with the binder composition to obtain the metal solder paste.
[0015] In one embodiment, preparing the binder composition includes: adding a thickener to a solvent and stirring to obtain a solution A; mixing a dispersant, the flocculant and the solution A and stirring to obtain the binder composition.
[0016] In one embodiment, preparing the alloy powder composition includes: mixing hydride powder and copper-silver alloy powder and centrifuging to obtain the alloy powder composition; wherein, in terms of mass percentage, the hydride is 3% to 5%, and the copper-silver alloy is 95% to 97%.
[0017] In a third aspect, the present invention provides a power device, comprising a ceramic solder, a metal solder and the metal solder paste as described in the first aspect, wherein the metal solder paste is disposed between the ceramic solder and the metal solder.
[0018] In a fourth aspect, the present invention provides a method for manufacturing a power device, comprising: placing a metal solder paste on the surface of a ceramic weld and drying it; connecting the metal weld with the ceramic weld, the metal weld being in contact with the metal solder paste, and obtaining the power device after sintering.
[0019] The present invention mixes a binder composition containing a flocculant with an alloy powder composition, and utilizes the flocculant to solve the powder stratification problem that often occurs in the alloy powder composition, thereby improving the storage stability of the metal solder paste. Furthermore, during the screen printing process, good powder distribution can improve the uniformity of the metal solder paste on the screen printing sheet and further improve the active metal brazing quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 is a flow chart of a method for preparing a metal solder paste according to an embodiment;
[0022] Figure 2 is a flow chart of preparing a binder composition and an alloy powder composition according to an embodiment;
[0023] Figure 3 The present invention is a flow chart of a method for manufacturing a power device according to an embodiment. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.
[0026] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0027] The present invention provides a metal solder paste, comprising an alloy powder composition and a binder composition, wherein the binder composition comprises a flocculant. The present invention mixes the binder composition containing the flocculant with the alloy powder composition, and the flocculant can be used to solve the powder stratification problem that often occurs in the alloy powder composition, thereby improving the storage stability of the metal solder paste. Furthermore, in the screen printing process, good powder distribution can improve the uniformity of the metal solder paste on the screen printing sheet, and further improve the active metal brazing quality.
[0028] Specifically, the flocculant provided by the present invention is an organic controlled flocculant. The organic controlled flocculant has multiple organic functional groups. In the slurry system, multiple adsorption functional groups separated from each other can form bridges between different powder particles. When the centrifugally mixed adhesive composition contacts the adhesive composition, several terminal adsorption functional groups of the flocculant can be quickly adsorbed on the surfaces of two adjacent powders with different properties to form an integral network. The two powders with originally inconsistent sedimentation speeds in the network will move as a whole under the restriction of the bridge, thereby effectively solving the problem of metal solder paste stratification caused by different sedimentation speeds.
[0029] In one embodiment, in the metal solder paste, the alloy powder composition accounts for 80% to 90% by mass, and the binder composition accounts for 10% to 20% by mass.
[0030] Optionally, the proportion of the alloy powder composition can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, or 90%.
[0031] Optionally, the binder composition may account for 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%.
[0032] In one embodiment, the flocculant includes one or more of polybasic long alkyl chain carboxylic acids and derivatives thereof, polybasic carboxylic acid polymers and copolymers thereof.
[0033] In a specific embodiment, the flocculant is a polyvalent long alkyl chain carboxylic acid and its derivatives, such as citric acid, tartaric acid, butane tetracarboxylic acid, etc., and other polyvalent carboxylic acid polymers and copolymers thereof, such as low molecular weight unsaturated polyvalent carboxylic acid polymer and polysiloxane copolymers, alkyl alcohol ammonium salts of acidic polymers, etc. In other specific embodiments, the flocculant can also be BYK-P104, ANTI-TERRA-204, etc. from BYK.
[0034] The common features of the above types of flocculants include multiple carboxylic acid or its derivative salt functional groups, multiple siloxane functional groups, which will form non-covalent bonds such as hydrogen bonds with polar functional groups on the surface of the alloy powder composition, thereby adsorbing on the powder, and these functional groups are spaced far apart, which effectively inhibits all functional groups from adsorbing on the same particle surface, thereby achieving a bridge effect between different powder particles. Taking citric acid as an example, citric acid is an organic weak acid with a large number of carboxyl groups. The H atoms on the carboxyl groups can form hydrogen bonds with polar functional groups on the surface of the alloy powder composition, thereby adsorbing the powder, but the multiple carboxyl groups on citric acid are spaced far apart and are not located in the same plane, so that different powder particles can be connected and evenly dispersed.
[0035] In one embodiment, in the binder composition, the flocculant accounts for 1% to 10% by mass.
[0036] Optionally, the mass proportion of the dispersant can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%.
[0037] In one embodiment, the binder composition further comprises, by weight percentage, 1% to 10% of a dispersant, 1% to 10% of a thickener, and 80% to 95% of a solvent.
[0038] It should be explained that in the binder composition provided by the present invention, the types, functions and effects of the flocculant and the dispersant are different. The polar affinity groups in the structure of the flocculant are not only concentrated in a small area of the molecule, but are distributed at the relatively far molecular ends or branched tails, so that they can be effectively adsorbed on the surfaces of different particles, playing the role of a bridge between powder particles.
[0039] Optionally, the mass proportion of the dispersant can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%.
[0040] Optionally, the mass proportion of the thickener can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%.
[0041] Optionally, the mass proportion of the solvent can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, or 95%.
[0042] In one embodiment, the dispersant includes one or two of stearic acid and polyethylene glycol, the thickener includes one or more of ethyl cellulose, polyvinyl alcohol, and acrylic resin, and the solvent includes one or more of pineneol, tributyl citrate, diethylene glycol butyl ether, and diethylene glycol butyl ether acetate.
[0043] Optionally, in other specific embodiments, the dispersant may be polyethylene glycol including polyethylene glycol 200 (molecular weight) and polyethylene glycol 400 (molecular weight), or DISPERBYK-168 from BYK.
[0044] In one embodiment, the alloy powder composition includes 3% to 5% hydride and 95% to 97% copper-silver alloy in terms of mass percentage. When the proportions of the components of the alloy powder composition are within the above range, the metal solder paste can be ensured to have good eutectic spreading and chemical bonding, thereby improving the welding strength of the welding layer.
[0045] Optionally, the mass proportion of hydride may be 3%, 3.5%, 4%, 4.5%, or 5%.
[0046] Optionally, the mass proportion of the copper-silver alloy may be 95%, 95.5%, 96%, 96.5%, or 97%.
[0047] In the prior art, traditional solder paste generally uses a mixture of silver, copper and titanium, and needs to use three kinds of silver powder, copper powder and titanium powder respectively. The preparation process of the ternary alloy powder is complicated and the production cost is high, which limits the application prospects of the silver, copper and titanium active solder paste. The present invention uses a metal solder paste prepared from hydride powder and silver-copper alloy powder. The preparation process of hydride powder and silver-copper alloy powder is relatively simple and the production cost is low. Using these two powders to replace the silver-copper-titanium ternary alloy powder can reduce the raw material cost by about 50%.
[0048] In one embodiment, the hydride includes one or both of titanium hydride and zirconium hydride, and the copper-silver alloy includes one or more of silver-copper, copper-phosphorus-silver, and copper-tin-phosphorus-silver. The above two metal materials can meet the requirements of the alloy powder composition in the metal solder paste, and both the titanium hydride powder and the silver-copper alloy powder are products with relatively simple preparation processes and low production costs, which are conducive to large-scale industrial production.
[0049] Since the density of silver-copper alloy powder is much greater than that of hydride powder, the sedimentation rate of silver-copper alloy powder in the solder paste system is faster than that of hydride powder, resulting in serious powder static stratification. The silver-copper alloy powder in the lower layer of the solder paste is aggregated, while the hydride powder is aggregated in the upper layer. During the screen printing process, the two powders cannot be evenly distributed on the surface of the ceramic sheet. The proportion of silver-copper alloy powder in some areas is high, and the proportion of hydride powder in some areas is high, resulting in the occurrence of flower defects in the solder paste during the screen printing process. In the subsequent brazing process, due to the uneven distribution of hydride powder, the thickness difference between the nitride and silicide transition layers generated by the reaction of the solder layer and silicon nitride ceramic is too large, so there are many holes between the solder layer and the ceramic; and the area with low silver-copper alloy content leads to weak bonding between the solder layer and the copper foil, which is generally manifested as poor peeling strength. The addition of flocculants can form bridges between different powder particles. When the two powders after centrifugal mixing come into contact with the binder, several terminal adsorption groups of the flocculant can be quickly adsorbed on the surfaces of the two adjacent powders with different properties, forming an overall network. The two powders with originally inconsistent sedimentation speeds in the network will move as a whole under the restriction of the bridge, thus effectively solving the problem of solder paste stratification caused by different sedimentation speeds.
[0050] In one embodiment, the particle size D50 of the hydride is 1 μm to 20 μm, and the particle size D50 of the copper-silver alloy is 5 μm to 50 μm. The particle size D50 of the hydride and the particle size D50 of the copper-silver alloy satisfy the above ranges, which can reduce the difficulty of particle manufacturing, prevent particle agglomeration, and increase the dispersibility of the particles.
[0051] Optionally, the particle size D50 of the hydride can be 1 μm, 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, or 20 μm.
[0052] Optionally, the particle size D50 of the copper-silver alloy can be 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, or 50 μm.
[0053] In one embodiment, the present invention also provides a method for preparing a metal solder paste, please refer to Figure 1 , including the following steps:
[0054] Step S10, preparing an alloy powder composition and a binder composition respectively, wherein the binder composition includes a flocculant.
[0055] Step S20, mixing the alloy powder composition with the binder composition to obtain a metal solder paste.
[0056] Specifically, the preparation method provided by the present invention is different from the method in the prior art in that the alloy powder composition and the binder composition are prepared separately, and the alloy powder composition can be mixed evenly by high-speed centrifugation, which is different from the traditional method of adding two or more metal powders one after another. The advantage of the preparation method is that the alloy powder composition has better dispersibility, and the flocculant is more easily combined with the alloy powder, and then a bridge effect is achieved.
[0057] Optionally, in step S20, the alloy powder composition is added to the binder composition, including: weighing a formulated amount of the binder composition and adding it to a mixing device such as a power mixer, adding the formulated amount of the alloy powder composition in batches while stirring, mechanically mixing for 60 minutes to 90 minutes and vacuum degassing after the powder is completely added, then further dispersing the slurry with a three-roll grinder, and collecting the ground product to obtain a solder paste.
[0058] In one embodiment, the binder composition is prepared, please refer to Figure 2 , including the following steps:
[0059] Step S11, adding a thickener into the solvent and stirring to obtain solution A.
[0060] Step S12, mixing and stirring the dispersant, the flocculant and the solution A to obtain a binder composition.
[0061] Optionally, in step S11, the thickener is added to the solvent and stirred, specifically comprising: adding the thickener to the solvent, stirring at a high speed of 60° C. to 90° C. for 1 h to 2 h, until the thickener is completely dissolved to form a clear and transparent solution A.
[0062] Optionally, in step S12, a dispersant and a flocculant are added to solution A and stirred, specifically comprising: adding a dispersant and a controlled flocculant to solution A, and continuing stirring for 0.5 h to 1 h; after stopping stirring, quickly filtering to remove insoluble impurities, and the obtained adhesive composition can be used after standing at room temperature for more than 6 h.
[0063] In one embodiment, the alloy powder composition is prepared, please refer to Figure 2 , including the following steps:
[0064] Step S13, mixing the hydride powder and the copper-silver alloy powder and centrifuging to obtain an alloy powder composition.
[0065] Optionally, in step S13, the hydride powder and the copper-silver alloy powder are mixed and then centrifuged, specifically comprising: weighing the formulated amounts of two alloy powders (hydride powder and copper-silver alloy powder) into a centrifuge tank, sealing it and placing it in a high-speed centrifuge for centrifugation for 1 min to 10 min, with a centrifugal speed of 3000 rpm to 10000 rpm; after centrifugal mixing, wait for the powder to return to room temperature before use.
[0066] Among them, calculated by mass percentage, hydride is 3% to 5%, and copper-silver alloy is 95% to 97%.
[0067] High-speed centrifugal mixing can effectively physically homogenize two powders with large differences in density and size, so that the physical distance between the two types of powders can be shortened when the alloy powder composition is mixed with the binder composition. This can effectively solve the sedimentation and stratification problem caused by the difference in density and size of the two powders, improve the uniformity of screen printing and the final active metal brazing quality.
[0068] In one embodiment, the present invention further provides a power device, comprising a ceramic solder, a metal solder, and the metal solder paste provided in the above embodiment, wherein the metal solder paste is disposed between the ceramic solder and the metal solder.
[0069] Specifically, the power device may be a chip, a photovoltaic cell, etc. The ceramic welded object may be a ceramic sheet, specifically a nitride ceramic sheet, such as silicon nitride, aluminum nitride, etc. The metal welded object may be a metal sheet, such as oxygen-free copper foil, etc., and the thickness of the metal sheet may be 0.3 mm to 0.8 mm.
[0070] In one embodiment, after the power device is ultrasonically tested, the defective rate of holes of the ceramic weld and the metal weld is less than or equal to 3%, and the peel strength of the ceramic weld and the metal weld is greater than or equal to 15N / mm.
[0071] In one embodiment, the present invention also provides a method for manufacturing a power device, please refer to Figure 3 , including the following steps:
[0072] Step S100, placing metal solder paste on the surface of the ceramic object to be welded and drying it.
[0073] Step S200, connecting the metal solder and the ceramic solder, the metal solder and the metal solder paste are in contact, and a power device is obtained after sintering.
[0074] Optionally, in step S100, the metal solder paste is placed on the surface of the ceramic weld and dried, specifically including: printing the metal solder paste on both sides of the ceramic weld by screen printing, and the single-sided weight of the metal solder paste is 94 g / m 2 ~131.6g / m 2 , can be dried at 80℃ for 30min.
[0075] Optionally, in step S200, the metal weld is connected to the ceramic weld, and the metal weld is in contact with the metal solder paste and sintered, specifically including: covering the metal weld on the metal solder paste surface on both sides of the ceramic weld, placing it in a vacuum brazing furnace for degreasing and debinding sintering, and keeping the temperature at 800°C to 900°C for 2h to 3h, so as to achieve good welding between the metal weld and the ceramic weld.
[0076] The technical solution of the present invention is described in detail below through specific embodiments.
[0077] Example 1
[0078] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0079] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0080] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), terpineol (81.5%), stearic acid (3%) and citric acid (2%).
[0081] The preparation method of the metal solder paste provided in this embodiment is as follows:
[0082] 1) Prepare a mixed solvent of terpineol and tributyl citrate, add ethyl cellulose into the mixed solvent, and stir at 80° C. for 90 minutes.
[0083] 2) Stearic acid and citric acid were added to the solution of step 1), and the mixture was stirred for 30 minutes and then filtered and allowed to stand to obtain a binder composition.
[0084] 3) The titanium hydride powder and the silver-copper alloy powder were mixed in the above mass ratio, and centrifuged at 5000 rpm for 5 min to obtain an alloy powder composition.
[0085] 4) The alloy powder composition and the binder composition are mixed and dispersed using a three-roll mill to obtain a metal solder paste.
[0086] Example 2
[0087] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 90:10.
[0088] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0089] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), terpineol (81.5%), stearic acid (3%) and citric acid (2%).
[0090] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 is that the mass ratio of the alloy powder composition and the binder composition is different.
[0091] Example 3
[0092] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0093] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0094] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), pineneol (81.5%), stearic acid (3%) and tartaric acid (2%).
[0095] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 is that the type of flocculant is different.
[0096] Example 4
[0097] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0098] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0099] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), terpineol (84.5%), stearic acid (1%) and citric acid (1%).
[0100] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 is that the mass proportion of the flocculant is different.
[0101] Example 5
[0102] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0103] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0104] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), pineneol (81.5%), PEG (polyethylene glycol) 400 (3%) and citric acid (2%).
[0105] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 is that the type of dispersant is different.
[0106] Example 6
[0107] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0108] The alloy powder composition includes silver-copper alloy powder (95%) and titanium hydride powder (5%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0109] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), terpineol (81.5%), stearic acid (3%) and citric acid (2%).
[0110] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 is that the mass ratio of the alloy components is different.
[0111] Example 7
[0112] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0113] The alloy powder composition includes silver-copper alloy powder (96%) and zirconium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0114] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), terpineol (81.5%), stearic acid (3%) and citric acid (2%).
[0115] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 lies in the different types of alloy components.
[0116] Example 8
[0117] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0118] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 25.0 μm, and the average particle size D50 of the titanium hydride powder is 6.0 μm.
[0119] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), terpineol (81.5%), stearic acid (3%) and citric acid (2%).
[0120] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 is that the particle size D50 of the alloy powder is different.
[0121] Example 9
[0122] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0123] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0124] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), terpineol (81.5%), DISPERBYK-168 (3%) and BYK-P104 (2%).
[0125] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 lies in the different types of dispersant and flocculant.
[0126] Example 10
[0127] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0128] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0129] Calculated by mass percentage, the binder composition includes ethyl cellulose (5.5%), tributyl citrate (8.5%), terpineol (84.0%), DISPERBYK-168 (1%) and BYK-P104 (1%).
[0130] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 lies in the different mass ratios of the dispersant and the flocculant.
[0131] Embodiment 11
[0132] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 80:20.
[0133] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0134] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), terpineol (81.5%), stearic acid (3%) and citric acid (2%).
[0135] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 is that the mass ratio of the alloy powder composition and the binder composition is different.
[0136] Example 12
[0137] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0138] The alloy powder composition includes silver-copper alloy powder (97%) and titanium hydride powder (3%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0139] Calculated by mass percentage, the binder composition includes ethyl cellulose (5%), tributyl citrate (8.5%), terpineol (81.5%), stearic acid (3%) and citric acid (2%).
[0140] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 is that the mass ratio of the alloy components is different.
[0141] Embodiment 13
[0142] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0143] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0144] Calculated by mass percentage, the binder composition includes ethyl cellulose (4%), tributyl citrate (7.5%), terpineol (77.5%), stearic acid (1%) and citric acid (10%).
[0145] The preparation method of the metal solder paste provided in this embodiment is the same as that of Embodiment 1. The difference between the metal solder paste provided in this embodiment and Embodiment 1 is that the content of the flocculant is different.
[0146] Comparative Example 1
[0147] This embodiment provides a metal solder paste, including an alloy powder composition and a binder composition, with a mass ratio of 87:13.
[0148] The alloy powder composition includes silver-copper alloy powder (96%) and titanium hydride powder (4%) by mass percentage. The average particle size D50 of the silver-copper alloy powder is 20.0 μm, and the average particle size D50 of the titanium hydride powder is 5.0 μm.
[0149] Calculated by mass percentage, the binder composition includes ethyl cellulose (7%), tributyl citrate (8.5%), terpineol (81.5%) and stearic acid (3%).
[0150] The preparation method of the metal solder paste provided in this comparative example is the same as that of Example 1. The difference between the metal solder paste provided in this comparative example and Example 1 is that no flocculant is added.
[0151] The metal solder paste provided in Examples 1-13 and Comparative Example 1 was used in solder paste screen printing to bond the silicon nitride ceramic sheet and the oxygen-free copper foil. The metal solder paste was printed on both sides of the silicon nitride ceramic sheet, and the single-sided weight was controlled to be 112.8 g / m 2 , and dried at 80℃ for 30min. Cover the solder layer surface of both sides of the silicon nitride ceramic sheet with 0.3mm thick oxygen-free copper foil, place it in a vacuum brazing furnace for degreasing, debinding and sintering, and keep it at 850℃ for 2 hours. The obtained ceramic copper clad laminate was tested for hole detection and peel strength, and the test data are shown in Table 1.
[0152] Hole detection method: The defective hole rate of ceramic copper clad laminate adopts the method in GB / T39240-2020 "General Principles of Non-destructive Testing and Ultrasonic Testing", and is obtained by calculating the proportion of products with defective holes.
[0153] Peel strength test: The peel strength of the ceramic copper clad laminate is tested using GB / T11363-2008 "Test method for brazing joint strength".
[0154] Powder average particle size D50 test: GB / T 19077-2016 "Particle size distribution laser diffraction method" test, ultrasonic dispersion in anhydrous ethanol for 5 minutes, test in industrial alcohol as a dispersion medium, and take particle size D50 as the average particle size.
[0155] Sedimentation uniformity: The sample is left to stand to allow the solids in the metal solder paste to settle. By observation, the sample sedimentation uniformity can be divided into "excellent" and "poor". Among them, for samples with "excellent" sedimentation uniformity, the sediment is uniform in color and does not appear stratified; for samples with "poor" sedimentation uniformity, the sediment is stratified and obvious color unevenness can be observed. It needs to be explained that since different metal powders in the solder paste have different densities and colors, in the sediment, if the sedimentation uniformity of the sample is "poor", the sedimentation speed of different metal powders is different, which will produce stratified color difference.
[0156] Silk screen appearance: The samples are printed on both sides of the silicon nitride ceramic sheet. Through observation, the solder paste morphology on the silicon nitride ceramic sheet can be divided into two types: "uniform" and "flowering". Among them, the sample with "uniform" silk screen appearance has a uniform solder paste coating without wavy patterns; the sample with "flowering" silk screen appearance has an uneven solder paste coating and obvious wavy patterns can be observed. It needs to be explained that the wavy pattern is "flowering", and because different metal powders in the solder paste have different densities and colors, this phenomenon will occur if the alloy powders in the solder paste are not well mixed.
[0157] Table 1
[0158]
[0159]
[0160] From the test results of Examples 1-13 and Comparative Example 1 in Table 1, it can be seen that the adhesive composition in Comparative Example 1 does not add a controlled flocculant, resulting in the two powders in the metal solder paste settling at different speeds due to the difference in density. The silver-copper alloy powder in the lower layer of the solder paste aggregates, while the titanium hydride powder in the upper layer aggregates. Therefore, during the silk-screen printing process, the two powders cannot be evenly distributed on the surface of the ceramic sheet. The proportion of silver-copper alloy powder in some areas is high, and the proportion of titanium hydride powder in some areas is high, resulting in the solder paste having flower defects during the silk-screen printing process. In the subsequent brazing process, due to the uneven distribution of titanium hydride powder, the thickness difference between the titanium nitride and titanium silicide transition layers generated by the reaction of the solder layer and silicon nitride ceramics is too large, so that more holes are generated between the solder layer and the ceramic; and the area with low silver-copper alloy content leads to weak bonding between the solder layer and the copper foil, which is generally manifested as poor peeling strength.
[0161] In contrast, the binder compositions in Examples 1-13 are all added with controlled flocculants, so that the alloy powders in the alloy powder compositions have good dispersion, are not prone to aggregation, and the powders do not have stratification problems, thereby improving the storage stability of the metal solder paste; and during the silk-screen printing process, good powder distribution can improve the uniformity of the metal solder paste on the silk-screen sheet and further improve the quality of active metal brazing.
[0162] In the description of the embodiments of the present invention, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0163] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope covered by the present invention.
Claims
1. A metal solder paste, characterized in that: The invention comprises an alloy powder composition and a binder composition, wherein the binder composition comprises a flocculant.
2. The metal solder paste according to claim 1, characterized in that: In the metal solder paste, the alloy powder composition accounts for 80% to 90% by mass, and the binder composition accounts for 10% to 20% by mass.
3. The metal solder paste according to claim 1, characterized in that: The flocculant includes one or more of polybasic long alkyl chain carboxylic acids and derivatives thereof, polybasic carboxylic acid polymers and copolymers thereof.
4. The metal solder paste according to claim 1, characterized in that: In the binder composition, the flocculant accounts for 1% to 10% by mass.
5. The metal solder paste according to claim 1, characterized in that: Calculated by mass percentage, the binder composition further comprises 1% to 10% of a dispersant, 1% to 10% of a thickener, and 80% to 95% of a solvent.
6. The metal solder paste according to claim 5, characterized in that: The dispersant includes one or two of stearic acid and polyethylene glycol, the thickener includes one or more of ethyl cellulose, polyvinyl alcohol, and acrylic resin, and the solvent includes one or more of pineol, tributyl citrate, diethylene glycol butyl ether, and diethylene glycol butyl ether acetate.
7. The metal solder paste according to claim 1, characterized in that: Calculated by mass percentage, the alloy powder composition includes 3% to 5% of hydride and 95% to 97% of copper-silver alloy.
8. The metal solder paste according to claim 7, characterized in that: The hydride includes one or both of titanium hydride and zirconium hydride, and the copper-silver alloy includes one or more of silver-copper, copper-phosphorus-silver, and copper-tin-phosphorus-silver.
9. The metal solder paste according to claim 7, characterized in that: The particle size D50 of the hydride is 1 μm to 20 μm, and the particle size D50 of the copper-silver alloy is 5 μm to 50 μm.
10. A method for preparing a metal solder paste, characterized in that: include: preparing an alloy powder composition and a binder composition respectively, wherein the binder composition comprises a flocculant; The alloy powder composition is mixed with the binder composition to obtain the metal solder paste.
11. The preparation method according to claim 10, characterized in that: The binder composition is prepared, comprising: Adding the thickener to the solvent and stirring to obtain solution A; The dispersant, the flocculant and the solution A are mixed to obtain the binder composition.
12. The preparation method according to claim 10, characterized in that: The alloy powder composition is prepared, comprising: mixing the hydride powder and the copper-silver alloy powder and centrifuging to obtain the alloy powder composition; Wherein, calculated by mass percentage, the hydride is 3% to 5%, and the copper-silver alloy is 95% to 97%.
13. A power device, characterized in that: The invention comprises a ceramic solder, a metal solder and the metal solder paste according to any one of claims 1 to 9, wherein the metal solder paste is arranged between the ceramic solder and the metal solder.
14. A method for manufacturing a power device, characterized in that: include: placing the metal solder paste on the surface of the ceramic soldering object and drying it; The metal solder is connected to the ceramic solder, the metal solder is in contact with the metal solder paste, and the power device is obtained after sintering.
Citation Information
Cited By
Soldering paste, ceramic copper-clad plate and method for preparing ceramic copper-clad plate
CN119820169A
Metal soldering paste and preparation method therefor, and power device
WO2025232838A1