Polyamide profiled section fiber and fiber comprising core-sheath composite yarn

By using polyamide special-shaped cross-section fibers and core-sheath type composite yarn structures in sports clothing, the problem of insufficient water-repellent performance and durability of sports clothing during intense movements and washing processes is solved, and water-repellent performance, resistance to rupture and washing are achieved. Improvement of dyeing fastness.

CN118749036APending Publication Date: 2024-10-08TORAY INDUSTRIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380019856.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-27
Filing Date
2023-05-19
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Sportswear fabrics undergo complex deformation during intense movements and washing processes, resulting in insufficient water repellency and durability. Existing fibers have poor practical durability in terms of friction and breakage, and are prone to fading after washing.

Method used

Polyamide special-shaped cross-section fiber is used, and there are multiple grooves on the periphery of the fiber cross-section. The ratio of the curvature radius of the entrance corner of the groove to the diameter of the circumscribed circle is less than 0.030, and the ratio of the groove depth to the diameter of the circumscribed circle is between 0.10 and 0.30. Combined with the core-sheath type composite yarn structure, the core is configured with polyamide polymer. After the sheath is dissolved and removed, the fiber elongation and strength change within a specific range, ensuring water-repellent performance and durability.

Benefits of technology

It provides textiles or braids with excellent water repellency and durability, practical durability that resists breakage or friction, and high wash and dye fastness, and can maintain functionality in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118749036A_ABST
    Figure CN118749036A_ABST
Patent Text Reader

Abstract

Provided is a fabric or a knitted fabric having excellent water repellency, practical durability, and dyeing fastness when used in clothing, said fabric or knitted fabric being used in clothing applications, and a polyamide multifilament having a profiled cross-section, said polyamide multifilament being used in clothing applications. A polyamide profiled cross-sectional fiber having a profiled cross-sectional shape in which a plurality of grooves are present on the outer periphery of the fiber cross-sectional surface of a single fiber, and the radius of curvature d of the entrance corner of each groove, the depth H of each groove, and the diameter D of the circumcircle of the fiber cross-sectional surface satisfy the following formulae (1) and (2), and the amount of rigid amorphous particles being 35%-55% (inclusive). D / D < = 0.030... Formula (1) 0.10 < = (H / D) < = 0.30... Formula (2)
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyamide multifilament with a profiled cross section used in clothing applications. More specifically, by using a multifilament containing polyamide fibers with a profiled cross section having specific grooves in clothing applications, a woven or knitted fabric having excellent water repellency, practical durability, and excellent color fastness can be provided. Background Art

[0002] Synthetic fibers such as polyamide and polyester have excellent mechanical and chemical properties and are therefore widely used for clothing and industrial purposes.

[0003] In sports applications such as mountaineering, hiking, and winter sports, high water repellency and practical durability are required, and further, fastness to washing is required.

[0004] In order to impart a water-repellent function to a fiber product, generally, after the fiber is woven into a cloth, the fiber or the fiber product surface layer is treated with a so-called water-repellent agent to form a water-repellent film to impart a water-repellent function.

[0005] In order to form an excellent water-repellent film, in addition to studying advanced processing technologies such as the composition of the agent or the processing conditions or process methods for firmly fixing it, we also studied the following technology, that is, the technology of forming a special surface morphology on the fabric as a base material to physically improve the water-repellent performance or its durability, aiming at the so-called Lotus effect, by making the fiber profile.

[0006] For example, Patent Document 1 proposes a composite fiber having a protrusion shape with protrusions and grooves alternately in the core and having a so-called gear-shaped cross section. Patent Document 2 proposes a composite fiber having a cross section with grooves in the core and a wide width of the groove being 1.3 times or more of the width of the groove entrance. Patent Document 3 proposes a fiber having 20 or more grooves with a groove depth of more than 2 times the groove width on the fiber surface.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2016-129467

[0010] Patent Document 2: Japanese Patent Application Publication No. 2019-26944

[0011] Patent Document 3: Japanese Patent Laid-Open No. 2003-129327 Summary of the invention

[0012] Problems to be solved by the invention

[0013] In sportswear applications, textiles or knitted fabrics are subject to complex deformation due to the intense movements during wearing. In addition, since the frequency of washing increases, practical durability is required to resist deformation, friction or cracking, and washing durability to maintain functionality or prevent fading.

[0014] However, the fiber described in Patent Document 1 or Patent Document 2 is a fabric containing polyamide fibers having a gear-shaped cross section or a teardrop-shaped slit cross section after the sheath component is eluted and removed, and although the water-repellent performance and the washing durability of the water-repellent performance are excellent, the practical durability against friction or tearing is poor, and fading due to washing occurs. In addition, although the fiber described in Patent Document 3 also exhibits water-repellent performance due to the grooves, the protrusions formed by the grooves are easily peeled off from the base due to friction or deformation accompanying wearing due to the deep grooves, the practical durability against friction is poor, the washing durability of the water-repellent performance due to washing is also poor, and fading occurs.

[0015] The present invention is an invention for solving the above-mentioned problems, and is a polyamide profiled cross-section fiber having excellent water-repellent performance and water-repellent durability, practical durability against cracking or friction, and excellent washing and dyeing fastness, and a fiber including a core-sheath type composite yarn that can provide the polyamide profiled cross-section fiber.

[0016] Technical means of solving problems

[0017] In order to solve the above-mentioned problems, the present invention adopts the following structure.

[0018] (1) A polyamide profiled cross-section fiber having a plurality of grooves on the outer periphery of a fiber cross-section of a single fiber, wherein the curvature radius d of the entrance corner of the groove, the groove depth H and the circumscribed circle diameter D of the fiber cross-section satisfy the following formula (1) and the following formula (2), and the rigid amorphous content is 35% or more and 55% or less,

[0019] d / D≦0.030…Formula (1)

[0020] 0.10≦(H / D)≦0.30…Formula (2).

[0021] (2) A fiber comprising a core-sheath type composite yarn, having a core-sheath type cross-sectional shape in which a thermoplastic polymer soluble in alkali or hot water is arranged in the sheath portion and a polyamide polymer is arranged in the core portion, the cross-sectional shape of the core portion is a cross-sectional shape having a plurality of grooves, and the curvature radius d of the entrance corner of the groove portion, the groove portion depth H and the circumscribed circle diameter D of the cross-sectional shape of the core portion satisfy the following formula (1) and the following formula (2),

[0022] d / D≦0.030…Formula (1)

[0023] 0.10≦(H / D)≦0.30…Formula (2)

[0024] The elongation and strength of the sheath before and after dissolution and removal satisfy the following equations (3) and (4):

[0025] Fiber elongation Ea after sheath dissolution and removal / Fiber elongation Eb before sheath dissolution and removal ≦ 1.30…Formula (3)

[0026] Fiber strength Sa after dissolution and removal of the sheath / fiber strength Sb before dissolution and removal of the sheath≧0.95…Formula (4).

[0027] Effects of the Invention

[0028] The polyamide profiled cross-section fiber and the fiber comprising the core-sheath type composite yarn of the present invention can provide a textile or knitted fabric having excellent water-repellent performance and water-repellent durability, practical durability against cracking or friction, and excellent washing and dyeing fastness, even in a usage environment where elongation, bending friction, etc. or harsh abrasion are applied when the fiber product is used. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] [ Figure 1 ] are cross-sectional views for explaining the polyamide profiled cross-section fiber of the present invention. (a) is a cross-sectional view of a single fiber of the polyamide profiled cross-section fiber, showing the circumscribed circle diameter D and the groove depth H. (b) and (c) are cross-sectional forms of an embodiment of the core-sheath type composite yarn of the present invention, wherein (b) has a sheath polymer disposed only in the groove portion of the polyamide profiled cross-section fiber, and (c) has a sheath polymer disposed in the groove portion of the polyamide profiled cross-section fiber and in a manner covering the entire core polymer.

[0030] [ Figure 2 ] is a schematic diagram for illustrating the curvature radius d of the entrance corner of the groove portion of the polyamide profiled cross-section fiber of the present invention.

[0031] [ Figure 3 ] is a schematic diagram of one embodiment of a manufacturing apparatus that can be preferably used in the manufacturing method of the core-sheath type composite yarn of the present invention. DETAILED DESCRIPTION

[0032] Hereinafter, the present invention will be described in further detail.

[0033] The polyamide referred to in the present invention is a high molecular weight resin including a so-called hydrocarbon group linked to a main chain via an amide bond.

[0034] The polyamide has excellent spinning properties and mechanical properties, and is preferably polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polyundecanamide (nylon 11), polypentamethylene adipamide (nylon 56), polypentamethylene sebacamide (nylon 510), polyhexamethylene sebacamide (nylon 610), and copolymers containing these as main components. In terms of difficulty in gelling and good spinning properties, polycaproamide (nylon 6) is further preferred.

[0035] The term "mainly" means, for example, that in polycaproamide, the ε-caprolactam unit constituting polycaproamide accounts for 80 mol% or more, and preferably 90 mol% or more. Other components are not particularly limited, and examples thereof include monomers constituting polydodecanoamide, polyhexamethylene adipamide, polyhexamethylene azelaic acid amide, polyhexamethylene sebacic acid amide, polyhexamethylene dodecanoamide, polymeta-xylylene adipamide, polyhexamethylene terephthalamide, polyhexamethylene isophthalamide, and the like, i.e., units of aminocarboxylic acids, dicarboxylic acids, diamines, and the like.

[0036] Usually, titanium oxide is mostly used as a matting agent for polyamide. In the polyamide of the present invention, titanium oxide may also be included as a matting agent. The titanium oxide content can be appropriately set within the range that does not hinder the effect of the present invention, and its preferred range is 0 wt % to 2 wt %. In addition, in addition to the titanium oxide, various additives may also be included within the range that does not hinder the effect of the present invention. If the additives are exemplified, stabilizers such as manganese compounds, heat-resistant agents, flame retardants, etc. can be listed.

[0037] The cross-sectional shapes of the single fibers and the core of the core-sheath type composite yarn constituting the polyamide profiled cross-sectional fiber of the present invention are shown in FIG. Figure 1 (a)~(c).

[0038] The cross-sectional shape has a plurality of grooves formed on the periphery. Through the grooves, an air layer is introduced between the water droplets and the fiber surface, thereby obtaining water-repellent properties. Furthermore, during water-repellent processing, since the inside of the grooves is not rubbed from the outside, the water-repellent agent that penetrates into the grooves is not easy to fall off, thereby showing water-repellent durability. The preferred number of grooves is 3 to 16.

[0039] The shape of the groove portion is such that the curvature radius d of the groove entrance corner, the groove depth H, and the circumscribed circle diameter D of the fiber cross section satisfy the following equations (1) and (2).

[0040] d / D≦0.030…Formula (1)

[0041] 0.10≦(H / D)≦0.30…Formula (2)

[0042] By setting the shape of the groove portion to the predetermined range, a surface morphology exhibiting water-repellent properties as a woven or knitted fabric is provided and the detachment of the water-repellent agent is suppressed, thereby exhibiting excellent water-repellent durability even in a severe use environment.

[0043] The ratio of the curvature radius d of the inlet corner of the groove to the circumscribed circle diameter D of the fiber cross section (hereinafter referred to as d / D) is 0.030 or less. The inlet corner of the groove is the acute angle portion near the inlet of the groove in the fiber cross section of the polyamide profiled cross section fiber (refer to Figure 2 The so-called circumscribed circle diameter D of the fiber cross section is the circumscribed circle diameter in the fiber cross section of the polyamide profiled cross section fiber ( Figure 1 (a) D).

[0044] By setting d / D to 0.030 or less, when water droplets come into contact with the fibers, it is difficult for the water droplets to enter the grooves, and the air taken in acts by pushing up the water droplets, so that the air layer can be maintained and the water repellent performance can be maintained. If d / D exceeds 0.030, water droplets easily invade the grooves, and the structural water repellent performance cannot be exerted. Preferably, d / D is 0.025 or less. More preferably, d / D is 0.022 or less.

[0045] The ratio of the groove depth H to the diameter D of the circumscribed circle of the fiber cross section (hereinafter referred to as H / D) is 0.10 or more and 0.30 or less. The groove depth H is the length from the circumscribed circle to the bottom surface of the groove in the fiber cross section of the polyamide profiled cross-section fiber ( Figure 1 (a) H).

[0046] By setting H / D to the prescribed range, even if the water droplets are subjected to their own weight or water pressure, the water droplets cannot reach the depth of the groove, so the water repellency can be maintained and the water repellency durability can be exerted. In addition, from the perspective of water drop intrusion, the larger the H / D, the better. When it is less than 0.10, the structural water repellency cannot be exerted due to the intrusion of water, and the water repellency durability is reduced. On the other hand, when H / D exceeds 0.30, the shape of the groove cannot be maintained due to deformation or destruction of the protrusion forming the groove when subjected to external force, and the water repellency durability is reduced. Preferably, H / D is greater than 0.12 and less than 0.28. It is further preferred that H / D is greater than 0.15 and less than 0.25.

[0047] The rigid amorphous content of the polyamide profiled cross-section fiber of the present invention is 35% to 55%. The rigid amorphous content is the amorphous content determined by the method described in Example 1, which is the amorphous content in which the molecular motion is frozen above the glass transition temperature (Tg) in the intermediate state between crystallization and movable amorphous, and becomes a fluid state at a temperature higher than Tg. (For example, refer to Shi Shimin, "DSC (3) - Glass Transition Behavior of Polymers -", ​​Journal of the Fiber Society, Vol. 65, No. 10 (2009))

[0048] By setting the rigid amorphous content to the specified range, practical durability against cracking or friction can be obtained, and a textile or woven fabric with excellent washing and dyeing fastness can be obtained. When the rigid amorphous content is less than 35%, the orientation of the polyamide is not fully advanced, the fiber strength is insufficient and it becomes easy to break, and the washing and dyeing fastness is poor. When the rigid amorphous content exceeds 55%, due to the insufficient crystallization of the entire fiber structure, the fiber strength is insufficient and it is easy to break, and the washing and dyeing fastness is poor. In addition, the orientation of the polyamide on the fiber surface is advanced, and the wear resistance is poor. Preferably, the rigid amorphous content is 38% to 52%.

[0049] In addition, according to the description in paragraph

[0149] of Patent Document 1, in the core-sheath composite fiber of nylon 6 and copolymerized polyethylene terephthalate (PET), since the elongation change rate before and after the dissolution of the sheath component is large, which is 1.48, it is considered difficult to apply stress to nylon 6, the orientation is not promoted, the rigid amorphous content becomes low and is less than 35%, and the washing and dyeing fastness is low.

[0050] The polyamide profiled cross-section fiber of the present invention can be obtained by dissolving and removing the sheath component from a composite yarn having a core-sheath type cross-section shape in which a polyamide polymer is arranged in a core portion and a thermoplastic polymer dissolved in alkali or hot water is arranged in a sheath portion in a high-order processing step. The cross-section shape of the core portion is the same as that of the polyamide profiled cross-section fiber of the present invention.

[0051] The sheath component of the core-sheath type composite yarn of the present invention includes a thermoplastic polymer soluble in alkali or hot water, and the core component includes a polyamide polymer.

[0052] The core component and the sheath component are preferably combined as the dissolution rate ratio relative to the solvent (alkali or hot water) is larger, and the dissolution rate ratio is preferably 10 times or more, and the polymer can be selected based on the range of 3000 times or less. More preferably, the dissolution rate ratio is 100 times or more, and further preferably 1000 times or more.

[0053] As the sheath component, for example, a polymer that can be melt-formed and is more easily soluble than the core component, such as polyethylene terephthalate and its copolymers, polylactic acid, copolymers of polyamide, polystyrene and its copolymers, polyethylene, polyvinyl alcohol, etc., is selected. In the composite spinning through the same die, the core component polyamide needs to have heat resistance under melt spinning conditions, and the sheath component is preferably polyethylene terephthalate and its copolymers or polylactic acid.

[0054] The cross-sectional shape of the core of the core-sheath composite yarn of the present invention is a special-shaped cross-section, and by forming a sharp cross-section, a high water-repellent performance can be exhibited. However, if it is a sharp cross-section, stress is easily concentrated, and it is easy to turn white for impact or friction. Therefore, the core component is selected from a polyamide with high wear resistance. The preferred core components are polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polyundecanamide (nylon 11), polypentamethylene adipamide (nylon 56), polypentamethylene sebacamide (nylon 510), and polyhexamethylene sebacamide (nylon 610).

[0055] In the fiber comprising the core-sheath composite yarn of the present invention, the elongation change (Ea / Eb) before and after the sheath is dissolved and removed is the fiber elongation Ea after the sheath is dissolved and removed / the fiber elongation Eb before the sheath is dissolved and removed ≤ 1.30. By setting Ea / Eb to the prescribed range, a textile or knitted fabric having excellent washing and color fastness is obtained. If Ea / Eb exceeds 1.30, the washing and color fastness is poor. Preferably, Ea / Eb is 1.10 or less.

[0056] In addition, in the fiber comprising the core-sheath composite yarn of the present invention, the strength change before and after the sheath is dissolved and removed (Sa / Sb) is the fiber strength Sa after the sheath is dissolved and removed / the fiber strength Sb before the sheath is dissolved and removed ≧0.95. By setting Sa / Sb to the specified range, a textile or knitted fabric with practical durability resistant to rupture or friction is obtained. When Sa / Sb is less than 0.95, the fiber strength is insufficient and becomes easy to rupture, and the practical durability is poor. The preferred Sa / Sb is 1.00 or more.

[0057] Next, an example of the method for producing the polyamide modified-cross-section fiber of the present invention will be described in detail.

[0058] The polyamide profiled cross-section fiber of the present invention can be obtained by manufacturing a core-sheath type composite yarn including a core component having a profiled cross-section of a polyamide polymer and a sheath component of a thermoplastic polymer soluble in alkali or hot water, and dissolving and removing the sheath component in an advanced processing step.

[0059] Hereinafter, a method for producing fibers including core-sheath type composite yarns and a method for eluting and removing the sheath component will be described.

[0060] Figure 3 This is a diagram showing one embodiment of a production apparatus preferably used in a method for producing fibers including core-sheath type composite yarns.

[0061] Here, as a method for spinning the fiber including the core-sheath type composite yarn of the present invention, composite spinning by melt spinning is suitable from the viewpoint of improving productivity. Fiber including the core-sheath type composite yarn can also be obtained by solution spinning or the like.

[0062] First, polyamide and easily soluble thermoplastic polymer are melted, metered and transported by a gear pump, and finally extruded from the ejection hole provided in the composite spinning die 1 to form each filament. Figure 3 As shown, in order to suppress the contamination of the die over time, the ejected filaments are cooled and solidified to room temperature by a gas supply device 2 for blowing steam and a cooling device 3. Thereafter, an oil agent is applied by an oil supply device 4, and each filament is bundled by a fluid nozzle device 5 to form a multifilament, which is stretched by a traction roller 6 and a stretching roller 7 and then wound by a winding device 8.

[0063] In the production of the polyamide modified-section fiber and the fiber including the core-sheath type composite yarn of the present invention, the melt viscosity of the polyamide resin chips used is preferably in the range of 300 poise to 2000 poise. The measurement method is described in the following Example 1.

[0064] The higher the melt viscosity of the polyamide resin chips as the core component, the more easily they are subjected to stress on the spinning line, and the more advanced the fiber structure formation of the polyamide is. By setting the predetermined range, the rigid amorphous amount, elongation change Ea / Eb, and strength change Sa / Sb can be obtained.

[0065] In addition, from the perspective of spinning properties, if the melt viscosity of the polyamide resin chips is below 1800 poise, the extrusion pressure of the molten polymer during spinning and its rising rate over time can be suppressed, which can reduce the excessive load on the production equipment or extend the die replacement cycle, thereby ensuring productivity, and is therefore more preferred.

[0066] In the production of the polyamide modified-section fiber and the fiber including the core-sheath composite yarn of the present invention, the melt viscosity of the easily soluble thermoplastic polymer resin chips used is preferably in the range of 300 poise to 1500 poise. The measurement method is described in the following Example 1.

[0067] The lower the melt viscosity of the easily soluble thermoplastic polymer resin chips as the sheath component, the less likely they are to be subjected to stress on the spinning line, and the more advanced the fiber structure formation of the core component polyamide is. By setting the predetermined range, the rigid amorphous amount, elongation change Ea / Eb, and strength change Sa / Sb can be obtained.

[0068] In the production of the polyamide profiled cross-section fiber and the fiber including the core-sheath type composite yarn of the present invention, it is important to control the orientation of each polymer component before stretching in order to achieve the desired rigid amorphous content. From the perspective of increasing the stress on the polyamide at the solidification point where stress begins to be applied to the ejected polymer after the composite spinning, or reducing the solidification point difference with the easily soluble thermoplastic polymer, the melting point difference between the core component and the sheath component is preferably 50° C. or less, although it depends on the composite ratio, ejection amount, and specific heat.

[0069] In the production of the polyamide profiled cross-section fiber and the fiber including the core-sheath type composite yarn of the present invention, the melting temperature is preferably melted in the range of a temperature 20°C higher than the melting point (Tm) of the polyamide and the easily soluble polymer (Tm) (Tm+20°C) or higher and a temperature 95°C higher than Tm (Tm+95°C) or lower. By setting it in the above-mentioned predetermined range, the melt viscosity is suitable for melt spinning, so stable spinning can be performed.

[0070] In the production of the polyamide profiled cross-section fiber and the fiber including the core-sheath type composite yarn of the present invention, the ratio of the core component to the sheath component when the core-sheath type composite yarn is spun can be selected in the range of 50 / 50 to 90 / 10 in terms of weight ratio based on the ejection amount. In the core-sheath ratio, if the core ratio is increased, it is suitable from the perspective of the productivity of the core-sheath type composite yarn. Among them, as a range that can be produced in a good balance while efficiently and stably maintaining the long-term stability of the core-sheath type cross-section and the profiled cross-section, the core-sheath ratio is more preferably 70 / 30 to 90 / 10.

[0071] In order to achieve the desired amount of rigid amorphous particles in the production of the polyamide profiled cross-section fiber of the present invention, it is important to control the orientation of the polyamide as the core before stretching when spinning the fiber including the core-sheath type composite yarn, that is, to optimize the spinning conditions of spinning draft and cooling.

[0072] The spinning draft of the spinning conditions is the ratio of the pulling roller speed to the ejection line speed (hereinafter referred to as the draft ratio), and is preferably controlled to be 75 to 300. The smaller the draft ratio, the more difficult it is to promote the orientation of the polyamide, and thus the rigid amorphous content is lower. On the other hand, the larger the draft ratio, the easier it is to promote the orientation of the polyamide, but from the perspective of the yarn forming property, the yarn breakage increases and the productivity is significantly reduced, so the draft ratio is preferably 300 or less. If the draft ratio is set to 75 or more, the orientation of the polyamide is promoted, the desired rigid amorphous content can be achieved, the orientation difference between the core component and the sheath component polymer can be suppressed, and the elongation change Ea / Eb and the strength change Sa / Sb can be reduced.

[0073] The cooling of the spinning conditions is preferably to increase the solidification point of the ejected polymer after the composite spinning, and it is preferable to cool efficiently. By increasing the solidification point, the orientation during spinning is promoted, the rigid amorphous is improved, and the difference in the solidification point of the polymers of the core component and the sheath component is reduced to reduce the orientation difference, thereby suppressing the elongation change Ea / Eb and the strength change Sa / Sb. In addition, by quickly solidifying the fiber cross section formed by the composite spinning die, the desired profile cross section can be obtained.

[0074] The ejected polymer entering the cooling zone is solidified as close to the upper end of the cooling zone as possible. Preferably, the vertical distance LS from the lower surface of the spinning die to the upper end of the cooling air blowing portion of the cooling device 3 (hereinafter referred to as the cooling start distance LS) is set to 30 mm to 120 mm.

[0075] By setting the cooling start distance LS to 120 mm or less, the solidification point is increased and the orientation during spinning is promoted, the rigid amorphous content is increased, and the solidification point difference between the core component and the sheath component polymer is reduced to reduce the orientation difference, thereby suppressing the elongation change Ea / Eb and the strength change Sa / Sb. In addition, by quickly solidifying the fiber cross section formed by the composite spinning die, the desired profile cross section can be obtained. When the cooling start distance LS is 30 mm or more, the orientation during spinning can be moderated, the oriented crystallization during extension can be promoted, and the strength can be obtained.

[0076] In addition, from the perspective of the Nusselt heat exchange cooling method, as an effective method to bring the solidification point closer to the upper end, it is preferred to increase the cooling air speed. The prescribed range also depends on the single fiber fineness, but it is preferably in the range of 30m / min to 50m / min at the lower end of the cooling area.

[0077] By setting the cooling air speed to 30 m / min or more, the heat exchange rate of the polymer becomes faster, and the solidification point is close to the upper end surface of the cooling area. Therefore, the difference in the solidification point of the polymer of the core component and the sheath component becomes smaller, and the desired rigid amorphous amount is obtained. On the other hand, from the perspective of workability, the cooling air speed is preferably 50 m / min or less.

[0078] In addition, as described above, the cooling air temperature in the cooling zone is also an important factor in heat exchange, and the cooling air temperature is preferably 20° C. or less. By setting the cooling air temperature to 20° C. or less, the heat exchange rate of the polymer becomes faster, and the solidification point is close to the upper end surface of the cooling zone, thereby increasing the rigid amorphous content.

[0079] The polyamide profiled cross-section fiber of the present invention is prepared into a woven or knitted fabric having the fiber containing the core-sheath type composite yarn in at least a portion, and a thermoplastic polymer dissolved in alkali or hot water as a sheath component is dissolved and removed using alkali or hot water, thereby obtaining a woven or knitted fabric having the polyamide profiled cross-section fiber in at least a portion.

[0080] The so-called dissolution and removal of the sheath component refers to dissolving and removing more than 99% of the sheath component using an alkali or hot water as a solvent. Examples of the alkali described herein include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, etc., and preferably a strong alkali (pH value = 10 to 14) such as sodium hydroxide and potassium hydroxide is used. In addition, the alkali concentration and temperature in the dissolution and removal can be set arbitrarily. For example, in the case of sodium hydroxide, it is preferably treated at 80°C to 100°C using a 1.0 wt% to 8.0 wt% aqueous solution.

[0081] Example

[0082] A. Melt Viscosity

[0083] For the resin chip sample, the hole diameter is 1.0 mm, the hole length is 10.00 mm, the melting temperature is 290°C, and the shear rate is 1216 sec. -1 The value measured by a capillary flow tester under the conditions of is set as melt viscosity (poise).

[0084] B. Rigid amorphous amount

[0085] The rigid amorphous content of the fiber sample was measured using a differential scanning calorimeter Q1000 manufactured by TA Instruments as a measuring device.

[0086] The difference (ΔHm-ΔHc) between the heat of fusion ΔHm and the heat of cold crystallization ΔHc obtained by differential scanning calorimetry (hereinafter referred to as DSC), the specific heat difference ΔCp obtained by temperature modulation DSC, and the theoretical value when the polyamide is 100% crystalline (completely crystalline) and the theoretical value when the polyamide is 100% amorphous (completely amorphous) are used.

[0087] Here, ΔHm0 is the heat of fusion of polyamide (completely crystalline), and ΔCp0 is the specific heat difference before and after the glass transition temperature (Tg) of polyamide (completely amorphous).

[0088] The crystallinity Xc and the movable amorphous amount Xma are determined based on the following formula. The rigid amorphous amount Xra is calculated from Xc and Xma.

[0089] The rigid amorphous content was calculated from the average value of these two measurements.

[0090] Xc(%)=(ΔHm-ΔHc) / ΔHm0×100

[0091] Xma(%)=ΔCp / ΔCp0×100

[0092] Xra(%)=100-(Xc+Xma).

[0093] C. Section shape

[0094] Perform any of the following treatments on the fiber sample.

[0095] ■ Make the fully aligned fiber sample pass through the hole with a diameter of about 0.3mm to 1.0mm opened on the copper plate, and use a razor to cut the front and back of the copper plate to make the fiber cross section;

[0096] or

[0097] ■Embed the fiber sample with an embedding agent such as epoxy resin, and slice it with a microtome to produce a fiber cross section.

[0098] The obtained fiber cross sections were observed using a transmission microscope at a magnification sufficient to observe one single fiber, and three fibers were randomly selected and photographed.

[0099] Based on each image captured, for all grooves in the same image, the curvature radius d of the two entrance corners of one groove was measured in μm using image processing software (WINROOF), and the average value (d1, d2, ... dn) was calculated. The d of one single yarn is the average value of d1, d2, ... dn rounded to the second decimal place.

[0100] Similarly, the groove depth H located in one groove and the circumscribed circle diameter D (H1, H2, ... Hn, D1, D2, ... Dn) of the monofilament (core component) are measured in μm. H and D of one monofilament are the average values ​​of the measured values ​​rounded off to the second decimal place.

[0101] For the images of the single-filament segments (3 pieces) extracted in the above operation, simple numerical averages of the respective values ​​(d, H, D) were repeatedly used to obtain the respective values ​​(d / D, H / D).

[0102] D.Total fineness

[0103] (a) Fibers comprising core-sheath composite yarns

[0104] For the fiber sample, a 1.125m / week gauge was rotated 200 times at a tension of 1 / 30cN×displayed dtex to make a ring-shaped skein, which was dried in a hot air dryer (105±2°C×60 minutes), and the mass of the skein was weighed on a balance, and the fineness was calculated by multiplying the value by the official moisture regain. In addition, the official moisture regain of nylon 6 is set to 4.5%.

[0105] (b) Polyamide profiled fiber

[0106] After removing more than 99% of the sheath component of the core-sheath composite yarn, the yarn was dried in a hot air dryer (105±2°C×60 minutes), and the mass of the skein was weighed on a balance. The fineness was calculated by multiplying the value by the official moisture regain. In addition, the official moisture regain of nylon 6 is set to 4.5%.

[0107] E. Strength and elongation

[0108] The tensile strength and elongation of the fiber samples were measured according to Japanese Industrial Standards (JIS) L1013 (2021), and the tensile strength-elongation curve was drawn.

[0109] The test conditions were as follows: the test machine was a constant speed extension type, the gripping interval was 50 cm, and the tensile speed was 50 cm / min. In addition, when the tensile strength at the time of cutting was less than the maximum strength, the maximum tensile strength and the elongation at that time were measured.

[0110] The elongation and strength are calculated using the following formula.

[0111] Elongation = elongation at break (%)

[0112] Strength = tensile strength at break (cN) / total fineness (dtex).

[0113] F. Elongation change Ea / Eb, strength change Sa / Sb

[0114] The fibers including the core-sheath type composite yarn collected under various spinning conditions in the examples and comparative examples were placed on a gauge at 1.125 m / period, rotated 10 times to remove the hank, and after removing 99% or more of the sheath component using an elution bath (bath ratio 100) filled with a solvent that dissolves the sheath component, the elongation and strength were measured as described in the above item E. The value obtained by dividing the strength Sa or elongation Ea after elution by the strength Sb or elongation Eb before elution was defined as the elongation change Ea / Eb and the strength change Sa / Sb.

[0115] Here, the sheath component was removed by immersing the film in a 6.0 wt % sodium hydroxide aqueous solution heated to 95° C. for 30 minutes.

[0116] G. Fabric Evaluation

[0117] (a) Water repellency

[0118] For the textile fabric produced by the same method as in Example 1, 10 pieces were cut out in a sample size of 20 cm × 20 cm to prepare fabric samples. For each sample, a circle with a diameter of 11.2 cm was drawn in the center, and the circle was expanded in a manner that the area was expanded by 80%, and the sample was mounted on a test piece holding frame used in the water repellency test (JIS L1092), and a spray test (JIS L1092 (2020) "Test method for water repellency of fiber products") was performed, and the grade was determined, and the average value of the grade determination results of the 10 samples was set as the water repellency performance.

[0119] S: Level 4 or above

[0120] A: Level 3 or above

[0121] B: Less than level 3

[0122] C: Level 2 or below

[0123] Level 3 and above are considered qualified.

[0124] (b) Washing durability of water-repellent finish

[0125] The textile fabric produced by the same method as in Example 1 was washed using the C4M method described in JIS L1930 (2014) "Test Methods for Home Laundering of Textile Products". Evaluation was performed with the number of washes being 0 and 50. In addition, the water repellency was evaluated according to the above-mentioned item G (a).

[0126] S: Level 4 or above

[0127] A: Level 3 or above

[0128] B: Less than level 3

[0129] C: Level 2 or below

[0130] In the grade determination of the washing frequency of 50 times, grades 3 and above were regarded as pass.

[0131] (c) Tear strength

[0132] For the woven fabric produced by the same method as in Example 1, the tear strength at three random locations in the transverse direction was measured in accordance with JIS L1096 (2020) “Textile and knitted fabrics test methods” (8.17A method), and the average value was measured.

[0133] S: 4.5N or more

[0134] A: 4.1N or more and less than 4.5N

[0135] B: 3.7N or more and less than 4.1N

[0136] C: less than 3.7N

[0137] Evaluation was performed in four stages, and S and A were considered pass.

[0138] (d) Wear resistance

[0139] Regarding the abrasion method, the appearance retention tester described in JIS L1076 (2012) "Test method for pilling of textiles and knitted fabrics" was used, and the bottom area of ​​the upper holder was set to about 13 square centimeters, the number of frictions was set to 90 rpm, and the pressing load was set to 7.36 N. The textile produced by the same method as in Example 1 was fixed on the upper holder and the lower friction plate and abraded for 10 minutes. After abrasion, the fibrillation of the single fiber of the textile placed on the upper holder was observed at 50 times using a microscope VHX-2000 manufactured by Keyence Corporation.

[0140] At this time, the surface changes of the textile before and after the abrasion treatment were confirmed, and the fibrillation condition was evaluated in three stages. The case where the entire textile surface was fibrillated before and after the treatment was set as "not possible" and set to "C", the case where fibrillation was confirmed in part was set as "good" and set to "B", and the case where fibrillation was not confirmed was set as "good" and set to "A".

[0141] (e) Washing fastness

[0142] The textile fabric produced by the same production method as in Example 1 was tested in accordance with JIS L0844 (2011) "Test method for color fastness to washing" A-1 method.

[0143] S: Level 4 or above

[0144] A: Level 3 or above

[0145] B: Less than level 3

[0146] C: Level 2 or below

[0147] Color discoloration of level 3 or above is considered acceptable.

[0148] [Example 1]

[0149] Nylon 6 (N6) chips having a melt viscosity of 1500 poise, a melting point of 225° C. and no titanium oxide as a core component were dried by a conventional method to a moisture content of 0.03% by mass or less.

[0150] Polyethylene terephthalate (PET) chips having a melt viscosity of 850 poise, a melting point of 260° C., and containing no titanium oxide as a thermoplastic polymer of the sheath component were dried by a conventional method to a moisture content of 0.015% by mass or less.

[0151] The obtained N6 chips and PET chips were melted at 290°C, respectively, with the core:sheath weight ratio being 80:20, and the composite spinning die (aperture 0.22 mm, 72 holes) was used to form a Figure 1 The material was ejected in the manner shown in the cross section of (b) (ejection amount: 44.4 g / min).

[0152] Spinning is used Figure 3 The spinning was carried out using a composite spinning machine of the form shown.

[0153] Each filament discharged from the composite spinning die 1 was passed through an annular cooling device 3 blowing cooling straightened air at a cooling start distance LS of 100 mm, a cooling air temperature of 18° C., and a cooling air speed of 35 m / min to cool and solidify the filaments to room temperature.

[0154] Then, oil is applied at the oil supply position Lg of 1000 mm from the lower surface of the spinning die, and the filaments are bundled to form multifilaments, and convergence is applied by the fluid nozzle device 5. Convergence is applied by spraying high-pressure air on the traveling filaments in the fluid nozzle device 5.

[0155] Thereafter, the fiber was stretched at a draft ratio of 100 and a stretching ratio of 2.2 between a take-up roll 6 and a stretching roll 7, and wound up by a winding device 8 to obtain a fiber including a core-sheath type composite yarn having 66 dtex and 36 filaments.

[0156] The obtained fibers including the core-sheath type composite yarn were used for warp yarns and weft yarns, and were woven with a warp density of 188 yarns / 2.54 cm and a weft density of 155 yarns / 2.54 cm in a plain weave.

[0157] The obtained raw fabric was dyed and water-repellent processed under the following conditions (a) to (g) to obtain a woven fabric having a warp density of 200 yarns / 2.54 cm and a weft density of 160 yarns / 2.54 cm.

[0158] (a) Refining: Noigen WS 5 ml / L, sodium hydroxide 5 g / L, bath ratio 1:50, 95°C × 60 minutes

[0159] (b) Intermediate setting: 180°C x 1 minute

[0160] (c) Dissolution and removal treatment (elution of sheath components): 6.0 wt% sodium hydroxide aqueous solution, 95°C x 30 minutes

[0161] (d) Dyeing: Acid dye (Nylosan Blue-GFL167% (Sandoz)) 1.0% owf, 98°C x 60 minutes

[0162] (e) Fixing treatment: synthetic tannin (Nylonfix 501 manufactured by Senka) 3 g / l, 80°C x 20 minutes

[0163] (f) Finishing setting: 200℃×1 minute

[0164] (g) Water-repellent processing: The target textile was immersed in a treatment solution of 5.0 wt% of Neoseed NR-158 (manufactured by Nikka Chemical Co., Ltd.), 0.3 wt% of Beckamine M-3 (manufactured by DIC Corporation), 0.3 wt% of Catalyst ACX (manufactured by DIC Corporation), 1 wt% of isopropyl alcohol, and 93.5 wt% of water, and the solution was squeezed out using a squeezer at a squeeze rate of 60%, and then dried at 130°C for 1 minute and cured at 170°C for 35 seconds to obtain a water-repellent processed fabric sample. In addition, when the fiber after dissolution is nylon, a fixation treatment was performed. The fixing treatment was carried out using 5% owf Nylonfix 501 (manufactured by Senka Co., Ltd.) under the reaction conditions of 80°C x 30 minutes and a bath ratio of fabric:water of 1:20.

[0165] Table 1 shows the results of evaluation of woven fabrics using the obtained polyamide modified-section fibers.

[0166] [Example 2] [Comparative Example 1] [Comparative Example 4]

[0167] The spinning conditions were changed as shown in Table 1, except that the draft ratio was changed and the rigid amorphous content was changed, and a fiber including a core-sheath type composite yarn of 66 dtex and 36 filaments was obtained by the same method as in Example 1 to obtain a woven fabric. The evaluation results are shown in Table 1.

[0168] [Table 1]

[0169] [Table 1]

[0170]

[0171] [Example 3] [Comparative Example 2]

[0172] A fiber including a core-sheath type composite yarn of 66 dtex and 36 filaments was obtained by the same method as in Example 1 except that the cooling air speed was changed as shown in Table 2 and the fiber properties including the rigid amorphous content were changed. A woven fabric was obtained. The evaluation results are shown in Table 2.

[0173] [Example 4] [Comparative Example 3]

[0174] A fiber including a core-sheath type composite yarn of 66 dtex and 36 filaments was obtained by the same method as in Example 1 except that the cooling start distance LS was changed as shown in Table 2 and the fiber properties including the rigid amorphous content were changed. A woven fabric was obtained. The evaluation results are shown in Table 2.

[0175] [Table 2]

[0176] [Table 2]

[0177]

[0178] [Example 5]

[0179] The thermoplastic polymer as the sheath component was changed to a copolymerized PET crumb (melt viscosity 750 poise, melting point 240° C.) obtained by copolymerizing 8.0 mol % of 5-sodium sulfoisophthalic acid and 10 wt % of polyethylene glycol having a molecular weight of 1000. A fiber including a core-sheath type composite yarn of 66 dtex and 36 filaments was obtained by the same method as in Example 1 to obtain a woven fabric. The evaluation results are shown in Table 3.

[0180] [Example 6] [Example 7]

[0181] The core component polyamide polymer was changed to N66 chips (melt viscosity 550 poise, melting point 265°C) and N610 chips (melt viscosity 570 poise, melting point 225°C) as shown in Table 3, the ejection amount was changed to 48.4 g / min, and the stretching ratio was changed to 2.4 times. A fiber containing a core-sheath type composite yarn of 66 dtex and 36 filaments was obtained by the same method as in Example 1 to obtain a woven fabric. The evaluation results are shown in Table 3.

[0182] [Comparative Example 5]

[0183] The polyamide polymer as the core component was N6 crumbs having a melt viscosity of 1200 poise, a melting point of 225°C, and no titanium oxide. The thermoplastic polymer as the sheath component was copolymerized PET crumbs (melt viscosity of 450 poise, melting point of 240°C) obtained by copolymerizing 8.0 mol% of 5-sodium sulfoisophthalic acid and 10 wt% of polyethylene glycol having a molecular weight of 1000. The crumbs were melted at 270°C, the core:sheath weight ratio being 8:2, and the composite spinning die (aperture 0.3 mm, 24 holes) was formed. Figure 1 The fiber was ejected in the manner of the cross section of (b) (ejection amount 29.4 g / min). The melt-ejected filaments were cooled and solidified, and then an oil agent was applied, and the filaments were wound at a spinning speed of 1200 m / min to obtain undrawn fibers. Furthermore, the undrawn fibers were stretched 2.92 times between rollers heated to 90°C and 130°C (stretching speed 800 m / min), and 84 dtex, 24 filaments of core-sheath composite fibers were obtained to obtain textiles. The evaluation results are shown in Table 3.

[0184] [Table 3]

[0185] [Table 3]

[0186]

[0187] Explanation of symbols

[0188] 1: Composite spinning die

[0189] 2: Gas supply device

[0190] 3: Cooling device

[0191] 4: Oil supply device

[0192] 5: Fluid nozzle device

[0193] 6: Traction roller

[0194] 7: Extension roller

[0195] 8: Coiler

[0196] LS: Cooling start distance

[0197] Lg: Oil supply position

[0198] d: The radius of curvature of the groove entrance corner

[0199] D: Circumscribed circle diameter of the fiber cross section

[0200] H: Groove depth

Claims

1. A polyamide profiled cross-section fiber, wherein a plurality of grooves are present on the outer periphery of the fiber cross section of a single fiber, and The curvature radius d of the inlet corner of the groove, the groove depth H and the circumscribed circle diameter D of the fiber cross section satisfy the following equations (1) and (2), and The rigid amorphous content is 35% or more and 55% or less. d / D≦0.030…Formula (1) 0.10≦(H / D)≦0.30…Formula (2) 2. A fiber comprising a core-sheath type composite yarn, having a core-sheath type cross-sectional shape in which a thermoplastic polymer soluble in alkali or hot water is arranged in the sheath portion and a polyamide polymer is arranged in the core portion, The cross-sectional shape of the core is a special cross-sectional shape having a plurality of grooves, and the curvature radius d of the entrance corner of the groove, the groove depth H and the circumscribed circle diameter D of the cross-sectional shape of the core satisfy the following equations (1) and (2): d / D≦0.030…Formula (1) 0.10≦(H / D)≦0.30…Formula (2) The elongation and strength before and after the sheath is dissolved and removed satisfy the following equations (3) and (4). Fiber elongation Ea after sheath dissolution and removal / Fiber elongation Eb before sheath dissolution and removal ≦ 1.30…Formula (3) Fiber strength Sa after dissolution and removal of the sheath / fiber strength Sb before dissolution and removal of the sheath≧0.95…Formula (4).

Citation Information

Patent Citations

  • Specific cross section yarn

    JP2003129327A

  • Sheath-core composite fiber

    JP2019026944A

  • Core-sheath conjugated fiber, slit fiber, and method for manufacturing these fibers

    WO2016129467A1