Far infrared transmitting member and method for manufacturing far infrared transmitting member

By using the post-oxidation sputtering method to form a high-hardness NiOx layer in the far-infrared transmission film, the problem of insufficient scratch resistance of the existing transmission film is solved, and a combination of high transmittance and high scratch resistance is achieved.

CN118748984APending Publication Date: 2024-10-08AGC INC

Patent Information

Application Number
CN202380025398.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-07
Filing Date
2023-02-17
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing far-infrared transmission films have deficiencies in scratch resistance. In particular, the nickel oxide film has low indentation hardness and is prone to scratches and scratches.

Method used

The post-oxidation sputtering method is used to form a NiOx layer with NiOx as the main component on the substrate. A high-hardness NiOx layer is formed through a lamination step and an oxidation step to ensure transmittance and scratch resistance.

Benefits of technology

Appropriate far-infrared transmission is achieved, and the scratch resistance is significantly improved. The indentation hardness reaches more than 10GPa, which enhances the mechanical strength of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748984A_ABST
    Figure CN118748984A_ABST
Patent Text Reader

Abstract

The present invention appropriately permits transmission of far infrared rays and improves scratch resistance. The far-infrared-ray-transmitting member (20) includes a base material (30) that permits far-infrared ray transmission, and a first functional film (32) that is formed on the base material (30) and has a NiOx layer (34) having NiOx as the main component, the average transmittance of light having a wavelength of 8 [mu] m to 12 [mu] m being 50% or more, and the average transmittance of light having a wavelength of 8 [mu] m to 12 [mu] m being 50% or more. And the maximum value (Hmax) of the indentation hardness within the indentation depth range from 40 nm to 110 nm (inclusive) from the surface of the functional film as measured by a nanoindentation method is 10 GPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a far-infrared ray transmitting member and a method for producing the far-infrared ray transmitting member. Background Art

[0002] For example, when a far infrared sensor is mounted on a vehicle or the like, a far infrared transmission member having a functional film formed thereon for appropriately causing far infrared rays to enter the far infrared sensor is sometimes provided. For example, Patent Document 1 describes that an infrared transmission film containing a metal oxide having zinc oxide as a main component is formed on a substrate. In addition, for example, Non-Patent Document 1 describes that a nickel oxide film is formed on a Si substrate as a far infrared transmission film.

[0003] For a far-infrared transmitting film used to increase the amount of transmitted light of far-infrared rays, high scratch resistance is important, but for example, according to non-patent document 1, the indentation hardness of the nickel oxide film formed on the Si substrate by RF magnetron sputtering is as low as 6.1 GPa, so it is expected that scratches and scratches will easily occur.

[0004] Prior art literature

[0005] Non-patent literature

[0006] Non-patent document 1: Hyun Bin Shim et al., Controlling the infrared opticalproperties of rf-sputtered NiO films for application of infrared window, Infrared Physics and Technology 72 (2015), 135-139

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2017-151408 Summary of the invention

[0009] Problems to be solved by the invention

[0010] Such a far-infrared ray transmitting member is required to appropriately allow far-infrared ray transmission and to improve scratch resistance.

[0011] An object of the present invention is to provide a far-infrared transmitting member and a method for producing the far-infrared transmitting member which appropriately allows far-infrared transmission and can improve scratch resistance.

[0012] Means used to solve problems

[0013] The far infrared ray transmitting member disclosed in the present invention comprises a substrate and a functional film, wherein the substrate allows far infrared ray to be transmitted, and the functional film is formed on the substrate and has one or more layers of NiO x NiO as the main component x The far-infrared ray transmitting member has an average transmittance of light of a wavelength of 8 μm to 12 μm of 50% or more, and a maximum value H of an indentation hardness within a range of an indentation depth of 40 nm or more and 110 nm or less from the surface of the functional film measured by a nanoindentation method. max More than 10GPa.

[0014] In the method for manufacturing a far infrared ray transmitting member disclosed in the present invention, a NiO film is formed on a substrate that allows far infrared ray transmission by a post-oxidation sputtering method. x NiO as the main component x layer, thereby manufacturing a far-infrared transmitting member.

[0015] Effects of the Invention

[0016] According to the present invention, it is possible to appropriately allow far infrared rays to be transmitted and to improve scratch resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram which shows the state which mounted the vehicle glass of this embodiment on the vehicle.

[0018] Figure 2 It is a schematic plan view of the vehicle glass according to the present embodiment.

[0019] Figure 3 For along Figure 2 Cross-sectional view along line AA.

[0020] Figure 4 For along Figure 2 Cross-sectional view of the BB section.

[0021] Figure 5 It is a schematic cross-sectional view of the far-infrared transmissive member of this embodiment.

[0022] Figure 6 It is a schematic diagram for explaining the manufacturing method of the far-infrared transmissive member of this embodiment.

[0023] Figure 7 It is a schematic cross-sectional view of a far-infrared transmissive member according to another example of the present embodiment. DETAILED DESCRIPTION

[0024] The preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. It should be noted that the present invention is not limited to the embodiments, and in addition, when there are multiple embodiments, the embodiments are also combined to form the embodiments. In addition, the numerical values ​​include the range of rounding.

[0025] (vehicle)

[0026] Figure 1 Schematic diagram showing a state where the vehicle glass of this embodiment is mounted on a vehicle. Figure 1 As shown, the vehicle glass 1 of this embodiment is mounted on a vehicle V. The vehicle glass 1 is a window member applied to the front glass of the vehicle V. That is, the vehicle glass 1 is used as the front window of the vehicle V, in other words, as a windshield. A far-infrared camera CA1 and a visible light camera CA2 are mounted inside (inside) the vehicle V. It should be noted that the inside (inside) of the vehicle V refers to, for example, the interior of the vehicle V where the driver's seat is set.

[0027] The vehicle glass 1, the far-infrared camera CA1 and the visible light camera CA2 constitute the camera unit 100 of the present embodiment. The far-infrared camera CA1 is a camera for detecting far-infrared rays, and captures a thermal image of the outside of the vehicle V by detecting far-infrared rays from the outside of the vehicle V. The visible light camera CA2 is a camera for detecting visible light, and captures an image of the outside of the vehicle V by detecting visible light from the outside of the vehicle V. It should be noted that the camera unit 100 may also have, for example, LiDAR and millimeter wave radar in addition to the far-infrared camera CA1 and the visible light camera CA2. The far-infrared rays here refer to, for example, electromagnetic waves in a wavelength band of 8μm to 13μm, and the visible light refers to, for example, electromagnetic waves in a wavelength band of 360nm to 830nm. In addition, 8μm to 13μm here refers to 8μm or more and 13μm or less, and 360nm to 830nm refers to 360nm or more and 830nm or less, and the same applies to the following text. In addition, the far infrared rays may be set to electromagnetic waves in the wavelength range of 8 μm to 12 μm.

[0028] (Glass for vehicles)

[0029] Figure 2 It is a schematic plan view of the vehicle glass according to the present embodiment. Figure 3 For along Figure 2 Cross-sectional view along line AA. Figure 4 For along Figure 2 The sectional view of the BB section. Figure 2As shown, hereinafter, the upper edge of the vehicle glass 1 is referred to as the upper edge portion 1a, the lower edge of the vehicle glass 1 is referred to as the lower edge portion 1b, the side edge on one side of the vehicle glass 1 is referred to as the side edge portion 1c, and the side edge on the other side of the vehicle glass 1 is referred to as the side edge portion 1d. The upper edge portion 1a is an edge portion located on the upper side in the vertical direction when the vehicle glass 1 is mounted on the vehicle V. The lower edge portion 1b is an edge portion located on the lower side in the vertical direction when the vehicle glass 1 is mounted on the vehicle V. The side edge portion 1c is an edge portion located on the lateral side of one side when the vehicle glass 1 is mounted on the vehicle V. The side edge portion 1d is an edge portion located on the lateral side of the other side when the vehicle glass 1 is mounted on the vehicle V.

[0030] Hereinafter, in the direction parallel to the surface of the vehicle glass 1, the direction from the upper edge 1a to the lower edge 1b is set as the Y direction, and the direction from the side edge 1c to the side edge 1d is set as the X direction. In the present embodiment, the X direction is orthogonal to the Y direction. The direction orthogonal to the surface of the vehicle glass 1, that is, the thickness direction of the vehicle glass 1 is set as the Z direction. The Z direction is, for example, the direction from the outer side of the vehicle V to the inner side of the vehicle V when the vehicle glass 1 is mounted on the vehicle V. The X direction and the Y direction are along the surface of the vehicle glass 1, but, for example, when the surface of the vehicle glass 1 is a curved surface, they can also be directions tangent to the surface of the vehicle glass 1 at the center point O of the vehicle glass 1. The center point O refers to the center position of the vehicle glass 1 when the vehicle glass 1 is observed from the Z direction.

[0031] A light-transmitting area A1 and a light-shielding area A2 are formed on the vehicle glass 1. The light-transmitting area A1 is an area occupying the central part of the vehicle glass 1 when viewed from the Z direction. The light-transmitting area A1 is an area for ensuring the driver's field of vision. The light-transmitting area A1 is an area that allows visible light to be transmitted. The light-shielding area A2 is an area formed around the light-transmitting area A1 when viewed from the Z direction. The light-shielding area A2 is an area that blocks visible light. A far-infrared ray transmission area B and a visible light transmission area C are formed in the light-shielding area A2a, which is a part on the side of the upper edge 1a in the light-shielding area A2.

[0032] The far infrared transmission area B is an area where far infrared rays are allowed to be transmitted, and is an area where the far infrared camera CA1 is set. That is, the far infrared camera CA1 is set at a position overlapping with the far infrared transmission area B when viewed from the optical axis direction of the far infrared camera CA1. The visible light transmission area C is an area where visible light is allowed to be transmitted, and is an area where the visible light camera CA2 is set. That is, the visible light camera CA2 is set at a position overlapping with the visible light transmission area C when viewed from the optical axis direction of the visible light camera CA2.

[0033] Since the far-infrared transmission area B and the visible light transmission area C are formed in the light-shielding area A2, the light-shielding area A2 blocks far infrared rays in the area other than the area where the far-infrared transmission area B is formed, and blocks visible light in the area other than the area where the visible light transmission area C is formed. The far-infrared transmission area B and the visible light transmission area C form a light-shielding area A2a around them. By providing the light-shielding area A2a around them, it is preferable to protect various sensors from the influence of sunlight. Since the wiring of various sensors cannot be seen from the outside of the vehicle, it is also preferable from the viewpoint of appearance design.

[0034] like Figure 3 As shown, the vehicle glass 1 includes a glass substrate 12 (first glass substrate), a glass substrate 14 (second glass substrate), an intermediate layer 16, and a light shielding layer 18. In the vehicle glass 1, the glass substrate 12, the intermediate layer 16, the glass substrate 14, and the light shielding layer 18 are stacked in this order in the Z direction. The glass substrate 12 and the glass substrate 14 are fixed (bonded) to each other by the intermediate layer 16.

[0035] As the glass substrates 12 and 14, for example, soda-lime glass, borosilicate glass, aluminosilicate glass, etc. can be used. The intermediate layer 16 is an adhesive layer that bonds the glass substrate 12 and the glass substrate 14. As the intermediate layer 16, for example, a polyvinyl butyral (hereinafter also referred to as PVB) modified material, an ethylene-vinyl acetate copolymer (EVA) type material, a polyurethane resin material, a vinyl chloride resin material, etc. can be used. In more detail, the glass substrate 12 includes a surface 12A and another surface 12B, and the other surface 12B is in contact with a surface 16A of the intermediate layer 16 and fixed (bonded) to the intermediate layer 16. The glass substrate 14 includes a surface 14A and another surface 14B, and the one surface 14A is in contact with the other surface 16B of the intermediate layer 16 and fixed (bonded) to the intermediate layer 16. It can be seen that the vehicle glass 1 is a laminated glass in which the glass substrate 12 and the glass substrate 14 are stacked. However, the vehicle glass 1 is not limited to laminated glass, and may be a structure including only one of the glass substrate 12 and the glass substrate 14. In this case, the intermediate layer 16 may not be provided. Hereinafter, when the glass substrates 12 and 14 are not distinguished, they are described as the glass substrate 10.

[0036] The light-shielding layer 18 includes a surface 18A and another surface 18B, and the surface 18A is in contact with and fixed to the other surface 14B of the glass substrate 14. The light-shielding layer 18 is a layer that blocks visible light. As the light-shielding layer 18, for example, a ceramic light-shielding layer or a light-shielding film can be used. As the ceramic light-shielding layer, for example, a ceramic layer including a conventionally known material such as a black ceramic layer can be used. As the light-shielding film, for example, a light-shielding polyethylene terephthalate (PET) film, a light-shielding polyethylene naphthalate (PEN) film, a light-shielding polymethyl methacrylate (PMMA) film, etc. can be used.

[0037] In the present embodiment, the side of the vehicle glass 1 on which the light shielding layer 18 is provided is the inner side (vehicle interior side) of the vehicle V, and the side of the vehicle glass 1 on which the glass substrate 12 is provided is the outer side (vehicle exterior side) of the vehicle V, but the present invention is not limited thereto, and the light shielding layer 18 may be provided on the outer side of the vehicle V. In the case of a laminated glass composed of the glass substrates 12 and 14 , the light shielding layer 18 may be formed between the glass substrates 12 and 14 .

[0038] (Light-shielded area)

[0039] The light-shielding region A2 is formed by providing the light-shielding layer 18 on the glass substrate 10. That is, the light-shielding region A2 is a region where the glass substrate 10 has the light-shielding layer 18. That is, the light-shielding region A2 is a region where the glass substrate 12, the intermediate layer 16, the glass substrate 14, and the light-shielding layer 18 are stacked. On the other hand, the light-transmitting region A1 is a region where the glass substrate 10 does not have the light-shielding layer 18. That is, the light-transmitting region A1 is a region where the glass substrate 12, the intermediate layer 16, and the glass substrate 14 are stacked but the light-shielding layer 18 is not stacked.

[0040] (Far infrared transmission area)

[0041] like Figure 3 As shown, the vehicle glass 1 is formed with an opening 19 that passes through from one surface (here, the surface 12A) to the other surface (here, the surface 14B) in the Z direction. A far-infrared ray transmitting member 20 is provided in the opening 19. The region where the opening 19 is formed and the far-infrared ray transmitting member 20 is provided is a far-infrared ray transmitting region B. That is, the far-infrared ray transmitting region B is a region where the opening 19 and the far-infrared ray transmitting member 20 arranged in the opening 19 are provided. Since the light shielding layer 18 does not allow far infrared rays to be transmitted, the light shielding layer 18 is not provided in the far-infrared ray transmitting region B. That is, in the far-infrared ray transmitting region B, the glass substrate 12, the intermediate layer 16, the glass substrate 14, and the light shielding layer 18 are not provided, and the far-infrared ray transmitting member 20 is provided in the formed opening 19. The far-infrared ray transmitting member 20 will be described later.

[0042] (Visible light region)

[0043] like Figure 4 As shown, like the light-transmitting region A1, the visible light-transmitting region C is a region where the glass substrate 10 does not have the light-shielding layer 18 in the Z direction. That is, the visible light-transmitting region C is a region where the glass substrate 12, the intermediate layer 16, and the glass substrate 14 are stacked but the light-shielding layer 18 is not stacked.

[0044] like Figure 2 As shown, the visible light transmission area C is preferably arranged near the far infrared transmission area B. Specifically, the center of the far infrared transmission area B when observed from the Z direction is referred to as the center point OB, and the center of the visible light transmission area C when observed from the Z direction is referred to as the center point OC. When the shortest distance between the far infrared transmission area B (opening 19) and the visible light transmission area C when observed from the Z direction is set to the distance L, the distance L is preferably greater than 0 mm and less than or equal to 100 mm, and more preferably greater than 10 mm and less than 80 mm. By positioning the visible light transmission area C relative to the far infrared transmission area B within this range, the far infrared camera CA1 and the visible light camera CA2 can be used to capture images of nearby positions, and the perspective distortion amount in the visible light transmission area C can be suppressed, so that the visible light camera CA2 can be used to appropriately capture images. By using the far infrared camera CA1 and the visible light camera CA2 to capture images of nearby positions, the load when performing calculations on the data obtained from each camera can be reduced, and the wiring of the power supply and signal cables can also become appropriate.

[0045] like Figure 2 As shown in FIG. 1 , the visible light transmission region C and the far infrared transmission region B are preferably located in a position aligned along the X direction. That is, the visible light transmission region C is preferably aligned with the far infrared transmission region B in the X direction, and is not located on the Y direction side of the far infrared transmission region B. By arranging the visible light transmission region C in a manner aligned with the far infrared transmission region B in the X direction, the visible light transmission region C can be arranged near the upper edge portion 1a. Therefore, the field of vision of the driver in the light transmission region A1 can be appropriately ensured.

[0046] (Far infrared ray transmitting component)

[0047] Hereinafter, the far-infrared ray transmitting member 20 provided in the far-infrared ray transmitting region B will be specifically described. Figure 5 FIG. 4 is a cross-sectional schematic diagram of the far-infrared transmission component of this embodiment. Figure 5As shown, the far-infrared ray transmission member 20 has a substrate 30, a first functional film 32 as a functional film formed on the substrate 30, and a second functional film 36 formed on the substrate 30. In the present embodiment, the first functional film 32 is formed on one surface 30a of the substrate 30. The surface 30a is a surface that becomes the outer side of the vehicle when mounted on the vehicle glass 1. In addition, the second functional film 36 is formed on the other surface 30b of the substrate 30. The surface 30b is a surface that becomes the inner side of the vehicle when mounted on the vehicle glass 1. However, the second functional film 36 is not an indispensable structure, and a layer other than the substrate 30 may not be provided on the surface 30b.

[0048] In the present embodiment, the far-infrared ray transmitting member 20 is disposed in the light shielding region A2 of the vehicle glass 1 as the window member of the vehicle V, but is not limited thereto, and may be disposed on any external member of the vehicle V, such as an external member for a pillar of the vehicle V. That is, the far-infrared ray transmitting member 20 may be disposed on the window member of the vehicle, may be disposed on the external member for a pillar of the vehicle, or may be disposed in the light shielding region of the external member for the vehicle. In addition, the far-infrared ray transmitting member 20 is not limited to being disposed on the vehicle V, and may be used for any purpose.

[0049] (Base material)

[0050] The substrate 30 is a component that allows far-infrared rays to be transmitted. The internal transmittance of the substrate 30 for light with a wavelength of 10 μm (far-infrared rays) is preferably 50% or more, more preferably 60% or more, and further preferably 70% or more. In addition, the average internal transmittance of the substrate 30 for light with a wavelength of 8 μm to 12 μm (far-infrared rays) is preferably 50% or more, more preferably 60% or more, and further preferably 70% or more. By making the internal transmittance of the substrate 30 for light with a wavelength of 10 μm and the average internal transmittance for light with a wavelength of 8 μm to 12 μm within this numerical range, far-infrared rays can be appropriately allowed to be transmitted, so that, for example, the performance of the far-infrared camera CA1 can be fully utilized. It should be noted that the average internal transmittance here refers to the average value of the internal transmittance of light of each wavelength in the band (here 8 μm to 12 μm).

[0051] The internal transmittance of the substrate 30 is the transmittance after deducting the surface reflection losses on the incident side and the emission side, and is well known in the art, and can be measured by a commonly performed method. The measurement is performed, for example, as follows.

[0052] A pair of flat plate samples (first sample and second sample) composed of substrates of the same composition and different thicknesses are prepared. The two surfaces of the flat plate samples are parallel to each other and optically polished. The external transmittance of the first sample including surface reflection loss is set to T1, the external transmittance of the second sample including surface reflection loss is set to T2, the thickness of the first sample is set to Td1 (mm), and the thickness of the second sample is set to Td2 (mm), where Td1 < Td2. At this time, the internal transmittance τ at the thickness Tdx (mm) can be calculated by the following formula (1).

[0053] τ=exp[-Tdx×(lnT1-lnT2) / ΔTd]……(1)

[0054] In addition, the external transmittance of infrared light can be measured by, for example, a Fourier transform infrared spectrometer (manufactured by ThermoScientific, trade name: Nicolet iS10).

[0055] The refractive index of the substrate 30 for light with a wavelength of 10 μm is preferably 1.5 or more and 4.0 or less, more preferably 2.0 or more and 4.0 or less, and further preferably 2.2 or more and 3.5 or less. In addition, the average refractive index of the substrate 30 for light with a wavelength of 8 μm to 12 μm is preferably 1.5 or more and 4.0 or less, more preferably 2.0 or more and 4.0 or less, and further preferably 2.2 or more and 3.5 or less. By having the refractive index and the average refractive index of the substrate 30 within this numerical range, far-infrared light can be appropriately allowed to pass through, so that, for example, the performance of the far-infrared camera CA1 can be fully exerted. It should be noted that the average refractive index here refers to the average value of the refractive index of light of each wavelength in the band (here 8 μm to 12 μm). The refractive index can be determined, for example, by fitting an optical model using polarization information obtained using an infrared spectroscopic ellipsometer (manufactured by JA Woollam, IR-VASE-UT) and a spectral transmission spectrum obtained using a Fourier transform infrared spectrometer.

[0056] The thickness D1 of the substrate 30 is preferably 0.5 mm or more and 5 mm or less, more preferably 1 mm or more and 4 mm or less, and further preferably 1.5 mm or more and 3 mm or less. When the thickness D1 is within this range, the strength can be ensured, and far infrared rays can be appropriately allowed to be transmitted. It should be noted that the thickness D1 can also be said to be the length in the Z direction from the surface 30a of the substrate 30 to the surface 30b.

[0057] The material of the substrate 30 is not particularly limited, and examples thereof include Si, Ge, ZnS, and chalcogenide glass. It can be said that the substrate 30 preferably includes at least one material selected from the group consisting of Si, Ge, ZnS, and chalcogenide glass. By using such a material for the substrate 30, it is possible to appropriately allow far infrared rays to be transmitted.

[0058] The preferred composition of chalcogenide glass is the following composition:

[0059] In atomic %, it contains:

[0060] Ge+Ga: 7%~25%,

[0061] Sb: 0%~35%,

[0062] Bi: 0%~20%,

[0063] Zn: 0%~20%,

[0064] Sn: 0%~20%,

[0065] Si: 0%~20%,

[0066] La: 0%~20%,

[0067] S+Se+Te: 55%~80%,

[0068] Ti: 0.005%~0.3%,

[0069] Li+Na+K+Cs: 0%~20%,

[0070] F+Cl+Br+I:0%~20%.

[0071] Furthermore, the glass preferably has a glass transition temperature (Tg) of 140°C to 550°C.

[0072] It should be noted that Si and ZnS are more preferably used as the material of the substrate 30 .

[0073] (First functional film)

[0074] The first functional film 32 is formed on the surface 30a of the vehicle outer side of the substrate 30. The first functional film 32 includes one or more layers of NiO x Layer 34. Figure 5 In the example, the first functional film 32 has only NiO x Layer 34, no other layers. Figure 5 In the example, NiO x The layer 34 is located on the outermost side (the side farthest from the substrate 30 ) in the first functional film 32 .

[0075] However, the first functional film 32 is not limited to having only NiO x The first functional film 32 may be formed of NiO x The substrate 30 side of the layer 34 has another layer (adhesion layer), which will be described in detail later. x The layer 34 has other layers (color adjustment layer, outermost layer 39) on the side opposite to the substrate 30 (vehicle outer side). In this case, NiO x Layer 34 is not the outermost layer.

[0076] (NiO x layer)

[0077] NiO x Layer 34 is made of NiO x The main component here may refer to a layer with respect to NiO x The content of the entire layer 34 is 50 mass % or more. NiO x In layer 34, relative to NiO x Layer 34 overall, NiO x The content of NiO is 50% by mass or more and 100% by mass or less, preferably 70% by mass or more and 100% by mass or less, and more preferably 90% by mass or more and 100% by mass or less. x Layer 34 is preferably NiO alone x , that is, except for unavoidable impurities, NiO x The content of NiO is 100% by mass. x As for layer 34, NiO x When the content of is within this range, far infrared rays can be appropriately allowed to be transmitted and the scratch resistance can be improved.

[0078] It should be noted that nickel oxide is known to have various compositions depending on the valence of nickel, and x can take any value from 0.5 to 2. In addition, the valence may not be a single one, but may be a mixture of two or more valences. In this embodiment, as NiO x , NiO is preferably used.

[0079] NiO x The layer 34 may contain a minor component other than NiO as a main component. x As minor components, oxides that allow far infrared rays to pass through are preferred, and examples include ZrO2, ZnO, Bi2O3, and CuO x At least one of .

[0080] NiO xThe thickness D2 of the layer 34 is preferably 300 nm or more and 2000 nm or less, more preferably 400 nm or more and 1500 nm or less, and further preferably 1000 nm or more and 1300 nm or less. x The length in the Z direction from the surface of the layer 34 on the Z direction side to the surface on the side opposite to the Z direction.

[0081] In addition, NiO x The ratio of the thickness D2 of the layer 34 to the thickness D1 of the substrate 30 is preferably 0.02% to 0.4%, more preferably 0.02% to 0.3%, and even more preferably 0.03% to 0.08%.

[0082] In addition, NiO x The ratio of the thickness D2 of the layer 34 to the thickness D3 of the first functional film 32 is more preferably 50% or more and 100% or less, further preferably 60% or more and 100% or less, and further preferably 70% or more and 100% or less. It should be noted that the thickness D3 of the first functional film 32 can also be said to be the length in the Z direction from the surface of the first functional film 32 on the Z direction side to the surface on the side opposite to the Z direction.

[0083] When the thickness D2 is within this range, far infrared rays can be appropriately allowed to be transmitted, and scratch resistance can be appropriately improved.

[0084] NiO x The surface of the layer 34 opposite to the substrate 30 is referred to as the surface 34a. The surface 34a is the surface exposed to the outside, and in this embodiment, it can also be said to be the surface on the outside of the vehicle. In this case, NiO x The arithmetic mean roughness Ra (surface roughness) of the surface 34a of the layer 34 is preferably 6 nm or less, more preferably 0.5 nm or more and 6 nm or less, further preferably 0.5 nm or more and 5 nm or less, further preferably 0.5 nm or more and 4 nm or less, and most preferably 0.5 nm or more and 3 nm or less. When the arithmetic mean roughness Ra of the surface 34a is within this range, the change in the dynamic friction coefficient and the surface roughness before and after scratching can be reduced, and the scratch resistance can be more appropriately improved. It should be noted that the arithmetic mean roughness Ra refers to the arithmetic mean roughness Ra specified in JIS B 0601:2001.

[0085] It should be noted that the NiO x The arithmetic mean roughness Ra of the surface 34a of the layer 34 is the average roughness Ra of the surface 34a of the layer 34. x Layer 34 is the outermost layer (NiO xHowever, as described later, in the case of NiO x When another layer (outermost layer 39) is formed outside the layer 34, the arithmetic mean roughness Ra of the surface 39a of the outermost layer 39 may be the same as that of the NiO x The arithmetic mean roughness Ra of the surface 34 a of the layer 34 is the same value.

[0086] NiO x Layer 34 can allow far infrared rays to be transmitted. NiO x The extinction coefficient of the layer 34 for light having a wavelength of 10 μm is preferably 0.4 or less, more preferably 0.1 or less, further preferably 0.05 or less, and further preferably 0.04 or less. The extinction coefficient can be determined, for example, by fitting an optical model using polarization information obtained using an infrared spectroscopic ellipsometer (manufactured by JA Woollam, IR-VASE-UT) and a spectral transmission spectrum obtained using a Fourier transform infrared spectrometer.

[0087] NiO x The refractive index of the layer 34 for light (visible light) with a wavelength of 550 nm is preferably 2.0 to 2.5, and more preferably 2.0 to 2.3. x The refractive index of layer 34 for visible light is within this numerical range, which can improve the NiO x The film density of the layer 34 can more appropriately improve the scratch resistance. The refractive index of light with a wavelength of 550 nm can be determined by fitting an optical model using polarization information obtained using a spectroscopic ellipsometer (M-2000 manufactured by JA Woollam) and spectral transmittance measured based on JIS R3106.

[0088] NiO x The extinction coefficient of layer 34 for light (visible light) with a wavelength of 550 nm is preferably 0.04 or more, more preferably 0.06 or more, further preferably 0.08 or more, and most preferably 0.10 or more. x When the extinction coefficient of the layer 34 for visible light is within this numerical range, the reflectance dispersion of visible light can be appropriately suppressed, and an appearance with secured design properties can be achieved.

[0089] (Second functional film)

[0090] The second functional film 36 provided on the surface 30b of the vehicle interior side of the substrate 30 is a layer that allows far infrared rays to be transmitted. The second functional film 36 may have the same structure as the first functional film 32. That is, for example, the far infrared ray transmitting member 20 may have a substrate 30, NiO, and the like stacked in this order from the substrate 30 toward the vehicle interior side. x Layer 34.

[0091] (Characteristics of far-infrared transmitting components)

[0092] As described above, the far infrared ray transmitting member 20 has a NiO layer formed on the surface 30a of the substrate 30. x The far infrared ray transmitting member 20 is formed by forming the first functional film 32 of the NiO layer 34. x The layer 34 can appropriately allow far infrared rays to be transmitted and can appropriately improve scratch resistance.

[0093] The transmittance of the far-infrared ray transmitting member 20 to light of 10 μm is preferably 50% or more, more preferably 65% ​​or more, and further preferably 70% or more. In addition, the average transmittance of the far-infrared ray transmitting member 20 to light of wavelength 8 μm to 12 μm is preferably 50% or more, more preferably 65% ​​or more, and further preferably 70% or more. When the transmittance and the average transmittance are within this range, the function as an infrared ray transmitting member can be appropriately exerted.

[0094] The reflectivity of the far-infrared transmissive component 20 to light of 10 μm is preferably 15% or less, more preferably 10% or less, and further preferably 5% or less. In addition, the average reflectivity of the far-infrared transmissive component 20 to light of wavelength 8 μm to 12 μm is preferably 15% or less, more preferably 10% or less, and further preferably 5% or less. By having the reflectivity and average reflectivity within this range, the function as an infrared transmissive component can be properly exerted. It should be noted that the average reflectivity refers to the average value of the reflectivity of light of each wavelength in the band (here 8 μm to 12 μm). The reflectivity can be measured, for example, using a Fourier transform infrared spectrometer (manufactured by ThermoScientific, Nicolet iS10).

[0095] The surface 20A (at the outer side of the vehicle) of the far infrared ray transmitting member 20 Figure 5 In the example, NiO x The hardness of the surface 34a of the layer 34 is 10 GPa or more, preferably 12 GPa or more, more preferably 13 GPa or more, and most preferably 15 GPa or more. When the hardness of the surface 20A is within this range, the scratch resistance can be appropriately improved.

[0096] The hardness of the surface 20A refers to the indentation hardness (indentation hardness) within the range of an indentation depth of 40 nm or more and 110 nm or less, measured by a nanoindentation method (continuous rigidity measurement method) using a nanoindenter. More specifically, the indentation hardness refers to a value obtained from a displacement-load curve of the measuring indenter from the time when a load is applied to the time when a load is removed, and is specified in ISO 14577.

[0097] The indentation hardness can be measured as follows. Specifically, using the iMicro nanoindenter manufactured by KLA, the indentation depth h (nm) corresponding to the indentation load P (mN) is continuously measured throughout the entire process from the start of the load application to the removal of the load at the measurement site, and a Ph curve is prepared. Then, the indentation hardness H (GPa) is calculated based on the prepared Ph curve.

[0098] H=P / A ……(2)

[0099] In formula (2), P is the indentation load (mN), A is the projected area of ​​the indenter (μm 2 ).

[0100] In this embodiment, the maximum value H of the indentation hardness H in the range of indentation depth of 40 nm or more and 110 nm or less is set to max As the hardness of the surface 20A.

[0101] The Young's modulus E of the far-infrared transmitting member 20 is preferably 210 GPa or more and 300 GPa or less, more preferably 220 GPa or more and 300 GPa or less, and further preferably 230 GPa or more and 300 GPa or less. max Ratio H to Young's modulus E max / E is preferably 0.045 or more and 0.120 or less, more preferably 0.050 or more and 0.120 or less, further preferably 0.060 or more and 0.120 or less, and particularly preferably 0.070 or more and 0.120 or more. The maximum value H of the indentation hardness H of the surface 36a is max The Young's modulus E and the Young's modulus E can be measured by the nanoindentation method. The maximum value H of the Young's modulus E and the indentation hardness H of the far-infrared transmitting member 20 is max Ratio H to Young's modulus E max When / E is within this range, the film is less likely to break and is easily restored, so that a film with strong damage resistance is obtained and scratch resistance is improved.

[0102] The Δa*b* of the far-infrared ray transmitting member 20 is preferably 5 or less, more preferably 4 or less, further preferably 3 or less, particularly preferably 2 or less, and most preferably 1 or less. Δa*b* refers to the distance from the origin coordinates of a*b* in the CIE-Lab colorimetric system obtained from the 5-degree incident visible light reflection spectrum. That is, Δa*b* is calculated using the following formula (3). When Δa*b* is within this range, the visible light reflected from the far-infrared ray transmitting member 20 becomes a neutral color, and an appearance that ensures the design of the appearance can be obtained.

[0103] Δa*b*=(a* 2 +b* 2) 0.5 …… (3)

[0104] A* and b* are chromaticity coordinates of reflected light in the CIE-Lab colorimetric system when standard light source D65 is used as illumination light, and can be calculated based on JIS Z 8781-4 using spectral reflectance measured based on JIS R3106.

[0105] In particular, the far infrared ray transmitting member 20 has NiO whose extinction coefficient in the visible light region changes depending on the degree of oxidation. x In the case of a film, it is possible to suppress the NiO x Changes in a* and b* are associated with changes in the degree of oxidation of the film.

[0106] In addition, preferably Figure 3 The surface 20A of the vehicle outer side of the far-infrared transmission member 20 shown is formed flush (continuously) with the surface of the vehicle outer side of the shading area A2. In other words, the far-infrared transmission member 20 is installed in a manner that the surface 20A of the vehicle outer side is continuous with the surface 12A of the glass substrate 12. By making the surface 20A of the far-infrared transmission member 20 continuous with the surface 12A of the glass substrate 12 in this way, it is possible to suppress the wiping effect of the wiper from being impaired. In addition, it is possible to suppress the possibility of damaging the design of the vehicle V due to the height difference, and the accumulation of sand and dust at the height difference. In addition, the far-infrared transmission member 20 is preferably formed in accordance with the curved surface shape of the vehicle glass 1 to which it is applied. There is no particular limitation on the molding method of the far-infrared transmission member 20, and grinding or mold molding is selected according to the curved surface shape and the member.

[0107] The shape of the far-infrared ray transmitting member 20 is not particularly limited, but is preferably a plate-like shape that matches the shape of the opening 19. That is, for example, when the opening 19 is circular, the far-infrared ray transmitting member 20 is preferably a disk-like shape (cylindrical shape). In addition, from the viewpoint of appearance design, the surface shape of the far-infrared ray transmitting member 20 on the outside of the vehicle can be processed to match the curvature of the outer surface shape of the glass substrate 12. In addition, for reasons such as achieving a wide angle of view of the far-infrared camera CA1 and improving mechanical properties, the far-infrared ray transmitting member 20 can be made into a lens shape. When such a structure is made, even if the area of ​​the far-infrared ray transmitting member 20 is small, it is possible to effectively focus the far infrared rays, so it is preferred. In this case, the number of the lens-shaped far-infrared ray transmitting members 20 is preferably 1 to 3, and typically preferably 2. In addition, the lens-shaped far-infrared ray transmitting member 20 is particularly preferably pre-aligned and made into a module, and integrated with a housing or a bracket that glues the far-infrared camera CA1 to the vehicle glass 1.

[0108] For the vehicle glass 1 of this embodiment, it is preferable to have a structure in which the area of ​​the opening 19 on the surface on the vehicle inner side is smaller than the area of ​​the opening 19 on the surface on the vehicle outer side, and the shape of the far-infrared ray transmitting member 20 is also consistent with it so that the area on the surface on the vehicle inner side is smaller than the area on the surface on the vehicle outer side. By making such a structure, the strength against the impact from the vehicle outer side is improved. Further, in the case where the vehicle glass 1 of this embodiment is a laminated glass having a glass substrate 12 (vehicle outer side) and a glass substrate 14 (vehicle inner side), the opening 19 is formed by overlapping the opening 12a of the glass substrate 12 and the opening 14a of the glass substrate 14. In this case, the area of ​​the opening 12a of the glass substrate 12 can be made larger than the area of ​​the opening 14a of the glass substrate 14, and the far-infrared ray transmitting member 20 having the same size as the opening 12a of the glass substrate 12 is arranged in the opening 12a of the glass substrate 12.

[0109] In addition, if Figure 3 As shown, regarding the far infrared ray transmitting member 20, the length d1 of the longest straight line among the straight lines connecting any two points in the surface of the vehicle outer side is preferably 80 mm or less. The length d1 is more preferably 70 mm or less, and further preferably 65 mm or less. In addition, the length d1 is preferably 60 mm or more. In addition, as Figure 3 As shown, regarding the opening 19 of the far-infrared transmission area B, the length d2 of the longest straight line connecting any two points in the surface on the outside of the vehicle is preferably 80 mm or less. The length d2 is more preferably 70 mm or less, and further preferably 65 mm or less. In addition, the length d2 is preferably 60 mm or more. The length d2 can also be said to be the length of the longest straight line connecting any two points on the outer periphery of the opening 19 on the surface (surface 12A) on the outside of the vehicle of the vehicle glass 1. By keeping the length d1 of the far-infrared transmission member 20 and the length d2 of the opening 19 within this range, the reduction in the strength of the vehicle glass 1 can be suppressed, and the perspective distortion around the opening 19 can also be suppressed. It should be noted that when the shape of the surface on the outside of the vehicle of the far-infrared transmission member 20 is circular, the lengths d1 and d2 are lengths equivalent to the diameter of the surface on the outside of the vehicle. In addition, the lengths d1 and d2 herein refer to the lengths when the vehicle glass 1 is mounted on the vehicle V. For example, when the glass is bent to form a shape to be mounted on the vehicle V, the lengths d1 and d2 are the lengths after the bending process. The same applies to the description of dimensions and positions other than the lengths d1 and d2 unless otherwise specified.

[0110] (Method for manufacturing infrared-transmitting member)

[0111] Next, a method for manufacturing the far infrared ray transmitting member 20 will be described. In this embodiment, NiO is formed on the substrate 30 by post-oxidation sputtering. x The far-infrared transparent member 20 is manufactured by forming the layer 34. Hereinafter, a method for manufacturing the far-infrared transparent member 20 will be specifically described. However, the far-infrared transparent member 20 may be manufactured by any manufacturing method so as to have the above-mentioned characteristics.

[0112] Figure 6 FIG. 2 is a schematic diagram for explaining a method for manufacturing a far-infrared transmitting member according to the present embodiment. Figure 6 As shown, in the present manufacturing method, the substrate 30 is arranged in the first space SP1 (step S10). In the first space SP1, a target T is arranged and connected to the inert gas supply unit M1. The target T is NiO laminated on the substrate 30. x The substrate 30 is a raw material for forming the NiO layer 34. x The surface 30a of one side of the layer 34 is arranged in the first space SP1 so as to face the target T. The inert gas supply unit M1 is a device for supplying the inert gas G into the first space SP1, so that the first space SP1 is filled with the inert gas G. As the inert gas G, argon gas is used, but it is not limited to this, and for example, a rare gas other than argon gas may be used.

[0113] After the substrate 30 is arranged in the first space SP1, an inert gas G is introduced into the first space SP1 where the target T and the substrate 30 are arranged, thereby performing sputtering, so that Ni contained in the target T is stacked on the surface 30a of the substrate 30 (step S12; stacking step). Specifically, in this step, in a state where the first space SP1 is made vacuous, an inert gas G is introduced into the first space SP1 from the inert gas supply unit M1. Then, the inert gas G is ionized by applying a negative voltage to the target T, and the ionized inert gas G collides with the surface of the substrate 30. As a result, the components (atoms, molecules) contained in the target T, in this case, Ni contained in the target T, are ejected from the target T and stacked on the surface 30a of the substrate 30. Hereinafter, the stack containing Ni stacked on the surface 30a of the substrate 30 is described as a stack 34A.

[0114] It should be noted that the component ejected from the target T and stacked in the form of the stacked body 34A is not limited to Ni, and other atoms, molecules, and other components contained in the target T (such as NiO x ) may also be ejected from the target T and stacked in the form of a stacked body 34A. That is, the stacked body 34A can be said to be a layer containing at least Ni.

[0115] In the stacking step, as described above, the inert gas G is introduced into the first space SP1 while the first space SP1 is in a vacuum state. The vacuum here may refer to, for example, adjusting the pressure to 10Pa or less, and the same applies to the following. In addition, in the stacking step, the inert gas G is preferably introduced in such a manner that the pressure in the first space SP1 is preferably less than 0.5Pa, more preferably less than 0.4Pa, and more preferably less than 0.3Pa. That is, in this step, it is preferably set in such a manner that the gas pressure in the first space SP1 containing the inert gas G is within the above-mentioned range. By adjusting the first space SP to such a gas pressure, the energy loss of the sputtered particles can be reduced, and a high-hardness and smooth NiO can be formed. x The layer 34 can improve the scratch resistance.

[0116] Next, the base material 30 on which the stacked body 34A is stacked is disposed in the second space SP2 (step S14). The second space SP2 is connected to the oxygen supply unit M2. The oxygen supply unit M2 is a device for supplying oxygen O.

[0117] After the substrate 30 is disposed in the second space SP2, oxygen plasma (plasma-like oxygen) is generated in the second space SP2, thereby oxidizing the stacked body 34A stacked on the substrate 30, thereby forming NiO on the substrate 30. x Specifically, in a state where the second space SP2 is in a vacuum state, oxygen O is supplied from the oxygen supply unit M2 into the second space SP2, and the oxygen O in the second space SP2 is plasmatized to generate oxygen plasma. In the second space SP2, the generated oxygen plasma contacts the stacked body 34A stacked on the substrate 30 and oxidizes the stacked body 34A, thereby forming NiO on the substrate 30. x That is, Ni contained in the stacked body 34A is oxidized by oxygen plasma to become NiO x It is believed that the volume expansion of the film occurs during the oxidation process, and the hardness increases due to the high density. As a result, the stacked body 34A becomes a NiO x NiO as the main component x Layer 34, thereby forming NiO on the substrate 30 x Layer 34. It should be noted that not only oxygen plasma but also oxygen radicals and oxygen ions may be generated to cause oxidation.

[0118] The target T contains Ni. For the target T, the Ni content is preferably 50 atomic % or more and 100 atomic % or less, more preferably 60 atomic % or more and 100 atomic % or less, 70 atomic % or more and 100 atomic % or less, or 80 atomic % or more and 100 atomic % or less, relative to the entire target T. When the Ni content in the target T is within this range, the volume expansion rate of the film in the oxidation process can be increased, and the film density becomes higher, so that a high-hardness NiO can be formed. x Layer 34 can improve the scratch resistance. It should be noted that the target T may contain NiO x As components other than Ni.

[0119] In the oxidation step, based on a total flow rate of 80 sccm, it is preferred to supply oxygen O of 10 sccm or more and 60 sccm or less to the second space SP2, and the supplied oxygen O is plasmatized to form oxygen plasma. Further, in the oxidation step, oxygen O of more preferably 20 sccm or more and 60 sccm or less, and further preferably 20 sccm or more and 40 sccm or less can be supplied to the second space SP2. The amount of oxygen required varies depending on the size of the chamber (equivalent to the size of the second space SP2), so the oxygen flow rate ratio in the total amount of gas in the second space SP2 is preferably 10% or more and 75% or less, more preferably 12% or more and 75% or less, and further preferably 25% or more and 50% or less. In other words, in the oxidation step, it can be said that it is preferred to plasmatize oxygen O at a flow rate within the above range to form oxygen plasma. By setting the supply amount of oxygen O within the above range, Ni can be appropriately oxidized, thereby forming high-hardness NiO without reducing the transmittance and average transmittance of far-infrared rays. x The layer 34 can improve the scratch resistance.

[0120] In the oxidation step, oxygen plasma can be generated by any method, for example, by providing an electrode in the second space SP2 and applying a voltage to the electrode, thereby plasmatizing the oxygen O in the second space SP2 to generate oxygen plasma. In this case, the power applied to the electrode is preferably 2 kW or more and 4 kW or less, and more preferably 3 kW or more and 4 kW or less. By setting the applied power within the above range, Ni can be appropriately oxidized to form NiO with high hardness. x The layer 34 can improve the scratch resistance.

[0121] In this embodiment, the processes of step S10 to step S16 may be repeated to form a NiO film in a gradually thickening manner. x Layer 34.

[0122] It should be noted that, in the present embodiment, the first space SP1 and the second space SP2 are isolated and separate spaces (rooms), and the NiO is formed by performing the above-mentioned stacking step and oxidation step while moving the substrate 30 from the first space SP1 to the second space SP2 or from the second space SP2 to the first space SP1. x The substrate 30 may be moved between the first space SP1 and the second space SP2 by any method. For example, the substrate 30 may be mounted on the surface of a rotatable drum to form the first space SP1 and the second space SP2 in a manner arranged along the rotation direction of the drum. In this case, the substrate 30 moves from the first space SP1 to the second space SP2 (or from the second space SP2 to the first space SP1) by the rotation of the drum.

[0123] In addition, the first space SP1 and the second space SP2 may be the same space (room). In this case, the substrate 30 may be placed in the space, and after forming a vacuum, a voltage may be applied to the target T while introducing an inert gas G to perform sputtering, and then oxygen plasma may be supplied into the space to oxidize the stack 34A to form NiO. x Layer 34.

[0124] (Effect)

[0125] As described above, the far infrared ray transmitting member 20 of the present embodiment includes a substrate 30 that allows far infrared rays to be transmitted and a functional film (first functional film 32) formed on the substrate 30 and having a NiO x NiO as the main component x Layer 34. The far-infrared transmissive member 20 has an average transmittance of 50% or more to light having a wavelength of 8 μm to 12 μm, and a hardness of 10 GPa or more as measured by a nanoindentation method.

[0126] Here, the far-infrared transmitting member is required to appropriately allow far-infrared transmission and improve scratch resistance. x NiO as the main component x Layer 34 can appropriately allow far infrared rays to pass through and improve scratch resistance. Further, diamond-like carbon (DLC) can also improve scratch resistance, but the film forming process of DLC is limited and elastic modulus control is required, so the load in the film forming process becomes high. In contrast, by using NiO as in this embodiment, x NiO as the main component x The layer 34 can reduce the load in the film forming step and improve the scratch resistance.

[0127] In the manufacturing method of this embodiment, NiO is formed on the substrate 30 that allows far infrared rays to pass through by post-oxidation sputtering. x NiO as the main component x The far infrared ray transmitting member 20 is manufactured by forming the layer 34. By using the post-oxidation sputtering method, a high-hardness NiO layer having a hardness of 10 GPa or more measured by the nanoindentation method can be formed. x The layer 34 can therefore appropriately allow far infrared rays to be transmitted, and can improve scratch resistance.

[0128] In addition, the manufacturing method of this embodiment preferably includes a stacking step and an oxidation step. In the stacking step, an inert gas G is introduced into the first space SP1 where the target T containing Ni and the substrate 30 are arranged, thereby stacking the stack 34A containing Ni in the target T on the substrate 30. In the oxidation step, the substrate 30 stacked with the stack 34A is arranged in the second space SP2, and oxygen plasma is generated in the second space SP2, thereby oxidizing the stack 34A stacked on the substrate 30, thereby forming NiO on the substrate 30. x By using the post-oxidation sputtering method as described above, it is possible to form a NiO layer having a hardness of 10 GPa or more as measured by the nanoindentation method. x The layer 34 can therefore appropriately allow far infrared rays to be transmitted, and can improve scratch resistance.

[0129] (Other examples)

[0130] Next, another example of the stacked structure of the far-infrared transmissive member 20 will be described.

[0131] (Outermost layer)

[0132] Figure 7 FIG. 2 is a cross-sectional schematic diagram of another example of a far-infrared transmission member of the present embodiment. Figure 7 As shown, the first functional film 32 may have an outermost layer 39. The outermost layer 39 is provided in the first functional film 32 with NiO x The side of the layer 34 opposite to the substrate 30 (NiO in this embodiment) x The outermost layer 39 is a layer on the outer side of the first functional film 32 (the side closest to the outside of the vehicle in this embodiment). In other words, the outermost layer 39 is the outermost layer of the far-infrared transmission member 20 and is exposed to the outside. Therefore, the surface 39a of the outermost layer 39 on the outer side of the vehicle becomes the surface 20A of the far-infrared transmission member 20.

[0133] It should be noted that in Figure 7 In the example, the first functional film 32 has only NiO xThe first functional film 32 may include a NiO layer 34 and an outermost layer 39, but is not limited thereto, and may further include at least one of a hue adjustment layer and an adhesion layer described later. x In addition to the layer 34, it also has an outermost layer 39, at least one of a color phase adjustment layer and an adhesive layer.

[0134] The outermost layer 39 preferably has a hardness equal to that of NiO x When the outermost layer 39 is provided, the maximum value H of the indentation hardness H of the far infrared ray transmitting member 20 is max By forming such a hard outermost layer 39 on the surface, the far infrared ray transmitting member 20 can be appropriately protected from damage caused by wiper wiping, sand and dust, and the like.

[0135] The refractive index of the outermost layer 39 for light (visible light) with a wavelength of 550 nm is preferably 2.5 or less, more preferably 1.5 or more and 2.5 or less, and further preferably 1.7 or more and 2.4 or less. In addition, the average refractive index of the outermost layer 39 for light with a wavelength of 380 nm to 780 nm is preferably 2.5 or less, more preferably 1.5 or more and 2.5 or less, and further preferably 1.7 or more and 2.4 or less. By having the refractive index and average refractive index of the outermost layer 39 for visible light within this numerical range, the reflection of visible light can be suppressed, thereby making the far-infrared transmissive member 20 inconspicuous.

[0136] The refractive index of the outermost layer 39 for light (far-infrared light) with a wavelength of 10 μm is preferably 0.5 or more and 3.5 or less, more preferably 0.7 or more and 2.5 or less, and further preferably 1.0 or more and 2.5 or less. In addition, the average refractive index of the outermost layer 39 for light with a wavelength of 8 μm to 12 μm is preferably 0.5 or more and 3.5 or less, more preferably 0.7 or more and 2.5 or less, and further preferably 1.0 or more and 2.5 or less. By making the refractive index and average refractive index of the outermost layer 39 for far-infrared light within this numerical range, the reflection of far-infrared light can be suppressed, thereby appropriately allowing the transmission of far-infrared light.

[0137] The outermost layer 39 can allow far infrared rays to pass through. The extinction coefficient of the outermost layer 39 for light with a wavelength of 10 μm is preferably 0.4 or less, preferably 0.2 or less, and more preferably 0.1 or less. The average extinction coefficient of the outermost layer 39 for light with a wavelength of 8 μm to 12 μm is preferably 0.4 or less, preferably 0.2 or less, and more preferably 0.1 or less. When the extinction coefficient and the average extinction coefficient are within this range, far infrared rays can be appropriately allowed to pass through.

[0138] In addition, the thickness of the outermost layer 39 is preferably 0.01 μm or more and 1 μm or less, more preferably 0.02 μm or more and 0.5 μm or less, and further preferably 0.05 μm or more and 0.3 μm or less. By having the thickness within this range, the reflection of far infrared rays and visible light can be appropriately suppressed. It should be noted that the thickness of the outermost layer 39 can also be said to be the length in the Z direction from the surface of the outermost layer 39 on the Z direction side to the surface on the side opposite to the Z direction.

[0139] The material of the outermost layer 39 is arbitrary, but preferably includes, for example, a material selected from ZrO2, Al2O3, TiO2, Si3N 4、 At least one material selected from the group consisting of AlN, MgF 2 , YF 3 and diamond-like carbon. By using such a material for the outermost layer 39 , the chemical stability of the far infrared ray transmitting member 20 can be ensured, and the far infrared ray transmitting member 20 can be appropriately protected.

[0140] In order to protect the far infrared ray transmission member 20 from the influence of water, the outermost layer 39 preferably has water barrier properties. The water barrier properties of the outermost layer 39 vary depending on the material, crystal structure, and film thickness. In addition, from the perspective of water barrier properties, the outermost layer 39 is preferably an amorphous structure. In addition, the outermost layer 39 is preferably a low friction coefficient. In addition, the outermost layer 39 may have a wettability improvement function.

[0141] It should be noted that the outermost layer 39 may also be NiO x The layer 34 is similarly formed by post-oxidation sputtering, but the present invention is not limited thereto and may be formed by any method, for example, by sputtering other than post-oxidation sputtering (eg, reactive sputtering) or evaporation.

[0142] (Hue adjustment layer)

[0143] In the first functional film 32, NiO x Between the layer 34 and the outermost layer 39 (NiO x A hue adjustment layer is provided on the vehicle outer side of the layer 34. The hue adjustment layer is a layer for suppressing the interference color of the far-infrared transmissive member 20 by reducing the difference in reflectivity (reflectivity dispersion) for visible light of different wavelengths, thereby ensuring the design of the appearance.

[0144] The hue adjustment layer can allow far infrared rays to pass through. The hue adjustment layer may be composed of only one layer or a plurality of layers.

[0145] The hue adjustment layer can be combined with NiO x The layer 34 is similarly formed by post-oxidation sputtering, but the present invention is not limited thereto and may be formed by any method, for example, by sputtering other than post-oxidation sputtering (eg, reactive sputtering) or evaporation.

[0146] The refractive index of the hue adjustment layer for light with a wavelength of 550nm (visible light) can be compared with that of NiO x The layer 34 has a different refractive index for light (visible light) with a wavelength of 550 nm. The refractive index of the hue adjustment layer for light (visible light) with a wavelength of 550 nm is preferably 2.2 or more and 2.5 or less, and more preferably 2.3 or more and 2.4 or less. When the refractive index of the hue adjustment layer for visible light is within this numerical range, the reflection dispersion of visible light can be suppressed, thereby making the far-infrared transmissive member 20 inconspicuous.

[0147] The hue adjustment layer can allow far infrared rays to pass through. The extinction coefficient of the hue adjustment layer for light with a wavelength of 10 μm is preferably 0.4 or less, preferably 0.2 or less, and more preferably 0.1 or less. When the extinction coefficient is within this range, far infrared rays can be appropriately allowed to pass through.

[0148] The thickness of the hue adjustment layer is preferably 5 nm to 100 nm, more preferably 10 nm to 60 nm, and even more preferably 20 nm to 50 nm. x The ratio of the thickness D2 of the layer 34 is preferably 0.5% or more and 10% or less, more preferably 1% or more and 6% or less, and further preferably 2% or more and 5% or less. When the thickness of the hue adjustment layer is within this range, far infrared rays can be appropriately allowed to be transmitted, while the reflection dispersion of visible light can be suppressed, so that the far infrared ray transmission member 20 is not conspicuous. It should be noted that the thickness of the hue adjustment layer can also be said to be the length in the Z direction from the surface of the hue adjustment layer on the Z direction side to the surface on the side opposite to the Z direction.

[0149] In this example, the hue adjustment layer includes a first layer and a second layer, wherein the second layer is disposed on the NiO x On the layer 34 side (outside the vehicle).

[0150] In this example, the first layer is a layer with ZrO2 as the main component. In the first layer, the content of ZrO2 is 50% by mass or more and 100% by mass or less, preferably 70% by mass or more and 100% by mass or less, and more preferably 90% by mass or more and 100% by mass or less relative to the first layer as a whole. In addition, the first layer is preferably ZrO2 alone, that is, the content of ZrO2 is 100% by mass except for unavoidable impurities. The first layer may contain a minor component, which is a component other than ZrO2 as the main component. As a minor component, an oxide that allows far infrared light to be transmitted is preferably used, and examples thereof include: NiO x 、ZnO、Bi2O3、CuO x .

[0151] The first layer can allow far infrared rays to pass through. The extinction coefficient of the first layer for light with a wavelength of 10 μm is preferably 0.10 or less, more preferably 0.05 or less, and further preferably 0.04 or less.

[0152] The refractive index of the first layer for light (visible light) having a wavelength of 550 nm is preferably 2.05 or more, more preferably 2.05 or more and 2.40 or less, further preferably 2.10 or more and 2.30 or less, particularly preferably 2.15 or more and 2.25 or less.

[0153] The thickness of the first layer is preferably 10 nm to 40 nm, more preferably 15 nm to 35 nm, and even more preferably 20 nm to 30 nm. x The ratio of the thickness D2 of the layer 34 is preferably 1% to 4%, more preferably 1.5% to 3.5%, and even more preferably 2% to 3%.

[0154] In this case, the second layer is made of materials and has the same properties as NiO x The second layer is the same layer as the NiO layer 34. However, the thickness of the second layer is preferably 5 nm to 40 nm, more preferably 5 nm to 25 nm, and even more preferably 10 nm to 30 nm. x The ratio of the thickness D2 of the layer 34 is preferably 0.5% to 4%, more preferably 0.5% to 2.5%, and even more preferably 1% to 3%.

[0155] In this example, the hue adjustment layer is composed of two layers, the first layer and the second layer, but is not limited thereto, and a laminate of multiple first layers and second layers may be stacked. The hue adjustment layer is preferably a layer obtained by alternately stacking the first layer and the second layer 2n (n is a natural number greater than 1) layers from the substrate 30 side. Regarding the film thickness ratio of each layer in the hue adjustment layer, it is preferred that the film thickness ratio of the layer with a low refractive index for light (visible light) with a wavelength of 550nm is high. By keeping the stacking order and the number of layers of the hue adjustment layer within this range, the reflection dispersion of visible light can be suppressed, thereby making the far-infrared ray transmitting component 20 inconspicuous.

[0156] However, the composition of the color adjustment layer is not limited to the first layer including ZrO2 as a main component and the material and NiO x The second layer, which is the same as the layer 34, may have any configuration.

[0157] (Adhesion layer)

[0158] In NiO x An adhesion layer may be formed between the layer 34 and the substrate 30. The adhesion layer is to allow the substrate 30 to be attached to the NiOx The layer 34 is a film that adheres to the substrate 30 and the NiO x The adhesion of layer 34 is improved.

[0159] The refractive index of the adhesive layer for light with a wavelength of 10 μm is preferably 1.0 to 4.3, more preferably 1.5 to 4.3, and even more preferably 1.5 to 3.8. When the refractive index is within this range, reflection of far infrared rays can be appropriately suppressed.

[0160] In addition, the thickness of the adhesive layer is preferably 0.05 μm or more and 0.5 μm or less, more preferably 0.05 μm or more and 0.3 μm or less, and further preferably 0.05 μm or more and 0.1 μm or less. When the thickness of the adhesive layer is within this range, the reflection of far infrared rays can be appropriately suppressed, and the substrate 30 and NiO can be made to be close to each other. x The thickness of the adhesive layer can also be referred to as the length in the Z direction from the surface of the adhesive layer on the Z direction side to the surface on the side opposite to the Z direction. In addition, the thickness of the adhesive film 40 is preferably thicker than NiO. x The thickness D2 of the layer 34 is thin. By making the thickness of the adhesive film 40 thinner than the thicknesses of these layers, the influence on the optical performance can be reduced.

[0161] The adhesive layer can allow far infrared rays to pass through. The extinction coefficient of the adhesive layer for light with a wavelength of 10 μm is preferably 0.4 or less, preferably 0.2 or less, and more preferably 0.1 or less. When the extinction coefficient is within this range, far infrared rays can be appropriately allowed to pass through.

[0162] The material of the adhesion layer is arbitrary, but preferably includes, for example, a material selected from Si, Ge, MgO, NiO x , CuO x At least one material selected from the group consisting of ZnS, Al2O3, ZrO2, SiO2, TiO2, ZnO and Bi2O3, more preferably ZrO2. The adhesion layer may contain such a material to appropriately adhere the substrate 30 and the hue adjustment layer.

[0163] It should be noted that the adhesion layer can also be made of NiO x The layer 34 is similarly formed by post-oxidation sputtering, but the present invention is not limited thereto and may be formed by any method, for example, by sputtering other than post-oxidation sputtering (eg, reactive sputtering) or evaporation.

[0164] (Example)

[0165] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited thereto. Tables 1 and 2 are tables showing the far-infrared transmitting members of the respective Examples.

[0166] [Table 1]

[0167]

[0168] [Table 2]

[0169]

[0170] (Example 1)

[0171] A far infrared ray transmitting member was produced using the data in Table 3 of Non-Patent Document 1. NiO was formed on both sides of a substrate made of Si (100 orientation, P type) mirror-polished on both sides by RF magnetron sputtering. x The thickness of the substrate is 0.525 mm, and the NiO x The thickness of the layer was 1200 nm. It should be noted that the thickness of the substrate was measured using a digital vernier caliper (CD-15CX, manufactured by Mitutoyo Co., Ltd.). In addition, the thickness of the functional film was evaluated using a stylus-type surface profiler (Dektak XT-S, manufactured by BRUKER).

[0172] (Example 2)

[0173] As shown in Table 1, in Example 2, NiO was formed on a substrate made of Si (FZ grade) by reactive sputtering using a carousel type sputtering apparatus. x Film (first film). Substrate, NiO x The thickness of the film was set to the thickness shown in Table 1.

[0174] NiO x The film formation conditions were as follows, and some of the conditions are also shown in Table 1. The film formation pressure was adjusted by the APC valve opening of the turbomolecular pump.

[0175] (Film formation conditions of Example 2)

[0176] Ni content of target: element ratio 61%

[0177] Target: Ni (30 mass%) + NiO (70 mass%) mixed target

[0178] Sputtering gas: Ar

[0179] Ar flow rate: 120sccm

[0180] Reactive gas: O2

[0181] Oxygen flow rate: 30sccm

[0182] Input power (output power): 3000W

[0183] Substrate temperature: room temperature

[0184] (Example 3)

[0185] As shown in Table 1, in Example 3, NiO was formed on the same substrate as in Example 2 by post-oxidation sputtering using a load-lock sputtering apparatus (RAS-1100BII, manufactured by SHINCRON Corporation). x Film (first film). Substrate, NiO x The thickness of the film was set to the thickness shown in Table 1.

[0186] NiO x The film formation conditions are as follows, and some of the conditions are also shown in Table 1. In addition, RF power is the power applied to the electrode when plasma is generated.

[0187] (Film formation conditions of Example 3)

[0188] Ni content of target: element ratio 61%

[0189] Target: Ni (30 mass%) + NiO (70 mass%) mixed target

[0190] [Layering steps]

[0191] Sputtering power: 6kW

[0192] Sputtering gas: Ar

[0193] Ar flow rate: 150sccm

[0194] [Oxidation step]

[0195] Reactive gas: Ar+O2

[0196] Oxygen flow rate: 10sccm

[0197] Argon gas flow rate: 70sccm

[0198] Substrate temperature: room temperature

[0199] (Example 4~Example 9)

[0200] In Examples 4 to 9, NiO was formed by the same method as in Example 3 except for the conditions shown in Table 1. x Membrane (first membrane).

[0201] (Example 4)

[0202] [Oxidation step]

[0203] Reactive gas: Ar+O2

[0204] Oxygen flow rate: 10sccm

[0205] Argon gas flow rate: 70sccm

[0206] Substrate temperature: room temperature

[0207] (Example 5)

[0208] [Oxidation step]

[0209] Reactive gas: Ar+O2

[0210] Oxygen flow rate: 25sccm

[0211] Argon gas flow rate: 55sccm

[0212] Substrate temperature: room temperature

[0213] (Example 6)

[0214] [Oxidation step]

[0215] Reactive gas: Ar+O2

[0216] Oxygen flow rate: 40sccm

[0217] Argon gas flow rate: 40sccm

[0218] Substrate temperature: room temperature

[0219] (Example 7)

[0220] [Oxidation step]

[0221] Reactive gas: Ar+O2

[0222] Oxygen flow rate: 60sccm

[0223] Argon gas flow rate: 20sccm

[0224] Substrate temperature: room temperature

[0225] (Example 8)

[0226] [Oxidation step]

[0227] Reactive gas: Ar+O2

[0228] Oxygen flow rate: 10sccm

[0229] Argon gas flow rate: 70sccm

[0230] Substrate temperature: room temperature

[0231] (Example 9)

[0232] [Oxidation step]

[0233] Reactive gas: Ar+O2

[0234] Oxygen flow rate: 60sccm

[0235] Argon gas flow rate: 20sccm

[0236] Substrate temperature: room temperature

[0237] (Example 10~Example 11)

[0238] In Examples 10 and 11, NiO was formed on the same substrate as in Example 3 by the same method as in Example 3 except for the conditions shown in Table 2. x The thickness of the substrate and each layer is set to the thickness shown in Table 2. It should be noted that the physical property values ​​recorded in Table 2 represent the physical property values ​​of the layer that becomes the outermost layer when observed from the substrate. It should be noted that the process conditions recorded in Table 2 represent the process conditions of NiO x film forming conditions.

[0239] (Example 10~Example 11)

[0240] (NiO x film forming conditions)

[0241] [Layering steps]

[0242] Sputtering power: 6kW

[0243] Sputtering gas: Ar

[0244] Ar flow rate: 120sccm

[0245] [Oxidation step]

[0246] Reactive gas: Ar+O2

[0247] Oxygen flow rate: 10sccm

[0248] Argon gas flow rate: 70sccm

[0249] Substrate temperature: room temperature

[0250] (Film formation conditions of ZrO2 film)

[0251] [Layering steps]

[0252] Target: Zr target

[0253] Sputtering power: 6kW

[0254] Sputtering gas: Ar

[0255] Sputtering gas flow rate: 150sccm

[0256] [Oxidation step]

[0257] Reactive gas: O2

[0258] Oxygen flow rate: 100sccm

[0259] RF power: 4kW

[0260] Substrate temperature: room temperature

[0261] Film forming pressure: 0.21Pa

[0262] (Average transmittance of light with a wavelength of 8μm to 12μm)

[0263] The physical property values ​​of the far-infrared transmissive member of each example were measured.

[0264] The NiO formed on the Ge substrate was measured x The infrared transmittance (FIR-T) of the film is used as a physical property value. As a measurement method, a Fourier transform infrared spectrometer (manufactured by ThermoScientific, trade name: Nicolet iS10) was used to measure the transmittance of light of each wavelength of 2500nm to 25000nm, and the refractive index and extinction coefficient of the film were analyzed based on the measured transmittance. Based on the values ​​obtained by the analysis, optical simulation was used to calculate the average transmittance of the film structure at a wavelength of 8μm to 12μm when used as a far-infrared transmission component. The optical simulation was performed using simulation software (manufactured by Hulinks Co., Ltd., TFCalc).

[0265] (Arithmetic mean roughness Ra)

[0266] The first film (NiO x The arithmetic mean roughness Ra of the surface of the film is taken as the physical property value.

[0267] (The maximum value of the indentation hardness H max )

[0268] The first film (NiO x The indentation hardness H of the surface of the first functional film was taken as the physical property value. Regarding the indentation hardness H, the indentation hardness H in the film thickness direction (depth direction) of the first functional film was measured by the nanoindentation method using an iMicro nanoindenter (manufactured by KLA). The measurement conditions are as follows.

[0269] ・Indenter: Bosch Indenter

[0270] ・Actuator: IF50

[0271] ・Measurement method: Continuous rigidity measurement method

[0272] ・Maximum press load: 50mN

[0273] ・Strain rate: 0.2% / second

[0274] ・Poisson's ratio of the sample: 0.25

[0275] ・Number of measurement points: 15 to 20 points per substrate

[0276] As the maximum value of the indentation hardness H max , the maximum value of the indentation hardness H within the indentation depth range of 40nm to 110nm is adopted.

[0277] Tables 1 and 2 show the measurement results of the physical property values ​​of each example.

[0278] As shown in Table 1, NiO x Example 1 and NiO layer formed by reactive sputtering x In Example 2 of the layer, the maximum value of the indentation hardness H was obtained. max NiO has a low mechanical strength of 10 GPa or less. x On the other hand, NiO is formed by post-oxidation sputtering. x In Examples 3 to 11 of the layer, the maximum value of the indentation hardness H was obtained. max NiO with high mechanical strength of more than 10GPa x Among them, NiO is formed by post-oxidation sputtering. x In Examples 5 to 7 and 9, the maximum value H of the indentation hardness H was obtained, and the O2 gas flow rate ratio in the reaction process area during film formation was set to 25% or more. max NiO has a very high mechanical strength of more than 12 GPa x layer.

[0279] (evaluate)

[0280] The far-infrared transmitting components of each example were evaluated. As an evaluation, a wiper test was performed and the number of scratches formed in the wiper test was measured. Specifically, for the first film (NiO x The wiper test was performed on the surface of the wiper film under the following conditions, and then the sliding part where the wiper slid was observed in a dark field using an optical microscope DSX500 (manufactured by OLYMPUS) at a magnification of 350. In the dark field observation, the number of scratches in the 1.8 mm area perpendicular to the sliding direction was measured.

[0281] The wiper test was conducted in the following manner: the surface on the side farthest from the substrate (outermost side) was worn using a transverse wear tester under the test conditions shown below. A wiper rubber (genuine Toyota product, model 85214-47170) was installed on the transverse wear tester, and a dust solution was dripped between the wiper and the sample, and reciprocating friction was performed while applying a contact load to the wiper. The wiper width was 20 mm, the stroke width was 40 mm, the number of strokes was 2500 reciprocating times, and the load was equivalent to 50 g. The dust solution was prepared by mixing the 8th type of JIS test powder 1 with pure water at a mass ratio of 3:100, and 2 ml of the dust solution was dripped onto the sliding part. The substrate was cleaned every 500 reciprocating times, and the dust solution was dripped again, and a total of 2500 reciprocating frictions were performed.

[0282] In the wiper test, the case where the number of scratches is 5 or less is evaluated as passing, and the case where the number of scratches is more than 5 is evaluated as failing. As shown in Table 1, in Example 2 as a comparative example, it is presumed that the maximum value H of the indentation hardness H is max On the other hand, it is known that in Examples 3 to 11 as embodiments, the wiper test is passed, and far infrared rays can be properly allowed to pass and scratch resistance can be improved.

[0283] (optional comments)

[0284] As an optional evaluation, Δa*b* was evaluated for the far-infrared transmissive components of Examples 10 and 11. The reflectance spectrum in the visible light region was measured using U4100 (manufactured by Hitachi, Ltd.) based on JIS R3106, and the chromaticity coordinates L*a*b* of the reflected light in the CIE-Lab colorimetric system when the standard light source D65 was used as the illumination light were obtained based on JIS Z 8781-4, and Δa*b* was calculated based on the above formula (3). When Δa*b* is 5 or less, the visible light reflected from the far-infrared transmissive component 20 becomes a neutral color, and an appearance that ensures the design of the appearance can be formed. As shown in Table 2, in Example 11, by adding a hue adjustment layer, Δa*b* is reduced, and the design of the appearance is improved.

[0285] The embodiments of the present invention have been described above, but the embodiments are not limited to the contents of the embodiments. In addition, the above-mentioned constituent elements include elements that can be easily thought of by those skilled in the art, substantially the same elements, and elements of so-called equivalent scopes. In addition, the above-mentioned constituent elements can be appropriately combined. In addition, various omissions, substitutions or changes of constituent elements can be performed within the scope of the gist of the above-mentioned embodiments.

[0286] Description of symbols

[0287] 1. Glass for vehicles

[0288] 10, 12, 14 Glass substrate

[0289] 20 Far infrared transmission components

[0290] 30 Base material

[0291] 32. First functional film (functional film)

[0292] 34 NiO x layer

[0293] 36 Second functional film

Claims

1. A far infrared ray transmitting member, wherein: The far infrared ray transmitting component comprises: a substrate that allows far infrared rays to be transmitted; and Functional film, the functional film is formed on the substrate and has one or more layers of NiO x NiO as the main component x layer, The far-infrared ray transmitting member has an average transmittance of 50% or more for light with a wavelength of 8 μm to 12 μm. The maximum value H of the indentation hardness within a range of 40 nm to 110 nm from the surface of the functional film measured by a nanoindentation method. max More than 10GPa.

2. The far-infrared ray transmitting member according to claim 1, wherein The maximum value of the indentation hardness H max Ratio H to Young's modulus E max / E is greater than or equal to 0.045 and less than or equal to 0.

120.

3. The far-infrared ray transmitting member according to claim 1 or claim 2, wherein: The far-infrared transmitting member has an arithmetic mean roughness Ra of 6 nm or less.

4. The far-infrared transmitting member according to any one of claims 1 to 3, wherein The NiO x The extinction coefficient of the layer for light with a wavelength of 10 μm is 0.4 or less.

5. The far-infrared transmitting member according to any one of claims 1 to 4, wherein The NiO x The layer is formed on the outermost side.

6. The far-infrared transmitting member according to any one of claims 1 to 5, wherein The far-infrared ray transmitting member is mounted on a vehicle.

7. The far-infrared ray transmitting member according to claim 6, wherein The far infrared ray transmitting member is arranged on a window member of a vehicle.

8. The far-infrared ray transmitting member according to claim 6 or claim 7, wherein: The far-infrared ray transmitting member is disposed on a pillar outer member of a vehicle.

9. The far-infrared transmitting member according to any one of claims 6 to 8, wherein The far-infrared ray transmitting member is disposed in a light shielding region of the vehicle exterior member.

10. A method for manufacturing a far-infrared transmitting member, wherein: A NiO substrate is formed on a substrate that allows far infrared rays to transmit by a post-oxidation sputtering method. x NiO as the main component x layer, thereby manufacturing a far-infrared transmitting member.

11. The method for manufacturing a far-infrared transmissive member according to claim 10, wherein: The manufacturing method comprises the following steps: a lamination step of introducing an inert gas into a first space in which a target containing Ni and the substrate are arranged, thereby laminating a laminate containing Ni in the target on the substrate; and The oxidation step comprises placing the substrate on which the laminate is stacked in a second space, generating oxygen plasma in the second space, thereby oxidizing the laminate stacked on the substrate, and forming the NiO on the substrate. x layer.

12. The method for manufacturing a far-infrared transmissive member according to claim 11, wherein: In the stacking step, the pressure in the first space is adjusted to be less than 0.5 Pa.

13. The method for manufacturing a far-infrared transmissive member according to claim 11 or claim 12, wherein: In the lamination step, a member having a Ni content of 50% or more and 100% or less in atomic weight ratio is used as the target.

14. The method for producing a far-infrared transmissive member according to any one of claims 11 to 13, wherein: In the oxidation step, oxygen gas having an oxygen flow rate ratio of 10% to 75% of the total amount of gas in the second space is converted into plasma to form the oxygen plasma.

Citation Information

Patent Citations

  • Plasma Processing Apparatus

    CN107230608A

  • Vehicle exterior trim part and vehicle exterior trim part with far infrared camera

    CN114126924A

  • Heat-resistant light shielding film, method for manufacturing the same, diaphragm and light quantity adjusting device

    JP2008197610A

  • Laminated reflective film, manufacturing method therefor, and optical reflector having the same

    JP2015212736A

  • Nd filter and method for manufacturing the same

    JP2018036325A

Cited By

  • Front windshield and automobile

    US12686251B2