Oxychlorination process

By activating the catalyst in the fluidized bed reactor, the problem of increased side reactions in the oxychlorination process is solved, the selectivity and product purity of 1,2-dichloroethane are improved, and the process efficiency is improved.

CN118748989APending Publication Date: 2024-10-08OXYETHYLENE LLP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023512.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-19
Filing Date
2023-01-19
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Although the existing oxychlorination process improves the catalytic activity of converting ethylene into 1,2-dichloroethane (EDC) at high temperatures, it also promotes the occurrence of side reactions, leading to the formation of CO, CO2 and chlorinated hydrocarbons. Reduced EDC selectivity and product purity.

Method used

By using an activated catalyst in a fluidized bed reactor, the catalyst is first heated and activated without ethylene conversion to ensure that the catalyst reaches a temperature of more than 150°C under fluidized conditions and remains in this state for more than 6 hours. , to improve the selectivity of EDC and reduce the generation of by-products.

Benefits of technology

It is possible to improve the selectivity and product purity of EDC without reducing the HCl conversion rate, reduce the generation of by-products, and improve process efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005008119180000151
    Figure BDA0005008119180000151
  • Figure BDA0005008119180000152
    Figure BDA0005008119180000152
  • Figure BDA0005008119180000161
    Figure BDA0005008119180000161
Patent Text Reader

Abstract

A process for the production of 1, 2-dichloroethane, the process comprising (i) providing a fluidizable catalyst; (ii) charging the fluidizable catalyst into a fluidized bed reactor; (iii) fluidizing the catalyst within the reactor; (iv) heating the catalyst in the fluidized bed reactor to a temperature greater than 150 DEG C for more than 6 hours while fluidizing the catalyst in the reactor, where the fluidizing and heating steps are carried out without conversion of ethylene; and (v) after the heating step, converting ethylene to 1, 2-dichloroethane in the presence of a catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims the benefit of U.S. Provisional Application No. 63 / 300,799, filed on January 19, 2022, which is incorporated herein by reference. Technical Field

[0002] Embodiments of the present invention provide an oxychlorination process using an activated catalyst. Background Art

[0003] Ethylene dichloride, also known as 1,2-dichloroethane (EDC), can be produced by the oxychlorination of ethylene. The oxychlorination process converts ethylene to EDC by a reaction involving hydrochloric acid and oxygen (or an oxygen-containing species). Water is produced as a by-product. Both fixed bed and fluidized bed processes are commercially available. Fluidized bed processes are typically characterized by a more uniform temperature distribution throughout the reactor because the fluidized bed has enhanced transport characteristics, allowing for gradual catalyst changes while in operation without shutting down the reactor.

[0004] Industrial oxychlorination processes are typically run with excess ethylene to minimize unreacted hydrochloric acid (HCl). As will be appreciated by those skilled in the art, the presence of HCl in the product stream is detrimental because it is not easily removed and can degrade the performance of downstream equipment. HCl conversion is also temperature dependent, with higher temperatures resulting in higher HCl conversion. Therefore, the operating temperature of industrial processes is typically above 220°C. While high temperatures result in increased catalytic activity for the oxidation of ethylene to EDC, unfortunately, higher temperatures also promote undesirable side reactions resulting in the formation of CO and CO2, as well as chlorinated hydrocarbons. In other words, EDC selectivity, as an indicator of the conversion of ethylene to EDC, decreases with increasing byproduct concentrations in the product stream. Among the chlorinated hydrocarbon byproducts, 1,1,2-trichloroethane, trichloroacetaldehyde, ethyl chloride, chloroform, and carbon tetrachloride are common and are typically oxidized as waste streams. In addition, heavier chlorinated organic byproducts may also be produced, thereby reducing not only the selectivity to EDC but also the purity of the product because the heavy chlorinated organic byproducts are not easily separated.

[0005] It would therefore be desirable to reduce the operating temperature of any given catalytic system without reducing HCl conversion, thereby increasing EDC selectivity without a corresponding loss in process efficiency. Summary of the invention

[0006] One or more embodiments of the present invention provide a method for producing 1,2-dichloroethane, the method comprising (i) providing a fluidizable catalyst; (ii) loading the fluidizable catalyst into a fluidized bed reactor; (iii) fluidizing the catalyst in the reactor; (iv) while fluidizing the catalyst in the reactor, heating the catalyst in the fluidized bed reactor to a temperature exceeding 150° C. for more than 6 hours, wherein the fluidizing and heating steps are performed without converting ethylene; and (v) after the heating step, converting ethylene into 1,2-dichloroethane in the presence of the catalyst. DETAILED DESCRIPTION

[0007] Embodiments of the present invention are based at least in part on the discovery of an oxychlorination process that is carried out in a fluidized bed in the presence of an activated catalyst. According to aspects of the present invention, the catalyst is activated before ethylene is converted to 1,2-dichloroethane. In one or more embodiments, activation typically includes heating the catalyst for a sufficient period of time under fluidized conditions without ethylene conversion. It has been observed that by activating the catalyst, the amount of ethylene converted to 1,2-dichloroethane (i.e., EDC selectivity) is increased relative to other conversion products without negatively affecting process efficiency. In other words, activation of the catalyst allows for efficient production of 1,2-dichloroethane while reducing the production of undesirable byproducts. Process Overview and Reactor Configuration

[0008] In one or more embodiments, the oxychlorination process of the present invention is carried out in a fluidized bed reactor, which is suitable for containing and fluidizing the catalyst. Fluidized bed reactors and processes for preparing 1,2-dichloroethane (EDC) by oxychlorination of ethylene are generally known, as disclosed in U.S. Patent No. 5,292,703 and U.S. Patent Publication Nos. 2009 / 0054708, 2009 / 0298682, 2010 / 0274061, 2006 / 0129008 and 2004 / 0192978, which are incorporated herein by reference. In one or more embodiments, the fluidized bed reactor includes a reaction zone in which the conversion of ethylene to EDC is carried out. In one or more embodiments, the reactor is equipped with a temperature control element, such as a steam coil, which can be used to heat or cool the reactor, particularly the reaction zone.

[0009] In one or more embodiments, at least a portion of the fluidized bed reactor includes a fluidizable catalyst composite. The catalyst composite, which may be referred to as a catalyst, includes a catalytic material impregnated on a solid support. The catalytic material (usually a catalytic metal compound) and the solid support will be described in more detail below.

[0010] In one or more embodiments, ethylene, hydrochloric acid, oxygen and / or oxygen-containing material and optional inert gas are sent to reactor as one or more fluid streams. These fluid streams can be injected into reactor under conditions of, for example, force and / or speed, so that catalyst complex is fluidized in bed. In other words, as will be appreciated by those skilled in the art, fluid streams make catalyst complex suspend and mix by reactor (such as reaction zone) in a certain way and make its behavior similar to fluid. In one or more embodiments, reactant and / or gas feed are sent to reactor bottom, and enter reaction zone by one or more distribution elements. In one or more embodiments, the product stream comprising EDC, ethylene by-products, water, unreacted reactant and optional inert gas leaves reactor by an outlet located at or near reactor top.

[0011] In one or more embodiments, the reactor is configured for a once-through process, whereby any unreacted ethylene in the product stream is discharged or otherwise removed. Alternatively, the reactor is configured for a cyclic process, whereby unreacted ethylene is circulated back to the reactor. In one or more embodiments, the product stream is separated to separate non-condensable components, liquid organic matter, and water-soluble compounds. For example, the product stream can be directed to a quenching system that condenses EDC and hydrochloric acid to form a gaseous non-condensable stream and a liquid stream. The liquid stream can be subjected to liquid-liquid separation to separate EDC from aqueous components. The non-condensable stream can contain ethylene, oxygen, and nitrogen and other gaseous components and can be circulated back to the reactor. Catalyst complex

[0012] As described above, the catalyst (which may be referred to as a catalyst composite or catalyst particles) includes a support impregnated with a catalytic metal compound; that is, a support on which a catalytic metal compound is deposited. In one or more embodiments, the catalytic metal compound includes a copper compound, and optionally one or more complementary catalytic metal compounds, which may also be referred to as a co-catalyst. Catalysts that can be used for oxychlorination are generally known, as described in U.S. Patent Publication No. 2014 / 0128643 and U.S. Patent No. 5,292,703, which are incorporated herein by reference. Carrier material

[0013] In one or more embodiments, the support is typically a fluidizable high surface area support material that can be prepared from silica, magnesia, diatomaceous earth, clay, Fuller's earth, alumina, zeolite, or a combination thereof. According to one or more embodiments, the support can be a high surface area powder (e.g., γ, δ, or θ alumina powder), including particles, granules, and / or spheres (e.g., amorphous or colloidal alumina microspheres or nanospheres). In an embodiment, the alumina support can be activated or can be a transitional alumina produced by calcining a hydrated or hydroxylated precursor alumina. These activated aluminas can be identified by the ordered structure observed in their X-ray diffraction patterns, which indicates that the mixed phase material contains minimal or no low surface area or crystalline phase α-alumina.

[0014] Those skilled in the art understand that alpha-alumina can be identified by the crystalline phase determined by x-ray diffraction. The higher surface area activated alumina is generally defined as the gamma alumina phase, but the phase transition can be a continuum of varying percentages of a variety of mixed phases (such as, but not limited to, delta and theta phases) based on the selected calcination temperature to achieve the desired support surface area. In a particular embodiment, gamma-alumina is used as a support. Alumina supports (e.g., gamma-alumina powders) may be referred to as fluidizable alumina supports or fluidizable alumina support materials.

[0015] In one or more embodiments, a useful gamma-alumina support is a powder having at least 90%, or at least 95%, or at least 98%, or at least 99%, or at least 99.995% gamma phase. In these or other embodiments, a useful gamma-alumina support has a surface area of ​​about 50 m 2 / g to about 250m 2 / g, or about 70m 2 / g to about 225m 2 / g, or about 100m 2 / g to about 215m 2 / g, or about 150m 2 / g to about 205m 2 According to an embodiment, a useful alumina support (e.g., γ-alumina powder) has a surface area of ​​at least 80 m 2 In these or other embodiments, useful fluidizable alumina supports may have a compacted bulk density of about 0.5 g / cm 3 To about 4.0g / cm 3 , or about 0.75g / cm 3 To about 3.0g / cm 3 , or about 1.0 g / cm 3 To about 2.0g / cm 3 , or about 0.7 g / cm 3 To about 1.3g / cm3 , or about 3.65g / cm 3 In these or other embodiments, a useful alumina support may have a pore volume of about 0.1 cm 3 / g to about 2cm 3 / g, or about 0.2cm 3 / g to about 1cm 3 / g, or about 0.3cm 3 / g to about 0.75cm 3 / g. In these or other embodiments, the particle size distribution of the fluidizable alumina support material can be such that (a) about 90% to about 100% by volume of the particles have a diameter less than about 150 μm, or less than about 140 μm, or less than about 125 μm, or less than about 110 μm; (b) about 50 to about 60% by volume of the particles have a diameter less than about 75 μm, or less than about 70 μm, or less than about 65 μm, or less than about 60 μm; and (c) about 20 to about 35% by volume of the particles have a diameter less than about 45 μm, or less than about 40 μm, or less than about 35 μm, or less than about 30 μm, as described in Malvern Instruments, Inc. The material sample is dispersed in 100 mL of deionized water for 1 minute at room temperature (about 20° C. to about 25° C.) and pressure (about 1 atmosphere) using a magnetic stirrer to form a suspension, and then 4 mL of the suspension is diluted with 130 mL of deionized water and analyzed using the analyzer at 2500 rpm (at room temperature and pressure).

[0016] Useful alumina supports are commercially available. For example, useful supports are available under the trade name SCCa-57 / 170 and SCCa-25 / 200 (Sasol). These aluminas are high-purity activated aluminas that are easy to fluidize, relatively stable, mechanically strong and wear-resistant.

[0017] In some non-limiting embodiments, the alumina support may contain additional components. Examples of these additional components include, but are not limited to, lanthanum (La), cerium (Ce), titanium (Ti), silicon (Si), etc., which are dispersed throughout the alumina support as trace components prior to impregnation with the active catalyst formulation. For example, the alumina support may contain about 0.005 wt % to about 0.50 wt % of one or more additional components.

[0018] It is also recognized that, in addition to alumina (Al2O3) (and additional components), some alumina support materials may contain small amounts of impurities of other metals, such as metal oxides, e.g., less than about 0.02 wt% sodium oxide, less than about 0.05 wt% iron oxide (Fe2O3), less than about 0.3 wt% titanium dioxide, less than about 0.2 wt% silicon dioxide, etc. In addition, it is known that Ti compounds may remain in the alumina during the alumina production process. Catalytic materials

[0019] As described above, the catalyst complex typically includes one or more metal compounds. In one or more embodiments, the metal compound includes a combination of a copper compound and one or more complementary metal compounds (i.e., a co-catalyst). For example, in one or more embodiments, the metal compound (also referred to as a catalytic metal compound) may include a copper compound, an alkaline earth metal compound (e.g., a magnesium compound), an optional alkali metal compound (e.g., a potassium compound), and a transition metal compound (e.g., a manganese compound or a rhenium compound). Other exemplary catalytic metal compound combinations may include copper compounds, alkaline earth metal compounds (e.g., magnesium compounds), optional alkali metal compounds (e.g., potassium compounds), and rare earth metal compounds (e.g., lanthanum compounds). Other exemplary catalytic metal compound combinations include copper compounds, alkaline earth metal compounds (e.g., magnesium compounds), and optional alkali metal compounds (e.g., potassium compounds). Other exemplary catalytic metal compound combinations may include copper compounds, alkaline earth metal compounds (e.g., magnesium compounds), optional alkali metal compounds (e.g., potassium compounds), and zirconium compounds (e.g., zirconium oxychloride).

[0020] In one or more embodiments, the copper compound is a water-soluble salt, such as copper chloride (e.g., copper II chloride). Other copper salts that can be converted to chlorides during the oxychlorination process, such as nitrates, carbonates, sulfates, or other halide salts, such as bromide salts, or combinations thereof, may also be used.

[0021] In one or more embodiments, useful alkali metal compounds include water-soluble salts, such as alkali metal chlorides. Other alkali metal salts can also be used, which can be converted into chloride salts during oxychlorination, such as nitrates, carbonates, sulfates or other halide salts, such as bromide salts, or combinations thereof. In particular embodiments, the alkali metal compound includes potassium salts, such as potassium chloride, potassium nitrate, potassium bromate, potassium carbonate or potassium sulfate. In a specific embodiment, the alkali metal compound is potassium chloride. In one or more embodiments, the alkali metal compound can include potassium chloride and one or more additional alkali metal compounds, such as lithium chloride. In other embodiments, the catalytic metal compound includes a potassium compound and contains no or only trace amounts (e.g., less than 1 ppm by weight) of other alkali metal compounds.

[0022] In one or more embodiments, useful alkaline earth metal compounds include water-soluble salts, such as alkaline earth metal chlorides. Other alkaline earth metal salts can also be used, which can be converted into chloride salts in the oxychlorination process, such as nitrates, carbonates, sulfates or other halide salts, such as bromide salts, or combinations thereof. In a specific embodiment, the alkaline earth metal compound includes a magnesium salt, such as magnesium chloride, magnesium nitrate, magnesium bromate, magnesium carbonate or magnesium sulfate. In a specific embodiment, the alkaline earth metal compound is magnesium chloride. In one or more embodiments, the alkaline earth metal compound can include a magnesium compound and one or more additional alkaline earth metal compounds, such as compounds of calcium, strontium, barium or mixtures thereof. In a specific embodiment, the catalytic metal compound includes a magnesium compound, and does not contain or contains only trace amounts (e.g., less than 1ppm by weight) of other alkaline earth metal compounds.

[0023] In one or more embodiments, useful transition metal compounds include water-soluble salts such as transition metal chlorides (e.g., chlorides or oxychlorides). Other salts may also be used, which can be converted into chloride salts such as nitrates, carbonates, sulfates or other halide salts such as bromide salts, or combinations thereof, during the oxychlorination process. Useful transition metal compounds include manganese compounds such as manganese chlorides and / or rhenium compounds. Other useful transition metal compounds include zirconium compounds such as zirconium oxychloride. In one or more embodiments, the catalytic metal compound may include a combination of a transition metal compound and one or more other transition metal compounds. In other embodiments, the catalytic metal compound includes a transition metal compound (e.g., zirconium oxychloride) and contains no or only trace amounts (e.g., less than 0.005 wt %) of other transition metal compounds. In one or more embodiments, the catalytic metal compound includes zirconium and does not contain manganese (Mn) or rhenium (Re).

[0024] In one or more embodiments, useful rare earth metal compounds include water-soluble salts, such as rare earth metal halides (such as chlorides). Other salts can also be used, which can be converted into chloride salts, such as nitrates, carbonates, sulfates or other halide salts, such as bromide salts, during oxychlorination. Useful rare earth metal compounds include lanthanum compounds, such as lanthanum chloride. Other useful rare earth metal compounds include cerium, neodymium and praseodymium compounds. In one or more embodiments, the catalytic metal compound may include a combination of a rare earth metal compound and one or more other rare earth metal compounds. In other embodiments, the catalytic metal compound includes a rare earth metal compound and contains no or only trace amounts (e.g., less than 0.005 wt %) of other rare earth metal compounds. In one or more embodiments, the catalytic metal compound includes a lanthanide metal and does not contain manganese (Mn) or rhenium (Re). Catalytic metal loading

[0025] As will be appreciated by those skilled in the art, the amount of deposited copper metal is generally based on the desired activity and the specific fluidization characteristics of the support for fluidized bed catalyst applications. In one or more embodiments, the catalyst composite comprises from about 1 wt % to about 10 wt % copper metal, based on the gross weight of the catalyst composition. In one or more embodiments, the catalyst comprises greater than 2.0 wt % copper (atomic copper), based on the gross weight of the catalyst, or greater than 3.0 wt % copper (atomic copper) in other embodiments. In these or other embodiments, the catalyst comprises less than 6.0 wt % copper, based on the gross weight of the catalyst, or less than 8.0 wt % copper in other embodiments, or less than 10 wt % copper in other embodiments.

[0026] When the catalyst includes an alkali metal compound, based on the gross weight of the catalyst composition, the catalyst composite may include about 0.5 wt % to about 5.0 wt %, or about 0.75 wt % to about 4.0 wt %, or about 1.0 wt % to 3.0 wt % of an alkali metal (e.g., atomic potassium). In one or more embodiments, based on the gross weight of the catalyst, the catalyst includes an alkali metal greater than 0.5 wt %, or in other embodiments, an alkali metal greater than 0.75 wt %. In one or more embodiments, based on the gross weight of the catalyst composition, the catalyst includes an alkali metal (e.g., potassium metal) less than 5.0 wt %, or less than 4.0 wt %, or less than 3.0 wt %. If additional alkali metals are included, the catalyst may contain additional alkali metals of about 0.005 wt % to about 10.0 wt %.

[0027] When the catalyst includes an alkaline earth metal compound, based on the catalyst composition gross weight, the catalyst composite may include about 0.5 wt % to about 5.0 wt %, or about 0.75 wt % to about 4.0 wt %, or about 1.0 wt % to 3.0 wt % of alkaline earth metal (e.g., atomic magnesium). In one or more embodiments, based on the gross weight of the catalyst, the catalyst includes an alkaline earth metal greater than 0.5 wt %, or in other embodiments, an alkaline earth metal greater than 0.75 wt %. In one or more embodiments, based on the gross weight of the catalyst composition, the catalyst includes an alkaline earth metal (e.g., magnesium) less than 5.0 wt %, or less than 4.0 wt %, or less than 3.0 wt %. If additional alkaline earth metals are included, the catalyst may contain additional alkaline earth metals of about 0.005 wt % to about 10.0 wt %.

[0028] When the catalyst includes a transition metal compound, based on the gross weight of the catalyst composition, the catalyst composite may include about 0.1 wt % to about 3.0 wt %, or about 0.3 wt % to about 2.5 wt %, or about 0.5 wt % to 2.0 wt % of a transition metal (e.g., atomic manganese). In one or more embodiments, based on the gross weight of the catalyst, the catalyst includes a transition metal greater than 0.1 wt %, or in other embodiments, a transition metal greater than 0.3 wt %. In one or more embodiments, based on the gross weight of the catalyst composition, the catalyst includes a transition metal less than 3.0 wt %, or less than 4.0 wt %, or less than 2.0 wt % of a transition metal (e.g., manganese metal). If additional transition metals are included, the catalyst may contain additional transition metals of about 0.005 wt % to about 10.0 wt %.

[0029] When the catalyst includes a rare earth metal compound, based on the gross weight of the catalyst composition, the catalyst composite may include about 0.1 wt % to about 3.0 wt %, or about 0.3 wt % to about 2.5 wt %, or about 0.5 wt % to 2.0 wt % of a rare earth metal (e.g., atomic lanthanum). In one or more embodiments, based on the gross weight of the catalyst, the catalyst includes a rare earth metal greater than 0.1 wt %, or greater than 0.3 wt % of a rare earth metal in other embodiments. In one or more embodiments, based on the gross weight of the catalyst composition, the catalyst includes less than 3.0 wt %, or less than 4.0 wt %, or less than 2.0 wt % of a rare earth metal (e.g., lanthanum metal). In one or more embodiments, additional rare earth metals may be included, and the catalyst may contain additional transition metals of about 0.005 wt % to about 10.0 wt %.

[0030] In a particular embodiment, the catalyst comprises a zirconium salt, such as zirconium oxychloride, zirconium carbonate or zirconium hydroxide. Based on the gross weight of the catalyst composition, the catalyst may comprise about 0.1 wt % to about 3.0 wt %, or about 0.5 wt % to about 2.0 wt %, or about 0.75 wt % to 1.0 wt % of zirconium as a metal. According to an embodiment, based on the gross weight of the catalyst composition, the catalyst may comprise a zirconium metal less than 3.0 wt %, or less than 2.0 wt %, or less than 1.0 wt %. If an additional transition metal is included, the catalyst may contain an additional transition metal of about 0.005 wt % to about 10.0 wt %.

[0031] Those skilled in the art will appreciate that the final catalyst composition containing catalytic metals (e.g., copper compounds, alkaline earth metal compounds, and transition metal compounds) is easily fluidized. In one or more embodiments, relatively small amounts or trace amounts of any other metals may be present in the catalyst composition. Typically, the content of these metals (if present) may be less than about 0.005 weight percent based on the total weight of the catalyst composition. Preparation of catalyst complex

[0032] The catalyst used in the present invention can be prepared by conventional techniques.

[0033] For example, the metal compound can be impregnated on an alumina carrier. This can be achieved by introducing an aqueous solution of a water-soluble salt (i.e., a metal compound) into the carrier. The wetted carrier can then be dried and optionally calcined. A single solution can be used, or multiple solutions can be used in succession in other embodiments to impregnate the carrier with the metal compound. For example, an alkaline earth metal compound, a transition metal compound, and any other metal compound (and optionally dried and calcined) can be first introduced, and then a copper compound is introduced into the carrier that has been impregnated with other metal compounds. In this regard, U.S. Patent Publication Nos. 2014 / 0275661 and 2017 / 0137351 are incorporated herein by reference.

[0034] Those skilled in the art will appreciate that the impregnation solution can be prepared by dissolving the desired amount of metal salt in water while stirring (e.g., manually stirring or vigorously mixing) at room temperature or, optionally, at an elevated temperature (e.g., about 40°C to about 60°C). Once dissolved, the metal salt solution can be introduced into the alumina support (i.e., the impregnation support). For example, the solution can be slowly introduced into a tumbler containing the support (e.g., rotating at a speed of about 90 revolutions per minute). The salt solution is dripped or sprayed onto the support within 30 minutes. After impregnation, the wet catalyst is typically dried. This can include pre-drying, which can be achieved by heating the catalyst in a steam bath (e.g., the catalyst in a ceramic tray or other container can be optionally heated in a steam bath for about 1 to about 3 hours). Whether or not pre-dried, the catalyst can be heated in an oven to remove all or substantially all of the water. For example, the catalyst can be heated in an oven at an ambient temperature of about 100°C to 180°C, or 110°C to 150°C, or 100°C, 105°C, 110°C, or 115°C. In this heating step, the catalyst can be exposed to these elevated temperatures for about 2 hours to about 30 hours, or about 10 hours to about 28 hours, or about 20 hours to about 25 hours. After drying, the dried catalyst can be sieved (e.g., sieved hot) using a 500 μm sieve, or a 475 μm sieve, or a 450 μm sieve, or a 400 μm sieve, or a 350 μm sieve, or a 300 μm sieve. The dried catalyst can be hot sieved at a temperature of about 100° C. to about 200° C. or 130° C. The final catalyst material can be packaged (e.g., bottled).

[0035] Those skilled in the art will appreciate that specific properties of the catalyst, such as surface area and pore volume, can be modified by the deposition of metal salts. For example, the final surface area of ​​the catalyst composition described herein can be from about 20 to about 220 m 2 / g, or about 60 to about 180m 2 / g, about 70 to about 170m 2 / g, or about 80m 2 / g to about 150m 2 / g, or about 150m 2 / g to about 215m 2 / g. Catalyst activation

[0036] As described above, the catalyst compositions described herein can be activated. In one or more embodiments, the catalyst is activated in a reactor bed while being heated and fluidized with a fluidizing gas comprising one or more of air, oxygen-enriched air, nitrogen-enriched air, nitrogen, and combinations thereof.

[0037] When implementing the method of one or more embodiments of the present invention, the catalyst is placed in a reactor (i.e., a fluidized bed reactor), and this step can be referred to as loading the catalyst into the reactor. After the catalyst is loaded into the reactor, the catalyst is activated. In one or more embodiments, the activation of the catalyst includes heating the catalyst so that the catalyst composite reaches a threshold temperature for a threshold time under fluidized conditions (while fluidizing the catalyst). In one or more embodiments, the catalyst is heated to a temperature greater than 150°C, a temperature greater than 170°C in other embodiments, a temperature greater than 190°C in other embodiments, and a temperature greater than 210°C in other embodiments. In these embodiments, the temperature of the catalyst (under fluidized conditions) is maintained for more than 6 hours, more than 12 hours in other embodiments, more than 24 hours in other embodiments, and more than 36 hours in other embodiments.

[0038] As described above, activation is performed in the substantial absence of ethylene conversion or EDC production. According to aspects of the present invention, activation of the catalyst is performed in the substantial absence of hydrochloric acid, the amount of which has no significant effect on the practice of the present invention or is less. In one or more embodiments, the amount of hydrochloric acid present when the catalyst is activated is less than 100 ppm, in other embodiments less than 50 ppm, and in other embodiments less than 25 ppm. In these or other embodiments, activation of the catalyst is performed in the substantial absence of ethylene, the amount of which has no significant effect on the practice of the present invention or is less. In one or more embodiments, the amount of ethylene present when the catalyst is activated is less than 100 ppm, in other embodiments less than 50 ppm, and in other embodiments less than 25 ppm.

[0039] In one or more embodiments, the catalyst is activated while fluidizing the catalyst in the presence of a fluidizing gas stream comprising oxygen or an oxygen-containing gas. In these or other embodiments, the catalyst is activated while fluidizing the catalyst in the presence of a fluidizing gas stream comprising an inert gas such as argon or nitrogen. In a specific embodiment, the catalyst is activated while fluidizing the catalyst in the presence of a fluidizing gas stream comprising an inert gas and substantially free of oxygen or an oxygen-containing gas.

[0040] As known to those skilled in the art, conventional techniques can be used to heat the catalyst in the reactor, which may be affected by the reactor temperature control element (e.g., a coil or tube comprising a heat transfer fluid). In the reactor, the temperature of the catalyst can be determined by one or more thermocouples, which are located in a thermal well in the fluidized bed, which is in contact with the fluidized material. In order to perform these measurements according to the embodiments of the present invention, it is assumed that the fluidized bed is balanced at a macroscopic level, so it is assumed that the temperature of the fluidized material (including gas phase and solid phase) at the location of the thermal well is equal to or close to the temperature of the catalyst complex (i.e., particles). Similarly, conventional techniques can be used to fluidize the catalyst, which may be affected by injecting a pressurized gas stream into the reactor under conditions suitable for the fluidized catalyst.

[0041] In one or more embodiments, the oxychlorination process is started after the catalyst is activated in the reactor before the properties of the catalyst undergo detrimental changes. Those skilled in the art will appreciate that the oxychlorination process is started by feeding ethylene, hydrochloric acid and oxygen or an oxygen-containing substance into the reactor (i.e., the reactant feed is put into the reactor). In one or more embodiments, the reactant feed is fed into the reactor without interrupting the fluidization of the catalyst. In these or other embodiments, the reactant feed is fed into the reactor before the catalyst is cooled (after activation), and the cooling is greater than 50°C, greater than 35°C in other embodiments, greater than 20°C in other embodiments, and greater than 10°C in other embodiments. In these or other embodiments, the reactant feed is fed into the reactor and cooled to a temperature below 110°C, below 120°C in other embodiments, below 130°C in other embodiments, and below 140°C in other embodiments before the catalyst is cooled.

[0042] In one or more embodiments, the activation of the catalyst occurs before the catalyst is used in the oxychlorination process. In other embodiments, the catalyst is activated after being used in the oxychlorination process. For example, the oxychlorination process using a particular catalyst is paused and the catalyst is activated according to the present invention. In one or more embodiments, the reaction is paused by at least interrupting the hydrochloric acid feed. In other embodiments, the reaction is paused by interrupting the hydrochloric acid feed and the ethylene feed.

[0043] Without being bound by any particular theory, it is believed that the activation of the catalyst according to the present invention can remove excess hydration water and some chlorine in the catalyst, such as hydrochloric acid. Therefore, the activation process may also change the surface chemistry of the catalyst, making it more effective in certain applications. Although embodiments of the present invention require that the catalyst be fluidized during the activation process, and keep heated and fluidized until the oxychlorination process begins, it is believed that as long as the catalyst can be maintained in an anhydrous environment until the oxychlorination process starts, the activation of the catalyst may be carried out outside the reactor. For example, it is believed that if the activated catalyst is maintained under anoxic conditions (such as nitrogen purging or nitrogen covering) during storage, transportation and loading into the reactor, the benefits of the present invention can be achieved. It is also believed that if the catalyst is maintained at a threshold temperature during storage, transportation and loading into the reactor, the benefits of the present invention can be achieved. Oxychlorination process

[0044] The catalyst composition of the present invention is an efficient catalyst for oxychlorinating ethylene to EDC. The reaction process temperature varies from about 170°C to about 260°C, in other embodiments from about 180°C to about 250°C, and in other embodiments from about 190°C to about 240°C. The reaction pressure varies from atmospheric pressure to up to about 200 psig. The contact time for fluidized bed and fixed bed catalysis can vary from about 5 seconds to about 50 seconds (the contact time here is defined as the ratio of the reactor volume occupied by the catalyst to the volume flow rate of the feed gas at the reactor control temperature and top pressure), and in other embodiments from about 5 seconds to about 35 seconds. Based on the number of moles of HCl fed to the reactor, the ratio of ethylene, HCl and oxygen reactants can be about 1.0 to about 2.0 moles of ethylene and about 0.5 to about 0.9 moles of oxygen per 2.0 moles of HCl. As previously described, modern oxychlorination processes attempt to operate within a stoichiometric ratio range of about 1 to about 2 moles of HCl to 1 mole of ethylene.

[0045] As described above, the oxychlorination process of the present invention converts ethylene to 1,2-dichloroethane (EDC) in the presence of an activated catalyst. Typically, the reaction is carried out in the presence of two moles of hydrochloric acid and half a mole of oxygen to produce EDC and water. In one or more embodiments, the oxychlorination catalyst of the present invention can be advantageously used in an oxychlorination process wherein the molar ratio of oxygen to hydrogen chloride (O2 / 2HCl) is close to a stoichiometric feed rate of 0.5. In one or more embodiments, the process operates at a molar ratio of oxygen to hydrogen chloride (O2 / 2HCl) of less than 0.9, in other embodiments less than 0.64, in other embodiments less than 0.58, in other embodiments less than 0.55, and in other embodiments less than 0.52. In one or more embodiments, the process operates at a molar ratio of oxygen to hydrogen chloride (O2 / 2HCl) of about 0.50 to about 0.80, in other embodiments about 0.51 to about 0.70, in other embodiments about 0.52 to about 0.60, and in other embodiments about 0.53 to about 0.58.

[0046] In those embodiments where recycle is performed, the ratio of HCl to ethylene may be less than 2. In those embodiments where a single pass process is performed, the ratio of HCl to ethylene may be higher and may be close to or closer to 2, resulting in an overall operating range of about 1 to about 2 moles of HCl to ethylene.

[0047] The operating temperature of the oxychlorination process described herein may be at or above conventional operating temperatures (e.g., 220° C.). In other embodiments, the operating temperature of the oxychlorination process may be below 218° C., below 215° C. in other embodiments, or below 212° C. in other embodiments. In one or more embodiments, the temperature at which the oxychlorination process of the present invention is carried out is a temperature of about 180 to 220° C., in other embodiments, about 190 to about 218° C., in other embodiments, about 195 to about 215° C., and in other embodiments, about 200 to about 210° C.

[0048] In these or other embodiments, the reaction pressure can vary from about atmospheric pressure to up to about 200 psig. The contact time for fluidized bed and fixed bed catalysis can vary from about 10 seconds to about 50 seconds (the contact time is defined as the ratio of the reactor volume occupied by the catalyst to the volume flow of the feed gas under the reactor control temperature and top pressure), and can be about 20 seconds to about 35 seconds. Based on the number of moles of HCl fed into the reactor, the ratio of ethylene, HCl and oxygen reactants can be about 1.0 moles to about 2.0 moles of ethylene and about 0.5 moles to about 0.9 moles of oxygen per 2.0 moles of HCl. Typical oxychlorination processes attempt to operate within the stoichiometric ratio range of about 1 mole to about 2 moles of HCl to 1 mole of ethylene. Process characteristics

[0049] The process of the present invention advantageously provides efficient conversion of ethylene to EDC. Those skilled in the art will appreciate that the conversion to EDC can be measured by conversion of hydrochloric acid. According to aspects of the present invention, when oxychlorination is carried out at a temperature greater than 220°C, activation of the catalyst according to the embodiments described herein results in an increase in EDC yield of more than 0.1%, in other embodiments more than 0.25%, in other embodiments more than 0.5%, in other embodiments more than 0.75%. In other embodiments, when oxychlorination is carried out at a temperature of about 200°C to 220°C, activation of the catalyst according to the embodiments described herein results in an increase in EDC yield of more than 1.0%, in other embodiments more than 1.25%, in other embodiments more than 1.5%, in other embodiments more than 2.0%. Example

[0050] To illustrate the practice of the present invention, the following examples were prepared and tested. However, these examples should not be considered to limit the scope of the present invention. The claims are used to define the present invention.

[0051] A series of laboratory-scale continuous oxychlorination reactions (i.e., runs) were performed. The equipment and procedures used in each run were essentially the same, except as described below. Likewise, the preparation of each catalyst was similar, except as described below.

[0052] The catalyst used in each run was prepared by impregnating an alumina support with the catalyst impregnation solution. The alumina support was obtained under the trade name SCCa 25 / 200 (Sasol) and was characterized by a pore volume of 0.44 mL / g and a surface area of ​​203 m 2 The particle size distribution (psd) of the carrier is characterized in that 1.4% of the particles are smaller than 22 microns, 7.1% of the particles are smaller than 31 microns, 23% of the particles are smaller than 44 microns, 79% of the particles are smaller than 88 microns, and 94% of the particles are smaller than 125 microns.

[0053] The catalyst impregnation solution is prepared by dissolving the metal chloride in water and then distributing the solution evenly throughout the support. The volume of the solution is selected to match 95% + / - 3% of the support pore volume. The impregnated catalyst is then dried at temperatures up to 150°C to remove most of the moisture and then dried in an oven at 110°C for another 16 hours. The following table lists the metals used and the amount of each metal used in each run. For clarity, the metals are provided in weight percentages, which represent the weight of each metal relative to the entire catalyst composition (e.g., copper as a weight percentage of metal relative to the total weight of the catalyst composition, the total weight of the catalyst composition including the total weight of all metal chlorides and the support).

[0054] When multiple reactors are used, each reactor has an inner diameter of approximately 2 cm and is filled with catalyst to achieve a fluidized bed height of approximately 99 + / - 2.5 cm. The reactors are equipped with a central thermocouple in the fluidized bed and external electric heaters to maintain the reaction temperature at the desired temperature. Each reactor is configured to communicate with analytical equipment suitable for measuring HCl in the feed and product streams and N2, C2H4, O2, CO in the product stream. x Specifically, HCl in the feed and product gases was measured by titration, N2, C2H4, O2, CO x and chlorinated hydrocarbons were measured by GC (HP 6890 series; column types - 1) Vocol glass capillary column (60 meters; inner diameter 0.75 mm; film thickness 1.5 microns. 2) 80 / 100 Porapak N column (12 x 1 / 8 inches, stainless steel). 3) 60 / 80 molecular sieve, 5 angstroms (6 feet x 1 / 8 inches); Detectors - 2 TCD detectors. Detector B (Vocal column) Detector A (molecular sieve / Porapak); One TCD is used to detect light gases such as O2, N2, and CO from the molecular sieve column, and heavier gases such as CO2 and ethylene from the Porapak column, as well as lighter chlorinated hydrocarbons such as vinyl chloride and ethyl chloride. The second TCD is used to detect the remaining heavier chlorinated hydrocarbons in the Vocol column starting with chloroform, including EDC and other heavier chlorinated by-products.

[0055] In the oxychlorination process, unless otherwise specified in the table below, the reactor is operated at atmospheric pressure and continuous temperature, and the feed gas stream contains 11.4NL / h of N2, 3.75NL / h of ethylene, 7.12NL / h of HCl and 2.55NL / h of O2. Data are collected at continuous temperature and interpolated over the temperature range. Specifically, after balancing the reaction conditions at any given set temperature, data related to EDC selectivity (the number of moles of ethylene converted to EDC relative to the total number of moles of ethylene converted) and HCl conversion are collected. The reaction temperature is then increased (usually about 3-5°C) and the reaction is allowed to reach equilibrium, and data related to EDC selectivity and HCl conversion are collected again. Once the data is interpolated, the reactions are compared (based on HCl conversion) at the same performance levels of 98% and 97% selectivity of ethylene to EDC. These comparisons are shown in the table below.

[0056] In connection with the present invention, runs were performed with and without catalyst activation. Generally, those catalysts that were activated were fluidized at elevated temperatures with feed gas streams containing nitrogen and oxygen (unless otherwise specified) in the ratios and times shown in the table below. For those runs without activation, the column was loaded with catalyst and the reactor was fluidized with nitrogen and brought to a temperature of about 200° C. Within no more than about 2 hours after reaching the target temperature, the ethylene, oxygen, and HCl feeds were started and the oxychlorination reaction was carried out.

[0057] To achieve the same EDC selectivity as the activated catalyst, the unactivated catalyst runs at a higher temperature and has a lower HCl conversion. Activation is indicated by the catalyst showing a higher HCl conversion at a lower operating temperature to achieve the same EDC selectivity. The overall performance is improved because the unactivated catalyst needs to be operated at a higher temperature to achieve the same HCl conversion as the activated catalyst, resulting in a lower percent selectivity for EDC. Dataset I - Runs 1-6

[0058] The first set of data is summarized in Table I below and generally shows the effect of catalyst activation as well as the effect of catalyst metal ratio.

[0059] As shown in Table I, Runs 1 and 2, Runs 3 and 4, and Runs 5 and 6, respectively, used the same catalyst, Runs 1, 3, and 5 were not activated, and Runs 2, 4, and 6 were activated according to the present invention. Comparison of Run 2 with Run 1 shows that by activating the catalyst, higher HCl conversion can be achieved at lower temperatures with the same EDC selectivity. Similar results are shown when Run 4 (activated) is compared to Run 3 (not activated), and Run 6 (activated) is compared to Run 5 (not activated). The data also shows a general trend that at lower copper loadings, higher temperatures are generally required to achieve the desired selectivity, but the advantages of the present invention are maintained, namely that the activation of the catalyst allows for lower temperatures while achieving the desired HCl conversion and EDC selectivity for each catalyst. Finally, the data shows that activation can be achieved regardless of whether oxygen is present in the feed stream during activation; Run 6 was activated with only nitrogen feed and achieved results comparable to activation occurring in the presence of a mixture of nitrogen and oxygen. Table I Data Set II - Runs 7-8

[0060] The second set of data, summarized in Table II below, shows that reactor run time does not achieve the same effect as catalyst activation, i.e., data for Run 7 was collected after about 50 days of reactor operation (under oxychlorination conditions) at various temperatures (and about 16 days of sporadic room temperature fluidization with nitrogen while shutting off the HCl and ethylene feeds). Despite having been run for an extended period of time, Run 7 did not achieve the benefits observed with Run 8, which was activated in accordance with the present invention; again, this is evidenced by the higher HCl conversions achieved at lower temperatures at the target EDC selectivity. Table II Data Set III - Runs 9-12

[0061] The third set of data is summarized in Table III and shows the relationship between catalyst activation and time and temperature. Each run represents a set of data collected continuously from the same reactor (i.e., after the reactor was run, the data of the previous run was collected). Specifically, for Run 9, the catalyst was fluidized with a nitrogen / oxygen mixture at 200°C for about 64 hours, then the oxygen, ethylene and HCl flows were started and the oxychlorination reaction was carried out for about 104 hours. The oxygen, ethylene and HCl feeds were then turned off and the catalyst was fluidized with a nitrogen / oxygen mixture at 200°C for 64 hours. After about 64 hours, the oxygen, ethylene and HCl feeds were turned on again and the oxychlorination was continued for about 104 hours, which represents Run 10. Runs 11 and 12 followed the same pattern, except that Run 12 heated the catalyst to 230°C for 64 hours under fluidization. Comparison of Run 12 with Run 9 shows that heating the catalyst at 200°C for 64 hours does not activate the catalyst to the same extent as a longer time at 200°C (see Runs 10 and 11) or a longer time at higher temperatures (see Run 12). However, it should be noted that Runs 10 and 11 show a trend that activation at 200 °C eventually improves the performance of the catalyst as activation time increases. Table III Data Set IV - Runs 13-16

[0062] The fourth set of data, summarized in Table V below, shows that the catalyst must be activated in the reactor under fluidized conditions. The catalyst used in Runs 14 and 16 was activated according to the present invention, while the catalyst used in Runs 13 and 15 was attempted to be activated in an oven at 230°C for 64 hours. The catalyst used in Run 13 was cooled to 110°C for 24 hours before being loaded into the reactor, while the catalyst used in Run 15 was transferred directly from the oven to the reactor. As shown in the data, neither of the catalysts heated in the oven (Runs 13 and 15) activated in the same manner as the catalysts activated according to the present invention (Runs 14 and 16). Table IV Data set V - runs 17-20

[0063] The fifth set of data is summarized in Table V below, showing that the findings associated with the present invention can be extended to other catalyst systems. For example, catalysts using potassium and rare earth metals, i.e., catalyst systems known for oxychlorination, can benefit from the practice of the present invention. One catalyst used in the present experiments (Runs #17 and #18) contained 1.5 wt % lanthanum, 0.5 wt % cerium, and 0.5 wt % praseodymium (expressed as 2.5 wt % rare earth in Table V). As shown in the data, activation of the catalyst according to the present invention (i.e., Run #18) provided higher HCl conversion at lower temperatures at the same EDC selectivity compared to the same system without activation (i.e., Run #17). Catalysts containing copper and magnesium also showed similar results (Runs #19 and #20). Table V

[0064] Various modifications and alterations will become apparent to those skilled in the art without departing from the scope and spirit of the invention.The present invention is not to be unduly limited to the illustrative embodiments set forth herein.

Claims

1. A method for producing 1,2-dichloroethane, the method comprising: (i) providing a fluidizable catalyst; (ii) loading the fluidizable catalyst into a fluidized bed reactor; (iii) fluidizing the catalyst within the reactor; (iv) heating the catalyst in a fluidized bed reactor to a temperature greater than 150° C. for more than 6 hours while fluidizing the catalyst in the reactor, wherein the fluidizing and heating steps are performed without conversion of ethylene; and (v) after the heating step, converting the ethylene to 1,2-dichloroethane in the presence of a catalyst.

2. The method of claim 1, wherein the heating step is performed for more than 12 hours.

3. A method as claimed in any one of the preceding claims, wherein the heating step is carried out for more than 24 hours.

4. The method of any one of the preceding claims, wherein the heating step is performed for more than 36 hours.

5. A method as claimed in any one of the preceding claims, wherein the heating step heats the catalyst to a temperature in excess of 170°C.

6. A process as claimed in any one of the preceding claims, wherein the heating step heats the catalyst to a temperature in excess of 190°C.

7. A method as claimed in any one of the preceding claims, wherein the heating step heats the catalyst to a temperature in excess of 210°C.

8. A method as claimed in any one of the preceding claims, further comprising the step of feeding oxygen to the reactor.

9. The process as claimed in any one of the preceding claims, wherein the step of converting ethylene to 1,2-dichloroethane comprises the step of feeding ethylene to a reactor.

10. The process as claimed in any one of the preceding claims, wherein the step of converting ethylene to 1,2-dichloroethane comprises the step of feeding hydrochloric acid to the reactor.

11. A method as claimed in any one of the preceding claims, wherein the heating and fluidising steps are carried out in the substantial absence of hydrochloric acid.

12. The method according to any one of the preceding claims, wherein the heating step is carried out in the presence of oxygen and / or an oxygen-containing gas and / or an inert gas.

13. The process of any one of the preceding claims, wherein the heating step provides a heated catalyst, and wherein the temperature of the catalyst is maintained in excess of 150°C, at least until the ethylene feed step.

14. A process as claimed in any preceding claim, wherein the fluidisable catalyst comprises a support impregnated with a catalytic metal species.

15. A method as claimed in any preceding claim, wherein the catalytic metal species comprises copper.

16. A method as claimed in any preceding claim, wherein the catalytic metal species comprises copper, magnesium and zirconium.

17. A process as claimed in any one of the preceding claims wherein the ethylene is contacted with the catalyst in the reaction zone of the reactor.

18. A process as claimed in any preceding claim further comprising the step of recovering 1,2-dichloroethane from the effluent stream of the reactor.

19. A process as claimed in any preceding claim wherein the support is high surface area alumina.